Coating material and method for inactivating bacteria or viruses
The coating material with a high-reflectance layer and photocatalyst layer enhances light exposure to photocatalysts, effectively inactivating bacteria and viruses by maximizing photocatalytic action from the start and sustaining it over time.
Patent Information
- Application Number
- JP2023181969
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-23
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2039-04-08
AI Technical Summary
Existing photocatalyst-based coatings struggle to efficiently inactivate bacteria and viruses due to insufficient light penetration, limiting their photocatalytic effectiveness.
A coating material with a base material having a coating layer with a reflectance of 85% or more for light at 555 nm, combined with a photocatalyst layer, enhances light exposure by reflecting and diffusing light to activate the photocatalyst, thereby increasing the photocatalytic action.
The coating material efficiently inactivates bacteria and viruses by maximizing light exposure to the photocatalyst, achieving high photocatalytic effects from the initial stage and maintaining them over time, including antifouling and hydrophilic actions.
Smart Images

Figure 0007576141000007 
Figure 0007576141000008 
Figure 0007576141000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates generally to a coating material and a method for inactivating bacteria or viruses, and more particularly to a coating material including a photocatalytic layer and a method for inactivating bacteria or viruses using the coating material. [Background technology]
[0002] Photocatalysts have photocatalytic actions such as hydrophilic action, antifouling action, and inactivation action of bacteria or viruses. Of these photocatalytic actions, the inactivation action of bacteria or viruses has attracted attention. In addition, a coating film containing a photocatalyst is provided on a colored substrate to impart a photocatalytic action to the substrate. For example, the photocatalytic colored coated article of Patent Document 1 includes a substrate, a colored coating film, and a photocatalytic coating film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-149855 A Summary of the Invention [Problem to be solved by the invention]
[0004] Since the photocatalytic action is expressed by the photoexcitation action caused by irradiating the photocatalyst with light, the photocatalytic action can be expressed efficiently by increasing the amount of light that reaches the photocatalyst. Therefore, by increasing the amount of light that reaches the photocatalyst, it becomes easier to express the inactivation action of bacteria or viruses by the photocatalyst.
[0005] An object of the present disclosure is to provide a coating material that can increase the amount of light that reaches a photocatalyst and efficiently exerts a photocatalytic action, and a method for inactivating bacteria or viruses using this coating material. [Means for solving the problem]
[0006] The coating material of the present disclosure includes a substrate having at least a portion of its surface constituted by a coating layer having a reflectance of 85% or more for light with a wavelength of 555 nm, and a photocatalyst layer located on the coating layer.
[0007] The method for inactivating bacteria or viruses disclosed herein involves irradiating the photocatalyst layer of the covering material with light, thereby activating the photocatalyst and inactivating bacteria or viruses. Effect of the Invention
[0008] The coating material of the present disclosure allows light to reach the photocatalyst efficiently, allowing the photocatalytic action to be exerted efficiently, and the coating material of the present disclosure can also be used to inactivate bacteria or viruses. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a coating material according to a first embodiment. [Diagram 2] FIG. 2 is a schematic explanatory diagram showing a case where the covering material shown in FIG. 1 is irradiated with light. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a coating material according to a second embodiment. [Figure 4] FIG. 4 is a schematic explanatory diagram showing a case where the covering material shown in FIG. 3 is irradiated with light. [Diagram 5] FIG. 5 is a graph showing the percentage of color difference ΔE versus elapsed time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] 1. Overview 1, a coating material 1 according to an embodiment of the present disclosure includes a substrate 2 and a photocatalytic layer 3. At least a portion of the surface of the substrate 2 is configured with a coating layer 21 having a reflectance of 85% or more for light with a wavelength of 555 nm. The photocatalytic layer 3 is located on the coating layer 21.
[0011] In the covering material 1 of this embodiment, the reflectance of the covering layer 21 at light with a wavelength of 555 nm is 85% or more, so that the covering layer 21 easily reflects light. The photocatalyst 30 contained in the photocatalyst layer 3 exerts a photocatalytic action when exposed to visible light, and therefore not only light that directly hits the photocatalyst layer 3 but also light that passes through the photocatalyst layer 3 and is reflected by the covering layer 21 can reach the photocatalyst 30. Therefore, light can efficiently reach the photocatalyst 30, and the photocatalytic action can be efficiently exerted.
[0012] In the following description, "reflectance" is defined as a percentage of the light reflectance measured according to the 60-degree specular gloss measurement method described in JIS K 5600-4-7 (1999), with the gloss of a reference surface taken as 100. The upper limit of specular gloss is 100%.
[0013] 2. Details of the covering material 2-1. First embodiment 2-1-1. Composition of coating material The configuration of the coating material 1 according to the first embodiment will be described in detail below. The coating material 1 according to the first embodiment includes a substrate 2 and a photocatalytic layer 3, and further includes an intermediate protective layer 4 provided between the substrate 2 and the photocatalytic layer 3. Therefore, in the coating material 1, the intermediate protective layer 4 and the photocatalytic layer 3 are laminated in this order on the substrate 2.
[0014] (1) Base material At least a portion of the surface of the substrate 2 is formed with the coating layer 21. That is, the entire surface of the substrate 2 may be formed with the coating layer 21, or a portion of the surface of the substrate 2 may be formed with the coating layer 21. In this embodiment, the entire surface of the substrate 2 is formed with the coating layer 21. The substrate 2 includes a base material 20, a coating layer 21, and an undercoat layer 23 provided between the base material 20 and the coating layer 21.
[0015] (i) Base material There is no particular limitation on the material of the base material 20. The base material 20 may be formed from one or more materials selected from the group consisting of metals, ceramic materials, hydraulic materials such as cement, resin molding materials such as plastics, and carbon materials. When the base material 20 is a metal plate, examples of the metal plate include steel plates, stainless steel plates, aluminum plates, zinc plates, copper plates, and alloy plates thereof.
[0016] The base material 20 in this embodiment is a plated steel sheet 22. That is, the base material 2 includes the plated steel sheet 22 and a coating layer 21 provided on the plated steel sheet 22.
[0017] Examples of the plated steel sheet 22 include various plated steel sheets such as hot-dip galvanized steel sheet, electrolytic galvanized steel sheet, alloyed hot-dip galvanized steel sheet, aluminum plated steel sheet, aluminum-zinc alloy plated steel sheet, zinc-aluminum-magnesium alloy plated steel sheet, zinc-aluminum-magnesium-silicon alloy plated steel sheet, zinc-magnesium alloy plated steel sheet, tin plated steel sheet, lead plated steel sheet, and chrome plated steel sheet.
[0018] The surface of the plated steel sheet 22 may be subjected to a chemical conversion treatment. Examples of the chemical conversion treatment include coating chromate treatment, electrolytic chromate treatment, zinc phosphate treatment, and a recently developed hexavalent chromium treatment. This includes non-chromate treatments that do not contain chromate.
[0019] (ii) Undercoat layer 23 The undercoat layer 23 is provided on the base material 20. The undercoat layer 23 covers the base material 20. Therefore, the undercoat layer 23 is in direct contact with the base material 20. In this embodiment, the base material 20 is a plated steel sheet 22, so the undercoat layer 23 is in direct contact with the plated steel sheet 22. The undercoat layer 23 may be a single layer or may be composed of multiple layers. In addition, it is not limited to the case where the base material 20 and the undercoat layer 23 are in direct contact with each other, and for example, an appropriate layer may be interposed between the base material 20 and the undercoat layer 23. The undercoat layer 23 can be formed from an undercoat paint.
[0020] The thickness of the undercoat layer 23 is preferably 5 μm or more and 30 μm or less. When the thickness of the undercoat layer 23 is 5 μm or more, the processability of the undercoat layer 23, the adhesion to the base material 20, and the reflectivity of the coating layer 21 can be improved. When the thickness of the undercoat layer 23 is 30 μm or less, the occurrence of popping (small bubble-like bulges or holes) during application of the undercoat paint can be suppressed. The thickness of the undercoat layer 23 is more preferably 10 μm or more and 25 μm or less, and particularly preferably 12 μm or more and 22 μm or less. When the undercoat paint cannot be applied in one go due to the occurrence of popping, it may be applied in two or more steps.
[0021] The undercoat paint may contain, for example, a polyester resin, a curing agent, and a white pigment. If necessary, the undercoat paint may contain known materials such as pigment components such as extender pigments, coloring pigments, and chromate-based or chromate-free anti-rust pigments, curing catalysts, pigment dispersants, surface conditioners, matting agents, and organic solvents, as long as the reflectance of light at a wavelength of 555 nm is not impaired by 85% or more.
[0022] The number average molecular weight of the polyester resin contained in the undercoat paint is preferably from 2000 to 30000, more preferably from 3000 to 25000, even more preferably from 19000 to 26000, and even more preferably from 20000 to 23000. In this specification, the number average molecular weight is a value obtained by converting the number average molecular weight measured using gel permeation chromatography (GPC) based on the molecular weight of standard polystyrene. Specifically, a gel permeation chromatograph "HLC8120GPC" (product name, manufactured by Tosoh Corporation) is used, and four columns "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (product names, all manufactured by Tosoh Corporation) are used, and measurements can be performed under the following conditions: mobile phase tetrahydrofuran, measurement temperature 40°C, flow rate 1 mL / min and detector RI.
[0023] The polyester resin contained in the undercoat paint preferably has a hydroxyl group. The hydroxyl value of the polyester resin is preferably in the range of 10 to 200 mgKOH / g, particularly 60 to 185 mgKOH / g, from the viewpoint of adhesion of the resulting coating film. The acid value of the polyester resin is preferably 30 mgKOH / g or less, preferably in the range of 1 to 20 mgKOH / g, from the viewpoint of finish.
[0024] The polyester resin contained in the undercoat paint can usually be produced by an esterification reaction or transesterification reaction between a polybasic acid component and a polyhydric alcohol component. As the polybasic acid component, for example, an alicyclic polybasic acid component, an aliphatic polybasic acid component, an aromatic polybasic acid component, etc. can be used.
[0025] The alicyclic polybasic acid component is generally a compound having one or more alicyclic structures (mainly 4- to 6-membered rings) and two or more carboxyl groups in one molecule, an acid anhydride of the compound, and an esterification product of the compound. Examples of the alicyclic polybasic acid component include alicyclic polycarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, 3-methyl-1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, and 1,3,5-cyclohexanetricarboxylic acid; anhydrides of these alicyclic polybasic carboxylic acids; and lower alkyl esterification products of these alicyclic polybasic carboxylic acids. The alicyclic polybasic acid component can be used alone or in combination of two or more kinds.
[0026] As the alicyclic polybasic acid component, particularly, 1,2-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic anhydride, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, and 4-cyclohexene-1,2-dicarboxylic anhydride can be preferably used. Among them, from the viewpoint of hydrolysis resistance, 1,2-cyclohexanedicarboxylic acid and 1,2-cyclohexanedicarboxylic anhydride can be particularly preferably used.
[0027] The aliphatic polybasic acid component is generally an aliphatic compound having two or more carboxyl groups in one molecule, an acid anhydride of the aliphatic compound, and an esterification product of the aliphatic compound, such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecane diacid, dodecane diacid, brassylic acid, octadecanedioic acid, citric acid, etc.; anhydrides of these aliphatic polybasic carboxylic acids; lower alkyl esterification products of these aliphatic polybasic carboxylic acids, etc. The aliphatic polybasic acid component can be used alone or in combination of two or more kinds.
