Apparatus for controlling thickness variations in layers of material formed using physical vapor deposition - Patents.com

A rotating magnetic field assembly during pulsed DC physical vapor deposition addresses film thickness uniformity issues in BAW devices by reducing short-range ripples, ensuring precise control and improved yield through efficient ion beam trimming.

JP7575866B2Active Publication Date: 2024-10-30SPTS TECH LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019169176
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-18
Filing Date
2019-09-18
Publication Date
2024-10-30
Estimated Expiration
2039-09-18

AI Technical Summary

Technical Problem

Existing methods for controlling film thickness uniformity in bulk acoustic wave (BAW) devices during physical vapor deposition fail to achieve the required accuracy and uniformity, leading to frequency deviations and yield loss due to short-range thickness variations (SRTV), which are difficult to correct with current ion beam trimming techniques.

Method used

A magnet assembly with a rotating magnetic field generating arrangement is used to guide ions during pulsed DC physical vapor deposition, creating a varying magnetic field strength along the radial direction to improve thickness and stress uniformity, allowing for more effective ion beam trimming.

Benefits of technology

The solution significantly reduces short-range ripples in film thickness variations, enabling precise control within ±0.1% and achieving superior within-wafer stress uniformity, facilitating faster and cost-effective trimming processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575866000001
    Figure 0007575866000001
  • Figure 0007575866000002
    Figure 0007575866000002
  • Figure 0007575866000003
    Figure 0007575866000003
Patent Text Reader

Abstract

To provide a magnet assembly for controlling ions used for forming a material layer on a substrate during a pulse DC physical vapor deposition process.SOLUTION: The device and method for incorporating a magnet assembly are provided in order to control the thickness variation of a material layer formed by pulse DC physical vapor deposition. The magnet assembly includes a magnetic field formation arrangement forming a magnetic field in the vicinity of a substrate and means for rotating the magnetic field formation arrangement inducing ions around a rotational axis to the substrate. The magnetic field formation arrangement includes a plurality of magnets constituted for an array extended around the rotational axis, and the array of the magnets is constituted so as to form variation magnetic field intensity in the radial direction to the rotation axis.SELECTED DRAWING: Figure 9
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an apparatus and method for controlling thickness variations in a material layer formed by pulsed DC physical vapor deposition. [Background technology]

[0002] Bulk Acoustic Wave (BAW) devices are used in mobile phones and other wireless devices to enable reception and / or transmission of certain radio frequencies. These devices utilize the piezoelectric effect to generate a mechanical resonance from an electrical input, and conversely, can use the mechanical resonance to generate an electrical output.

[0003] BAW devices typically comprise multiple layers of materials that are deposited and patterned on a silicon (Si) substrate using standard semiconductor thin-film processing techniques. Physical vapor deposition (PVD) is commonly used to deposit both the top and bottom metal electrodes and the piezoelectric dielectric layer (e.g., AlN or AlScN).

[0004] Factors that determine the performance of the fabricated devices include the electrical, mechanical, physical and acoustic properties of the piezoelectric material. In a manufacturing environment, the process is usually controlled by monitoring the film thickness and film stress. Very precisely controlled film thickness, excellent thickness uniformity and good within wafer stress uniformity result in high yields of functional devices and good bonding rates per wafer, typically defined as the mechanical energy stored in the device in response to an electrical input or vice versa.

[0005] One of the main causes of yield loss during BAW fabrication is frequency shift. The operating frequency of the BAW filter is determined by the thickness of the piezoelectric layer, since this determines the resonant frequency. Assuming a constant sound speed and density, the thickness accuracy and uniformity of the piezoelectric layer is required to be on the order of 0.1%. However, this degree of within-wafer uniformity cannot be achieved during the deposition process, and as a result, it is common in the industry to correct the film thickness after deposition by selectively trimming areas of the wafer with a localized etching step. Typically, an ion beam, which produces a constant etch rate, is scanned along the surface of the wafer at a controlled speed to ensure that the ion beam removes a precise amount of material at each location.

