PVD system with remote arc discharge plasma assisted process.

The coating system with multiple magnetrons and a central cathode rod enhances versatility by enabling various coating applications like plasma-enhanced magnetron sputtering and cathodic arc deposition, addressing the limitations of traditional cathodic arc systems.

JP7576391B2Active Publication Date: 2024-10-31VAPOR TECHNOLOGIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2019122235
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-24
Filing Date
2019-06-28
Publication Date
2024-10-31
Estimated Expiration
2039-06-28

AI Technical Summary

Technical Problem

Existing cathodic arc systems are limited to one or a few applications due to high capital costs and lack of versatility.

Method used

A coating system with multiple magnetrons surrounding a central cathode rod and a plasma source, capable of operating in various modes such as plasma-enhanced magnetron sputtering, cathodic arc plasma deposition, and ionic cleaning, utilizing a central cathode rod and remote anode configuration for enhanced ionization and plasma generation.

Benefits of technology

The system achieves versatility in multiple coating applications, including sputtering, cathodic arc deposition, and plasma-enhanced magnetron sputtering, with improved efficiency and adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576391000001
    Figure 0007576391000001
  • Figure 0007576391000002
    Figure 0007576391000002
  • Figure 0007576391000003
    Figure 0007576391000003
Patent Text Reader

Abstract

To provide a coating system having improved versatility.SOLUTION: An arc coating system includes a coating chamber having a surrounding chamber wall, a top wall and a bottom wall. The surrounding chamber wall, the top wall and the bottom wall specify a coating cavity and a chamber center. A plasma source is arranged on the chamber center, and the plasma source includes a center cathode rod, and a plurality of cathode rods surrounding the center cathode rod. The coating system further includes a sample holder for holding a plurality of substrates to be coated. The sample holder is characterized by being rotatable around the chamber center at a first distance from the chamber center.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] In at least one embodiment, the present invention relates to an arc evaporation system and related methods. [Background technology]

[0002] Physical vapor deposition (PVD) and low pressure chemical vapor deposition (CVD) sources are used for coating deposition and surface treatment. Over the past 25 years, cathodic arc evaporation (i.e., a type of physical deposition) has been established as a reliable source of highly ionized plasma for the deposition of reactive and unreacted coatings from conductive target materials such as zirconium, titanium, titanium, chromium, aluminum, copper, and their alloys. The highly ionized plasma and associated electron beam generated in the arc evaporation process are also used in surface preparation techniques such as ion sputtering, etching, implantation, and diffusion processes. In a typical cathodic arc coating process, an electric arc evaporates material from a cathode target. The vaporized material then condenses on a substrate to form a coating. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] U.S. Pat. No. 9,412,569 Summary of the Invention [Problem to be solved by the invention]

[0004] Although cathodic arc systems work well, such systems are typically limited to one or a few applications. Due to the relatively high capital costs for coating systems, and arc deposition in particular, it is desirable for any given system to be able to operate in many different applications. Such applications include sputtering only, cathodic arc deposition only, sputtering + cathodic arc simultaneously, etc.

[0005] Thus, there is a need for a coating system with improved versatility. [Means for solving the problem]

[0006] The present invention, in at least one embodiment, solves one or more problems of the prior art by providing a coating system comprising a plurality of magnetrons surrounding a central cathode rod. The coating system comprises a coating chamber having a peripheral chamber wall, a top wall, and a bottom wall. The peripheral chamber wall, the top wall, and the bottom wall define a coating cavity and a chamber center. A plasma source is disposed at the chamber center, the plasma source comprising a central cathode rod and a plurality of cathode rods surrounding the central cathode rod. The coating system also comprises a sample holder for holding a plurality of substrates to be coated. Featured, the sample holder is adapted to rotate about the chamber center at a first distance from the chamber center.