[0028] As the aliphatic polybasic acid component, it is preferable to use a dicarboxylic acid having an alkylene chain with 4 to 18 carbon atoms. Examples of the dicarboxylic acid having an alkylene chain with 4 to 18 carbon atoms include adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassylic acid, and octadecanedioic acid, and among these, adipic acid can be preferably used.
[0029] The aromatic polybasic acid component is generally an aromatic compound having two or more carboxyl groups in one molecule, an acid anhydride of the aromatic compound, and a lower alkyl ester of the aromatic compound, such as, for example, aromatic polycarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, trimellitic acid, pyromellitic acid, etc.; anhydrides of these aromatic polybasic carboxylic acids; and lower alkyl esters of these aromatic polybasic carboxylic acids. The aromatic polybasic acid component can be used alone or in combination of two or more kinds.
[0030] As the polyhydric alcohol component, a polyhydric alcohol having two or more hydroxyl groups in one molecule can be suitably used. Examples of the polyhydric alcohol component (a2) include alicyclic diols, aliphatic diols, aromatic diols, and trihydric or higher polyhydric alcohols.
[0031] The alicyclic diol is generally a compound having one or more alicyclic structures (mainly 4- to 6-membered rings) and two hydroxyl groups in one molecule. Examples of the alicyclic diol include dihydric alcohols such as 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, hydrogenated bisphenol A, and hydrogenated bisphenol F; polylactone diols obtained by adding lactone compounds such as ε-caprolactone to these dihydric alcohols; and the like, which can be used alone or in combination of two or more kinds.
[0032] The above-mentioned aliphatic diol is generally an aliphatic compound having two hydroxyl groups in one molecule. Examples of the aliphatic diol include ethylene glycol, propylene glycol, diethylene glycol, trimethylene glycol, tetraethylene glycol, triethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-butanediol, 3-methyl-1,2-butanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,2-pentanediol, 1,5-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,3-dimethyltrimethylene glycol, tetramethylene glycol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,4-hexanediol, 2,5-hexanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, neopentyl glycol; and polyether diol compounds such as polyethylene glycol, polypropylene glycol, and polybutylene glycol. These can be used alone or in combination of two or more.
[0033] The aromatic diol is generally an aromatic compound having two hydroxyl groups in one molecule. Examples of the aromatic diol include ester diol compounds such as bis(hydroxyethyl) terephthalate; alkylene oxide adducts of bisphenol A; and the like, which can be used alone or in combination of two or more kinds.
[0034] Examples of trihydric or higher polyhydric alcohols include trihydric or higher alcohols such as glycerin, trimethylolethane, trimethylolpropane, diglycerin, triglycerin, 1,2,6-hexanetriol, pentaerythritol, dipentaerythritol, sorbitol, and mannitol; polylactone polyol compounds obtained by adding lactone compounds such as ε-caprolactone to these trihydric or higher alcohols; and tris(hydroxyalkyl)isocyanurates such as tris(2-hydroxyethyl)isocyanurate, tris(2-hydroxypropyl)isocyanurate, and tris(2-hydroxybutyl)isocyanurate. Of these, trimethylolpropane is particularly preferred.
[0035] The method for producing the polyester resin is not particularly limited, but for example, the polyester resin can be produced by reacting an acid component having the above-mentioned polybasic acid component as an essential component with a polyhydric alcohol component in a nitrogen gas flow at 150 to 250°C for 5 to 10 hours to carry out an esterification reaction or an ester exchange reaction. In this esterification reaction or ester exchange reaction, the above-mentioned acid component and alcohol component may be added at once or in several portions. In addition, after synthesizing a carboxyl group-containing polyester resin first, a part of the carboxyl groups in the carboxyl group-containing polyester resin may be esterified using the above-mentioned alcohol component. Furthermore, after synthesizing a polyester resin first, an acid anhydride may be reacted to perform half esterification.
[0036] In the above esterification or transesterification reaction, a catalyst may be used to promote the reaction. Known catalysts such as dibutyltin oxide, antimony trioxide, zinc acetate, manganese acetate, cobalt acetate, calcium acetate, lead acetate, tetrabutyl titanate, and tetraisopropyl titanate can be used as the catalyst.
[0037] The polyester resin may be modified with a fatty acid, an oil, a monoepoxy compound, a monoalcohol compound, a polyisocyanate compound, or the like during the preparation of the resin, or after the esterification reaction or the transesterification reaction.
[0038] Examples of the fatty acids include coconut oil fatty acids, cottonseed oil fatty acids, hempseed oil fatty acids, rice bran oil fatty acids, fish oil fatty acids, tall oil fatty acids, soybean oil fatty acids, linseed oil fatty acids, tung oil fatty acids, rapeseed oil fatty acids, castor oil fatty acids, dehydrated castor oil fatty acids, safflower oil fatty acids, and other fatty acids; lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, and the like.
[0039] Examples of fats and oils include coconut oil, cottonseed oil, hemp seed oil, rice bran oil, fish oil, tall oil, soybean oil, linseed oil, tung oil, rapeseed oil, castor oil, dehydrated castor oil, and safflower oil.
[0040] Examples of the polyisocyanate compound used for the modification include aliphatic diisocyanate compounds such as lysine diisocyanate, hexamethylene diisocyanate, and trimethylhexane diisocyanate; alicyclic diisocyanate compounds such as hydrogenated xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane-2,4-diisocyanate, methylcyclohexane-2,6-diisocyanate, 4,4'-methylenebis(cyclohexylisocyanate), and 1,3-(isocyanatomethyl)cyclohexane; Examples of the isocyanate include organic polyisocyanates themselves, such as aromatic diisocyanate compounds such as tolylene diisocyanate, xylylene diisocyanate, and diphenylmethane diisocyanate; polyisocyanates having three or more valences, such as lysine triisocyanate; and adducts of these organic polyisocyanates with polyhydric alcohols, low molecular weight polyester resins, water, etc., as well as cyclized polymers (e.g., isocyanurates) and biuret-type adducts of the above-mentioned organic diisocyanates. These can be used alone or in combination of two or more.
[0041] The proportion of the polyester resin in the total amount of resin contained in the undercoat paint is more preferably from 85% by mass to 100% by mass, and particularly preferably from 90% by mass to 100% by mass.
[0042] The curing agent contained in the undercoat paint can be any curing agent that can react with the hydroxyl groups of the polyester resin by heating to cure the resin, and examples of such curing agents include melamine resins, benzoguanamine resins, urea resins, and polyisocyanate compounds.
[0043] Examples of the melamine resin include partially or fully etherified melamine resins in which some or all of the methylol groups of methylolated melamine are etherified with a monohydric alcohol having 1 to 8 carbon atoms, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, i-propyl alcohol, n-butyl alcohol, i-butyl alcohol, 2-ethylbutanol, 2-ethylhexanol, etc.
[0044] Commercially available melamine resins include, for example, Cymel 202, Cymel 232, Cymel 235, Cymel 238, Cymel 254, Cymel 266, Cymel 267, Cymel 272, Cymel 285, Cymel 301, Cymel 303, Cymel 325, Cymel 327, Cymel 350, Cymel 370, Cymel 701, Cymel 703, Cymel 1141 (all manufactured by Daicel-Allnex), and U-Ban 20SE60 (manufactured by Mitsui Chemicals, Inc.).
[0045] The benzoguanamine resin may be a methylolated benzoguanamine resin obtained by reacting benzoguanamine with an aldehyde. Examples of the aldehyde include formaldehyde, paraformaldehyde, acetaldehyde, and benzaldehyde. The benzoguanamine resin may also be etherified with one or more alcohols. Examples of the alcohol used for etherification include monohydric alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, 2-ethylbutanol, and 2-ethylhexanol. Among these, a benzoguanamine resin obtained by etherifying at least a part of the methylol group of a methylolated benzoguanamine resin with a monohydric alcohol having 1 to 4 carbon atoms is preferable.
[0046] Specific examples of the benzoguanamine resin include methyl-etherified benzoguanamine resins such as Mycoat 102, Mycoat 105, Mycoat 106 (all manufactured by Mitsui Chemicals), Nikalac SB-201, Nikalac SB-203, Nikalac SB-301, Nikalac SB-303, and Nikalac SB-401 (all manufactured by Sanwa Chemical); mixed etherified benzoguanamine resins of methyl ether and ethyl ether such as Cymel 1123 (manufactured by Daicel-Allnex); mixed etherified benzoguanamine resins of methyl ether and butyl ether such as Mycoat 136 (manufactured by Mitsui Chemicals), Nikalac SB-255, Nikalac SB-355, Nikalac BX-37, and Nikalac BX-4000 (all manufactured by Sanwa Chemical); and butyl-etherified benzoguanamine resins such as Mycoat 1128 (manufactured by Mitsui Chemicals).
[0047] Urea resins are obtained by the condensation reaction of urea with formaldehyde, and can be dissolved or dispersed in a solvent or water.
[0048] Examples of the polyisocyanate compound include compounds having two or more isocyanate groups in one molecule, such as aromatic diisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and naphthalene diisocyanate; aliphatic diisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, dimer acid diisocyanate, and lysine diisocyanate; methylene bis(cyclohexyl isocyanate), isophorone diisocyanate, and methyl diisocyanate; Examples of the polyisocyanates include alicyclic diisocyanates such as ethyl cyclohexane diisocyanate, cyclohexane diisocyanate, and cyclopentane diisocyanate; biuret-type adducts and isocyanuric ring-type adducts of the polyisocyanates; and free isocyanate group-containing prepolymers obtained by reacting these polyisocyanates with low- or high-molecular-weight polyol compounds (e.g., acrylic polyol, polyester polyol, polyether polyol, etc.) in an excess of isocyanate groups.
[0049] Furthermore, as the polyisocyanate compound, there can also be used a blocked polyisocyanate compound in which the free isocyanate groups of the above-mentioned polyisocyanate compounds are blocked with a blocking agent such as a phenol compound, an oxime compound, an active methylene compound, a lactam compound, an alcohol compound, a mercaptan compound, an acid amide compound, an imide compound, an amine compound, an imidazole compound, a urea compound, a carbamic acid compound, or an imine compound.
[0050] In addition, in order to accelerate the curing of the undercoat resin binder, a curing catalyst can be blended as necessary. When the curing agent is an amino resin, examples of the curing catalyst include strong acids and neutralized products of strong acids, and representative examples include sulfonic acid compounds that are strong acids such as p-toluenesulfonic acid, dodecylbenzenesulfonic acid, dinonylnaphthalenesulfonic acid, and dinonylnaphthalenedisulfonic acid, and amine neutralized products of these sulfonic acid compounds.
[0051] When the curing agent is a blocked polyisocyanate compound, examples of the curing catalyst include curing catalysts that promote dissociation of the blocking agent of the blocked polyisocyanate compound, which is the curing agent, such as organometallic catalysts such as tin octoate, dibutyltin di(2-ethylhexanoate), dioctyltin di(2-ethylhexanoate), dibutyltin dilaurate, dibutyltin oxide, dioctyltin oxide, and lead 2-ethylhexanoate.
