Accelerated evaluation method for anodes
An accelerated evaluation method for anodes in water electrolysis systems simulates renewable energy fluctuations by combining constant current and potential cycles with linear sweep voltammetry, effectively assessing durability and enhancing stability under variable power conditions.
Patent Information
- Application Number
- JP2020193246
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-20
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-11-20
AI Technical Summary
Existing methods are inadequate for rapidly evaluating the durability of anodes used in water electrolysis under conditions of large output fluctuations, such as those encountered with renewable energy sources, leading to performance deterioration.
An accelerated evaluation method involving repeated cycles of applying a constant oxidation current and maintaining a constant potential, combined with linear sweep voltammetry and optional open circuit potential holding, simulates the effects of renewable energy fluctuations to assess anode durability.
This method allows for rapid and accurate evaluation of anode durability under conditions mimicking renewable energy, extending the lifespan and stability of anodes in water electrolysis systems.
Smart Images

Figure 0007576260000001 
Figure 0007576260000002 
Figure 0007576260000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an accelerated evaluation method for an anode used in, for example, water electrolysis. [Background technology]
[0002] Hydrogen is suitable for storage and transportation, and is a secondary energy with a small environmental impact, so hydrogen energy systems that use hydrogen as an energy carrier are attracting attention. Currently, hydrogen is mainly produced by steam reforming of fossil fuels. However, from the perspective of global warming and the problems of fossil fuel depletion, it is important to produce hydrogen by water electrolysis using renewable energy such as solar power and wind power, among other fundamental technologies. Water electrolysis is low-cost and suitable for large-scale production, making it a promising technology for hydrogen production.
[0003] Currently, practical water electrolysis can be broadly divided into two types. One is alkaline water electrolysis, in which a highly concentrated alkaline aqueous solution is used as the electrolyte. The other is solid polymer water electrolysis, in which a solid polymer membrane (SPE) is used as the electrolyte. For large-scale hydrogen production by water electrolysis, it is said that alkaline water electrolysis, which uses inexpensive materials such as nickel and other iron-based metals, is more suitable than solid polymer water electrolysis, which uses electrodes that use large amounts of expensive precious metals. Recently, development of water electrolysis using anion exchange membranes has also progressed. In the case of water electrolysis using anion exchange membranes, the same electrode materials as those used in alkaline water electrolysis can be used.
[0004] High-concentration alkaline aqueous solutions become more conductive as the temperature rises, but they also become more corrosive. For this reason, the upper limit of the operating temperature is limited to around 80 to 90°C. Through the development of materials for the electrolysis cell and various piping materials that can withstand high temperatures and high-concentration alkaline aqueous solutions, as well as the development of low-resistance diaphragms and electrodes with enlarged surface areas and catalysts, the electrolysis performance has improved to a current density of 0.3 to 0.4 Acm. -2 The output voltage has improved to about 1.7 to 1.9 V (efficiency 78 to 87%).
[0005] Nickel-based materials that are stable in highly concentrated alkaline aqueous solutions are used as anodes for alkaline water electrolysis, and it is known that nickel-based anodes have a lifespan of several decades or more in alkaline water electrolysis using a stable power source. However, when renewable energy is used as the power source, harsh conditions such as frequent start-stops and load fluctuations are often encountered, and the performance degradation of nickel-based anodes is an issue.
[0006] Both the nickel oxide production reaction and the reduction reaction of the produced nickel oxide proceed on the metal surface. Therefore, these reactions promote the detachment of the electrode catalyst formed on the metal surface. When the power supply for electrolysis is stopped, the electrolysis stops and the nickel-based anode is maintained at a potential lower than the oxygen evolution potential (1.23 V vs. RHE) and higher than the counter electrode, the cathode for hydrogen generation (0.00 V vs. RHE). In the electrolysis cell, electromotive forces are generated by various chemical species, and the anode potential is maintained low as the cell reaction proceeds, promoting the reduction reaction of nickel oxide.
[0007] In the case of an electrolysis stack in which a plurality of cells, such as an anode chamber and a cathode chamber, are combined, the current generated by the cell reaction leaks through the piping connecting the cells. As a measure to prevent such current leakage, for example, there is a method of continuing to flow a small current when the operation is stopped. However, in order to continue to flow a small current when the operation is stopped, special power supply control is required, and oxygen and hydrogen are constantly generated, which results in excessive effort in operation and management. In addition, in order to intentionally avoid a reverse current state, it is possible to prevent the cell reaction by draining the electrolyte immediately after stopping, but this is not considered to be an appropriate measure when operation with electricity with large output fluctuations such as renewable energy is assumed.
