Positive electrode for all-solid-state secondary battery and all-solid-state secondary battery

By employing lithium cobalt oxide modified with Al and M1 elements to stabilize the positive electrode in all-solid-state batteries, the internal resistance is reduced, enhancing load characteristics and discharge efficiency.

JP7576400B2Active Publication Date: 2024-10-31MAXELL LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020044548
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-13
Publication Date
2024-10-31
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

All-solid-state secondary batteries face challenges in achieving low resistance values, particularly at high discharge currents, due to the expansion of positive electrode active materials like lithium cobalt oxide, which disrupts contact with the solid electrolyte, increasing internal resistance and degrading load characteristics.

Method used

The use of lithium cobalt oxide (LiCo1-a-b-cAl a M1 b M2 c O2) as the positive electrode active material, where Al and M1 elements suppress the expansion of Co, maintaining good contact with the solid electrolyte and reducing internal resistance, combined with a reaction suppression layer to prevent oxidation of the electrolyte.

Benefits of technology

This configuration results in an all-solid-state secondary battery with lower internal resistance and improved load characteristics, enabling efficient discharge at high currents while maintaining stability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576400000003
    Figure 0007576400000003
  • Figure 0007576400000004
    Figure 0007576400000004
  • Figure 0007576400000005
    Figure 0007576400000005
Patent Text Reader

Abstract

To provide a positive electrode for an all-solid type secondary battery, which is low in resistance value, and an all-solid type secondary battery arranged by use of the positive electrode.SOLUTION: A positive electrode for an all-solid type secondary battery according to the present invention comprises a compact of a positive electrode mixture containing a positive electrode active material, a conductive assistant and a solid electrolyte. In the positive electrode, a lithium cobalt oxide represented by the following general formula (1) is included as the positive electrode active material: LiCo1-a-b-cAlaM1bM2cO2 (1). [In the general formula (1), M1 is at least one element selected from a group consisting of Mg, Ni and Na, and M2 is at least one element selected from a group consisting of Mn, Fe, Cu, Zr, Ti, Bi, Ca, F, P, Sr, W, Ba, Nb, Si, Zn, Mo, V, Sn, Sb, Ta, Ge, Cr, K, S and Er; 0<a<0.1, 0<b<0.1, a+b<0.1, and 0≤c.] An all-solid type secondary battery according to the present invention comprises the positive electrode for an all-solid type secondary battery according to the present invention.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode for an all-solid-state secondary battery having a low resistance value, and an all-solid-state secondary battery using the positive electrode. [Background technology]

[0002] In recent years, with the development of portable electronic devices such as mobile phones and notebook personal computers, and the practical application of electric vehicles, there has been a demand for small, lightweight secondary batteries with high capacity and high energy density.

[0003] Currently, lithium secondary batteries, particularly lithium ion secondary batteries, that can meet this demand use lithium-containing composite oxides such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) as the positive electrode active material, graphite or the like as the negative electrode active material, and an organic electrolyte solution containing an organic solvent and a lithium salt as the non-aqueous electrolyte.

[0004] Furthermore, with the further development of devices in which lithium-ion secondary batteries can be used, there is a demand for lithium-ion secondary batteries with longer life, higher capacity and higher energy density. At the same time, there is also a high demand for the reliability of lithium-ion secondary batteries with longer life, higher capacity and higher energy density.

[0005] However, since the organic electrolyte used in the lithium ion secondary battery contains an organic solvent, which is a flammable substance, the organic electrolyte may generate abnormal heat when an abnormality such as a short circuit occurs in the battery. In addition, with the recent trend toward higher energy density of lithium ion secondary batteries and an increasing amount of organic solvent in the organic electrolyte, there is a demand for even higher reliability of lithium ion secondary batteries.