[0052] As described above, the undercoat paint preferably contains a white pigment. In this case, the reflectance of the coating layer 21 can be improved. The undercoat paint preferably contains titanium oxide as a white pigment, and more preferably contains rutile titanium oxide. Rutile titanium oxide has a high refractive index, so the reflectance of the coating layer 21 can be further improved. In the undercoat paint, the solid content volume concentration of rutile titanium oxide is preferably 20% to 35%, more preferably 20% to 30%, and particularly preferably 22% to 28%. The average particle size of rutile titanium oxide contained in the undercoat paint is preferably 200 nm to 400 nm, and more preferably 250 nm to 350 nm. The average particle size of rutile titanium oxide is the arithmetic mean value of the particle sizes of the remaining rutile titanium oxide particles, obtained by observing the undercoat layer 23 at a magnification of 10,000 times with an electron microscope, excluding the smallest 20% and the largest 5%.
[0053] There are no particular limitations on the manufacturing method of titanium oxide, the presence or absence of surface treatment, or the type of surface treatment, but titanium oxide with as high a concealing property and a high degree of whiteness as possible is preferred, and among these, it is particularly preferred that rutile-type titanium oxide is manufactured by the chlorine method and is surface-treated with alumina, silica, titania, etc. Such titanium oxide is particularly preferred because of its high concealing property and high degree of whiteness.
[0054] Commercially available titanium oxide products include, for example, Ti-Pure R706, Ti-Pure R960, Ti-Pure R902+ (all of which are product names of DuPont, titanium oxide pigments produced by the chlorine method), Typeic CR-50, Typeic CR-60, Typeic CR-95 (all of which are product names of Ishihara Sangyo Kaisha, Ltd., titanium oxide pigments produced by the chlorine method), and CR-826 (product name of Tronox, titanium oxide pigments produced by the chlorine method).
[0055] The undercoat paint may contain a solvent, a leveling agent, a pigment dispersant, an anti-popping agent, etc. to improve the ease of painting.
[0056] The application method of the undercoat paint can be curtain coating, roll coating, dip coating, spray coating, etc. When the undercoat paint is precoated by coil coating, it is preferable to use the curtain coating method or roll coating method from the viewpoint of economy. When applying the roll coating method, a top-feed or bottom-feed method using three rolls is recommended to maximize the uniformity of the coating surface, but in practice, a normal bottom-feed method using two rolls (so-called natural reverse coating, natural coating) is also acceptable.
[0057] The curing conditions (baking conditions) for the undercoat paint are usually about 15 seconds to 30 minutes at a maximum material temperature (PMT) of 120 to 260°C. In the field of precoat painting, which is applied by coil coating, etc., the curing is usually performed in the range of 15 to 90 seconds at a maximum material temperature of 160 to 260°C.
[0058] (2) Covering layer The coating layer 21 is provided on the undercoat layer 23 and covers the undercoat layer 23. Therefore, the coating layer 21 covers the base material 20 and constitutes the surface of the substrate 2. The coating layer 21 contains a binder and a white pigment. The coating layer 21 in this embodiment is in direct contact with the undercoat layer 23, but is not limited thereto, and an appropriate layer may be interposed between the undercoat layer 23 and the coating layer 21.
[0059] The coating layer 21 has a high light reflectance. Specifically, the coating layer 21 has a reflectance of 85% or more for light with a wavelength of 555 nm. This configuration can be achieved, for example, by the coating layer 21 containing a high concentration of white pigment relative to the binder. When the coating layer 21 has a high concentration of white pigment relative to the binder, reflection is likely to occur not only at the white pigment-binder interface but also at the white pigment-air interface and the binder-air interface. Therefore, the light reflectance of the coating layer 21 can be increased. Moreover, the coating layer 21 preferably has a reflectance of 92.5% or more for light with a wavelength of 450 nm or more and 750 nm or less, and a reflectance of 95% or more for light with a wavelength of 555 nm. In this case, the coating layer 21 can efficiently reflect light. Furthermore, when the coating material 1 is used as a reflector, high illuminance can be obtained.
[0060] The covering layer 21 of this embodiment will now be described in more detail.
[0061] In the coating layer 21, the concentration of the white pigment is preferably 150 parts by volume or more relative to 100 parts by volume of the binder, more preferably 200 parts by volume or more, even more preferably 500 parts by volume or more, and even more preferably 800 parts by volume or more. In this case, the reflectance of the coating layer 21 can be improved without increasing the thickness of the coating layer 21. The concentration of the white pigment is preferably less than 1500 parts by volume relative to 100 parts by volume of the binder. In this case, the coating layer 21 can be prevented from becoming brittle, and the strength of the coating layer 21 can be ensured.
[0062] The coating layer 21 preferably has a porosity by volume of 5 vol% or more, more preferably 9 vol% or more, and even more preferably 20 vol% or more. The cross-sectional porosity is preferably 2% or more, more preferably 5% or more, and even more preferably 10% or more. In this case, the reflectance of the coating layer 21 can be improved without increasing the thickness of the coating layer 21. The coating layer 21 preferably has a porosity by volume of less than 35 vol%. The cross-sectional porosity is preferably less than 35%. In this case, the coating layer 21 can be prevented from becoming brittle, and the strength of the coating layer 21 can be ensured.
[0063] The concentration (part by volume) of the binder and the white pigment in the coating layer 21 and the porosity by volume can be measured by the following method. First, a part of the coating layer 21 is scraped off to confirm the components of the binder and the white pigment. The method for confirming the components is not particularly limited. For example, the components of the binder can be confirmed by methods such as FT-IR and NMR. For example, the components of the white pigment can be confirmed by methods such as XRD and FT-IR. Next, a sample with a certain area a and a certain thickness b is scraped off from the coating layer 21. The apparent volume c of this sample is a×b. Next, the mass d of the sample is measured using a weighing machine capable of measuring with three or more significant digits. Next, the entire sample is heated until the binder decomposes. Next, the mass e of the sample after heating is measured. The mass e corresponds to the mass of the white pigment, and the mass f of the binder can be calculated by subtracting the mass e from the mass d. Based on the specific gravity of these binder components, the mass f of the binder, the specific gravity of the white pigment components, and the mass e of the white pigment, it is possible to calculate the volume g of the binder that occupies the volume c, and the volume h of the white pigment. From these values, the concentration (parts by volume) of the binder and the white pigment, and the porosity by volume can also be calculated.
[0064] The porosity of the cross section of the coating layer 21 can be measured by the following method. First, a sample is scraped off from the coating layer 21, embedded in resin, and polished to form a smooth cross section perpendicular to the surface of the coating layer 21. This cross section is photographed at 10,000 times magnification using a scanning microscope. The porosity of the cross section can be determined by comparing the area of the white pigment and the area of the voids in the obtained image.
[0065] The thickness of the coating layer 21 is preferably 5 μm or more and less than 100 μm. When the thickness of the coating layer 21 is less than 100 μm, the coating layer 21 can be prevented from becoming brittle. From the viewpoint of the finished appearance, the thickness of the coating layer 21 is preferably 20 μm or more and 50 μm or less, and more preferably 25 μm or more and 35 μm or less. In this case, the light reflectance of the coating layer 21 can be improved, and the coating layer 21 can be prevented from becoming brittle, thereby ensuring the strength of the coating layer 21. Note that the coating layer 21 is not limited to being composed of a single layer, and may be composed of multiple layers.
[0066] The binder contained in the coating layer 21 may be a thermoplastic resin or a thermosetting resin. The binder may be a solid resin that has been thermally melted, a resin that has been dissolved in an organic solvent, or a solid resin that has been pulverized. The binder may be water-soluble or may be an emulsion type that has been dispersed in water. The binder may be an ultraviolet-curable resin or an electron beam-curable resin. The binder may contain a crosslinking agent. The binder may contain, for example, one or more selected from the group consisting of polyester resin, urethane resin, acrylic resin, epoxy resin, melamine resin, vinyl chloride resin, fluororesin, and silicone resin.
[0067] The white pigment contained in the coating layer 21 preferably contains rutile titanium oxide. That is, the coating layer 21 preferably contains rutile titanium oxide. Rutile titanium oxide has a high refractive index and therefore easily reflects light at the white pigment-binder interface. Therefore, by the coating layer 21 containing rutile titanium oxide as a white pigment, the light reflectance of the coating layer 21 can be improved. The rutile titanium oxide may be surface-treated with Al, Si, Zr, an organic substance, or the like. The coating layer 21 may contain commercially available rutile titanium oxide as a white pigment. Examples of commercially available rutile titanium oxide include the "Tipaque TM" series manufactured by Ishihara Sangyo Kaisha, Ltd. and the "Titanics" series manufactured by Teika Corporation. The coating layer 21 may contain a white pigment other than rutile titanium oxide.
[0068] The average particle size of the white pigment contained in the coating layer 21 is preferably 200 nm or more and 400 nm or less. In this case, the surface area of the white pigment can be increased, the reflectance of the coating layer 21 can be improved, and an increase in the transmittance of light on the long wavelength side can be suppressed.
[0069] The coating layer 21 can be formed from a coating paint containing the above-mentioned binder and white pigment. Specifically, the coating layer 21 is obtained by baking and drying a coating film of the coating paint. Examples of the coating method include roller curtain coating, curtain flow coating, air spray coating, die coater coating, dip coating, inkjet coating, and the like.
[0070] (3) Intermediate protective layer The intermediate protective layer 4 is provided between the substrate 2 and the photocatalytic layer 3, more specifically, between the coating layer 21 and the photocatalytic layer 3. Therefore, the intermediate protective layer 4 covers the coating layer 21 and is in direct contact with the coating layer 21.
[0071] The main component of the intermediate protective layer 4 is preferably silicon oxide or a siloxane polymer.
[0072] Silicon oxide includes silicon monoxide, silicon dioxide, and compounds with non-stoichiometric ratios of silicon and oxygen (e.g., SiO 1.5 , SiO 1.8 ) is included. The silicon oxide may be crystalline, amorphous, or quasicrystalline. The silicon oxide preferably contains amorphous silica. In this case, the flexibility of the intermediate protective layer 4 can be improved more than when the silicon oxide is crystalline silica.
[0073] The siloxane polymer preferably contains a dehydration condensate obtained by hydrolysis and subsequent condensation of at least one alkoxysilane selected from the group consisting of tetraalkoxysilanes having an alkoxy group with 1 to 4 carbon atoms, alkoxysilanes having an alkyl group with 1 to 12 carbon atoms, alkoxysilanes having an aryl group, and alkoxysilanes having both an alkyl group and an aryl group with 1 to 12 carbon atoms, with an alkoxysilane having an epoxy group or an alkoxysilane having an amino group. The condensate of the alkoxysilane is preferably one produced by hydrolyzing the alkoxysilane used as a raw material to produce a hydrolyzate, which is then condensed in a drying and baking (heat treatment) process. When the main component of the intermediate protective layer 4 is silicon oxide or a siloxane polymer, it is preferable to suppress deterioration of the intermediate protective layer 4 due to the photocatalytic action of the photocatalyst 30 contained in the photocatalyst layer 3. In particular, since the main component of the intermediate protective layer 4 is an inorganic-organic composite polymer that is a polysiloxane-based inorganic polymer mainly composed of amorphous silica or silicon and that contains a large amount of alkyl groups and aryl groups, the weather resistance, processability, and stability against photocatalysts of the intermediate protective layer 4 can be improved.
[0074] Examples of the alkyl group having 1 to 12 carbon atoms include methyl, ethyl, propyl, butyl, hexyl, 2-ethylhexyl, and dodecyl groups, and examples of the aryl group include phenyl, tolyl, xylyl, and naphthyl groups. Among these alkyl groups, methyl and phenyl groups are preferred. That is, the alkoxysilane having an alkyl group having 1 to 12 carbon atoms preferably includes an alkoxysilane having a methyl group, an alkoxysilane having a phenyl group, and an alkoxysilane having a methyl group and a phenyl group, and particularly preferably includes an alkoxysilane having a phenyl group. The siloxane polymer preferably includes two or more alkoxysilanes having different organic groups, and an alkoxysilane containing two or more different organic groups.