[0007] In another embodiment, a coating system having an external magnetic coil is provided. The coating system includes a coating chamber having a peripheral chamber wall, a top wall, and a bottom wall. The peripheral chamber wall, the top wall, and the bottom wall define a coating cavity and a chamber center. A plasma source is disposed at a center of the chamber, the plasma source including a central cathode rod. The coating system also includes a sample holder that holds a plurality of substrates to be coated. The sample holder is adapted to rotate about the chamber center at a first distance from the chamber center. A first coaxial magnetic coil is disposed outside the coating chamber, and a second coaxial magnetic coil is disposed outside the coating chamber.

[0008] Advantageously, the coating system described above can be used in several different applications. In one example, the coating system can be adapted for plasma-enhanced magnetron sputtering, which involves both ionization of a metal gaseous plasma by a remote arc discharge established between a central cathode rod and a remote anode positioned by the surrounding chamber wall, and ionization of a metal gaseous plasma further enhanced by a hollow cathode plasma generated inside a separate shield. In another application, the coating system can be adapted for cathodic arc plasma deposition, alone or in combination with magnetron sputtering enhanced by a densified hollow cathode plasma generated in a separate shield. In another application, the coating system can be adapted for ionic cleaning and ionic surface conditioning in a hollow cathode gaseous plasma generated in a negatively charged container of metal mesh. In yet another application, the coating system can be adapted for plasma-enhanced magnetron sputtering (plasma-assisted magnetron sputtering, PEMS). [Brief description of the drawings]

[0009] [Figure 1] 1A-1C are schematic cross-sectional and top views of a coating system including at least one separating shield and a plurality of cathode rods. [Figure 2A] 1A-1D are schematic cross-sectional and side views of a coating system including at least one separating shield and a plurality of cathode rods. [Figure 2B] 2B is a schematic cross-sectional and side view of a coating system including at least one separating shield perpendicular to the view of FIG. 2A. [Figure 2C] Schematic diagram showing the operation of multiple cathode rods during sputtering. [Diagram 3] Schematic cross-sectional and top view of a coating system having an external magnetic coil. [Figure 4A] FIG. 2 is a side view of a separator shield formed from parallel rods. [Figure 4B] FIG. 2 is a side view of a separator shield formed from parallel rods. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Reference will now be made in detail to presently preferred compositions, embodiments, and methods of the present invention, which constitute the best mode of practicing the invention currently known to the inventors. The figures are not necessarily to scale. However, it should be understood that the disclosed embodiments are merely exemplary of the invention, which may be embodied in various and alternative forms. Thus, the specific details disclosed herein should not be construed as limiting, but merely as representative basis for any aspect of the invention and / or for teaching those skilled in the art how to use the invention in various ways.

[0011] It is also to be understood that this invention is not limited to the specific embodiments and methods described below, as specific components and / or conditions may, of course, vary. Further, the terminology used herein is used only for the purpose of describing particular embodiments of the invention, and is not intended to be limiting in any way.

[0012] It should also be noted that as used in the specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. For example, reference to a singular element is intended to include the plural elements.

[0013] The term "comprising" is synonymous with the terms "including," "having," "containing," or "characterized by." These terms are inclusive and open-ended and do not exclude additional, unrecited elements or method steps. isn't it.

[0014] The phrase "consisting of" excludes any element, step, or ingredient not specified in the claim. When this phrase appears in a clause in the body of a claim rather than immediately following a preamble, it limits only the elements recited in that clause and does not exclude other elements from the claim as a whole.

[0015] The phrase "consisting essentially of" limits the scope of a claim to the particular materials or steps, and those that do not materially affect the basic and novel characteristics of the claimed subject matter.

[0016] With respect to the terms "comprising," "consisting," and "consisting essentially of," although one of these three terms is used in this specification, the subject matter of this disclosure and claims may include use of either of the other two terms.

[0017] Throughout this application, when publications are referenced, the disclosures of these publications in their entireties are hereby incorporated by reference into this application to more fully describe the state of the art to which this invention pertains.