[0006] The full width at half maximum (FWHM) of the ion beam is typically a few centimeters, and the scan pattern typically has line-to-line distances in the millimeter range. The ion beam diameter is small enough to compensate for thickness gradients that typically occur over several centimeters. The local removal rate is controlled by the dwell time of the ion beam at a given location on the wafer, and the required velocity profile or scan speed of the beam across the wafer is calculated from a thickness map of the deposited film. Summary of the Invention [Problem to be solved by the invention]

[0007] The trimming process can be difficult when local short range thickness variations (SRTV) are present. The need to use a narrow beam and the acceleration required to meet the required velocity profile can make trimming difficult. The scan speed limitation can be circumvented by slowing down the ion beam etching rate, but this impacts system throughput and increases device cost.

[0008] A magnetic field can be used at the wafer surface during deposition to control the sputtered film stress. Such a magnetic field can be generated using an array of continuously rotating permanent magnets integrated into the platen that supports the wafer during the deposition process.

[0009] An example of a magnetic array used to control intra-wafer stress during deposition of AlN and AlScN piezoelectric layers is shown in Figure 1. Figure 1 shows a helical array of button magnets 1, for which the modeled magnetic field components of a continuously rotated array are shown in Figure 2. The magnetic array is shown to provide uniform stress within the wafer and uniform film thickness across the wafer for films deposited using standard techniques. However, even though the overall thickness uniformity of the deposited films is small, typically <2% full range, there are short range thickness variations corresponding to short range ripples in the average magnetic field components as shown in Figure 2.

[0010] Referring to FIG. 3, a plot of the deposited film thickness (Å) across the diameter of a 200 mm wafer is shown. The plot shows that the helical array (shown in FIG. 1) produces a variation in the deposited layer thickness of about 150 Å for the nominal 10,000 Å deposition thickness of ALScN. FIG. 4 provides a close-up view of the film thickness variation over a distance of 3 mm, and referring to FIG. 4, it is clear that the SRTV is about 75 Å. To achieve acceptable device performance, the thickness of the piezoelectric layer needs to be controlled within ±0.1% (i.e., ±10 Å for a 10,000 Å film).

[0011] We have now devised a magnetic field assembly, apparatus and method that addresses at least some of the problems discussed above. [Means for solving the problem]

[0012] According to the present invention, as can be seen from a first aspect, there is provided a magnet assembly for steering ions used to form a layer of material on a substrate during a pulsed DC physical vapor deposition process, comprising a magnetic field generating arrangement for generating a magnetic field in the vicinity of the substrate, and means for rotating the magnetic field generating arrangement for steering the ions about an axis of rotation relative to the substrate, the magnetic field generating arrangement comprising a plurality of magnets arranged in an array extending about the axis of rotation, the array of magnets configured to generate a varying magnetic field strength along a radial direction relative to the axis of rotation.

[0013] In one embodiment, the array comprises two linear subarrays extending along a radial direction relative to the axis of rotation, the two subarrays being angularly spaced about the axis of rotation by approximately 180°.

[0014] In another embodiment, the array comprises at least three linear subarrays extending along a radial direction relative to the axis of rotation, the at least three subarrays being angularly spaced about the axis of rotation. The at least three subarrays may be angularly spaced about the axis of rotation by substantially the same angle.

[0015] In one embodiment, the array comprises a plurality of linear subarrays arranged in a side-by-side configuration. In an alternative embodiment, the array comprises a helical array about the axis of rotation. In yet another alternative, the array comprises a plurality of concentric substantially circular subarrays about the axis of rotation.

[0016] In one embodiment, at least two magnets of the array are arranged in a stacked configuration, for example the array comprises a first row of magnets and a second row of magnets disposed above the first row.

[0017] In one embodiment, the plurality of magnets are disposed within a cassette, which may be generally disk-shaped and includes at least one recess adapted to receive the plurality of magnets.

[0018] In one embodiment, the magnets in the well are configured into a first array and a second array, the second array being disposed above the first array.

[0019] In one embodiment, the at least one recess comprises a first recess and a second recess extending along a radial direction relative to the axis of rotation, the two recesses being angularly spaced apart about the axis of rotation by approximately 180°. Alternatively, the cassette comprises at least three recesses extending along a radial direction relative to the axis of rotation, the at least three recesses being angularly spaced apart about the axis of rotation. In one embodiment, the at least three recesses are angularly spaced apart about the axis of rotation by approximately the same angle.