[0075] When the intermediate protective layer 4 contains the inorganic-organic composite polymer, this inorganic-organic composite polymer preferably has methyl groups and / or phenyl groups bonded at a ratio of 0.05 to 1.5, and more preferably 0.05 to 1.2, per Si-O bond of 1. In this case, it is possible to impart appropriate flexibility to the intermediate protective layer 4 and to improve the photocatalytic activity of the photocatalytic layer 3 provided on the intermediate protective layer 4.
[0076] The intermediate protective layer 4 may contain a photocatalyst. In this case, the proportion of the photocatalyst in the intermediate protective layer 4 is preferably smaller than the proportion of the photocatalyst in the photocatalyst layer 3. The mass proportion of the photocatalyst to the entire intermediate protective layer 4 is preferably 0.05% or more and 20% or less, and more preferably 0.1% or more and 15% or less. In this case, even if the intermediate protective layer 4 is exposed due to deterioration of the photocatalyst layer 3, the photocatalytic action can be exerted by the photocatalyst contained in the intermediate protective layer 4. Furthermore, deterioration of the resin contained in the coating layer 21 due to the photocatalytic action of the photocatalyst contained in the intermediate protective layer 4 can be suppressed.
[0077] The thickness of the intermediate protective layer 4 is preferably from 0.1 μm to 3 μm, more preferably from 0.1 μm to 2.5 μm, and even more preferably from 0.3 μm to 2 μm.
[0078] The intermediate protective layer 4 can be formed by forming a coating film from a coating material for a protective layer containing the above-mentioned silicon oxide or siloxane polymer and, if necessary, a photocatalyst, and then heating and curing the coating film. The coating material for a protective layer can be applied by, for example, dip coating, spray coating, bar coating, roll coating, or spin coating. The heating conditions for the coating film of the coating material for a protective layer are preferably a heat treatment in a temperature range of 150°C to 400°C for about one hour to a few seconds.
[0079] (4) Photocatalyst layer The photocatalytic layer 3 is located on the coating layer 21 , and more particularly on the intermediate protective layer 4 .
[0080] The photocatalyst layer 3 preferably contains at least one of silicon oxide and a siloxane polymer.
[0081] The silicon oxide preferably includes, for example, amorphous silica.
[0082] The siloxane polymer preferably contains, for example, a resin made of a dehydration condensate obtained by hydrolysis and condensation of a tetraalkoxysilane having an alkoxy group with 1 to 4 carbon atoms, or an alkoxysilane having an epoxy group.
[0083] Examples of tetraalkoxysilanes having an alkoxy group having 1 to 4 carbon atoms include tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, tetra-i-butoxysilane, tetra-sec-butoxysilane, and tetra-tert-butoxysilane.
[0084] Examples of alkoxysilanes having an epoxy group include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltripropoxysilane, γ-glycidoxypropyltributoxysilane, 3,4-epoxycyclohexylmethyltrimethoxysilane, 3,4-epoxycyclohexylmethyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, etc. Among alkoxysilanes having an epoxy group, γ-glycidoxypropyltriethoxysilane is particularly excellent in handleability.
[0085] The resin made of the condensate of the alkoxysilane and the alkoxysilane is a resin that has high stability against photocatalysis and is mainly composed of inorganic components such as siloxane, which is an inorganic component, and a small amount of epoxy groups. Among them, alkoxysilanes having epoxy groups are preferable because they have the effect of lowering the baking temperature of the film. In general, when forming a polysiloxane-based film using only silicon alkoxide as a starting material, heat treatment at 400 to 500 ° C for several hours is required to efficiently carry out a series of processes from dehydration condensation to curing. When forming the photocatalyst layer 3, by introducing epoxy groups, it is possible to reduce the treatment temperature to about 150 to 200 ° C and shorten the heat treatment time, and the heat treatment conditions can be set to be suitable for coil coating.
[0086] The photocatalyst layer 3 preferably contains an inorganic polymer consisting of only tetraalkoxysilane and condensates of these alkoxysilanes. Tetraalkoxysilanes generate siloxane bonds containing hydroxyl groups through hydrolysis and dehydration condensation, and can be made to have only siloxane bonds by further aging or heat treatment, so that the photocatalyst layer 3 can be prevented from being deteriorated by the photocatalytic action of the photocatalyst 30.
[0087] The ratio of epoxy groups contained in the photocatalyst layer 3 is preferably 0 to 0.25, and more preferably 0 to 0.22, relative to 1 Si—O bond. In this case, the photocatalytic resistance of the photocatalyst layer 3 can be improved.
[0088] The photocatalyst layer 3 includes a photocatalyst 30. The photocatalyst 30 is a substance that exhibits a photocatalytic action when irradiated with light. A specific example of the photocatalyst 30 is titanium oxide. Examples of titanium oxide include rutile-type titanium oxide, anatase-type titanium oxide, and brookite-type titanium oxide. The photocatalyst 30 preferably contains anatase-type titanium oxide. That is, the photocatalyst layer 3 preferably contains anatase-type titanium oxide. This is because the photocatalytic activity of anatase-type titanium oxide is higher than that of other titanium oxides. In particular, the photocatalyst 30 is preferably a substance that exhibits a photocatalytic action by visible light. That is, the photocatalyst 30 is preferably a visible light excited photocatalyst. In this case, the photocatalytic action of the photocatalyst 30 can be exhibited by visible light, and the photocatalytic action of the photocatalyst 30 can be exhibited by light such as fluorescent light and LED. Examples of visible light excited photocatalysts include anatase type titanium oxide doped with anions such as nitrogen or sulfur, and anatase type titanium oxide carrying Pt particles.
[0089] When nitrogen is doped into titanium oxide crystals, depending on the state of the nitrogen present, one or more of the following can be obtained: (i) some of the oxygen sites of the titanium oxide crystal are replaced with nitrogen atoms, resulting in a Ti-ON structure, (ii) nitrogen atoms are present between the lattices of the titanium oxide crystal, and (iii) nitrogen atoms are present at the grain boundaries of the polycrystalline aggregate of the titanium oxide crystal. In particular, the photocatalyst (i) has a crystal structure stabilized by the Ti-ON structure, so it can exert a photocatalytic effect with both visible light and ultraviolet light, and can exert the photocatalytic effect for a long period of time.
[0090] The state of the photocatalyst 30 may be any of a powder, an aqueous sol or colloid dispersed in water, and an organic solvent sol or colloid dispersed in a polar solvent such as alcohol or a non-polar solvent such as toluene. When the photocatalyst 30 is an organic solvent sol or colloid, the photocatalyst paint may be diluted with water or an organic solvent depending on its dispersibility. In addition, the photocatalyst 30 may be surface-treated to improve the dispersibility of the photocatalyst 30.
[0091] When the photocatalyst 30 contains anatase type titanium oxide doped with nitrogen, it can be produced, for example, by the following methods (I) to (IV). (I) A method of heat treating titanium oxide or hydrous titanium oxide in an atmosphere containing at least one gas selected from the group consisting of ammonia gas, nitrogen gas, and a mixed gas of nitrogen gas and hydrogen gas. (II) A method of heat treating a titanium alkoxide solution in an atmosphere containing at least one gas selected from the group consisting of ammonia gas, nitrogen gas, and a mixed gas of nitrogen gas and hydrogen gas. (III) In the emulsion combustion method, a method in which ions or molecules containing nitrogen elements other than nitrate ions, such as ammonia and hydrazine, are present in the titanium salt aqueous solution or suspension, which is the aqueous phase of the emulsion, and the emulsion is sprayed and burned in an atmosphere in which the combustion components, including oil and surfactants, contained in the emulsion are completely burned and an amount of oxygen not exceeding the amount required for the metal ions or metal compounds contained in the aqueous solution to form their most stable oxides in the atmosphere is introduced into the reaction apparatus. (IV) In the emulsion combustion method, the titanium salt aqueous solution or suspension, which is the aqueous phase in the emulsion, does not contain ions or molecules containing nitrogen atoms other than nitrate ions, such as ammonia or hydrazine, but contains a nitrogen-containing gas other than nitrogen gas, such as ammonia, and the amount of oxygen introduced into the reaction apparatus is less than the required amount of oxygen, and the emulsion is sprayed and burned in this atmosphere. (V) A method of subjecting titanium nitride crystals or titanium oxynitride crystals to a heat treatment or plasma treatment in an oxidizing atmosphere containing oxygen, ozone, water molecules, or a compound containing a hydroxyl group. (VI) A method of heating a mixture of titanium oxide and a nitrogen compound that is adsorbed to titanium oxide at room temperature.
[0092] The primary particle diameter of the photocatalyst 30 is preferably 0.5 μm or less, more preferably 0.1 μm or less, and particularly preferably 0.05 μm or less. The lower limit of the primary particle diameter of the photocatalyst 30 is not particularly limited, but is, for example, 5 nm or more. The smaller the primary particle diameter of the photocatalyst 30, the more the photocatalytic action can be improved. In addition, the smaller the primary particle diameter of the photocatalyst 30, the more difficult it is to disperse, and aggregates of the particles of the photocatalyst 30 are formed. In many cases, no resin is present in the gaps between the aggregates. By forming an area in the photocatalyst layer 3 where no resin is present, the photocatalytic action such as antifouling action and inactivation action of bacteria or viruses can be effectively performed.
[0093] When the photocatalyst 30 is a fine particle, it is difficult to disperse the photocatalyst 30 in the photocatalyst layer 3, and the particles of the photocatalyst 30 may form aggregates. Usually, the resin component constituting the photocatalyst layer 3 is not present in the gaps between the aggregates, which is an advantage in that bacteria or viruses can easily reach the photocatalyst 30. In addition, it is desirable that the photocatalyst 30 is uniformly dispersed in the photocatalyst layer 3, but it is not necessarily required to be uniformly dispersed. When the photocatalyst 30 is not uniformly dispersed, the particles of the photocatalyst 30 form aggregates, the concentration of the photocatalyst 30 differs between the outermost surface and the inside, the content concentration of the photocatalyst material changes stepwise, etc., and even in these states, the photocatalyst 30 can be suitably used.
[0094] By varying the dispersion state of the photocatalyst 30 in the photocatalyst layer 3, it is possible to exhibit the photocatalytic action from the initial stage over a long period of time, and to suppress the deterioration of the resin contained in the photocatalyst layer 3. For example, it is preferable that the photocatalyst 30 contained in the photocatalyst layer 3 has a maximum value in the particle size distribution, one of the maximum values of the particle size distribution of the photocatalyst 30 is in the range of 0.5 μm to 5 μm, and one of the maximum values of the particle size distribution of the photocatalyst in the intermediate protective layer 4 is 0.2 μm or less. Since the photocatalyst 30 in the photocatalyst layer 3 exhibits a photocatalytic action, it is preferable that the activity is high, and as a result of the aggregation of fine particles of the photocatalyst 30, one of the maximum values of the particle size distribution is preferably in the range of 0.5 μm to 5 μm. The maximum value of the particle size distribution of the photocatalyst 30 in the photocatalyst layer 3 is more preferably 0.5 μm to 3 μm, and further preferably 0.6 μm to 2 μm. In addition, it is preferable that the maximum value of the particle size distribution of the photocatalyst in the intermediate protective layer 4 is 0.15 μm or less. The maximum value of the photocatalyst contained in the photocatalyst layer 3 and the intermediate protective layer 4 preferably does not exceed 20 μm, which is twice the total coating thickness, and more preferably does not exceed 10 μm. In the photocatalyst layer 3, the maximum value of the particle size distribution of the photocatalyst 30 is preferably less than 0.2 μm. In this case, the photocatalytic activity of the photocatalyst layer 3 is easily expressed from the initial stage.
