Metal powder for additive manufacturing and additive manufactured body
By employing metal powders with defined particle size distributions, the stability and density of additive manufacturing products are enhanced, addressing the issue of open pores and fluid leakage in existing technologies.
Patent Information
- Application Number
- JP2023188963
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-11-03
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2043-11-03
AI Technical Summary
Existing additive manufacturing technologies using metal powders with a relative density of 95% result in open pores, leading to issues such as fluid leakage in the manufactured products.
The use of metal powders with specific particle size distributions, characterized by a -63μm+45μm sieve particle size of 9% or more and a particle size D5 of 9μm or more, to stabilize the powder bed and achieve a relative density of 99% or more in the layered products.
This approach ensures the formation of a stable powder bed, resulting in high-density layered products with reduced porosity and prevents fluid leakage.
Smart Images

Figure 0007576143000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal powder for additive manufacturing and an additive manufactured product. [Background technology]
[0002] In the above technical field, Patent Document 1 discloses that when additive manufacturing is performed by forming a powder bed using a metal powder having characteristics defined by the average particle size D50 and TD (tap density), an additive manufacturing body with a relative density of 95% or more can be obtained. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-017639 Summary of the Invention [Problem to be solved by the invention]
[0004] However, at a relative density of 95%, open pores occur, which can lead to errors such as leakage when handling fluids in additive manufacturing applications. Therefore, in order to obtain high-density additive manufacturing objects with a relative density of 99% or more, it is necessary to form a more stable powder bed. An object of the present invention is to provide a technique for solving the above-mentioned problems. [Means for solving the problem]
[0005] In order to achieve the above object, the metal powder for additive manufacturing according to the present invention comprises: A metal powder for additive manufacturing containing copper as a main component, which is used for manufacturing an additive manufacturing body by an additive manufacturing method that forms a powder bed, Additive elements: Al: 0.01% by mass or more and 3.92% by mass or less; Si: 0.01% by mass or more 0.97% by mass or less, P: 0.01% by mass or more and 0.14% by mass or less, Cr: 0.01% by mass or more and 1.33% by mass or less, Fe: 0.01% by mass or more and 0.29% by mass or less, Ni: 0.06% by mass or more and 4.08% by mass or less, Zr: 0.04 Mass% or more 0.31 % by mass or less, Sn: in the range of 0.24 mass% or more and 5.09 mass% or less, Mg: in the range of 0.01 mass% or more and 0.21 mass% or less, and Zn: in the range of 0.01 mass% or more and 32.0 mass% or less, The balance is copper and unavoidable impurities, This metal powder for additive manufacturing has a -63μm+45μm sieve particle size (mass%) of 9% or more and a particle diameter D5 of 9μm or more. Another metal powder for additive manufacturing according to the present invention is This metal powder for additive manufacturing contains 50.88 mass% of the added element N, at least one of the elements Al, Si, Ti, Cr, Mn, Fe, Co, Nb, and Mo, with the remainder being nickel and unavoidable impurities, has a -63 μm+45 μm sieve particle size (mass%) of 9% or more, and a particle diameter D5 of 9 μm or more.