[0020] In another embodiment, the array comprises a plurality of linear depressions arranged in a side-by-side configuration, the plurality of linear depressions extending generally parallel to a diameter of the cassette. The linear depressions may extend around a periphery of the cassette.

[0021] In one embodiment, the depression comprises a helical depression about the axis of rotation, hi an alternative embodiment, the depression comprises a plurality of concentric substantially circular depressions about the axis of rotation.

[0022] In one embodiment, the magnet assembly further comprises at least one spacer for spacing the magnets within the recesses.

[0023] In one embodiment, the means for rotating the magnetic field comprises a spindle and a drive assembly for driving the spindle, the spindle being rotatably coupled at one end to the cassette and at the other end to the drive assembly.

[0024] In one embodiment, the north-south axes of the magnets in the array extend substantially parallel to one another, and preferably the north-south axes extend substantially perpendicular to the substrate, in use.

[0025] In one embodiment, the layer of material formed over the substrate comprises a piezoelectric layer, such as a layer formed from AlN or AlScN.

[0026] According to the present invention, as can be seen from a second aspect, there is provided an apparatus for controlling thickness variation of a material layer formed by pulsed DC physical vapour deposition comprising a chamber housing a target on which the material layer is formed and a substrate on which the material layer can be formed, the chamber having an inlet for introducing a gas into the chamber, a plasma generating arrangement for generating a plasma in the chamber, and a power supply for applying an RF bias voltage to the substrate, the apparatus further comprising a magnetic field generating arrangement for localising the plasma configured in use to generate a magnetic field for localising the plasma in the vicinity of the target to localise the plasma adjacent to the target, and a magnet assembly according to the first aspect.

[0027] In one embodiment, the magnetic field is not substantially adversely affected by the magnetic field that localizes the plasma.

[0028] In one embodiment, the magnetic field generating arrangement is positioned on a side of the substrate opposite the side of the substrate that faces the plasma.

[0029] According to the present invention, as can be seen from a third aspect, there is provided a method of controlling thickness variation in a layer of material formed by pulsed DC physical vapor deposition, comprising the steps of: Providing a chamber containing a target on which a layer of material is to be formed and a substrate on which a layer of material can be formed; placing a substrate on a magnet assembly according to a first aspect; introducing a gas into the chamber; generating a plasma in a chamber; applying a magnetic field to localize the plasma adjacent the target to substantially localize the plasma adjacent the target; applying an RF bias voltage to the substrate; applying a magnetic field from a magnet assembly proximate the substrate to selected regions of a material layer formed on the substrate for directing gas ions from the plasma to improve thickness uniformity of the material layer compared to when no magnetic field is present; rotating a magnetic field of a magnet assembly about an axis of rotation relative to the substrate; The present invention provides a method comprising:

[0030] In one embodiment, the radially varying magnetic field strength is greater near the periphery of the substrate than at the center of the substrate.

[0031] In one embodiment, the method further comprises rotating a magnetic field relative to the substrate while forming the layer of material.

[0032] In one embodiment, the method further comprises rotating the magnetic field about an axis extending substantially perpendicular to the substrate, for example by rotating the magnet assembly.

[0033] In one embodiment, the method further comprises a plurality of separate steps of forming a layer of material, the substrate being rotated relative to the magnet assembly before the start of each deposition step.

[0034] Although the invention has been described above, the invention extends to any inventive combination of the features set out above or hereinafter described. Illustrative embodiments of the invention will now be described in detail with reference to the accompanying drawings, but it should be understood that the invention is not limited to these precise embodiments.

[0035] Furthermore, even if other features and embodiments do not refer to a particular feature, it is contemplated that a particular feature described individually or as part of an embodiment may be combined with other individually described features or parts of other embodiments, and thus the invention extends to specific combinations not described above.