[0095] The ratio of the photocatalyst 30 contained in the photocatalyst layer 3 is preferably 50% or less, preferably 40% or less, and preferably 30% or less, in terms of mass ratio to the entire photocatalyst layer 3. In this case, it is possible to suppress deterioration of the resin contained in the photocatalyst layer 3 due to the photocatalytic action of the photocatalyst 30, while efficiently exerting the photocatalytic action of the photocatalyst 30. The lower limit of the ratio of the photocatalyst 30 contained in the photocatalyst layer 3 is not particularly limited as long as it can exert the photocatalytic action, but is preferably, for example, 0.05% or more, more preferably 0.2% or more, and even more preferably 0.5% or more.
[0096] The photocatalyst layer 3 may contain the photocatalyst 30 as it is, or may contain the photocatalyst 30 supported on the surface of a catalyst carrier. When the photocatalyst layer 3 contains a catalyst carrier, the area of direct contact between the photocatalyst 30 and the polymer component can be reduced, so that deterioration of the polymer component caused by the photocatalyst 30 can be suppressed. In addition, although it may be difficult to disperse the photocatalyst 30 depending on the polymer component, the photocatalyst 30 can be easily dispersed by using an appropriate catalyst unit. The photocatalyst layer 3 preferably contains an inorganic oxide that is stable against the photocatalyst 30 as a catalyst carrier, and preferably contains one or more selected from the group consisting of silicon oxide, aluminum oxide, magnesium oxide, zirconium oxide, iron oxide, and calcium oxide.
[0097] The photocatalyst layer 3 is substantially composed of silicon oxide or siloxane polymer and the photocatalyst 30. Therefore, if the content of the photocatalyst 30 is about 10%, the remainder can be silicon oxide or siloxane polymer. However, in order to improve the design, corrosion resistance, wear resistance, catalytic function, etc. of the photocatalyst layer 3, the photocatalyst layer 3 may contain color pigments, extender pigments, catalysts other than photocatalysts, rust prevention pigments, metal powders, high-frequency loss agents, aggregates, etc. The photocatalyst layer 3 may contain, for example, oxides such as SiO2, TiO2, Al2O3, composite oxides containing two or more metal elements as constituents, metal powders such as Zn powder, Al powder, etc. The photocatalyst layer 3 may also contain non-chromate rust prevention pigments such as calcium molybdate, calcium phosphomolybdate, and aluminum phosphomolybdate. The photocatalyst layer 3 may also contain Zn-Ni ferrite as a high-frequency loss agent. The photocatalyst layer 3 may also contain potassium titanate fiber as an aggregate. The amount of these components in the photocatalyst 30 is not particularly limited, but is preferably, for example, 30% or less, more preferably 20% or less, and particularly preferably 15% or less.
[0098] The photocatalyst layer 3 contains Si as a main element, but may contain one or more elements selected from the group consisting of B, Al, Ge, Ti, Y, Zr, Nb, and Ta as other elements. In particular, Al, Ti, Nb, and Ta can complete the solidification of the film at a low temperature or in a short time when an acid is added to the system as a catalyst. When these metal-containing alkoxides are added using an acid as a catalyst, the ring-opening speed of the epoxy increases, and the film can be cured at a low temperature in a short time. The photocatalyst layer 3 preferably contains an alkoxide of Ti, such as Ti-ethoxide or Ti-isopropoxide. In addition, in a system to which Zr is added, the alkali resistance of the film is significantly improved, and therefore it is preferably used in applications where alkali resistance is particularly required.
[0099] The thickness of the photocatalyst layer 3 is preferably 0.1 μm to 3 μm, more preferably 0.1 μm to 2.5 μm, even more preferably 0.3 μm to 2 μm, and particularly preferably 1 μm to 3 μm. In this case, the photocatalytic action of the photocatalyst 30 contained in the photocatalyst layer 3 can be particularly exhibited.
[0100] The total thickness of the photocatalyst layer 3 and the intermediate protective layer 4 is preferably 5 μm or less. In this case, the processability of the coating material 1 and the adhesion of the processed portion can be improved. The total thickness of the photocatalyst layer 3 and the intermediate protective layer 4 is more preferably 4 μm or less, and particularly preferably 3 μm or less. In this case, the processability of the photocatalyst layer 3 and the intermediate protective layer 4 can be improved. The lower limit of the total thickness of the photocatalyst layer 3 and the intermediate protective layer 4 is not particularly limited, but is preferably 0.1 μm or more, and more preferably 0.3 μm or more.
[0101] The photocatalyst layer 3 can be formed, for example, by forming a coating film from a photocatalyst paint containing the above-mentioned silicon oxide or siloxane polymer and the photocatalyst 30, and then heating and curing the coating film. The photocatalyst layer 3 may be formed on the intermediate protective layer 4 after the intermediate protective layer 4 is formed, or may be formed simultaneously with the intermediate protective layer 4 by forming a coating film of a coating film for a protective layer on the covering layer 21, forming a coating film of a photocatalyst paint on the coating film, and then heating and curing the two coating films. For example, a dip coating method, a spray coating method, a bar coating method, a roll coating method, or a spin coating method can be adopted as a method for applying the photocatalyst paint. The heating conditions for the coating film of the photocatalyst paint are preferably a heat treatment for about one hour to several seconds in a temperature range of 150°C to about 400°C.
[0102] 2-1-2. Photocatalysis The photocatalytic action exerted by the coating material 1 according to the first embodiment will be described with reference to FIG.
[0103] FIG. 2 is a diagram for explaining the photocatalytic action when the photocatalytic layer 3 of the covering material 1 shown in FIG. 1 is irradiated with light. According to FIG. 2, the photocatalytic action is expressed by the light that reaches the photocatalyst 30. In addition, a part of the light irradiated to the photocatalyst layer 3 passes through the photocatalyst layer 3. The light that passes through the photocatalyst layer 3 passes through the intermediate protective layer 4 and reaches the covering layer 21. Since the covering layer 21 of this embodiment has a reflectance of 85% or more for light with a wavelength of 555 nm, the light that reaches the covering layer 21 is efficiently reflected by the covering layer 21. The light reflected by the covering layer 21 passes through the intermediate protective layer 4 and reaches the photocatalyst layer 3 again. The photocatalytic action is also expressed by the light that is reflected by the covering layer 21 and reaches the photocatalyst layer 3. That is, in the covering material 1 of this embodiment, not only the light that is directly irradiated to the photocatalyst layer 3 but also the light that passes through the photocatalyst layer 3 and is reflected by the covering layer 21 can be made to reach the photocatalyst 30. Therefore, light can efficiently reach the photocatalyst 30, and the photocatalytic action of the photocatalyst 30 can be efficiently exerted. As a result, a high photocatalytic action can be exerted from the initial stage when the photocatalyst layer 3 is irradiated with light, and this photocatalytic action can be maintained for a long period of time.
[0104] In addition, since the photocatalyst 30 of this embodiment is a visible light excitation type photocatalyst, it can exert a photocatalytic action not only by ultraviolet light with a wavelength of 380 nm or less, but also by visible light with a wavelength of 400 nm or more. Therefore, in the covering material 1 of this embodiment, it can exert a photocatalytic action not only by sunlight containing a lot of ultraviolet light, but also by light from fluorescent lamps, xenon lamps, LEDs, etc. In particular, the covering layer 21 has a high reflectance of light with a wavelength of 555 nm, and 555 nm is almost the middle of the wavelengths in the visible light region (380-750 nm), so it can efficiently reflect light in the entire visible light region. Since the photocatalyst 30 of this embodiment is a visible light excitation type photocatalyst, the wavelength region of light that the covering layer 21 is likely to reflect overlaps with the wavelength region in which the photocatalyst 30 can exert a photocatalytic action. Therefore, the photocatalytic action of the photocatalyst 30 can be exerted by the visible light that reaches the photocatalyst 30 directly and the visible light that is reflected by the coating layer 21, and a high photocatalytic action can be exerted from the initial stage when the photocatalyst layer 3 is irradiated with visible light, and the photocatalytic action can be maintained for a long period of time.
[0105] The photocatalytic action exhibited by the coating material 1 of this embodiment includes hydrophilic action, antifouling action, inactivation of bacteria or viruses, etc. In particular, in this embodiment, the inactivation action of bacteria or viruses is easily exhibited, and compared with a coating material having a photocatalytic layer on the surface of a general color steel plate, the inactivation action of bacteria or viruses can be exhibited even at an early stage, and the inactivation action can be maintained for a long period of time. This can be achieved by the coating layer 21 having a reflectance of 85% or more for light with a wavelength of 555 nm, and is more easily achieved by the photocatalyst 30 being a visible light excited photocatalyst. The photocatalytic action exhibited by the coating material 1 also includes antifouling, hydrophilicity, decomposition of organic matter, etc.
[0106] 2-2. Second embodiment 2-2-1. Composition of coating material The coating material 1 according to the second embodiment differs from the coating material 1 according to the first embodiment in that it includes a coating layer 210 instead of the coating layer 21, but otherwise has the same configuration as the coating material 1 according to the first embodiment. For this reason, in the coating material 1 of this embodiment, an intermediate protective layer 4 and a photocatalytic layer 3 are laminated in this order on a substrate 2, as shown in FIG. 3. The substrate 2 also includes a base material 20, a coating layer 210, and an undercoat layer 23 provided between the base material 20 and the coating layer 210. For this reason, in the coating material 1 of this embodiment, a photocatalytic layer 3 is provided on the coating layer 210.
[0107] The coating layer 210 of this embodiment has a reflectance of 85% or more for light with a wavelength of 555 nm, similar to the coating layer 21, but it is particularly preferable that the diffuse reflectance of light with a wavelength of 555 nm is 85% or more. In this case, light that has passed through the photocatalyst layer and reached the coating layer 210 can be diffused and reflected over a wide range of the photocatalyst layer 3. This allows a particularly high photocatalytic effect to be exhibited from the initial stage of irradiating the photocatalyst layer 3 with light.
[0108] The term "diffuse reflectance" refers to the diffuse reflectance of light with a wavelength of 555 nm, not including specular reflection, measured by an integrating sphere. This diffuse reflectance is specified as a percentage of the diffuse reflectance of a wavelength of 555 nm measured using a diffuse reflectance measuring device that uses an integrating sphere, with a reference white plate taken as 100. Examples of diffuse reflectance measuring devices include the "CM-3700d" manufactured by Minolta Co., Ltd. (now Konica Minolta Inc.) and the "AVAL265" spectrophotometer manufactured by Shimadzu Corporation. The diffuse reflectance is measured in accordance with JIS Z 8722 geometric condition c, etc., and is measured using an integrating sphere (a sphere whose inner surface is coated with white paint such as barium sulfate that almost completely diffusely reflects light) under the condition of diffuse illumination and 8° direction reception, as a percentage of the reflectance of a wavelength of 555 nm, with a reference white plate (made of barium sulfate) taken as 100. The diffuse reflectance can be measured using the SCE (specular reflection excluded) method, which is a method of measuring light by removing specular reflection. In the SCE method, regular reflected light is removed and only diffuse reflected light is measured, so that the evaluation of color and gloss is close to that by the naked eye. The upper limit of the diffuse reflectance of the coating layer 210 is 100%.