[0006] In order to achieve the above object, the layered object according to the present invention comprises: The above A layered object produced by a layered manufacturing method in which a powder bed is formed using a metal powder for layered manufacturing, Additive elements: Al: 0.01% by mass or more and 3.92% by mass or less; Si: 0.01% by mass or more 0.97 % by mass or less, P: 0.01% by mass or more and 0.14% by mass or less, Cr: 0.01% by mass or more and 1.33% by mass or less, Fe: 0.01% by mass or more and 0.29% by mass or less, Ni: 0.06% by mass or more and 4.08% by mass or less, Zr: 0.04 Mass% or more 0.31 % or less by mass, Sn: in the range of 0.24% by mass or more and 0.97% by mass or less, Mg: in the range of 0.01% by mass or more and 0.21% by mass or less, and Zn: in the range of 0.01% by mass or more and 32.0% by mass or less, with the remainder being copper and unavoidable impurities, The layered object has a cross-sectional area ratio of 99.0% or more, calculated by subtracting the porosity of the cross section of the layered object from 100. In order to achieve the above object, another additive manufacturing method according to the present invention is an additive manufacturing method using the above-mentioned metal powder for additive manufacturing containing nickel as a main component, the additive manufacturing method comprising forming a powder bed, The alloy contains 50.88% by mass of an additional element N, which is at least one of the elements Al, Si, Ti, Cr, Mn, Fe, Co, Nb, and Mo, with the remainder being nickel and unavoidable impurities; The cross-sectional area ratio, calculated by subtracting the porosity of the cross section of the layered product from 100, is 99.0% or more. Effect of the Invention
[0007] According to the present invention, a stable powder bed can be formed to obtain a high-density layered object with a relative density of 99% or more. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a graph showing the relationship between the particle size distribution of the average particle size D50 and the particle size D5 corresponding to the particle size distribution and the −63 μm+45 μm sieve particle size (mass %). [Diagram 2] FIG. 1 is a diagram showing the evaluation results of powder beds in the present embodiment and the comparative example. [Diagram 3] FIG. 13 is a diagram showing the relationship between the particle size D5 and the −63 μm+45 μm sieve particle size (mass%) of metal powders for additive manufacturing in the present examples and comparative examples. [Figure 4] FIG. 4 is a diagram showing the particle size distribution in each region of FIG. 3, with the value of particle size D5 plotted on the horizontal axis. [Diagram 5] FIG. 11 is a diagram showing air leakage from a cylinder as an additive manufacturing body in this example and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. However, the components described in the following embodiment are merely examples, and are not intended to limit the technical scope of the present invention.
[0010] A copper alloy powder (alloy powder containing copper as a main component) will be described as the metal powder for additive manufacturing in this embodiment. Before that, the current state of copper alloy powder for additive manufacturing will be described.
[0011] <Current status of metal powders for additive manufacturing> Patent Document 1 discloses that when additive manufacturing is performed by forming a powder bed using metal powder with properties defined by the average particle size D50 and TD (tap density), an additive manufacturing body with a relative density of 95% or more can be obtained.
[0012] However, the average particle diameter D50 represents the median value in the particle size distribution of the powder. Therefore, as shown in the particle diameter distribution 110 in Figure 1, even for powders with the same average particle diameter D50, a broad powder diameter distribution 111 with a large amount of fine and coarse powder, and a sharp powder diameter distribution 112 with almost no fine or coarse powder are expected. Therefore, since the amount of fine and coarse powder cannot be clearly determined from the value of the average particle diameter D50, the powder bed may not be stabilized even if the average particle diameter D50 is adjusted, and the relative density of the additive manufacturing object falls below 99%, which can cause problems such as errors occurring due to leakage, especially when handling fluids.
[0013] Powder size distributions 113 and 114 in FIG. 1 are intermediate between broad powder size distribution 111 and sharp powder size distribution 112, and it is believed that among these distributions, there exists a powder size distribution in which a powder bed is stably generated and the relative density of the layered object is stabilized at 99% or more.
[0014] <Metal powder for additive manufacturing according to this embodiment> The inventors focused on the particle diameter D5 (μm), which indicates the size of fine particles that inhibit the powder bed, and the -63 μm+45 μm sieve particle size (mass %), which indicates the amount of coarse powder required to form a stable powder bed by improving the flowability and density of the powder bed, as characteristics that define the powder size distribution in which a powder bed is stably generated and the relative density of the layered manufactured object is stable at 99% or more. Here, the particle diameter D5 is a value obtained by a laser diffraction method, and the 63-45 μm sieve particle size is a value obtained by the sieving test method specified in JIS Z8815:1994.