[0036] The invention may be carried out in various ways and, by way of example only, embodiments of the invention will now be described with reference to the accompanying drawings, in which: [Brief description of the drawings]

[0037] [Figure 1] 2 is a schematic diagram of a spiral array of button magnets that does not form part of the present invention. [Diagram 2] 2 is a graphical representation of magnetic field components generated during rotation of the array shown in FIG. 1. [Diagram 3] 1 is a graphical representation of the thickness profile of an AlScN piezoelectric layer achieved across the diameter of a 200 mm wafer by using a "spiral" type array of magnets. [Figure 4] 4 is a graphical representation of the thickness profile of the AlScN piezoelectric layer shown in FIG. 3 across a 3 mm area of ​​the wafer. [Diagram 5] 1 is a schematic diagram of a magnet assembly according to one embodiment of the present invention having a linear array of magnets. [Figure 6] 6 is a graphical representation of magnetic field components generated during rotation of the array shown in FIG. 5. [Figure 7] 1 is a schematic diagram of a magnet assembly according to one embodiment of the present invention comprising an array of magnets arranged in a parallel array of linear rows. [Figure 8] 2 is a schematic diagram of a magnet assembly according to one embodiment of the present invention comprising an array of magnets arranged into a plurality of angularly spaced, radially extending rows. [Figure 9] 6 is a schematic diagram of the magnet assembly shown in FIG. 5 with a magnet stack configuration. [Figure 10] FIG. 10 is a plan view of a first layer of stacked magnets in the array of FIG. [Figure 11] FIG. 10 is a plan view of a second layer of stacked magnets in the array of FIG. [Figure 12] 10 is a graphical representation of the thickness profile of an AlScN piezoelectric layer achieved using the magnet assembly shown in FIG. [Figure 13] 13 is a graphical representation of the thickness profile of the AlScN piezoelectric layer shown in FIG. 12 over a 20 mm span of the layer. [Figure 14] 10 is a graphical representation of the stress profile of an ALScN layer deposited using the magnet assembly shown in FIG. [Figure 15] 1 is a schematic diagram of an apparatus according to one embodiment of the present invention. [Figure 16] 3 is a flow chart illustrating method steps according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS It has been discovered that embodiments of the present invention allow for a significant reduction in short range ripple in the average ion steering magnetic field component while providing a time averaged ion steering magnetic field component that is strong enough to provide superior in-wafer stress control.

[0039] Referring to Figure 5, there is shown a magnet assembly 100 according to an embodiment of the invention used to control the thickness variation of a material layer, e.g. an ALScN piezoelectric layer, deposited on a substrate 230 (see Figure 15) using a physical vapor deposition (PVD) process, e.g. pulsed DC PVD. The assembly 100 comprises a magnetic field generating arrangement 110 which generates a magnetic field in the vicinity of the substrate 230 during use. The magnetic field generating arrangement 110 comprises a plurality of magnets 111 arranged into an array 110 arranged around an axis of rotation 101 (out of page in Figure 9; see also Figure 15) of the assembly 100 relative to the substrate 230, such that during use the magnetic field varies along a radius 102 between the axis of rotation 101 and a periphery 103 of the arrangement 110.

[0040] The plurality of magnets 111 are disposed within a cassette 104, which is generally disc-shaped and includes at least one recess 105 adapted to receive the plurality of magnets 111 of the array 110. In a first embodiment, as shown in FIG. 5, the cassette 104 includes a single recess 105 having a first recess and a second recess extending along a diameter of the cassette 104, the recess being disposed on either side of a central portion of the cassette 104. In a second embodiment, as shown in FIG. 7, the cassette 104 includes a plurality of side-by-side recesses 105 extending parallel to the diameter of the cassette (FIG. 7). In this embodiment, the recesses extend along the cord of the cassette, with each recess extending around the periphery of the cassette 104.

[0041] In a third embodiment, as shown in Figure 8, a cassette 104 may include a plurality of radially extending recesses 105 angularly spaced about the periphery of the cassette. The angular spacing may be uniform, or the angular spacing may be adjusted to direct ions to suit a particular deposition process.

[0042] In the embodiment shown in Figures 5, 7 and 8, the magnets 111 may have a cube and / or rod shape and are movably insertable inside the recesses 105 so that a particular row of magnets 111 can be formed along each of the recesses to generate a desired variation in magnetic field strength along a radial direction relative to the axis of rotation 101. The magnets 111 used typically have a magnetic field strength on the order of millitesla (mT) and the magnetic field profile generated along the radius of the cassette 104 may be tailored by appropriately positioning the magnets 111. For example, magnets 111 having different magnetic field strengths may be appropriately positioned and separated from each other using non-magnetic spacers 106 if desired.