[0109] The covering layer 210 will be described in detail below.
[0110] In this embodiment, for example, the configuration of the first example or the configuration of the second example shown below can be adopted as the covering layer 210. Note that the configuration of the covering layer 210 is not limited to the configurations of the first example and the second example shown below.
[0111] (First Example) The first example of the coating layer 210 includes a binder resin and a pigment, and is therefore formed from a coating paint that includes a binder resin and a pigment.
[0112] The binder resin preferably contains a polyester resin (hereinafter, also referred to as polyester resin A) having a number average molecular weight of 19,000 or more and 28,000 or less. In the coating layer 210 of this embodiment, the pigment concentration in the coating paint is high, so the ability to bind the pigments together (binder) is excellent. It is necessary to ensure the binder ability. In this regard, by blending polyester resin A as a resin contained in the coating paint, it is possible to ensure the binder ability and improve the processability of the coating layer 210. In addition, when a polyester resin with a high number average molecular weight is used, the viscosity of the coating paint increases, and the solid content concentration in the coating paint tends to increase. In contrast, in the coating paint of this embodiment, since the pigment concentration is high and the resin concentration is relatively low, even if the number average molecular weight of the polyester resin A is within the above range, a viscosity suitable for forming a coating film can be ensured, and a coating film can be easily formed from the coating paint. Therefore, a thick coating film can be formed from the coating paint while suppressing the occurrence of popping (small bubble-like swelling or holes). Furthermore, since the number average molecular weight of the polyester resin is 19,000 or more, it is possible to impart excellent moldability to the coating material 1. Furthermore, since the number average molecular weight of the polyester resin is 28,000 or less, it is possible to ensure the scratch resistance of the coating layer 210 while imparting appropriate flexibility to the coating layer 210. The number average molecular weight of the polyester resin A is more preferably from 19,000 to 26,000, and particularly preferably from 20,000 to 23,000. The proportion of the polyester resin A relative to the total amount of the binder resin is preferably from 20% by mass to 100% by mass, more preferably from 30% by mass to 80% by mass, and particularly preferably from 40% by mass to 60% by mass.
[0113] It is also preferable that the binder resin contains a polyester resin (hereinafter, also referred to as polyester resin B) having a number average molecular weight of 2000 or more and 6000 or less and a hydroxyl value of 20 or more. In the coating layer 210 of this embodiment, it is considered that the resin is dispersed between the pigments. In this structure, by combining polyester resin A and polyester resin B, polyester resin B can enter gaps into which polyester resin A has difficulty entering. Therefore, polyester resin B functions as a binder between pigments or between pigments and polyester resin A, and can improve the strength, processability, and adhesion of the coating layer 210.
[0114] Furthermore, by having a number average molecular weight of 2000 or more, the strength of the coating layer 210 can be ensured, and the processability of the coating layer 210 can be improved. Furthermore, by having a number average molecular weight of 6000 or less, the polyester resin B can easily penetrate into the gaps between the pigments, and the adhesion of the coating layer 210 can be improved. The number average molecular weight of the polyester resin B is more preferably 2500 or more and 5000 or less, and particularly preferably 3000 or more and 4500 or less. Furthermore, by having a hydroxyl value of 20 or more, the number of crosslinking points increases, and therefore the adhesion of the coating layer 210 to the undercoat layer 23 can be improved. The hydroxyl value of the polyester resin B is more preferably 30 or more, and particularly preferably 40 or more. The upper limit of the hydroxyl value of the polyester resin B is not particularly limited, but is preferably, for example, 200 or less.
[0115] In the coating paint, the ratio of the mass of polyester resin B to the mass of polyester resin A (polyester resin B / polyester resin A) is preferably 0.25 or more and 4 or less. When this ratio is 0.25 or more, the adhesion of the coating layer 210 can be effectively improved. Furthermore, when this ratio is 4 or less, the processability of the coating layer 210 can be effectively improved. The mass ratio of polyester resin A to polyester resin B is more preferably 0.4 or more and 2.5 or less, and particularly preferably 0.65 or more and 1.5 or less.
[0116] The pigment contained in the coating paint preferably contains rutile titanium oxide. That is, it is preferable that the coating layer 210 contains rutile titanium oxide. Rutile titanium oxide has a higher refractive index than other pigments, so it is possible to increase the refractive index difference between the resin and air contained in the coating layer 210 and the rutile titanium oxide. By increasing this refractive index difference, it is possible to increase the diffuse reflectance of the coating layer 210.
[0117] The rutile titanium oxide particles may be particles alone, or may be rutile titanium oxide particles coated with silica, alumina, zirconia, zinc oxide, antimony oxide, organic substances, etc. Examples of the organic substances used for coating may include polyols such as pentaerythritol and trimethylolpropane, alkanolamines such as triethanolamine and organic acid salts of trimethylolamine, silicone resins, and silicones such as alkylchlorosilanes.
[0118] The average particle size of rutile-type titanium oxide is preferably 200 nm or more and 400 nm or less. In this case, the reflectance of the coating layer 210 can be improved, and light that has passed through the photocatalyst layer 3 and reached the coating layer 210 can be easily reflected toward the photocatalyst layer 3. In addition, light with a wavelength that easily activates the photocatalyst 30 contained in the photocatalyst layer 3 can be easily reflected by the coating layer 210. The average particle size of rutile-type titanium oxide is more preferably 250 nm or more and 350 nm or less. The average particle size of rutile-type titanium oxide is the arithmetic mean value of the particle sizes of the remaining rutile-type titanium oxides, which are obtained by observing the coating layer 210 at a magnification of 10,000 times with an electron microscope and excluding the smallest 20% and the largest 5% of the rutile-type titanium oxides projected in the field of view.
[0119] In the coating layer 210, the solid content volume concentration of the rutile titanium oxide is preferably 20% or more. In this case, even if the coating layer 210 is in a close-packed state with the rutile titanium oxide particles, the volume of the voids between the particles can be made larger than the volume of the resin. Since the refractive index of the voids is lower than the refractive index of the pigment and the refractive index of the resin, light is likely to be reflected at the interface between the pigment and the voids and at the interface between the resin and the voids. Therefore, by providing sufficient voids in the coating layer 210, the diffuse reflectance of the coating layer 210 can be improved. The solid content volume concentration of the rutile titanium oxide is more preferably 25% or more. In this case, the diffuse reflectance of the coating layer 210 can be further improved. The solid content volume concentration of the rutile titanium oxide is preferably 70% or less, more preferably 65% or less, and particularly preferably 40% or less. In this case, the strength of the coating layer 210 can be ensured, and the coating layer 210 can be prevented from becoming brittle.
[0120] The coating paint may contain a component having a larger average particle size and a lower refractive index than rutile titanium oxide (hereinafter, also referred to as a low refractive index component). In this case, the voids in the coating layer 210 can be increased, and light can be reflected at the interface with rutile titanium oxide. Therefore, the diffuse reflectance of the coating layer 210 can be effectively improved. The average particle size of the low refractive index component is preferably 1 μm or more and 10 μm or less, more preferably 3 μm or more and 8 μm or less, and more preferably 4 μm or more and 7 μm or less. The refractive index of the low refractive index component is preferably 0.5 or more lower than the refractive index of rutile titanium oxide, and more preferably 1 or more lower. The low refractive index component may contain, for example, one or more selected from the group consisting of silica, calcium carbonate, barium sulfate, zinc oxide, and resin powders such as acrylic, polyester, and PTFE. The solid content volume concentration of the low refractive index component in the coating layer 210 is 9 to 25%, and preferably 10 to 17%. In this case, the diffuse reflectance of the coating layer 210 can be improved while ensuring the workability and corrosion resistance of the coating layer 210.
[0121] The ratio of the voids in the coating layer 210 is preferably 0.02 to 1.1 times the solid content volume of the coating layer 210, more preferably 0.3 to 1.0 times, and particularly preferably 0.5 to 0.95 times. In this case, the workability and adhesion of the coating layer 210 can be ensured while improving the diffuse reflectance of the coating layer 210. The size of the voids in the coating layer 210 is, for example, 200 nm to 400 nm, and preferably 250 nm to 350 nm. In this case, the workability and corrosion resistance of the coating layer 210 can be ensured while improving the diffuse reflectance of the coating layer 210. However, since it is difficult to control the size of the voids in the coating layer 210, the size of the voids in the coating layer 210 is not particularly limited as long as extremely large voids are not generated and the diffuse reflectance of the coating layer 210 is not particularly affected.
[0122] The thickness of the coating layer 210 is preferably 5 μm or more and less than 100 μm. When the thickness of the coating layer 210 is less than 100 μm, the coating layer 210 can be prevented from becoming brittle. In terms of the finished appearance, the thickness is preferably 20 μm to 50 μm, and more preferably 25 μm to 35 μm. In this case, the light reflectance of the coating layer 210 can be improved, and the coating layer 210 can be prevented from becoming brittle, so that the strength of the coating layer 210 can be ensured. The thickness of the coating layer 210 is more preferably less than 50 μm. In this case, the occurrence of popliteal defects (small bubble-like bulges or holes) during the formation of the coating layer 210 can be prevented. The coating layer 210 is not limited to being composed of a single layer, and may be composed of multiple layers.
[0123] The center average roughness Ra of the interface between the coating layer 210 and the intermediate protective layer 4 is preferably 0.8 μm or more, more preferably 1.1 μm or more, and particularly preferably 1.6 μm or more. In this case, the adhesion between the coating layer 210 and the intermediate protective layer 4 can be improved, and the diffuse reflectance of the coating layer 210 can be improved. The center average roughness Ra of the interface between the coating layer 210 and the intermediate protective layer 4 is preferably 4 μm or more. In this case, the intermediate protective layer 4 and the photocatalyst layer 3 can be easily flattened, and the contamination resistance of the photocatalyst layer 3 can be improved. The center average roughness Ra of the interface between the coating layer 210 and the intermediate protective layer 4 can be increased, for example, by the following method. (a) The coating paint and the paint for forming the intermediate protective layer 4 are laminated in a wet state. (b) The pigment concentration of the covering layer 210 is made greater than the pigment concentration of the intermediate protective layer 4 . (c) Adding a pigment having a large average particle size to the coating layer 210. (d) Reducing the viscosity of the coating paint. (e) The difference in surface tension between the coating paint and the paint for forming the intermediate protective layer 4 must be reduced.
[0124] (Second example) The second example coating layer 210 is a coating layer with low gloss, and is preferably a matte coating layer. The second example coating layer 210 can be formed from, for example, a paint containing a resin binder containing a polyester resin and a hardener, titanium oxide, and organic polymer fine particles having an average particle size of 4 to 9 μm (hereinafter, also referred to as the second example paint).
[0125] As the polyester resin contained in the resin binder, the same components as the polyester resin contained in the undercoat layer 23 of the first embodiment can be used.
[0126] As the curing agent contained in the resin binder, the same component as the curing agent contained in the undercoat layer 23 of the first embodiment can be used, and for example, it is preferable to use the above amino resin, the above blocked isocyanate compound, etc. Furthermore, the paint of the second example may contain a component similar to the curing catalyst contained in the undercoat layer 23 of the first embodiment in order to accelerate curing.