[0006] In the circumstances described above, all-solid-state lithium secondary batteries that do not use organic solvents (all-solid-state secondary batteries) have attracted attention (Patent Documents 1, 2, etc.). All-solid-state secondary batteries use a molded body of a solid electrolyte that does not use an organic solvent instead of the conventional organic solvent-based electrolyte, and are highly safe with no risk of abnormal heat generation from the solid electrolyte. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-40531 A [Patent Document 2] JP 2017-168387 A Summary of the Invention [Problem to be solved by the invention]

[0008] Incidentally, the application fields of all-solid-state secondary batteries are expanding rapidly at present, and for example, applications requiring discharge at a large current value are considered, so that it is required to improve the load characteristics to meet this. One way to improve the load characteristics of all-solid-state secondary batteries is, for example, to reduce the resistance value of the positive electrode, and therefore there is a demand for the development of a technology to achieve this.

[0009] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a positive electrode for an all-solid-state secondary battery having a low resistance value, and an all-solid-state secondary battery using the positive electrode. [Means for solving the problem]

[0010] The positive electrode for an all-solid-state secondary battery of the present invention has a molded body of a positive electrode mixture containing a positive electrode active material, a conductive assistant, and a solid electrolyte, The positive electrode active material is represented by the following general formula (1): LiCo 1-a-b-c Al a M 1 b M 2 cO2(1) 〔In the general formula (1), M 1 is at least one element selected from the group consisting of Mg, Ni, and Na, and M 2 is at least one element selected from the group consisting of Mn, Fe, Cu, Zr, Ti, Bi, Ca, F, P, Sr, W, Ba, Nb, Si, Zn, Mo, V, Sn, Sb, Ta, Ge, Cr, K, S, and Er, where 0 < a < 0.1, 0 < b < 0.1, a + b < 0.1, and 0 ≤ c〕 and contains lithium cobalt oxide represented by the following formula.

[0011] Further, the all-solid-state secondary battery of the present invention has a positive electrode, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode, and is characterized in that the positive electrode has a positive electrode for an all-solid-state secondary battery of the present invention.

Advantages of the Invention

[0012] According to the present invention, it is possible to provide a positive electrode for an all-solid-state secondary battery having a low resistance value and an all-solid-state secondary battery using the positive electrode.

Brief Description of the Drawings

[0013] [Figure 1] It is a cross-sectional view schematically showing an example of the all-solid-state secondary battery of the present invention. [Diagram 2] It is a plan view schematically showing another example of the all-solid-state secondary battery of the present invention. [Diagram 3] It is a cross-sectional view taken along line I-I of Figure 2.

Modes for Carrying Out the Invention

[0014] <Positive Electrode for All-Solid-State Secondary Battery> The positive electrode for an all-solid-state secondary battery of the present invention has a molded body of a positive electrode mixture containing a positive electrode active material, a conductive assistant, and a solid electrolyte. And, as the positive electrode active material, lithium cobalt oxide (A) represented by the following general formula (1) is used.

[0015] LiCo 1-a-b-c Ala M 1 b M 2 c O2(1)

[0016] In the general formula (1), M 1 represents at least one element selected from the group consisting of Mg, Ni and Na; M 2 is at least one element selected from the group consisting of Mn, Fe, Cu, Zr, Ti, Bi, Ca, F, P, Sr, W, Ba, Nb, Si, Zn, Mo, V, Sn, Sb, Ta, Ge, Cr, K, S, and Er, and 0 <a<0.1、0<b<0.1、a+b<0.1、0≦cである。

[0017] When lithium cobalt oxide (A) is used as a positive electrode active material for a non-aqueous electrolyte secondary battery using an organic electrolyte, the Al and M contained in the material are 1 Lithium cobalt oxide (A) is a material that increases the internal resistance of a battery by the action of an additive element such as lithium cobalt oxide (A). However, in the case of a non-aqueous electrolyte secondary battery having an organic electrolyte, the electrolyte that transfers ions between the positive and negative electrodes is liquid (electrolytic solution), so the original internal resistance is small, and the increase in internal resistance due to lithium cobalt oxide (A) has almost no effect on the battery characteristics. On the other hand, in an all-solid-state secondary battery in which ions are transferred between the positive and negative electrodes by a solid electrolyte, it is expected that the increase in internal resistance due to the action of the positive electrode active material will cause a decrease in battery characteristics such as load characteristics.