[0043] The assembly 100 further comprises means 120 (see FIG. 15) for rotating the magnetic field generating arrangement 110 about the axis of rotation 101 relative to the substrate 230. The means 120 for rotating the magnetic field may comprise a spindle (not shown) rotatably coupled at one end to the cassette 104 and at the other end to a drive assembly (not shown).

[0044] The magnets 111 arranged in each of the recesses 105 may have different magnetic field strengths to generate a variation in the magnetic field profile along the radial direction. However, it is envisaged that this variation may be achieved by using magnets 111 with the same magnetic field strength but arranged at different heights relative to the surface of the cassette 104 using spacers 106, which effectively space the magnets 111 from the substrate 230 and adjust the magnetic field strength sensed by the substrate at the radial position. It is further envisaged that the depth may be such that two or more magnets 111 can be stacked (without extending above the surface of the cassette 104). In this regard, it is envisaged that each of the recesses 105 may comprise two or more rows of a sequence of magnets 111 and spacers 106, the rows being arranged one above the other. Thus, different radial positions of the substrate 230 may sense a magnetic field due to two stacked magnets arranged below the recess or near the surface of the cassette, or may sense very little magnetic field due to the stacked arrangement of the spacers 106 at the radial positions. Different options for configuring the magnets 111 and spacers 106 within each of the recesses 105 facilitate the generation of a number of the illustrated radial magnetic field profiles that guide the ions.

[0045] For example, referring to Figures 9-11 showing the assembly of the first embodiment, the plurality of magnets 111 may comprise a first row or layer 111a of magnets 111 and spacers arranged in a recess 105 extending along the diameter of the cassette 104, and a second row or layer 111b of magnets 111 and spacers 106 extending above the first row within the same recess 105. Referring to Figure 9, it is clear that the magnetic field strength at the ends of the recesses 105a,b, i.e., at the periphery of the cassette 104, is greater than in the center of the stacked arrangement of the two magnets 111 at each end 105a,b. The north-south axes of the magnets 111 of the array 110 may extend approximately parallel to each other so as to be approximately perpendicular to the substrate 230 during use. The time-averaged magnetic field achieved using embodiments of the present invention is strong enough at all points to control the within-wafer stress uniformity to typically ±50 MPa.

[0046] A typical stress profile for an aluminum nitride or scandium aluminum nitride piezoelectric layer has a significantly greater elongation in the center than at the edges. The invention described herein creates a very uniform stress profile in the deposited film by generating a strong ion-inducing magnetic field at the area where the film or material layer is most stressed, i.e., the edge of the wafer, where the strongest magnetic field is required.

[0047] It is important to minimize the interaction between the magnetic fields of adjacent magnets 111 so that the time-averaged magnetic field produces smooth variations as it rotates. Thickness and stress profiles of AlScN films deposited using an ion-guiding assembly according to an embodiment of the invention having multiple magnets arranged in a linear array (as shown in Figs. 9-11) are shown in Figs. 12-14. The graphs in Figs. 12 and 13 show that the easily varying magnetic field of the array produces a significantly smaller percentage change in thickness than that shown in Figs. 3 and 4, and Fig. 13 is the thickness range over the 20 mm section of Fig. 12. In Fig. 13, the thickness of the piezoelectric layer is controlled to within ±0.1% (i.e., ±10 Å for 10,000 Å) by a 3 mm scan. The SRTV is significantly reduced compared to the results shown in Fig. 4, making it much easier to correct the film thickness by ion beam trimming if necessary.

[0048] Figure 14 shows the stress profile (MPa) at the center of a wafer with an AlScN layer deposited using the assembly shown in Figure 9. The stress variation within the wafer is ±50 MPa, which is comparable to existing designs. The rate of change in wafer thickness is significantly smaller than that which can be achieved using existing techniques.

[0049] 15, there is shown a simplified diagram of an apparatus 200 according to one embodiment of the invention for controlling thickness variation of a material layer formed by pulsed DC physical vapor deposition. The apparatus 200 comprises a grounded process chamber 210 in which a physical vapor deposition process takes place. The chamber 210 is adapted to accommodate a target 220, such as aluminum or scandium aluminum nitride, from which a material layer is sputtered, and a platen 240 that supports a substrate 230, such as a silicon wafer. The chamber 210 has an inlet 250 for introducing gases, e.g., noble gases such as krypton, neon or argon, and reactive gases such as nitrogen, into the chamber to form a nitride film.