[0127] The titanium oxide contained in the paint of the second example can be the same as the titanium oxide contained in the undercoat layer 23 of the first embodiment. The content of titanium oxide in the paint of the second example is 100 parts by mass or more and 250 parts by mass or less, and preferably 140 parts by mass or more and 190 parts by mass or less, per 100 parts by mass of the resin binder component. In this case, the finish, high diffuse reflectance, and adhesion of the coating layer 210 of the second example can be improved in a well-balanced manner.
[0128] As described above, the paint of the second example contains organic polymer fine particles having an average particle diameter of 4 to 9 μm. This allows the coating layer 210 to have low gloss and high diffuse reflectance. Examples of the organic polymer fine particles include organic polymer fine particles of urea resin type obtained by pulverizing a resin obtained by a condensation reaction between urea and an aldehyde component, and organic polymer fine particles of acrylic resin type. The organic polymer fine particles may be hollow.
[0129] The average particle diameter of the organic polymer fine particles is 4 μm or more and 9 μm or more, and preferably 5 μm or more and 8 μm or less. In this case, the finish of the coating layer 210 can be improved while improving the diffuse reflectance of the coating layer 210. The average particle diameter of the organic polymer fine particles is the median diameter (d50) value of the volume-based particle size distribution measured by a laser diffraction scattering method using a Microtrack particle size distribution measuring device (product name "MT3300", manufactured by Nikkiso Co., Ltd.).
[0130] Commercially available organic polymer microparticles include Pargopack M3 (trade name, manufactured by Lonza Japan), GR-800 (trade name, manufactured by Negami Chemical Industries, Ltd.), Techpolymer MBX-5, and Techpolymer MBX-8 (all trade names, manufactured by Sekisui Chemical Co., Ltd.).
[0131] The content of the organic polymer fine particles in the second example coating material is preferably from 10 to 30 parts by mass, more preferably from 11 to 20 parts by mass, per 100 parts by mass of the resin binder component.
[0132] The thickness of the coating layer 210 of the second example is preferably 20 μm or more and 35 μm or less, and more preferably 25 μm or more and 33 μm or less. In this case, the hiding power of the coating layer 210 can be improved, and the coating material of the second example can be easily applied uniformly without unevenness.
[0133] The coating material of the second example may contain, as necessary, a matting agent such as silica, a solvent, a leveling agent, a surface conditioner, an ultraviolet absorber, a light stabilizer, a pigment dispersant, an anti-popping agent, and the like.
[0134] Examples of the coating method for the second example paint include curtain coating, roll coating, dip coating, spray coating, etc. When the second example paint is precoated by coil coating or the like, curtain coating and roll coating are recommended from the viewpoint of economy. When applying the roll coating method, a top-feed or bottom-feed method using three rolls is recommended to maximize the uniformity of the coating surface, but in practice, a bottom-feed method using a normal two-roll system (so-called natural reverse coating, natural coating) may also be used.
[0135] The curing conditions (baking conditions) of the coating material in the second example are, for example, a maximum material temperature of 160 to 260° C. and a time of 15 to 90 seconds.
[0136] The surface of the substrate 2 to which the coating layer 210 of the second example is applied has a 60 degree specular gloss within a range of 5 to 20%, preferably 6 to 15%. In this case, it is easy to obtain a high degree of diffuse reflected light. Furthermore, the coating layer 210 of the second example can achieve a diffuse reflectance of 85% or more, preferably 88% or more, at a light wavelength of 555 nm.
[0137] 2-2-2. Photocatalysis The photocatalytic action exerted by the coating material 1 according to the second embodiment will be described with reference to FIG.
[0138] In the covering material 1 of this embodiment, as in the covering material 1 according to the first embodiment, the reflectance of the covering layer 210 at a wavelength of 555 nm is 85% or more, so that not only the light directly irradiated onto the photocatalyst layer 3 but also the light that passes through the photocatalyst layer 3 and is reflected by the covering layer 210 can reach the photocatalyst 30. Therefore, light can efficiently reach the photocatalyst 30, and the photocatalytic action of the photocatalyst 30 can be efficiently exhibited.
[0139] Furthermore, in the covering material 1 of this embodiment, the covering layer 210 has a diffuse reflectance of 85% or more for light with a wavelength of 555 nm, so that light that has passed through the photocatalyst layer 3 and reached the covering layer 210 can be diffused over a wide range toward the photocatalyst layer 3 (see FIG. 4). Therefore, light can reach the photocatalyst 30 particularly efficiently, and the photocatalytic action of the photocatalyst 30 can be particularly efficiently exerted. As a result, a particularly high photocatalytic action can be exerted from the initial stage when the photocatalyst layer 3 is irradiated with light, and this photocatalytic action can be maintained for a particularly long period of time.
[0140] Of course, the photocatalytic action exhibited by the covering material 1 of this embodiment also includes a hydrophilic action, an antifouling action, a bacterial or viral inactivation action, etc. In the covering material 1 of this embodiment, even in the early stage after the photocatalytic layer 3 is irradiated with light, the bacterial or viral inactivation action can be exhibited particularly efficiently, and this inactivation action can be maintained for a long period of time.
[0141] 3. Methods for inactivating bacteria or viruses As described above, by using the covering material 1 of the first and second embodiments, bacteria or viruses can be inactivated.
[0142] For this reason, in the method for inactivating bacteria or viruses, the photocatalyst layer 3 of the above-mentioned covering material 1 is irradiated with light to activate the photocatalyst 30, thereby inactivating the bacteria or viruses. More specifically, by irradiating the photocatalyst layer 3 with light from a light source such as sunlight, a fluorescent lamp, or an LED lamp, the photocatalyst 30 is excited, and active oxygen having strong oxidizing power is generated on the surface of the photocatalyst layer 3. This active oxygen decomposes bacteria, viruses, etc., thereby inactivating the bacteria or viruses. In addition, since the active oxygen can decompose organic matter, it can also exhibit an antifouling effect.
[0143] The bacteria and viruses that can be inactivated by the photocatalytic action of the coating material 1 include blue mold (Penicillium pinohilum), Fusarium, Staphylococcus aureus, influenza A virus, cat mosquito virus, norovirus, Bacillus anyabhattai, Aeromicrobium sp, Marmorico sp, Bacillus sp, etc. Of course, the bacteria and viruses that can be inactivated by the photocatalytic action of the coating material 1 also include bacteria and viruses other than those mentioned above.
[0144] The coating material 1 exerts a bacterial or viral inactivation effect from the initial stage when the photocatalytic layer 3 is irradiated with light. As indicators for the exertion of a bacterial or viral inactivation effect from the initial stage when the photocatalytic layer 3 is irradiated with light, for example, the following indicators are considered.
[0145] As described above, the inactivation action of bacteria or viruses is exerted by active oxygen generated on the surface of the photocatalyst layer 3. This active oxygen can decompose not only bacteria or viruses but also organic matter such as methylene blue, so the decomposition ability of methylene blue can be used as an indicator of the inactivation action of bacteria or viruses. Therefore, if the decomposition ability of methylene blue is high in the early stage of irradiating the photocatalyst layer 3 with light, it can be considered that the inactivation action of bacteria or viruses is exerted from the early stage of irradiating the photocatalyst layer 3 with light.
[0146] The resolution of methylene blue can be measured, for example, by the following method. First, a dry coating film containing methylene blue at an arbitrary concentration and having an arbitrary thickness is provided on the photocatalyst layer 3. Next, the photocatalyst layer 3 is irradiated with a UV lamp at an arbitrary illuminance and for an arbitrary time. When methylene blue is decomposed by the photocatalytic effect, the color of the dry coating film changes, so the resolution of methylene blue can be measured based on the color difference ΔE of the dry coating film before and after irradiation with the UV lamp. The method for measuring the color difference ΔE is not particularly limited, but can be measured, for example, using a spectrophotometric colorimeter (product number CM-3700d) manufactured by Konica Minolta, Inc.
[0147] In the coating material 1 of the first and second embodiments, a dried coating film of methylene blue diluted 100 times (adhesion amount 44.4 mg / m 2 ) was provided on the photocatalyst layer 3, and 10.0±0.5 W / m 2 When the coating is irradiated with ultraviolet light at an irradiation intensity of 100 nm for 1 hour, it is preferable that the percentage of the color difference (ΔE) of the dry coating film after irradiation to the color difference (ΔE0) of the dry coating film before irradiation is 30% or more.
[0148] In particular, in the coating material 1 of the second embodiment, the dried coating film of methylene blue diluted 100 times (adhesion amount 44.4 mg / m 2 ) was provided on the photocatalyst layer 3, and ultraviolet rays were irradiated at 10.0±0.5 W / m 2 When the coating is irradiated for one hour at an illuminance of 100 nm, the percentage of the color difference (ΔE) of the dry coating film after ultraviolet irradiation to the color difference (ΔE0) of the dry coating film before ultraviolet irradiation is preferably 40% or more.
[0149] In the coating material 1 of the first and second embodiments, the deposition amount was 44.4 mg / m 2 A dry coating of methylene blue of 0.0±0.5 W / m was provided on the photocatalyst layer 3. 2 When the coating is exposed to ultraviolet light for 11 hours at an irradiation intensity of 100 nm, it is preferable that the percentage of the color difference (ΔE) of the dry coating film after irradiation to the color difference (ΔE0) of the dry coating film before irradiation increases by 6% or more per hour.
[0150] In the coating material 1 of the first and second embodiments, the deposition amount was 44.4 mg / m 2 A dry coating of methylene blue of 0.0±0.5 W / m was provided on the photocatalyst layer 3. 2 When the coating is irradiated with ultraviolet light at an irradiation intensity of 11 hours, the percentage of the color difference (ΔE) of the dry coating film after irradiation to the color difference (ΔE0) of the dry coating film before irradiation is preferably 60% or more, and more preferably 70% or more. EXAMPLES
[0151] The present invention will now be described in detail with reference to examples.
[0152] (Examples 1 and 2 and Comparative Examples 1 and 2) First, a 55% Al-Zn hot-dip plated steel sheet was prepared as a substrate.
[0153] Next, the undercoat paint shown in Table 1 below was applied onto the surface of the substrate to form a coating film, and then heated at 220° C. for about 1 minute to form the undercoat layer 23. The amount of the undercoat paint applied was 12.5 μm in terms of dry film thickness.
[0154] Next, a coating paint shown in Table 1 below was applied onto the undercoat layer 23 to form a coating film, and then heated at 220°C for about 1 minute to form a coating layer. The coating amount of the coating paint was 27.5 µm in dry film thickness. The reflectance and diffuse reflectance of the surface of the coating layer for light with a wavelength of 555 nm were the values shown in Table 1 below. The reflectance and diffuse reflectance of the coating layer were measured using a spectrophotometer (CM-3700d) manufactured by Konica Minolta.
[0155] Next, a coating material for the protective layer shown in Table 1 below was applied onto the undercoat layer 23 to form a coating film, and then heated at 200° C. for about 1 minute to form an intermediate protective layer. The coating amount of the coating material for the protective layer was 1.0 μm in terms of dry film thickness.
[0156] Next, the photocatalytic paint shown in Table 1 below was applied onto the intermediate protective layer to form a coating film, and then heated at 220°C for about 1 minute to form a photocatalytic layer. The amount of the photocatalytic paint applied was 1.0 μm in dry film thickness. Through the above process, a coating material was produced.