[0008] Conventionally, platinum group metals, platinum group metal oxides, valve metal oxides, iron group oxides, lanthanide group metal oxides, etc. have been used as catalysts (anode catalysts) for oxygen generation anodes used in alkaline water electrolysis. Other anode catalysts include nickel-based alloys such as Ni-Co and Ni-Fe; nickel with expanded surface area; spinel-based Co 3 O 4 , NiCo 2 O 4 , the perovskite-based LaCoO 3 , LaNiO 3 Conductive oxides (ceramic materials) such as those mentioned above; oxides of precious metals; and oxides of lanthanide metals and precious metals are also known.
[0009] As an oxygen generating anode used in high-concentration alkaline water electrolysis, an anode in which a lithium-containing nickel oxide layer is formed in advance on the surface of a nickel substrate is known (Patent Documents 1 and 2). In addition, an anode for alkaline water electrolysis in which a lithium-containing nickel oxide catalyst layer containing lithium and nickel at a predetermined molar ratio is formed on the surface of a nickel substrate (Patent Document 3) and an anode for alkaline water electrolysis in which a catalyst layer containing a nickel-cobalt oxide and an iridium oxide or ruthenium oxide is formed on the surface of a nickel substrate (Patent Document 4) have been proposed. However, even the anodes proposed in Patent Documents 1 to 4 tend to degrade in performance when power with large output fluctuations such as renewable energy is used as the power source, making it difficult to use them stably for a long period of time. For this reason, there is a demand for the development of an anode that can be used stably for a longer period of time even when power with large output fluctuations is used as the power source.
[0010] Since the service life of an electrode is 5 to 10 years, it was practically impossible to spend such a long time on the development and evaluation of electrodes. Therefore, a method for simulating actual electrolysis conditions such as alkaline water electrolysis and reproducing actual deterioration in a shorter time to evaluate anodes and anode catalysts in an accelerated manner is extremely important for developing anodes and anode catalysts as well as for quality control.
[0011] To date, methods that have been used to evaluate the durability of anode catalysts include using cyclic voltammetry or cyclic galvanograms multiple times in succession (Non-Patent Documents 1 and 2) and investigating using fluctuating currents such as sine waves (Non-Patent Document 3). Also, a test method has been proposed in which an appropriate potential interval is repeatedly operated to select non-precious metal catalysts (Patent Document 5). Furthermore, an accelerated test has been proposed in which a very large current is passed for a long period of time (Patent Document 6).
[0012] On the other hand, it has been reported that when the potential becomes more negative than the open circuit potential after the completion of the water electrolysis reaction, an electrochemical reduction reaction of the anode occurs on the surface, and the repeated transitions between reducing and oxidizing conditions accelerate the dissolution and peeling of the catalyst (Non-Patent Documents 4 and 5). [Prior art documents] [Patent documents]
[0013] [Patent Document 1] UK Patent Application Publication No. 864457 [Patent Document 2] U.S. Patent No. 2,928,783 [Patent Document 3] JP 2015-86420 A [Patent Document 4] JP 2017-190476 A [Patent Document 5] US Patent Application Publication No. 2016 / 199821 [Patent Document 6] U.S. Pat. No. 4,498,962 [Non-patent literature]
[0014] [Non-Patent Document 1] D.Delgado, F.Bizzotto, A.Zana, and M.Arenz, Chem. Phys. Chem., 2, 3147-3153(2019) [Non-Patent Document 2] Tsukada, Y; Kuroda, Y; Niiro, H; Fujii, Y; Fujimoto, N; Mitsushima, S; Electrochimica Acta (20200901), 353, pp.136544 [Non-Patent Document 3] Z.Dobo and ABPalotas, Int. J. Hydrogen Energy, 42, 5649-5656(2017) [Non-Patent Document 4] M.Bernt et al., Chemie Ing.Tech., 93, 31-39(2020) [Non-Patent Document 5] A. Weis et al., J. Electrochem. Soc., 166, F487-F497(2019) Summary of the Invention [Problem to be solved by the invention]
[0015] However, all of the evaluation methods used to date have been insufficient for accelerated evaluation of the durability of anodes powered by electricity with large output fluctuations, such as renewable energy sources. In other words, the current situation is that no practical method has been found to accelerate evaluation of the lifespan of anodes for water electrolysis, etc., by imitating the intermittent characteristics of renewable energy sources with large output fluctuations.