[0050] The apparatus 200 further comprises a magnet assembly 100 which can be positioned within a recess 241 in the platen 240. The platen 240 is positioned within the chamber 210 and oriented such that the wafer 230 can be positioned generally parallel to the target 220 on the platen surface 242 and the wafer axis 101 passing through the center of the wafer generally perpendicular to the wafer is generally aligned with the target axis extending generally perpendicular to the face of the target 220. However, in alternative embodiments, it is envisioned that the platen 240 and wafer 230 may be tilted relative to the target 220 and that the wafer axis 101 may not be aligned with the target axis. The apparatus 200 further comprises a plasma generating arrangement 260 for generating a plasma within the chamber 210 and a power supply 270 for applying an RF bias voltage to the substrate 230 via the platen 240. Typically, the platen 240 is driven at a conventional 13.56 MHz, although the invention is not so limited.

[0051] The plasma may be generated by applying pulsed (direct current) DC power from a DC power supply 262 between the target 220 and an anode ring disposed within the chamber 210. The operation of the power supplies 261, 270 is controlled by a controller 280 having a suitable graphical user interface (not shown). A magnetic field generating arrangement for localizing the plasma, such as a magnetron 262, is configured to generate a magnetic field in use for localizing the plasma in the vicinity of the target 220 to localize the plasma proximate to the target 220. The magnetron 263 is disposed outside the chamber 210 on the side of the target 220 opposite the side facing the substrate 230 and is arranged to rotate about an axis extending generally transverse to the target 220. The magnet assembly 100 is disposed on the side of the substrate opposite the side facing the target 220, the magnet assembly 100 extending over several centimeters above the substrate. There is no significant interaction between the magnetic field from the magnetron 290 proximate to the target 220 and the magnetic field from the magnet assembly 100 behind the substrate 230. The strength of the magnetic field that localizes the plasma is typically reduced to background levels near the substrate 230, so that ions drifting near the substrate will likely begin to be influenced, if not alone, by the magnetic field from the magnet assembly 100.

[0052] 16, a flow chart is shown outlining the steps involved in a method 300 of controlling thickness variation of a material layer formed by pulsed DC physical vapor deposition in accordance with one embodiment of the present invention. When it is desired to form a material layer, such as an aluminum nitride or scandium aluminum nitride layer, on a substrate 230, such as a silicon wafer, in step 301, the magnet assembly 100 including the cassette 104 and magnet array 110 is placed in a platen, and in step 302, the wafer 230 is placed on the platen above the array 110. In step 303, the aluminum target 220 is placed in the chamber 210, and in step 304, a gas (not shown), which may include nitrogen, argon, or a nitrogen / argon mixture, is introduced into the chamber 210 via the inlet 250.

[0053] The method 300 further comprises, in step 305, adjusting the magnetic field by manipulating the magnets 111 and the spacers 106 to adjust the radial magnetic field profile. The method further comprises, in step 306, rotating the cassette 104 to generate a non-uniform ion control magnetic field (B) across the surface of the wafer 230. In particular, the radially varying magnetic field may be stronger near the periphery of the substrate than at the center. The step 306 of rotating the magnetic field that guides ions relative to the substrate may be performed as the material layer is formed, and is performed about an axis that extends generally perpendicular to the substrate 230. The method 300 further comprises a number of separate steps of forming the material layer, with the substrate 230 being rotated relative to the ion control assembly 100 before beginning each deposition step.

[0054] Magnet 263 generates a magnetic field in the vicinity of target 220 to localize the plasma and gas ions around target 220. Such localization promotes interaction of the gas ions within target 220, thus promoting the liberation of aluminum atoms.