[0018] 1, 2A, 2B and 2C, schematic diagrams of a coating system having a plurality of cathode rods distributed around a central cathode are provided. The coating system 10 includes a coating chamber 12 that defines a central coating cavity 14. In a refinement, the coating chamber 12 includes a peripheral chamber wall 16, a top wall 18, and a bottom wall 20. In this context, "top" and "bottom" refer to the relative positions when the coating chamber is placed in its design position, i.e., the orientation in which it is to be used to coat a substrate. The chamber center 22 is a position that is approximately in the center of the chamber relative to the peripheral wall 16. In a further refinement, the peripheral chamber wall 16 is cylindrical with a circular cross section. The peripheral wall 16 includes a top edge 24 and a bottom edge 26. The top wall 18 is adjacent to the top edge 24, and the bottom wall 20 is adjacent to the bottom edge 26. In a refinement, the top wall 18 is a top flange located at a top edge 24 of the peripheral chamber wall and the bottom wall 20 is a bottom flange located at a bottom edge 26 of the peripheral chamber wall. The plasma source 30 is located at the chamber center. The sample holder 32 holds a number of substrates 34 to be coated. The sample holder 32 is rotatable along a direction f1 about the chamber center at a first distance d1 from the chamber center.

[0019] As shown in Figures 2A and 2B, the plasma source 30 can include a central cathode rod 60 and a central coil 62 that surrounds the central cathode rod 60. The central coil 62 is coaxially mounted around the cathode rod 60. The cathode rod 60 is powered by a power supply 64, while the central coil 62 is powered by a power supply 66. A control system 68 can be used to control the current flowing through the cathode rod 60 and the central coil 62. Typically, the current flowing is between 50 and 2000A.

[0020] Further, referring to Figs. 1, 2A, 2B and 2C, a schematic diagram of a coating system is provided that includes a plurality of cathode sputtering rods distributed around a central cathode. These rods can be advantageously used as magnetrons for magnetron sputtering. In this variation, the coating system 10 includes a plurality of cathode rods 72, 74, 76 and 78 (e.g., central cathode rod 60 and central coil 62) surrounding the plasma source 30. In one variation, the plurality of cathode rods includes 1 to 10 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10) rod-like cathodes having a longitudinal axis a1 aligned parallel to the surrounding chamber wall. In another refinement, the plurality of cathode rods includes an even number (e.g., 2, 4, 6, 8, etc.) of rod-like cathodes having a longitudinal axis a1 aligned parallel to the surrounding chamber wall. Fig. 3 shows a situation where there are four auxiliary cathode rods. Typically, each cathode rod of the plurality of cathode rods is rotatable about a longitudinal axis a2. Adjacent rods can be rotated in the same or opposite directions (i.e., clockwise or counterclockwise). In one refinement, a plurality of blocking shields 82, 84 are disposed between alternating pairs of cathode rods in the plurality of cathode rods.

[0021] As shown in FIG. 2C, the current can flow along the axis of the cylindrical magnetron source, with the current along each adjacent pair of cathode rods being directed in opposite directions I1 and I2. In this case, a focusing magnetic field is generated by a linear current flowing along the axis of the magnetron, and the magnetic field lines are in a plane perpendicular to the axis of the plasma source that focuses the metal vapor arc plasma from the plasma source device through the blocking shields 82, 84 toward the substrate to be coated in the coating chamber. In this coating deposition, the blocking shields 82, 84 are preferably positioned along the magnetic field lines generated by the linear current conducted along the magnetron sputtering source, which drives positively charged ions away from the region between the baffle and the cathode arc source toward the substrate to be coated in the deposition region of the coating chamber.

[0022] In one refinement, the coating system 10 comprises one or more separation shields. The first separation shield 40 is arranged around the chamber center at a second distance d2 from the chamber center. Typically, the second distance d2 is greater than the first distance. Alternatively, the second distance is smaller than the first distance. The first separation shield 40 is usually negatively charged. For this purpose, the system 10 includes a DC power supply 42 having a positive terminal 44 and a negative terminal 46 connected to the first separation shield 40 or to an RF power supply 47 (in which case the negative self-polarization potential creates an RF hollow cathode effect inside the hollow cathode vessel). A vacuum system 48 is in fluid communication with the coating chamber 12 and is used to maintain the vacuum during the coating deposition. In a variant described in more detail below, a remote anode 58 is arranged at a third distance d3 from the chamber center, which is moved away from the vessel established by the first separation shield 40.