[0018] However, the inventors have found through their studies that in an all-solid-state secondary battery using the lithium cobalt oxide (A) represented by the general formula (1) as the positive electrode active material, it is actually possible to reduce the internal resistance compared to a case where, for example, LiCoO2 is used as the positive electrode active material.

[0019] When a battery using LiCoO2 as the positive electrode active material is charged, the Co expands due to a change in valence. In a battery using an organic electrolyte, even if the volume of the positive electrode active material changes due to this, the electrolyte that transfers ions is liquid, so contact with the positive electrode active material is not lost. On the other hand, in an all-solid-state secondary battery, the electrolyte that transfers ions in the positive electrode is solid (solid electrolyte), so the volume of the positive electrode active material changes when the battery is charged and discharged, creating a gap between the solid electrolyte, and the internal resistance of the positive electrode and, ultimately, the battery increases.

[0020] However, in the case of the lithium cobalt oxide (A) represented by the general formula (1), even in a charged state, Al and the element M 1 Since the expansion of Co is suppressed by the action of the above, the expansion amount (volume change amount) of the entire positive electrode active material is small. Therefore, in an all-solid-state secondary battery using the positive electrode for an all-solid-state secondary battery of the present invention (the all-solid-state secondary battery of the present invention), the contact between the lithium cobalt oxide (A) and the solid electrolyte in the positive electrode is well maintained even during charging and discharging, so that the internal resistance can be kept low, resulting in excellent load characteristics.

[0021] Examples of positive electrodes for all-solid-state secondary batteries include a molded body (such as a pellet) obtained by molding a positive electrode mixture, and a structure in which a layer (positive electrode mixture layer) made of a molded body of a positive electrode mixture is formed on a current collector.

[0022] In lithium cobalt oxide (A), Al is an element that substitutes for the Co site, M 1 are elements that substitute for the Li site, and both have the effect of reducing the amount of expansion of Co (the amount of expansion of lithium cobalt oxide (A)) during charging.

[0023] Lithium cobalt oxide (A) is a compound containing the element M 1 At least one element selected from Mg, Ni, and Na may be contained as the lithium ion species. However, Mg is preferred since it has an ionic radius equivalent to that of the Li which it substitutes, and furthermore does not undergo a change in valence during charging and discharging.

[0024] In the lithium cobalt oxide (A), in order to suppress the expansion amount during charging, the amount of Al, a, is greater than 0 and less than 0.1, and the element M 1 The amount b of Al is greater than 0 and less than 0.1, and a+b is less than 0.1. The amount a of Al is preferably 0.005 or more, and the amount of element M 1 The amount b of element M is preferably 0.005 or more. Furthermore, the amount a of Al is preferably 0.08 or less. 1 The amount b is preferably 0.08 or less.

[0025] Lithium cobalt oxide (A) is a compound containing the element M 2 may or may not be contained (the amount c may be 0), but element M 2 If the amount of element M is too large, for example, the amount of Co may become small, and the capacity of the lithium cobalt oxide (A) may become small. 2 The amount c is preferably 0.05 or less.

[0026] The positive electrode active material may be composed of only lithium cobalt oxide (A), or may be used in combination with other positive electrode active materials. Examples of other positive electrode active materials that can be used in combination with lithium cobalt oxide (A) include active materials capable of absorbing and releasing lithium ions, similar to those used as positive electrode active materials in conventionally known lithium ion secondary batteries. However, when lithium cobalt oxide (A) is used in combination with other positive electrode active materials, it is preferable that the proportion of lithium cobalt oxide (A) in the total positive electrode active material is 60 mass% or more. Note that the entire positive electrode active material may be lithium cobalt oxide (A), so the upper limit of the preferred content of lithium cobalt oxide (A) in the total positive electrode active material is 100 mass%.