[0055] In step 307, an RF bias is applied to the wafer 230 by an RF power supply. Such an electrical bias results in an electric field oriented approximately perpendicular to the wafer surface and positive gas ions (during one half cycle of the RF voltage waveform) that begin to be attracted to the wafer 230. The ions impinge on the surface of the wafer 230, thus compressing the deposited layer of aluminum atoms, resulting in a more compressed layer. The density of ions impinging on the wafer 230 varies across the wafer 230 due to ion fluctuations created in the plasma. The plasma profile depends on the magnetic field from the magnetron, and regions of high magnetic field create concentrated regions of plasma and therefore concentrated regions of gas ions. It can be seen that magnetrons used in physical vapor deposition processes create regions of high ion density near the peripheral region of the target 230, resulting in more liberation (i.e., disintegration) of target material from the peripheral region than the central region. Furthermore, this increased ion density results in a greater concentrated bombardment of ions on the wafer 230 around the peripheral region than the central region.

[0056] However, the interaction of the RF bias voltage and the ion control magnetic field of the array 110 creates a force on the moving gas ions, the Lorentz force. The force depends on the cross product of the electric field created by the RF bias and the ion control magnetic field from the array 110. This force therefore acts to redirect or direct the ions preferentially to areas of the wafer 230, resulting in an increased ion density in those areas of the layer.

[0057] Embodiments of the present invention enable the fabrication of piezoelectric layers with thickness profiles that improve manufacturing costs and device performance. Furthermore, ion beam thickness trimming can be performed with wide ion beams, wide line spacings and small scan acceleration / deceleration rates, resulting in a fast and low cost trimming process.

Claims

1. a magnet assembly within a platen supporting a substrate for directing ions used to form a material layer on the substrate during a pulsed DC physical vapor deposition process, the magnet assembly being configured to be disposed within a recess in the platen; a magnetic field generating arrangement for generating a magnetic field adjacent and beneath the substrate; means for rotating the magnetic field generating arrangement about an axis of rotation relative to the substrate; the magnetic field generating arrangement comprises a plurality of magnets arranged in an array extending around the axis of rotation, the array of magnets being configured to generate a varying magnetic field strength along a radial direction relative to the axis of rotation; the array comprises a plurality of linear subarrays arranged in a parallel and stacked configuration; a cassette, the magnets being disposed within the cassette with a plurality of recesses adapted to receive the linear sub-arrays, the recesses being defined on an outer surface of the cassette, the substrate being disposed on a top portion of the cassette, the linear sub-arrays extending parallel to a diameter of the cassette, the magnets within the recesses being configured in a stacked configuration, the stacked array of magnets being configured such that the varying magnetic field strength is stronger near a periphery of the recesses within the cassette than at a center of the cassette, at least one of the recesses having first and second recess portions on either side of a center of the cassette, at least two of the recesses extending from one edge of a periphery to the other edge of the periphery, and all of the recesses being parallel to one another; at least one non-magnetic spacer for spacing the magnets in at least one of the recesses; A magnet assembly comprising:

2. A magnet assembly as described in claim 1, wherein the means for rotating the magnetic field comprises a spindle and a drive assembly driving the spindle, the spindle being rotatably coupled to the cassette at one end and to the drive assembly at the other end.

3. 1. An apparatus for controlling thickness variation of a material layer formed by pulsed DC physical vapor deposition, comprising: a chamber housing a target on which the layer of material is formed and a substrate on which the layer of material can be formed, the chamber having an inlet for introducing a gas into the chamber; a plasma generating arrangement for generating a plasma within the chamber; a power source for applying an RF bias voltage to the substrate; Equipped with a plasma-localizing magnetic field generating device configured to generate, during use, a plasma-localizing magnetic field proximate to the target to localize the plasma proximate to the target; Placement and A magnet assembly according to claim 1; The apparatus further comprises:

4. The apparatus described in claim 3, wherein the magnetic field is substantially unaffected by a magnetic field that localizes the plasma.

5. The apparatus of claim 3, wherein the magnetic field generating arrangement is positioned on a side of the substrate opposite the side of the substrate facing the plasma.

6. A magnet assembly as described in claim 1, wherein the linear subarrays are spaced apart from each other by portions of the cassette.

Citation Information

Patent Citations

  • Plane discharge electrode

    JP1986291971A

  • Method and device for sputtering

    JP1989279752A

  • Sputtering device

    JP1992131651U

  • Magnetron unit for sputtering apparatus and sputtering apparatus

    JP1997118980A

  • Method and device for improving coverage of side wall and bottom face in imp treatment by using magnetic field

    JP2001140071A