[0016] The present invention has been made in consideration of the problems of the conventional technology. The object of the present invention is to emulate electric power with large output fluctuations such as renewable energy, and to accurately evaluate the durability of an anode that uses such electric power with large output fluctuations as a power source in a short period of time. do The present invention provides an accelerated evaluation method for an anode, which enables the above-mentioned. [Means for solving the problem]
[0017] As a result of intensive research into solving the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by repeatedly applying a step of a constant density current and a step of maintaining a constant potential multiple times, and thus completed the present invention.
[0018] That is, according to the present invention, there is provided the following accelerated evaluation method for an anode. [1] A method for accelerating evaluation of the durability of an anode by electrochemically operating the anode in an aqueous electrolyte for a duration T e at 0.1A / cm 2 An oxidation current of J or more is applied to the anode. e Step and duration T min The anode is held at a constant potential lower than the open circuit potential at E min and e Step and E min An accelerated evaluation method for anodes in which each step is repeated more than 100 times. [2] The duration T e and the duration T min The accelerated evaluation method for an anode according to the above [1], wherein each of the above times is 120 s or less. [3] Said J e Step and min During the step, e The accelerated evaluation method for an anode according to [1] or [2], further comprising an LSV step of subjecting the anode to linear sweep voltammetry starting from a potential lower than the potential at the end of the step, wherein the scan rate SR of the linear sweep voltammetry is in the range of 50 to 500 mV / s. [4] Said J e The accelerated evaluation method for an anode according to [3], further comprising an OCP step between the LSV step and the LSV step, in which the anode is held at an open circuit potential, and the holding time at the open circuit potential is 10 to 60 s. [5] E. min The method for accelerated evaluation of an anode according to any one of [1] to [4] above, wherein in the step, the anode is held at a potential 0.6 to 1.0 V lower than the open circuit potential. [6] The method for accelerated evaluation of an anode according to any one of [1] to [5] above, wherein the anode is an oxygen generating electrode. Effect of the Invention
[0019] According to the present invention, it is possible to provide an accelerated anode evaluation method that can mimic electricity with large output fluctuations, such as renewable energy, and accurately evaluate the durability of an anode that is powered by such electricity with large output fluctuations in a shorter period of time. [Brief description of the drawings]
[0020] [Figure 1] 1 is a graph showing an embodiment of a method for accelerated evaluation of an anode of the present invention. [Diagram 2] 4 is a graph showing another embodiment of the accelerated evaluation method of an anode of the present invention. [Diagram 3] 1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 1. [Figure 4] 1 is a graph showing polarization curves at a holding potential of 0.5 V vs. RHE ((a)) and at a holding potential of 0.7 V vs. RHE ((b)) in Example 1. [Diagram 5] 1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 1. [Figure 6] 1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 2. [Figure 7] 13 is a graph showing polarization curves at durations Tmin of 10 s and 60 s in Example 2. [Figure 8] 1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 2. [Figure 9] 1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 3. [Figure 10]1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 3. [Figure 11] 1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 4. [Figure 12] 13 is a graph showing polarization curves at durations Tmin of 10 s and 60 s in Example 4. [Figure 13] 1 is a graph plotting electrode potential at an oxidation current of 0.1 A / cm2 versus cycle number in Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The accelerated evaluation method for an anode of the present invention (hereinafter, also simply referred to as the "evaluation method") is a method for evaluating the durability of an anode, such as an anode for alkaline water electrolysis (oxygen generating electrode), in an accelerated manner by electrochemical operation in an aqueous electrolyte. e at 0.1A / cm 2 Applying an oxidation current of J or more to the anode e Step and duration T min The anode is held at a constant potential lower than the open circuit potential at E min Step 3: e Step and E min Each step is repeated at least 100 times. The evaluation method of the present invention will be described in detail below.