[0027] The average particle size of the positive electrode active material is preferably 1 μm or more, more preferably 2 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less. The positive electrode active material may be either primary particles or secondary particles formed by agglomeration of primary particles. When a positive electrode active material having an average particle size in the above range is used, a large interface with the solid electrolyte can be obtained, and thus the load characteristics of the battery are further improved.

[0028] The average particle diameter of the positive electrode active material in this specification is the 50% diameter value (d 50 )

[0029] The positive electrode active material preferably has a reaction suppression layer on its surface for suppressing reaction with the solid electrolyte.

[0030] If the positive electrode active material and the solid electrolyte come into direct contact with each other in the positive electrode mixture compact, the solid electrolyte may oxidize to form a resistance layer, which may reduce the ionic conductivity in the compact. By providing a reaction suppression layer that suppresses the reaction with the solid electrolyte on the surface of the positive electrode active material and preventing direct contact between the positive electrode active material and the solid electrolyte, it is possible to suppress the reduction in the ionic conductivity in the compact due to the oxidation of the solid electrolyte.

[0031] The reaction suppression layer may be made of a material that has ion conductivity and can suppress the reaction between the positive electrode active material and the solid electrolyte. Examples of materials that can form the reaction suppression layer include oxides containing Li and at least one element selected from the group consisting of Nb, P, B, Si, Ge, Ti, and Zr, more specifically, Nb-containing oxides such as LiNbO3, Li3PO4, Li3BO3, Li4SiO4, Li4GeO4, LiTiO3, LiZrO3, and the like. The reaction suppression layer may contain only one of these oxides, or may contain two or more of them, and further, a plurality of these oxides may form a composite compound. Among these oxides, it is preferable to use Nb-containing oxides, and it is more preferable to use LiNbO3.

[0032] The reaction suppression layer is preferably present on the surface in an amount of 0.1 to 1.0 part by mass per 100 parts by mass of the positive electrode active material, in order to effectively suppress the reaction between the lithium cobalt oxide and the solid electrolyte.

[0033] Methods for forming a reaction suppression layer on the surface of a positive electrode active material include the sol-gel method, the mechanofusion method, the CVD method, the PVD method, and the like.

[0034] The content of the positive electrode active material in the positive electrode mixture is preferably 60 to 95 mass %.

[0035] The conductive assistant for the positive electrode can be a carbon material such as graphite (natural graphite, artificial graphite), graphene, carbon black, carbon nanofiber, carbon nanotube, etc. The content of the conductive assistant in the positive electrode mixture is preferably 1 to 10 mass %.

[0036] The solid electrolyte for the positive electrode is not particularly limited as long as it has lithium ion conductivity, and for example, a sulfide-based solid electrolyte, a hydride-based solid electrolyte, an oxide-based solid electrolyte, etc. can be used.

[0037] Examples of sulfide solid electrolytes include particles such as Li2S-P2S5, Li2S-SiS2, Li2S-P2S5-GeS2, and Li2S-B2S3-based glasses. In recent years, LGPS-based materials (Li 10 GeP2S 12 etc.) and argyrodite-based materials [such as those represented by Li6PS5Cl, Li 7-x+y PS 6-x Cl x+y (where 0.05 ≦ y ≦ 0.9, -3.0x + 1.8 ≦ y ≦ -3.0x + 5.7), Li 7-a PS 6-a Cl b Br c (where a = b + c, 0 < a ≦ 1.8, 0.1 ≦ b / c ≦ 10.0), etc.] can also be used. Among these, argyrodite-based materials with particularly high lithium ion conductivity and high chemical stability are preferably used.

[0038] Examples of hydride solid electrolytes include LiBH4, solid solutions of LIBH4 and the following alkali metal compounds (e.g., those with a molar ratio of LiBH4 to the alkali metal compound of 1:1 to 20:1). Examples of the alkali metal compounds in the solid solution include at least one selected from the group consisting of lithium halides (LiI, LiBr, LiF, LiCl, etc.), rubidium halides (RbI, RbBr, RbiF, RbCl, etc.), cesium halides (CsI, CsBr, CsF, CsCl, etc.), lithium amide, rubidium amide, and cesium amide.