[0023] The first separated shield 40 can establish a hollow cathode vessel surrounding both the centrally located metal vapor plasma source and the substrate 34. It can facilitate all stages of the coating deposition process compared to a system without a separated shield: (i) ionic cleaning and ionic surface conditioning stages in the hollow cathode gaseous plasma generated in the hollow cathode vessel, (ii) plasma assisted magnetron sputtering (PEMS) mode when magnetron sputtering is provided in the hollow cathode plasma cloud generated by the hollow cathode vessel, (iii) ionization of the metal gaseous plasma by a remote arc discharge established between a cylindrical cathode of a cathodic arc source and a remote anode positioned by the chamber wall and centrally located within the coating deposition region. (iv) cathodic arc plasma deposition mode alone or in combination with magnetron sputtering enhanced by a high density hollow cathode plasma generated inside a negatively charged hollow cathode vessel surrounding both the deposited plasma source and the substrate 34, allowing for an increase in density and electron temperature as well as concentration of high energy electrons in the region inside the negatively charged first separating shield during the deposition of the plasma.

[0024] In one variant, the coating system 10 further comprises a second separating shield 50. The second separating shield 50 is disposed at a fourth distance d4 from the chamber center, which is smaller than the first distance d1. In a further refinement, the substrate is biased to the same potential as the second separating shield 50. A DC power supply 52 can be used for this purpose. In one refinement, the first separating shield 40 and the second separating shield 50 are each independently a metal mesh screen. Typically, the first separating shield 40 is an outer metal mesh screen and the second separating shield 50 is an inner metal mesh screen. Typically, the outer mesh screen and the inner mesh screen each independently have openings between 1 mm and 50 mm. In one refinement, the outer mesh screen and the inner mesh screen each independently have openings between 5 mm and 20 mm. Here, the substrate to be coated is placed in a container established by a first separating shield that separates the substrate from the surrounding chamber wall and a second separating shield that separates the substrate from the central cathode rod. An opening smaller than 1 mm can prevent plasma from flowing across the metal mesh wall, while an opening larger than 50 mm can mitigate the generation of high density plasma due to the hollow cathode effect.

[0025] When the second isolation shield 50 is present, the substrate 34 is placed in a negative DC pulsed metal mesh container established between a first isolation shield (e.g., an outer mesh screen) that separates the substrate 34 from the peripheral wall 16, and a second isolation shield 50 that separates the substrate 34 from a centrally located plasma source. The substrate can be biased to the same potential as the first isolation shield 40 and / or second isolation shield 50 by simply electrically connecting the substrate to the metal mesh screen, or alternatively, the bias potential of the substrate 34 can be different from the potential of the metal mesh screen container, which may be provided by a separate substrate bias power supply (not shown).

[0026] In a variant, the first isolation shield 40 does not have to completely isolate the inner region from the grounded chamber wall. For example, with the isolation shield removed, the top and bottom of the container can be fully or partially open to the chamber. Alternatively, the first isolation shield 40 and / or the second isolation shield 50 can be partially manufactured from a metal sheet without openings. For example, the top and bottom walls of the metal mesh container can be made from a metal sheet without openings or can open into the chamber wall.

[0027] In another refinement shown in FIGS. 3A and 3B, one or both of the first separating shield 40 and the second separating shield 50 have a distance d between adjacent rods 54, typically between 1 mm and 50 mm. r A crossbar 56 may be used to hold the rods 54 around the chamber center 22.

[0028] As mentioned above, the coating system 10 may further include a remote anode 58 that may be positioned at a fourth distance d4 from the chamber center that is greater than the first distance d1 and the second distance d2. In one refinement, the system 10 may further include one or more additional remote anodes 54 distributed along the peripheral wall 16. The peripheral wall 16 may optionally include a recess 60 for the location of the remote anode. The presence of the remote anode allows the coating system to be operated in a remote arc assisted magnetron sputtering (RAAMS) mode, as described in U.S. Patent No. 5,399,992, the disclosure of which is incorporated herein by reference in its entirety.