[0015] Powder size distributions 111 to 114 of powders having the same average particle size D50 value are plotted on a graph 120 in which the horizontal axis represents the particle size D5 (μm) indicating the size of fine particles, and the vertical axis represents the amount of coarse powder required to form a stable powder bed, -63 μm+45 μm sieve particle size (mass%). Based on the results of the examples and comparative examples, a particle size threshold 121 (particle size D5 is 9 μm) and a sieve particle size threshold 122 (-63 μm+45 μm sieve particle size (mass%) is 9%) were obtained to separate powder size distribution 113 in which a powder bed is stably generated and the relative density of the layered product is stabilized at 99% or more from the other powder size distributions 111, 112, and 114.
[0016] Powders with a particle size D5 smaller than 9 μm and a -63 μm+45 μm sieve particle size (mass%) of 9% or more have a broad particle size distribution like powder size distribution 111. Therefore, segregation occurs during storage of the metal powder for additive manufacturing in the additive manufacturing device, and a stable powder bed cannot be formed until the additive manufacturing is completed.
[0017] Powders with a particle size D5 of 9 μm or more and a -63 μm + 45 μm sieve particle size (mass%) of less than 9% have a sharp particle size distribution like powder size distribution 112 and good fluidity. However, the particle size is too uniform, which reduces the density of the powder bed and leads to a decrease in relative density. In addition, powders produced by atomization methods, etc. require sieving within a very narrow particle size range, which is poor in productivity.
[0018] A powder with a particle size D5 smaller than 9 μm and a -63 μm+45 μm sieve particle size (mass%) of less than 9% is a powder with a particle size distribution that has a certain balance, such as powder size distribution 114. However, the powder as a whole is pulverized into fine powder, which impairs fluidity and makes it impossible to form a powder bed in the first place.
[0019] In this way, by using a metal powder having a particle size distribution 113 in which the -63 μm+45 μm sieve particle size (mass%) is 9% or more and the particle size D5 (volume distribution) measured by laser diffraction method is controlled to be 9 μm or more, high-density (relative density of 99% or more) additive manufacturing objects can be stably obtained.
[0020] [First embodiment] As the metal powder for additive manufacturing of the first embodiment, copper powder and copper alloy powder (alloy powder containing copper as a main component) will be described.
[0021] The copper powder of this embodiment contains copper and unavoidable impurities, such as elements P and Al, at 0.01 mass % or less.
[0022] In addition, the copper alloy powder of this embodiment contains 0.01 mass% or more and 32.0 mass% or less of an additive element M (at least one of the elements Mg, Al, Si, P, Cr, Fe, Ni, Zn, Zr, Ag, and Sn), with the remainder being copper and unavoidable impurities.
[0023] The additive element M is added to improve the properties of the copper alloy powder (fluidity, etc.), the properties during additive manufacturing (laser reflectance, laser absorptance, etc.), and the properties of the additive manufactured body (mechanical properties: strength, wear resistance, toughness, etc.; physical properties: electrical conductivity, heat resistance, etc.). However, in this embodiment, conditions have been found for specifying a copper alloy powder that produces a stable powder bed and stabilizes the relative density of the additive manufactured body at 99% or more.
[0024] Each element of the additive element M is added in the following range so that the total amount of the additive element M falls within the range of 0.01 mass% or more and 32.0 mass% or less. For example, Al is in the range of 0.01 mass% or more and 3.92 mass% or less, Si is in the range of 0.03 mass% or more and 0.97 mass% or less, P is in the range of 0.01 mass% or more and 0.14 mass% or less, Cr is in the range of 0.01 mass% or more and 0.29 mass% or less, Ni is in the range of 0.06 mass% or more and 4.08 mass% or less, Zr is in the range of 0.04 mass% or more and 0.31 mass% or less, Sn is in the range of 0.24 mass% or more and 5.09 mass% or less, etc.