[0022] The evaluation method of the present invention is a method for accelerated evaluation of the durability of an anode powered by electricity such as renewable energy, whose output fluctuates in a complex manner, and is mainly composed of a steady-state operation under an oxidation current and a low potential control that is reached when no power is supplied. FIG. 1 is a graph showing one embodiment of the accelerated evaluation method of an anode of the present invention. In the evaluation method of the embodiment shown in FIG. 1, the evaluation cycle is performed in an alkaline aqueous solution at room temperature to 100° C. for a duration T e 0.6A / cm 2 The oxidation current for water electrolysis is applied to the anode. eStep is then performed for duration T min Hold the anode at a constant potential lower than the open circuit potential at E min Steps are then carried out. e Step and E min Repeat each step at least 100 times.
[0023] Duration T e and duration T min are preferably set to 120 s (2 min) or less, more preferably set to 90 s or less, particularly preferably set to 60 s or less, and most preferably set to 45 s or less. If the time is longer than 120 s (seconds), the time required for evaluation becomes excessively long, and even if the time is longer than that, an increase in the rate of deterioration of the anode is not expected. min In the step, it is preferable to hold the anode at a potential 0.6 to 1.0 V less noble than the open circuit potential. If the anode is held at a potential more noble than this range, the degradation rate is likely to decrease. On the other hand, if the anode is held at a potential more noble than the above range, excessive reduction of the catalyst may be induced or hydrogen may be generated. For this reason, the degradation behavior may differ slightly from that in actual operation.
[0024] As shown in Figure 1, e Step and E min During the steps, J e It is preferable to further include an LSV step in which linear sweep voltammetry (LSV) is performed starting from a potential lower than the potential at the end of the step. This makes it possible to more appropriately simulate the actual fluctuation state of power with large output fluctuations such as renewable energy. Note that LSV is usually started from a potential near the open circuit potential ("1.5V" in FIG. 1). The scan rate SR of LSV is preferably in the range of 50 to 500 mV / s. If the scan rate SR is too slow, deterioration will accelerate, but the entire evaluation method may take longer, and power fluctuations that are unlikely to occur in reality may occur. On the other hand, if the scan rate SR is too fast, the significance of providing the LSV step may be lost.
[0025] FIG. 2 is a graph showing another embodiment of the accelerated evaluation method of the anode of the present invention. As shown in FIG. e It is preferable to further include an OCP step between the LSV step and the LSV step, in which the anode is held at an open circuit potential. By further providing an OCP step, it is possible to more appropriately simulate the actual fluctuation state of power with large output fluctuations, such as renewable energy. In the OCP step, it is preferable that the holding time for holding the open circuit potential is 10 to 60 s. If the holding time is too short, it may be difficult to obtain the effect of maintaining the open circuit potential. On the other hand, if the holding time is too long, the significance of providing the OCP step may be lost.
[0026] J e Step and E min The number of repetitions (number of cycles) of each step depends on the type of anode to be evaluated, but is 100 or more and preferably 10,000 or less. In addition, it is preferable to set the time of each step so that the total time required for the evaluation is about several hours to several hundred hours.
[0027] (anode) Next, an anode for alkaline water electrolysis will be described as an example of the anode to be evaluated. The anode for alkaline water electrolysis (hereinafter also simply referred to as "anode") includes, for example, a conductive substrate, an intermediate layer optionally formed on the surface of the conductive substrate, and a catalyst layer formed on the surface of the intermediate layer.
[0028] The conductive substrate is a conductor for passing electricity for electrolysis and is a member having a function as a carrier for supporting the intermediate layer and the catalyst layer. At least the surface of the conductive substrate (the surface on which the intermediate layer and the catalyst layer are formed) is made of nickel or a nickel-based alloy. That is, the conductive substrate may be entirely made of nickel or a nickel-based alloy, or only the surface may be made of nickel or a nickel-based alloy. Specifically, the conductive substrate may be one in which a coating of nickel or a nickel-based alloy is formed on the surface of a metal material such as iron, stainless steel, aluminum, or titanium by plating or the like.
[0029] The thickness of the conductive substrate is preferably 0.05 to 5 mm. The shape of the conductive substrate is preferably a shape having an opening for removing bubbles such as generated oxygen and hydrogen. For example, expanded mesh or porous expanded mesh can be used as the conductive substrate. When the conductive substrate has a shape with an opening, the aperture ratio of the conductive substrate is preferably 10 to 95%.