[0157] Details of the paints shown in Table 1 below are as follows. · KPP-76: Premer paint (product number KPP-76) manufactured by Kansai Paint Co., Ltd. Contains a resin binder and titanium dioxide pigment. · KP-217: White paint manufactured by Kansai Paint Co., Ltd. (product number KP-217). KP-217 + organic polymer microparticles: A mixture of white paint (product number KP-217) manufactured by Kansai Paint Co., Ltd. and acrylic resin beads (particle size 5μm), adjusted so that the gloss level after application and drying is 10. · MX-110F: White paint manufactured by Akzo Nobel Coatings Co., Ltd. (product number MX-110F). · VCT-02BSLB: Protective paint manufactured by Toyota Tsusho Vitex Co., Ltd. It contains raw materials including alkoxysilane and a substance with photocatalytic activity. · VCTII-02BSLC: Protective paint manufactured by Toyota Tsusho Vitex Co., Ltd. It contains raw materials including alkoxysilane and a substance that has photocatalytic activity in the visible light range.
[0158] [Table 1]
[0159] (evaluation) 1. Resolution of methylene blue The coating materials of Examples 1 and 2 and Comparative Examples 1 and 2 were irradiated with sunlight for 6 hours to bring the photocatalyst layers of Examples 1, 2 and Comparative Example 1 into an excited state, except for the coating material of Comparative Example 2 which did not contain a photocatalyst layer. Next, methylene blue diluted 100 times with pure water was applied to the surface of each coating material and dried, resulting in a deposition amount of 44.4 mg / m 2 A dry coating of methylene blue was then formed. Each coating was then irradiated with ultraviolet light. The irradiation intensity of the ultraviolet light was 10.0±0.5 W / m2 After the start of UV irradiation, the color difference of each coating material was measured at regular intervals and the percentage of the initial color difference ΔE0 was calculated. The results are shown in Table 2 and Figure 5.
[0160] [Table 2]
[0161] According to Table 2 and FIG. 5, the coating material of Comparative Example 1 has a larger percentage of color difference ΔE than the coating material of Comparative Example 2. This is considered to be because the coating material of Comparative Example 2 does not have a photocatalytic layer and is difficult to decompose methylene blue. The coating materials of Examples 1 and 2 also have a larger percentage of color difference ΔE than the coating material of Comparative Example 1, and in particular, the percentage of ΔE is larger from the beginning of ultraviolet irradiation. This is considered to be because the coating materials of Examples 1 and 2 have a coating layer with high reflectance in addition to the photocatalytic layer, and therefore can efficiently exert the photocatalytic effect from the beginning of ultraviolet irradiation. The coating material of Example 1 also has a larger percentage of color difference ΔE than the coating material of Example 2 11 hours and 21 hours after ultraviolet irradiation. This is considered to be because the coating layer of Example 1 has a higher diffuse reflectance than the coating layer of Example 2, and can particularly efficiently exert the photocatalytic effect.
[0162] 2. Inactivates bacteria, mold, and viruses The inactivation effects of bacteria, mold, and viruses were measured for the coating material of Example 1, which has particularly excellent decomposition ability for methylene blue, and Comparative Example 1, which has a lower decomposition ability for methylene blue than Example 1. The inactivation effects of bacteria, mold, and viruses were also measured for some of Comparative Example 2, which does not have the decomposition ability for methylene blue because it does not have a light-colored catalyst layer. The results are shown below.
[0163] (A) Mold and fungi The bacteria and molds shown in Table 3 below were placed on the surfaces of the covering materials of Example 1 and Comparative Examples 1 and 2. Next, using a fluorescent lamp with an illuminance of 1000 lx, each covering material was irradiated with fluorescent light through a UV cut filter for 24 hours. Then, the reduction rate was calculated from the number of live bacteria before and after the light irradiation. The results are shown in Table 3 below.
[0164] [Table 3]
[0165] According to Table 3, the covering material of Comparative Example 1 has a greater reduction rate in the viable bacteria count than the covering material of Comparative Example 2. This is believed to be because the covering material of Comparative Example 1 has a photocatalyst layer, and therefore the number of mold or bacteria can be reduced by the photocatalytic effect. Also, the covering material of Example 1 has a greater reduction rate in the viable bacteria count than the covering materials of Comparative Examples 1 and 2. This is believed to be because the covering material of Example 1 has a covering layer with high reflectance and diffuse reflectance in addition to a photocatalyst layer, and therefore can efficiently exert the photocatalytic effect from the beginning of ultraviolet irradiation and maintain this photocatalytic effect for a long period of time.
[0166] (a) Influenza A virus Influenza A viruses were placed on the surface of the covering materials of Example 1 and Comparative Examples 1 and 2. Next, using a fluorescent lamp with an illuminance of 3000 lx, each covering material was irradiated with fluorescent light through a UV cut filter for 8 hours. Then, the ratio of the number of live viruses 4 hours after the start of irradiation to the number of live viruses before irradiation and the ratio of the number of live viruses 8 hours after the start of irradiation were calculated. The results are shown in Table 4 below.
[0167] [Table 4]
[0168] According to Table 4, the covering material of Comparative Example 1 has a smaller ratio of live virus count than the covering material of Comparative Example 2. This is believed to be because the covering material of Comparative Example 1 has a photocatalyst layer, and the number of viruses can be reduced by the photocatalytic effect. The covering material of Example 1 also has a smaller ratio of live virus count than the covering materials of Comparative Examples 1 and 2. This is believed to be because the covering material of Example 1 has a covering layer with high reflectance and diffuse reflectance in addition to the photocatalyst layer, so that the photocatalytic effect is efficiently exerted from the early stage of ultraviolet irradiation and this photocatalytic action is maintained for a long period of time.
[0169] (c) Nekokashiri virus The feline mosquito virus was placed on the surface of the covering material of Example 1 and Comparative Examples 1 and 2. Next, using a fluorescent lamp with an illuminance of 3000 lx, each covering material was irradiated with fluorescent light through a UV cut filter for 8 hours. Then, the ratio of the number of live viruses 8 hours after the start of irradiation to the number of live viruses before irradiation was calculated. The results are shown in Table 5 below.
[0170] [Table 5]
[0171] According to Table 5, the covering material of Comparative Example 1 has a smaller ratio of live virus count than the covering material of Comparative Example 2. This is believed to be because the covering material of Comparative Example 1 has a photocatalyst layer, and the number of viruses can be reduced by the photocatalytic effect. The covering material of Example 1 also has a smaller ratio of live virus count than the covering materials of Comparative Examples 1 and 2. This is believed to be because the covering material of Example 1 has a covering layer with high reflectance and diffuse reflectance in addition to the photocatalyst layer, so that the photocatalyst effect is efficiently exerted from the beginning of ultraviolet irradiation and this photocatalyst effect is maintained for a long period of time.
[0172] (D) Bacteria collected from soil Four types of bacteria (Bacillus anyabhattai, Aeromicrobium sp, Marmorico sp, Bacillus sp) collected from soil were placed on the surface of the covering materials of Example 1 and Comparative Example 1. Next, using a fluorescent lamp with an illuminance of 1000lx, each covering material was irradiated with fluorescent light through a UV cut filter for 16 hours. Then, the reduction rate was calculated from the number of live bacteria before and after the light irradiation. The results are shown in Table 6 below.
[0173] [Table 6]
[0174] According to Table 6, the covering material of Example 1 exhibited a large reduction rate in the viable cell count, especially in the viable cell counts of Aeromicrobium sp, Marmorico sp, and Bacillus sp. This is believed to be because the covering material of Example 1 exhibits a photocatalytic effect efficiently from the beginning of ultraviolet irradiation due to its high reflectance and diffuse reflectance, and this photocatalytic effect is maintained for a long period of time. [Explanation of symbols]
[0175] 1 Covering material 2 Base material 21 Covering layer 22 Galvanized steel sheet 3 Photocatalyst layer 4 Intermediate protective layer
Claims
1. The present invention includes a substrate, at least a part of whose surface is constituted by a coating layer having a reflectance of 85% or more for light having a wavelength of 555 nm and a diffuse reflectance of 85% or more for light having a wavelength of 555 nm, and a photocatalyst layer located on the coating layer, the coating layer includes a binder resin and a pigment, the binder resin includes a polyester resin having a number average molecular weight of 19,000 or more and 28,000 or less, The photocatalyst layer contains at least one of silicon oxide and a siloxane polymer, On the photocatalyst layer, the adhesion amount was 44.4 mg / m 2 A dry coating film of methylene blue having a reflectance of 10.0±0.5 W / m 2 When ultraviolet light was irradiated for 11 hours at an irradiation intensity of 100 nm, the color difference (ΔE 0 ) the percentage of the color difference (ΔE) of the dry coating film after irradiation with the ultraviolet light increases by an average of 6% or more per hour; Covering material.
2. The present invention includes a substrate, at least a part of whose surface is constituted by a coating layer having a reflectance of 85% or more for light having a wavelength of 555 nm and a diffuse reflectance of 85% or more for light having a wavelength of 555 nm, and a photocatalyst layer located on the coating layer, the coating layer includes a binder resin and a pigment, the binder resin includes a polyester resin having a number average molecular weight of 19,000 or more and 28,000 or less, The photocatalyst layer contains at least one of silicon oxide and a siloxane polymer, On the photocatalyst layer, the adhesion amount was 44.4 mg / m 2 A dry coating film of methylene blue having a reflectance of 10.0±0.5 W / m 2 When ultraviolet light is irradiated for 1 hour at an irradiation intensity of 100 nm, the color difference (ΔE 0 ) the percentage of the color difference (ΔE) of the dried coating film after irradiating with the ultraviolet light for 1 hour to the color difference (ΔE) of the dried coating film after irradiating with the ultraviolet light for 1 hour is 30% or more; Covering material.
3. The present invention includes a substrate, at least a part of whose surface is constituted by a coating layer having a reflectance of 85% or more for light having a wavelength of 555 nm and a diffuse reflectance of 85% or more for light having a wavelength of 555 nm, and a photocatalyst layer located on the coating layer, the coating layer includes a binder resin and a pigment, the binder resin includes a polyester resin having a number average molecular weight of 19,000 or more and 28,000 or less, The photocatalyst layer contains at least one of silicon oxide and a siloxane polymer, On the photocatalyst layer, the adhesion amount was 44.4 mg / m 2 A dry coating film of methylene blue having a reflectance of 10.0±0.5 W / m 2 When ultraviolet light was irradiated for 11 hours at an irradiation intensity of 100 nm, the color difference (ΔE 0 ) the percentage of color difference (ΔE) of the dried coating film after 11 hours of irradiation with ultraviolet light is 60% or more; Covering material.
4. The coating layer contains rutile titanium oxide. The coating material according to any one of claims 1 to 3.
5. An intermediate protective layer is provided between the coating layer and the photocatalyst layer. The coating material according to any one of claims 1 to 4.
6. The substrate includes a plated steel sheet and the coating layer provided on the plated steel sheet. The coating material according to any one of claims 1 to 5.
7. The photocatalyst layer of the coating material according to any one of claims 1 to 6 is irradiated with light to activate the photocatalyst and inactivate bacteria or viruses. A method for inactivating bacteria or viruses.
Citation Information
Patent Citations
High reflectivity surface treated plate excellent in pollution resistance
JP1999181969A
Photocatalytic colored coated article
JP2001149855A
White coating metal plate having excellent processability, light reflectivity and light reflection continuity
JP2002011827A
Method for manufacturing light reflecting material and light reflecting material
JP2003154621A
Coated base material and its manufacturing method
JP2007290294A