[0025] <Method of manufacturing copper alloy powder> The method for producing the copper alloy powder for additive manufacturing of this embodiment is not particularly limited, but a method in which powder particles are rapidly cooled and solidified from a molten state, such as a gas atomization method, a water atomization method, a centrifugal atomization method, a plasma atomization method, a plasma rotating electrode method, etc., is preferable. From the viewpoint of mass production, the gas atomization method is particularly preferable. The produced powder can be classified under predetermined classification conditions by a known classification method to adjust it to a copper alloy powder for additive manufacturing of an appropriate particle size. As a classification device for performing classification, an air classifier can be suitably used. In addition, the copper alloy powder may be subjected to mechanical milling or the like. For example, a ball mill method, a bead mill method, a planetary ball mill method, an attritor method, and a vibration ball mill method are used.
[0026] <Manufacturing method of additive manufacturing> Various known metal additive manufacturing techniques can be used to produce copper alloy additive manufacturing objects. For example, in powder bed fusion, metal powder is spread on the modeling stage using a blade or roller to form a powder layer, and then a laser or electron beam is irradiated to a predetermined position of the powder layer to sinter and melt the metal powder, repeating this process to produce an additive manufacturing object. In the metal additive manufacturing process, it is necessary to control a large number of process parameters to obtain a high-quality additive manufacturing object. In the laser-based powder bed fusion method, there are many scanning conditions, such as laser output and laser scanning speed. Therefore, in setting the optimal scanning conditions, the main parameters are adjusted using energy density, which is an index that summarizes the main parameters. Energy density E [J / mm 3 The energy density is determined by E = P / (v × s × t), where P is the laser output, V is the laser scanning speed, S is the laser scanning pitch, and T is the powder layer thickness. In the laser-based powder bed fusion method, the energy density is 150 J / mm 3 More than 450J / mm 3 The preferred energy density is 150 J / mm 3 If the energy density is less than 450 J / mm, the powder layer will not melt or will not fuse properly, resulting in defects such as voids in the laminated object. 3If the temperature exceeds 100° C., sputtering occurs, making the surface of the powder layer unstable, and defects such as voids occur in the laminated body. In the electron beam type powder bed fusion method, when the powder layer is irradiated with an electron beam, if negative charges accumulate in the powder layer and charge up, the powder will fly up in a mist-like form, causing a smoke phenomenon, which leads to poor melting. Therefore, in order to prevent charge up, a preliminary process of preheating the powder layer and pre-sintering it is necessary. However, if the preheating temperature is too high, sintering will progress and cause necking, making it difficult to remove the remaining powder from inside the laminated body after molding. For this reason, in the copper alloy powder for additive manufacturing, the preheating temperature is preferably set to 400 to 800° C. Here, the metal additive manufacturing technology using the powder bed fusion method has been exemplified, but the general additive manufacturing method for producing an additive manufacturing body using the copper alloy powder for additive manufacturing of the present invention is not limited to this, and for example, an additive manufacturing method using a directed energy deposition method may be adopted.
[0027] <Method of measuring relative density> The relative density can be measured by (1) producing an additive manufacturing body using a 3D powder additive manufacturing machine and calculating the relative density (%) as a cross-sectional area ratio obtained by subtracting the porosity of the cross section of the additive manufacturing body from 100, or (2) producing an additive manufacturing body using a 3D powder additive manufacturing machine, measuring the density of the produced additive manufacturing body by Archimedes' method, and calculating the relative density (%) with the theoretical density (density of a melted material having the same composition as the additive manufacturing body) set to 100%. In this embodiment, the method (1) was adopted.
[0028] According to this embodiment, the copper powder or copper alloy powder for additive manufacturing is (1) The amount of coarse powder required to form a high-density, stable powder bed without reducing the apparent density as a powder characteristic is specified as the "-63μm+45μm sieve particle size (mass%)" obtained by "JIS Z8815:1994 Sieving Test Method"; (2) The particle size of fine powder that affects fluidity is specified as "D5 (μm)" by the laser diffraction method. It was possible to stably form a powder bed that would enable the production of additive manufacturing objects with high relative density (99% or more).