[0030] The catalyst layer is a layer having catalytic ability formed on the surface of the conductive substrate or on the surface of the intermediate layer. By interposing the intermediate layer, the catalyst layer is more firmly fixed on the conductive substrate. The type of catalyst contained in the catalyst layer is not particularly limited, and a catalyst having a catalytic ability according to the purpose can be selected and used. Specific examples of the catalyst include nickel cobalt spinel oxide (NiCo 2 O 4 ), lanthanoid nickel cobalt perovskite oxide, iridium oxide, ruthenium oxide, and lithium nickel cobalt oxide, etc. The lanthanoid nickel cobalt perovskite oxide is represented by the structural formula: XNi a Co 1-a O 3 (X represents at least one metal of lanthanum, cerium, and praseodymium, and 0 < a < 1).
[0031] The catalyst layer may be formed of one type of catalyst or may be formed of multiple types of catalysts. When multiple types of catalysts are used, multiple types of catalysts can be mixed to form one catalyst layer. In addition, multiple catalyst layers may be stacked to form a catalyst-type catalyst layer. When a stacked catalyst layer is used, each layer may be formed of one type of catalyst or each layer may be formed of multiple types of catalysts. For example, after a first layer made of lithium nickel oxide or nickel cobalt spinel oxide is formed on an intermediate layer, a second layer made of iridium oxide may be stacked on the first layer. The thickness and density of the catalyst layer are not particularly limited and may be appropriately set according to the use of the anode.
[0032] The anode can be manufactured by forming an intermediate layer, if necessary, on the surface of a conductive substrate, and then forming a catalyst layer. The catalyst layer can be formed, for example, by a pyrolysis method, electroplating, sputtering, ion plating, plasma spraying, etc. Hereinafter, a method for manufacturing an anode will be described using a method for forming a catalyst layer by a pyrolysis method as an example.
[0033] Before forming the catalyst layer, it is preferable to perform a chemical etching treatment on the conductive substrate in advance in order to remove contaminant particles such as metals and organic matter from the surface. The amount of wear of the conductive substrate due to the chemical etching treatment is 30 g / m 2 More than 400g / m 2 It is preferable that the surface of the conductive substrate is roughened in advance in order to increase the adhesion to the intermediate layer and the catalyst layer. Examples of the roughening method include blasting with powder, etching with an acid soluble in the substrate, and plasma spraying.
[0034] A precursor aqueous solution containing desired metal ions is applied to the surface of the conductive substrate that has been chemically etched. Examples of the application method include brush application, roller application, spin coating, and electrostatic coating. Next, if necessary, the conductive substrate to which the aqueous solution has been applied is dried. The drying temperature is preferably set to a temperature (for example, about 60 to 80° C.) that avoids rapid evaporation of the solvent.
[0035] Next, the conductive substrate with the aqueous precursor solution applied on its surface is heat-treated. This allows the catalyst layer to be formed on the surface of the conductive substrate. The heat treatment temperature can be set appropriately. Considering the decomposition temperature of the precursor and production costs, the heat treatment temperature is preferably 450 to 600°C, more preferably 450 to 550°C. For example, the decomposition temperature of lithium nitrate is about 430°C, and the decomposition temperature of nickel acetate is about 373°C. By setting the heat treatment temperature at 450°C or higher, each component can be decomposed more reliably. If the heat treatment temperature is set to more than 600°C, the oxidation of the conductive substrate is likely to proceed, and the electrode resistance may increase, leading to an increase in voltage loss. The heat treatment time may be set appropriately in consideration of the reaction rate, productivity, oxidation resistance of the catalyst layer surface, etc.
[0036] By appropriately setting the number of times the precursor aqueous solution is applied, the thickness of the catalyst layer to be formed can be controlled. The application and drying of the aqueous solution may be repeated for each layer, and the entire layer may be heat-treated after the top layer is formed, or the application and heat treatment (pretreatment) of the aqueous solution may be repeated for each layer, and the entire layer may be heat-treated after the top layer is formed. The temperature of the pretreatment and the temperature of the overall heat treatment may be the same or different. In addition, it is preferable that the time of the pretreatment is shorter than the time of the overall heat treatment. EXAMPLES
[0037] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following examples, an electrochemical cell (volume: 5 L) made of polytetrafluoroethylene (PTFE) was used. This electrochemical cell has three electrodes, using the evaluation target (anode) as the working electrode, the RHE as the reference electrode, and a spiral nickel wire as the counter electrode. The surface area of the working electrode is 1.0 cm 2The working electrode was connected to a Ni wire shielded with a heat shrink tube. The distance between the Luggin capillaries of the working electrode and the reference electrode was fixed to within approximately 1 cm. The counter electrode was placed in a cylindrical neutral diaphragm to prevent the hydrogen generated from diffusing into the electrolyte in the cell. The electrolyte was a 7.0 mol / L KOH aqueous solution. The electrolyte temperature was maintained at 80°C and 25°C during pretreatment (electrochemical activation) and accelerated evaluation, respectively. A Bio-Logic SAS potentiostat (model: VSP-300) controlled by dedicated software (EC-Lab V11.30) was used for electrochemical operation. For electrochemical pretreatment, the anode to be evaluated was used, and the anode was charged at 80°C for 2 hours at 1.0 A / cm. 2 Water electrolysis was carried out at a constant current of .