[0029] Referring to Figure 4, a schematic diagram of a coating system having external coaxial magnetic coils is provided. In this variation, the central coil 62 disposed within the cavity of the coating chamber 12 shown in Figures 2A and 2B is not present. Instead, the coaxial magnetic coils are disposed outside the coating chamber 12 but adjacent to the peripheral wall 16. For example, Figure 5 shows a first coaxial magnetic coil 90 disposed adjacent to a first wall outside the coating chamber and a second coaxial magnetic coil 92 disposed adjacent to a second wall outside the coating chamber. EXAMPLES

[0030] The following examples illustrate various embodiments of the invention. Those of ordinary skill in the art will recognize many variations that are within the spirit and scope of the claims.

[0031] Example 1 RAAMS deposition of TiN coating. The coating system shown in Figure 1 with four cylindrical magnetrons and a centrally located cylindrical cathodic arc source is used for this coating deposition process. Both the magnetrons and cathodic arc source are equipped with titanium targets. In the initial stage of ion cleaning, argon as a plasma generating gas is introduced into the vacuum chamber to a gas pressure in the range of 1 to 10 mTorr. A primary arc discharge is ignited by a mechanical trigger between the surface of the cathodic arc target and a grounded shield placed between the magnetron source. Then, a remote arc discharge is ignited between the cylindrical cathodic target and a remote anode placed by the wall of the vacuum coating deposition chamber. The current of the primary arc is set to 140 A, while its voltage is oscillating in the range of about 25 V to about 30 V. The current of the remote arc is set to 400 A, while its voltage is oscillating in the range of about 60 V to about 80 V. The current of the remote arc propagates from the cathode target through a chevron shield, which is impermeable to the heavy components of the vacuum arc plasma (metal ions, atoms, and macroparticles), but the electron flow of the remote arc discharge can move from the cylindrical cathode target towards a remote anode positioned by the coating chamber wall. The substrates to be coated are mounted on a rotating table, which allows them to rotate around the center of the coating chamber and simultaneously around their own axis. A bias voltage of -300V is applied to the rotating table with the substrates to be coated. The ion cleaning phase lasts for 30 minutes, followed by a remote arc assisted magnetron sputtering (RAAMS) deposition phase. At the start of the deposition phase, nitrogen is added to the chamber to make a mixture of about 30% N2 / remainder argon at a pressure ranging from 2 to 5 mTorr. The magnetron is driven at about 5 W / cm2 of the magnetron sputtering target. 2 The substrate bias during the TiN coating deposition stage is reduced to 100 V. For the deposition of a 5 μm thick TiN coating, the deposition of the TiN coating lasts for 3 hours.