[0029] [Second embodiment] As the metal powder for additive manufacturing of the second embodiment, nickel alloy powder (alloy powder containing nickel as the main component) will be described.
[0030] The nickel alloy powder of this embodiment contains 50.88 mass% of the additive element N (at least one of the elements Al, Si, Ti, Cr, Mn, Fe, Co, Nb, and Mo), with the remainder being nickel and unavoidable impurities.
[0031] The additive element N is added to improve the properties of the nickel alloy powder, the properties during additive manufacturing, and the properties (mechanical properties, physical properties) of the additive manufactured body. However, in this embodiment, conditions have been found to specify a nickel alloy powder that produces a stable powder bed and stabilizes the relative density of the additive manufactured body at 99% or more. Therefore, the range of the amount of each element of the additive element N to be added is not limited and can be selected appropriately.
[0032] The method for producing the nickel alloy powder, the method for producing an additive manufacturing body using the nickel alloy powder, and the method for measuring the relative density are similar to those for the copper alloy powder of the first embodiment, and therefore overlapping descriptions will be omitted.
[0033] According to this embodiment, the nickel alloy powder for additive manufacturing is (1) The amount of coarse powder required to form a high-density, stable powder bed without reducing the apparent density as a powder characteristic is specified as the "-63μm+45μm sieve particle size (mass%)" obtained by "JIS Z8815:1994 Sieving Test Method"; (2) The particle size of fine powder that affects fluidity is specified as "D5 (μm)" by the laser diffraction method. It was possible to stably form a powder bed that would enable the production of additive manufacturing objects with high relative density (99% or more).
[0034] [Other embodiments] The specification of the metal powder or alloy powder for additive manufacturing that forms a stable powder bed for obtaining a high-density additive manufacturing body with a relative density of 99% or more, with a -63 μm+45 μm sieve particle size (mass%) of 9% or more and a particle diameter D5 (μm) of 9 μm or more, is not limited to copper, nickel, or alloys thereof as shown in the above first and second embodiments. The specification of -63 μm+45 μm sieve particle size (mass%) of 9% or more and a particle diameter D5 (μm) of 9 μm or more is a general specification that does not depend on the type of metal or the type of alloy. EXAMPLES
[0035] Below, experiments were conducted on metals containing only unavoidable impurities or alloys with different main component elements, in various combinations of metals and elements, to examine the relationship between the -63μm+45μm sieve particle size (mass%) and particle diameter D5 (μm), the quality and stability of the powder bed formation, and the stable height of the relative density of the layered object. The experimental results are shown in [Tables 1A] to [Table 2B]. Here, Examples 101 to 122 and Comparative Examples 101 to 111 are the experimental results of copper powder or copper alloy powder, and Example 201 is the experimental result of nickel alloy powder.
[0036] [Table 1A] [Table 1B] [Table 2A] [Table 2B]
[0037] The quality of the powder bed formation shown in [Table 1A] to [Table 2B] (○: good, △: unstable, X: not good) was evaluated by forming a powder bed using metal powder for additive manufacturing or alloy powder for additive manufacturing, as shown in FIG. 2. In Example 110 (201 in FIG. 2), a uniform powder bed was formed (○). In Comparative Example 104 (202 in FIG. 2), powder clumps were partially generated and the powder bed was unstable (△). In Comparative Example 109 (203 in FIG. 2), a complete powder bed could not be formed and molding was not possible (X). The bold frame in [Table 2B] indicates -63 μm + 45 μm sieve particle size (mass%) or particle size D5 (μm) outside the specified range.
[0038] The relative densities of the additively manufactured objects shown in [Table 1A] to [Table 2B] were obtained by producing additively manufactured objects using a 3D powder additive manufacturing machine and calculating the relative density (%) as the cross-sectional area ratio obtained by subtracting the porosity of the cross section of the additively manufactured object from 100.