[0038] (Manufacturing anodes for alkaline water electrolysis) Nickel nitrate and cobalt nitrate were dissolved in pure water to obtain a coating solution with a nickel (Ni):cobalt (Co) molar ratio of Ni:Co=33.3:66.7. The obtained coating solution was applied to a substrate with a metal amount of 1 g / m 2 The coating solution was applied to the surface of a nickel substrate that had been surface-treated so as to obtain a catalyst layer (composition: NiCo) on the surface of the nickel substrate. The coating solution was then dried at room temperature for 10 minutes and at 60°C for 10 minutes. The coating solution was then thermally decomposed in an air-circulating electric furnace for 15 minutes at 350°C. The process from coating to thermal decomposition was repeated four times to form a catalyst layer (composition: NiCo) on the surface of the nickel substrate. 2 O 4 The amount of metal in the formed catalytic layer was 4 g / m. 2 It was.
[0039] Example 1 E min Step Impact: As shown in Figure 1, in order to simulate the actual fluctuations of electricity from renewable sources, e Step and E min During the steps, J eThe potential at the end of the step was held at 1.5 V vs. RHE, and an LSV step was performed from that potential at a scan rate of 500 mV / s. min = 0.3, 0.5, and 0.7 V, and the duration of this step T min The oxidation current was 0.1 A / cm for the number of cycles. 2 A graph plotting the electrode potential at 1000 V is shown in Fig. 3. The electrode potential values in Fig. 3 were calculated from the polarization curve (sweep rate: 5 mV / s) shown in Fig. 4.
[0040] As shown in Figure 3, E min At E = 0.3 V and 0.5 V, the change (deterioration) in the electrode potential was almost the same. min At E = 0.7 V, degradation is slower, and min As the value of J becomes more noble, the stress on the anode is reduced. As shown in Figure 5, the deterioration behavior of the electrode is e Based on the anode potential at each step, the electrode can be divided into three main regions: Region A, where the electrode shows stable catalytic performance, Region B, where the electrode rapidly deteriorates, and Region C, where the performance of the degraded catalyst becomes equivalent to that of the nickel substrate. Surface observation by SEM confirmed the consumption of the catalyst in the anode that had reached Region C.
[0041] Example 2 E min Step duration T min Impact: As shown in Figure 1, min The holding potential at the step (E min ) is fixed at 0.5V and duration T min The evaluation was carried out by changing only the oxidation current of 0.1 A / cm against the number of cycles. 2 A graph plotting the electrode potential at 1000 V is shown in Fig. 6. The electrode potential values in Fig. 6 were calculated from the polarization curve (sweep rate: 5 mV / s) shown in Fig. 7.
[0042] As shown in Figure 7, the duration T min If the duration is set to 60s, T minIt was observed that the deterioration progressed faster when the duration T min When the time t is set to 10 s, region A becomes much wider, and stable activity is maintained for more cycles. When the potential becomes more negative than the open circuit potential after the water electrolysis reaction is completed, it is assumed that an electrochemical reduction reaction occurs on the anode surface, causing degradation reactions of the electrode catalyst, such as dissolution and detachment. This degradation reaction is called E min Not only the holding potential of the step but also the duration T min It is also clear that it strongly depends on
[0043] Example 3 Effect of scan rate SR on LSV step: As shown in Figure 1, min The holding potential at the step (E min ) to 0.5V and duration T min The scan rate SR of the LSV step was changed while the time was fixed at 60 s. The oxidation current was 0.1 A / cm 2 Graphs plotting the electrode potential at 1000 mV / s are shown in Figures 9 and 10. Of the scan rates SR of 50 mV / s and 500 mV / s, the electrode showed better durability at 500 mV / s. Also, as shown in Figure 10, when the scan rate SR was 50 mV / s, region B appeared at a low cycle number. Thus, it is clear that slowing down the scan rate SR accelerates the progression of the deterioration reaction on the anode surface.