[0039] Examples of oxide solid electrolytes include Li7La3Zr2O 12 , LiTi(PO4)3, LiGe(PO4)3, LiLaTiO3, etc.

[0040] The solid electrolyte may be one or more of the above-mentioned examples. Among the above-mentioned solid electrolytes, it is more preferable to use a sulfide-based solid electrolyte because it has high lithium ion conductivity and also has a function of increasing the moldability of the positive electrode mixture.

[0041] The content of the solid electrolyte in the positive electrode mixture is preferably 4 to 30 mass %.

[0042] The positive electrode mixture may or may not contain a resin binder. Examples of the resin binder include fluororesins such as polyvinylidene fluoride (PVDF). However, since the resin binder acts as a resistance component in the positive electrode mixture, it is desirable that the amount of the resin binder is as small as possible. Therefore, it is preferable that the positive electrode mixture does not contain a resin binder, or if it does contain one, the content is 0.5 mass% or less. It is more preferable that the content of the resin binder in the positive electrode mixture is 0.3 mass% or less, and even more preferable that it is 0 mass% (i.e., no resin binder is contained).

[0043] When a current collector is used for the positive electrode, the current collector can be made of a metal foil such as aluminum or stainless steel, a punched metal, a net, an expanded metal, a foamed metal, a carbon sheet, or the like.

[0044] The positive electrode mixture compact can be formed, for example, by compressing a positive electrode mixture prepared by mixing a positive electrode active material, a conductive assistant, a solid electrolyte, and further a binder added as necessary, by pressure molding or the like.

[0045] In the case of a positive electrode having a current collector, the positive electrode can be produced by bonding a molded body of the positive electrode mixture formed by the above-mentioned method to the current collector by, for example, pressure bonding.

[0046] The thickness of the positive electrode mixture compact (in the case of a positive electrode having a current collector, the thickness of the positive electrode mixture compact per one side of the current collector; the same applies below) is preferably 200 μm or more from the viewpoint of increasing the capacity of the battery. In addition, the load characteristics of a battery are generally easily improved by making the positive electrode or negative electrode thinner, but according to the present invention, even when the positive electrode mixture compact is as thick as 200 μm or more, the load characteristics can be improved. Therefore, in the present invention, when the thickness of the positive electrode mixture compact is, for example, 200 μm or more, the effect is more remarkable. In addition, the thickness of the positive electrode mixture compact is usually 2000 μm or less.

[0047] <All-solid-state secondary battery> The all-solid-state secondary battery of the present invention has a positive electrode, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode, and the positive electrode is the positive electrode for the all-solid-state secondary battery of the present invention.

[0048] (Negative electrode) The negative electrode of the all-solid-state secondary battery has, for example, a molded body of a negative electrode mixture containing a negative electrode active material, a conductive assistant, a solid electrolyte, and the like. Examples of the negative electrode include a negative electrode consisting of the molded body alone and a negative electrode having a structure in which the molded body and a current collector are integrated together.

[0049] As the negative electrode active material, for example, one or a mixture of two or more of carbon-based materials capable of absorbing and releasing lithium, such as graphite, pyrolytic carbons, cokes, glassy carbons, fired organic polymer compounds, mesocarbon microbeads (MCMB), carbon fibers, etc., can be used. In addition, simple substances, compounds and alloys thereof containing elements such as Si, Sn, Ge, Bi, Sb, In, etc.; compounds capable of charging and discharging at a low voltage close to that of lithium metal, such as lithium-containing nitrides or lithium-containing oxides; lithium metal; and lithium / aluminum alloys can also be used as the negative electrode active material.

[0050] The content of the negative electrode active material in the negative electrode mixture is preferably 50 to 95 mass %.

[0051] The conductive assistant for the negative electrode can be a carbon material such as graphite (natural graphite, artificial graphite), graphene, carbon black, carbon nanofiber, carbon nanotube, etc. The content of the conductive assistant in the negative electrode mixture is preferably 1 to 10 mass %.