[0039] As shown in [Table 1A] to [Table 2B], in [Table 1A] and [Table 1B] (Examples 101 to 122, 201), for metals containing only unavoidable impurities or alloys with different main component elements, in various combinations of metals and elements, the -63 μm+45 μm sieve particle size (mass%) is 9% or more and the particle diameter D5 is 9 μm or more, so a high-density, stable powder bed is formed and additive manufacturing objects with a relative density of 99% or more are stably manufactured.
[0040] On the other hand, [Table 2A] and [Table 2B] show metal powders and alloy powders for various combinations of metals and elements containing only unavoidable impurities or alloys with different main component elements, in which the -63 μm+45 μm sieve particle size (mass%) was less than 9% and / or the particle size D5 was less than 9 μm, resulting in the formation of a spotty, unstable powder bed and preventing the production of an additive manufacturing object with a relative density of 99% or more.
[0041] Fig. 3 is a graph plotting the quality of the powder bed formation in [Table 1A] to [Table 2B] with particle diameter D5 on the horizontal axis and -63μm+45μm sieve particle size (mass%) on the vertical axis. As shown in Fig. 3, powder groups 311 to 314 of the powder bed formation quality and poor quality exist on the boundary of a threshold value, as in Fig. 1. Fig. 4 shows the powder diameter distribution with particle diameter D5 on the horizontal axis corresponding to powder groups 311 to 314 in Fig. 3.
[0042] 4, powders with a particle size D5 smaller than 9 μm and a −63 μm+45 μm sieve particle size (mass%) of 9% or more have a broad particle size distribution as shown by powder size distribution 311. Therefore, segregation occurs during storage of the metal powder for additive manufacturing in the additive manufacturing device, and a stable powder bed cannot be formed until the additive manufacturing is completed.
[0043] In Figure 4, a powder with a particle size D5 of 9 μm or more and a -63 μm + 45 μm sieve particle size (mass%) of less than 9% has a sharp particle size distribution like powder size distribution 312 and good fluidity. However, the particle size is too uniform, which reduces the density of the powder bed and leads to a decrease in relative density. In addition, powders produced by atomization or other methods require sieving within a very narrow particle size range, which is poor in productivity.
[0044] In Fig. 4, a powder having a particle size D5 smaller than 9 µm and a -63 µm + 45 µm sieve particle size (mass%) less than 9% is a powder with a particle size distribution that has a certain balance, such as powder size distribution 314. However, the powder as a whole is pulverized into fine powder, which impairs fluidity and makes it impossible to form a powder bed in the first place.
[0045] In this way, by using a metal powder having a particle size distribution of powder size distribution 313 in Figure 4, in which the -63 μm+45 μm sieve particle size (mass%) is 9% or more and the particle size D5 (volume distribution) measured by laser diffraction method is controlled to 9 μm or more, a high-density (relative density of 99% or more) additive manufacturing object can be stably obtained. EXAMPLES
[0046] Using the copper alloy powders of Example 110 and Comparative Example 102, cylinders with a maximum thickness of 2 mm and a minimum thickness of 1 mm were fabricated, and a leak check was performed using compressed air at 0.2 MPa. The results of the leak check using compressed air at 0.2 MPa are shown in FIG.
[0047] As shown in Fig. 5, a tube 501 having a maximum thickness of 2 mm and a minimum thickness of 1 mm was produced. Compressed air of 0.2 MPa was applied to this tube 501 to check for air leakage in water. There was no air leakage in tube 502 produced by additive manufacturing using the copper alloy powder of Example 110. On the other hand, air leakage occurred in tube 503 produced by additive manufacturing using the copper alloy powder of Comparative Example 102. It is believed that air leakage occurred because the relative density of tube 503 was in the 98% range, which resulted in open pores.