[0044] From the results of Examples 1 and 2, J e Step and E min We found the existence of a phenomenon in which the degradation of the electrode catalyst, such as dissolution and detachment, is accelerated depending on the number of cycles of the step. In addition, from the results of Example 3, we found the existence of a phenomenon in which the degradation reaction of the electrode catalyst is easily promoted by slowing down the scan rate SR of the LSV step, and the durability is significantly reduced. In other words, we confirmed that the scan rate SR of the LSV step is an effective factor for acceleration evaluation.
[0045] Example 4 Impact of OCP step: As shown in Figure 2, e Between the LSV step and the OCP step, an OCP step was further provided in which the anode was held at an open circuit potential. min The holding potential of the step is 0.5 V and the duration is T min The oxidation current was 0.1 A / cm2 versus the number of cycles. 2 A graph plotting the electrode potential at 2000 s is shown in Fig. 11. The electrode potential values in Fig. 11 were calculated from the polarization curve (sweep rate: 5 mV / s) shown in Fig. 12.
[0046] As shown in FIG. 11, it is clear that the interval between OCP steps has a significant effect on improving the durability of the electrode. Also, as shown in FIG. 13, it is clear that the range (area A) in which the anode exhibits stable catalytic activity is clearly expanded, and that the presence of the OCP step significantly reduces the rate of progression in the subsequent area (area B). In Example 4, a phenomenon was found in which the durability of the electrode catalyst is significantly improved by providing an OCP step. Although the reason for this is not entirely clear, it is believed that by maintaining an open circuit, the J e The structural changes in the catalyst layer that occurred during the step are alleviated and restored, and the E min It is speculated that the progression of deterioration at the step was suppressed. Since this phenomenon may occur in an actual device, by providing an OCP step, it is possible to establish an accelerated durability evaluation method that is more suited to the actual device. [Industrial Applicability]
[0047] INDUSTRIAL APPLICABILITY The accelerated evaluation method for an anode of the present invention is useful, for example, as a method for accelerated evaluation of an anode for alkaline water electrolysis, such as an oxygen generating electrode, which uses as a power source electric power with large output fluctuations, such as renewable energy.
Claims
1. A method for accelerated evaluation of the durability of an anode by electrochemically operating the anode in an aqueous electrolyte, comprising: Duration T e 0.1 A / cm 2 A constant density oxidation current of J or more is applied to the anode. e Steps and Duration T min The anode is held at a constant potential lower than the open circuit potential E min and Said J e Step and E min An accelerated evaluation method for an anode in which each step is repeated 100 times or more.
2. The duration T e and the duration T min 2. The method for accelerated evaluation of an anode according to claim 1, wherein each of the above times is 120 seconds or less.
3. Said J e Step and E min During the step, e The method further includes a LSV step of subjecting the anode to linear sweep voltammetry starting from a potential less noble than the potential at the end of the step; 3. The method for accelerated evaluation of an anode according to claim 1, wherein a scan rate SR of the linear sweep voltammetry is in the range of 50 to 500 mV / s.
4. Said J e and an OCP step between the LSV step and the LSV step, which holds the anode at an open circuit potential; 4. The method for accelerated evaluation of an anode according to claim 3, wherein the open circuit potential is maintained for a period of time of 10 to 60 seconds.
5. The above E min 5. The method for accelerated evaluation of an anode according to claim 1, wherein in the step, the anode is held at a potential 0.6 to 1.0 V lower than the open circuit potential.
6. 6. The method for accelerated evaluation of an anode according to claim 1, wherein the anode is an oxygen generating electrode.
Citation Information
Patent Citations
Fuel cell catalyst material acceleration evaluation method
CN111458398A
Improvements relating to hydrogen-oxygen cells particularly for use as electrolysers
GB864457A
Anode for alkali water electrolysis
JP2015086420A
Anode for alkali water electrolysis and manufacturing method of anode for alkali water electrolysis
JP2017190476A
Titanium base material, manufacturing method thereof, electrode for water electrolysis, and water electrolysis device
JP2019157273A