[0052] The negative electrode solid electrolyte may be one or more of the solid electrolytes listed above as examples of the solid electrolytes that may be included in the positive electrode mixture. Among the solid electrolytes listed above, it is more preferable to use a sulfide-based solid electrolyte, since it has high lithium ion conductivity and has the function of improving the moldability of the negative electrode mixture.

[0053] The content of the solid electrolyte in the negative electrode mixture is preferably 4 to 49 mass %.

[0054] The negative electrode mixture may or may not contain a resin binder. Examples of the resin binder include fluororesins such as polyvinylidene fluoride (PVDF). However, since the resin binder acts as a resistance component even in the negative electrode mixture, it is desirable that the amount of the resin binder is as small as possible. Therefore, it is preferable that the negative electrode mixture does not contain a resin binder, or if it does contain one, the content is 0.5 mass% or less. It is more preferable that the content of the resin binder in the negative electrode mixture is 0.3 mass% or less, and even more preferable that it is 0 mass% (i.e., no resin binder is contained).

[0055] When a current collector is used for the negative electrode, the current collector can be made of copper or nickel foil, punched metal, net, expanded metal, foamed metal; carbon sheet; or the like.

[0056] The negative electrode mixture compact can be formed, for example, by compressing, by pressure molding, a negative electrode mixture prepared by mixing a negative electrode active material, a conductive assistant, a solid electrolyte, and further a binder added as necessary.

[0057] In the case of a negative electrode having a current collector, the negative electrode can be produced by bonding a molded product of the negative electrode mixture formed by the above-mentioned method to the current collector by, for example, pressure bonding.

[0058] The thickness of the negative electrode mixture compact (in the case of a negative electrode having a current collector, the thickness of the positive electrode mixture compact per one side of the current collector. The same applies below) is preferably 200 μm or more from the viewpoint of increasing the capacity of the battery. In addition, the load characteristics of a battery are generally easily improved by making the positive electrode or negative electrode thinner, but according to the present invention, even if the negative electrode mixture compact is as thick as 200 μm or more, the load characteristics can be improved. Therefore, in the present invention, when the thickness of the negative electrode mixture compact is, for example, 200 μm or more, the effect is more remarkable. In the present invention, when the thickness of the positive electrode mixture compact is 200 μm or more and the thickness of the negative electrode mixture compact is 200 μm or more, the effect is particularly remarkable. In addition, the thickness of the negative electrode mixture compact is usually 3000 μm or less.

[0059] (Solid electrolyte layer) The solid electrolyte in the solid electrolyte layer may be one or more of the same solid electrolytes as those exemplified above for the positive electrode. However, in order to improve the battery characteristics, it is preferable to contain a sulfide-based solid electrolyte, and it is more preferable to contain a sulfide-based solid electrolyte in all of the positive electrode, negative electrode, and solid electrolyte layer.

[0060] The solid electrolyte layer may have a porous body such as a resin nonwoven fabric as a support.

[0061] The solid electrolyte layer can be formed by a method of compressing a solid electrolyte by pressure molding or the like; a method of applying a composition for forming a solid electrolyte layer, which is prepared by dispersing a solid electrolyte in a solvent, onto a substrate, a positive electrode, or a negative electrode, drying the composition, and, if necessary, performing pressure molding such as pressing.

[0062] It is preferable to select a solvent that does not deteriorate the solid electrolyte for use in the composition for forming the solid electrolyte layer. In particular, since sulfide-based solid electrolytes and hydride-based solid electrolytes undergo chemical reactions due to a small amount of water, it is preferable to use a non-polar aprotic solvent represented by a hydrocarbon solvent such as hexane, heptane, octane, nonane, decane, decalin, toluene, or xylene. In particular, it is more preferable to use an ultra-dehydrated solvent with a water content of 0.001 mass% (10 ppm) or less. In addition, fluorine-based solvents such as "Vertrel (registered trademark)" manufactured by Mitsui DuPont Fluorochemicals, "Zeorolla (registered trademark)" manufactured by Nippon Zeon Co., Ltd., and "Novec (registered trademark)" manufactured by Sumitomo 3M Co., Ltd., as well as non-aqueous organic solvents such as dichloromethane and diethyl ether can also be used.