Claims
1. A metal powder for additive manufacturing containing copper as a main component, which is used for manufacturing an additive manufacturing body by an additive manufacturing method that forms a powder bed, As additive elements, at least one of Al: in the range of 0.01 mass% or more and 3.92 mass% or less, Si: in the range of 0.01 mass% or more and 0.97 mass% or less, P: in the range of 0.01 mass% or more and 0.14 mass% or less, Cr: in the range of 0.01 mass% or more and 1.33 mass% or less, Fe: in the range of 0.01 mass% or more and 0.29 mass% or less, Ni: in the range of 0.06 mass% or more and 4.08 mass% or less, Zr: in the range of 0.04 mass% or more and 0.31 mass% or less, Sn: in the range of 0.24 mass% or more and 5.09 mass% or less, Mg: in the range of 0.01 mass% or more and 0.21 mass% or less, and Zn: in the range of 0.01 mass% or more and 32.0 mass% or less, with the remainder being copper and unavoidable impurities, A metal powder for additive manufacturing, having a -63 μm + 45 μm sieve particle size (mass%) of 9% or more and a particle diameter D5 of 9 μm or more.
2. A metal powder for additive manufacturing containing nickel as a main component, which is used for manufacturing an additive manufacturing body by an additive manufacturing method that forms a powder bed, A metal powder for additive manufacturing, containing 50.88% by mass of an added element N, at least one of the elements Al, Si, Ti, Cr, Mn, Fe, Co, Nb, and Mo, with the remainder being nickel and unavoidable impurities, having a -63 μm + 45 μm sieve particle size (mass %) of 9% or more, and a particle diameter D5 of 9 μm or more.
3. The -63 μm + 45 μm sieve particle size (mass%) is a value obtained by a sieving test method defined in JIS Z8815:1994, and the particle diameter D5 is a value obtained by a laser diffraction method. The metal powder for additive manufacturing according to claim 1 or 2.
4. 2. A layered object produced by a layered manufacturing method in which a powder bed is formed using the metal powder for layered manufacturing according to claim 1, As additive elements, at least one of Al: in the range of 0.01 mass% or more and 3.92 mass% or less, Si: in the range of 0.01 mass% or more and 0.97 mass% or less, P: in the range of 0.01 mass% or more and 0.14 mass% or less, Cr: in the range of 0.01 mass% or more and 1.33 mass% or less, Fe: in the range of 0.01 mass% or more and 0.29 mass% or less, Ni: in the range of 0.06 mass% or more and 4.08 mass% or less, Zr: in the range of 0.04 mass% or more and 0.31 mass% or less, Sn: in the range of 0.24 mass% or more and 0.97 mass% or less, Mg: in the range of 0.01 mass% or more and 0.21 mass% or less, and Zn: in the range of 0.01 mass% or more and 32.0 mass% or less, with the remainder being copper and unavoidable impurities, An additive manufacturing object having a cross-sectional area ratio of 99.0% or more, calculated by subtracting the porosity of the cross section of the additive manufacturing object from 100.
5. 3. A layered object produced by a layered manufacturing method in which a powder bed is formed using the metal powder for layered manufacturing according to claim 2, The alloy contains 50.88% by mass of an additional element N, which is at least one of the elements Al, Si, Ti, Cr, Mn, Fe, Co, Nb, and Mo, with the remainder being nickel and unavoidable impurities; An additive manufacturing object having a cross-sectional area ratio of 99.0% or more, calculated by subtracting the porosity of the cross section of the additive manufacturing object from 100.
Citation Information
Patent Citations
Magnesium alloy powder
JP2019056140A
Cu-BASED ALLOY POWDER
JP2021017639A
Copper alloy powder, layered / molded product, method for producing layered / molded product, and various metal parts
JP2023106573A
Cited By
Metal powder for additive manufacturing, and additively manufactured object
WO2025095041A1
Copper alloy mixed powder and method for evaluating same
WO2026094185A1