[0032] Example 2 RAAMS deposition of TiN / DLC two-segment coating The coating system shown in Figure 1 with four cylindrical magnetrons and a centrally located cylindrical cathodic arc source is used for this coating deposition process. Both the magnetrons and cathodic arc source are equipped with titanium targets. The metal mesh cage is electrically connected to a rotating table with a substrate to be coated in order to maintain equal potential between the cage and the substrate. The cage and the rotating table are connected to a DC bias power supply and a high voltage DC pulse power supply through a switch, so that either of these two power supplies can be connected to the metal cage and the rotating table with the substrate to be coated at different stages of the coating deposition process. In the initial stage of ion cleaning, argon as a plasma generating gas is introduced into the vacuum chamber to a gas pressure ranging from 1 to 10 millitorr. A primary arc discharge is ignited by a mechanical trigger between the surface of the cathodic arc target and a grounded shield located between the magnetron source. A remote arc discharge is then ignited between the cylindrical cathodic target and a remote anode located by the wall of the vacuum coating deposition chamber. The current of the primary arc is set to 140 A, while its voltage is oscillating within a range of about 25 V to about 30 V. The current of the remote arc is set to 400 A, while its voltage oscillates within the range of about 60 V to about 80 V. The current of the remote arc propagates from the cathode target through a chevron shield, which is impermeable to the heavy components of the vacuum arc plasma (metal ions, atoms, and macroparticles), but the electron flow of the remote arc discharge can move from the cylindrical cathode target towards a remote anode positioned by the coating chamber wall. The substrates to be coated are mounted on a rotating table, which allows them to rotate around the center of the coating chamber and simultaneously around their own axis. The DC pulse power supply is disconnected from the cage and a DC bias power supply is connected to the cage to apply a DC bias voltage of -300 V to the rotating table with the substrates to be coated during the ion cleaning phase. The ion cleaning phase lasts for 30 minutes, followed by a remote arc assisted magnetron sputtering (RAAMS) deposition phase.At the beginning of the deposition phase, nitrogen is added to the chamber to make a mixture of about 30% N2 / rest argon at a pressure ranging from 2 to 5 mTorr. The magnetron is powered at about 5 W / cm of the magnetron sputtering target. 2 The magnetron is turned on by a magnetron power supply with a power density of 100 V DC. The substrate bias during the TiN coating deposition stage is reduced to 100 V DC. For the deposition of a 1.5 μm thick TiN coating segment, the deposition of the TiN coating lasts for 1 h. After the deposition stage of the TiN coating segment is completed, the magnetron is turned off and an argon / nitrogen mixture as the reactive gas atmosphere is replaced with acetylene to a total pressure of 15 mTorr. The DC bias power supply is disconnected from the cage and a DC pulse bias power supply is connected to the cage and at the same time to the rotating table with the substrate to be coated. A negative DC pulse voltage with an amplitude of -5 kV and a frequency of 30 kHz is applied to the cage and the rotating table to establish a hollow cathode enhanced high density plasma cloud during the deposition of the top DLC coating segment. The deposition of the DLC segment lasts for 4 h, resulting in the deposition of a 5 μm thick DLC top segment layer.

[0033] Example 3 RAAMS-cathodic arc hybrid deposition of TiSiNC nanocomposite coatings A coating system shown in Figure 1 with four cylindrical magnetrons and a centrally located cylindrical cathodic arc source is used for this coating deposition process. Both the magnetrons and cathodic arc source are equipped with the same titanium target as in Example 1. An adjustable Venetian baffle is used between two magnetrons of two opposing pairs of magnetrons, while a solid metal shield is installed between the magnetrons of adjacent pairs of magnetrons as shown in Figure 1. In the initial stage of ion cleaning, argon as a plasma generating gas is introduced into the vacuum chamber to a gas pressure ranging from 1 to 10 mTorr. The primary arc discharge is ignited by a mechanical trigger between the surface of the cathodic arc target and a grounded shield placed between the magnetron source. In the stage of ion cleaning, the Venetian baffle is slightly open, allowing the electron flow to propagate freely through the array of Venetian baffles along the remote arc discharge established between the cylindrical cathodic target and the remote anode placed by the wall of the chamber while blocking the propagation of the heavy components of the cathodic arc into the coating deposition region between the centrally located plasma source and the chamber wall. A remote arc discharge is then ignited between the cylindrical cathode target and a remote anode positioned by the wall of the vacuum coating deposition chamber. The current of the primary arc is set to 140 A while its voltage is oscillating within the range of about 25 V to about 30 V. The current of the remote arc is set to 400 A while its voltage is oscillating within the range of about 60 V to about 80 V. The substrates to be coated are mounted on a rotating table, which allows them to rotate around the center of the coating chamber and simultaneously around their own axis. A bias voltage of -300 V is applied to the rotating table with the substrates to be coated and at the same time to a metal mesh cage electrically connected to the rotating table by a DC bias power supply that is turned on while the high voltage DC pulse power supply is turned off. The ion cleaning phase lasts for 30 minutes, followed by a remote arc assisted magnetron sputtering (RAAMS) deposition phase.At the beginning of the TiNSiC nanocomposite coating deposition stage, nitrogen and trimethylsilane (3MS) are added to the argon in the process chamber to create a reactive gas mixture with the composition 30% N2 / 10% 3MS / rest argon at a pressure ranging from 2 to 5 mTorr. The magnetron is set at approximately 5 W / cm of the magnetron sputtering target. 2 The magnetron is turned on by a magnetron power supply having a power density of 10 kV. The DC bias power supply is turned off while the high voltage DC pulse power supply is turned on and set to apply a negative pulse of 5 kV at a repetition frequency of 30 kHz. A current of about 300 A is conducted along the cylindrical magnetron and its direction is switched in opposite directions at each adjacent magnetron as shown in Figures 15i and 15k, which provides a focusing magnetic field between adjacent magnetrons as shown by the magnetic field lines of arrows in Figures 15i and 15k. The position of the strips of the Venetian baffle is adjusted so that the surface of the baffle is approximately tangential to the focusing magnetic field as shown in Figure 15k, creating a plasma transport passage between adjacent strips of the Venetian baffle array. The direction of magnetron sputtering metal atom flow is aligned with that of magnetically focused cathodic arc metal vapor plasma to provide a cathodic arc / magnetron hybrid process of nanocomposite TiNSiC coating deposition, which lasts for 5 h for the deposition of a 20 μm thick TiNSiC nanocomposite coating.

[0034] Although exemplary embodiments have been described above, these embodiments are not intended to describe all possible forms of the invention. Rather, the words used herein are words of description rather than limitation, and it is understood that various changes may be made without departing from the spirit and scope of the invention. Moreover, features of the various embodiments may be combined to form further embodiments of the invention.

Claims

1. a coating chamber having a peripheral chamber wall, a top wall and a bottom wall, said peripheral chamber wall, said top wall and said bottom wall defining a coating cavity and a chamber center; a plasma source disposed at the center of the chamber, the plasma source comprising a cylindrical central cathode rod powered by a first power source and a plurality of cathode rods surrounding the cylindrical central cathode rod, each of the plurality of cathode rods being a cylindrical magnetron having a longitudinal axis aligned parallel to the peripheral chamber wall, the cylindrical central cathode rod being a target; a sample holder adapted to hold a plurality of substrates to be coated and to rotate about the chamber center at a first distance from the chamber center; Equipped with A coating system, wherein each cathode rod of the plurality of cathode rods is rotatable about the longitudinal axis.

2. The coating system of claim 1 further comprising at least one remote anode positioned proximate the peripheral chamber wall and a second distance from the chamber center.

3. The coating system of claim 1 , wherein the plurality of cathode rods comprises 2 to 10 rod-shaped cathodes.

4. The coating system of claim 1 , further comprising a plurality of blocking shields, the blocking shields being disposed between alternating pairs of cathode rods within the plurality of cathode rods.

5. 10. The coating system of claim 1, further comprising a first separation shield disposed between the sample holder and the surrounding chamber wall, and a second separation shield disposed between the plasma source and the sample holder.

6. 6. The coating system of claim 5, wherein said first separator shield is an outer metal mesh screen and said second separator shield is an inner metal mesh screen.

7. 7. The coating system of claim 6, wherein the substrate is biased to the same potential as the inner metal mesh screen.

8. 8. The coating system of claim 7, further comprising a DC power supply having a positive terminal and a negative terminal, the negative terminal being connected to the first isolation shield.

9. 10. The coating system of claim 1 adapted for ionic cleaning and ionic surface conditioning in a hollow cathode gaseous plasma generated in a metal mesh negatively charged vessel.

10. 10. The coating system of claim 1 adapted for plasma assisted magnetron sputtering (PEMS).

11. 10. The coating system of claim 1, wherein the top wall is a top flange located at a top edge of the peripheral chamber wall and the bottom wall is a bottom flange located at a bottom edge of the peripheral chamber wall.

Citation Information

Patent Citations

  • Remote arc discharge plasma supporting process

    JP2017031501A

  • Remote arc discharge plasma assisted processes

    US9412569B2