[0063] The thickness of the solid electrolyte layer is preferably 100 to 300 μm.

[0064] (electrode body) The positive electrode and the negative electrode can be used in a battery in the form of a laminated electrode body in which the positive electrode and the negative electrode are laminated with a solid electrolyte layer interposed therebetween, or in the form of a wound electrode body in which this laminated electrode body is wound.

[0065] In forming the electrode body, it is preferable to pressure mold the positive electrode, the negative electrode, and the solid electrolyte layer in a laminated state, from the viewpoint of increasing the mechanical strength of the electrode body.

[0066] (Battery type) A cross-sectional view showing a schematic example of an all-solid-state secondary battery of the present invention is shown in Fig. 1. The battery 1 shown in Fig. 1 has a positive electrode 10, a negative electrode 20, and a solid electrolyte layer 30 interposed between the positive electrode 10 and the negative electrode 20 enclosed in an exterior body formed of an exterior can 40, a sealing can 50, and a resin gasket 60 interposed between them.

[0067] The sealing can 50 is fitted into the opening of the outer can 40 via a gasket 60, and the open end of the outer can 40 is tightened inward, whereby the gasket 60 comes into contact with the sealing can 50, sealing the opening of the outer can 40 and forming an airtight structure inside the element.

[0068] The outer can and the sealing can can be made of stainless steel or the like. The gasket can be made of polypropylene, nylon, or other materials. If heat resistance is required for the battery's intended use, heat-resistant resins with melting points exceeding 240°C, such as fluororesins such as tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), polyphenylene ether (PEE), polysulfone (PSF), polyarylate (PAR), polyethersulfone (PES), polyphenylene sulfide (PPS), and polyetheretherketone (PEEK), can also be used. If the battery is used in an application that requires heat resistance, a glass hermetic seal can be used for the sealing.

[0069] 2 and 3 are drawings that diagrammatically show another example of the all-solid-state secondary battery of the present invention. Fig. 2 is a plan view of the all-solid-state secondary battery, and Fig. 3 is a cross-sectional view taken along line II in Fig. 2.

[0070] The all-solid-state secondary battery 100 shown in Figures 2 and 3 houses an electrode assembly 200 consisting of a positive electrode, a solid electrolyte layer, and a negative electrode of the present invention in a laminate film exterior body 500 consisting of two sheets of metal laminate film, and the laminate film exterior body 500 is sealed at its outer periphery by heat fusing the upper and lower metal laminate films. In Figure 3, in order to avoid complicating the drawing, the layers constituting the laminate film exterior body 500 and the positive electrode, negative electrode, and separator constituting the electrode body are not shown separately.

[0071] The positive electrode of the electrode body 200 is connected to a positive electrode external terminal 300 within the battery 100, and although not shown, the negative electrode of the electrode body 200 is also connected to a negative electrode external terminal 400 within the battery 100. One end of the positive electrode external terminal 300 and the negative electrode external terminal 400 is drawn out to the outside of the laminate film exterior body 500 so that they can be connected to an external device or the like.

[0072] The form of the all-solid-state secondary battery may be one having an exterior body composed of an exterior can, a sealing can, and a gasket as shown in FIG. 1, that is, one generally referred to as a coin-type battery or a button-type battery, or one having an exterior body composed of a resin film or a metal-resin laminate film as shown in FIGS. 2 and 3, or one having an exterior body having a metallic, bottomed, tubular (cylindrical or rectangular) exterior can and a sealing structure that seals the opening of the can.

[0073] The lithium cobalt oxide (A) contained in the all-solid-state secondary battery of the present invention as a positive electrode active material has excellent stability in a high-voltage charging state. Therefore, the all-solid-state secondary battery of the present invention can be used by setting the end voltage during charging to about 4.2 V, as with conventional lithium ion secondary batteries having an organic electrolyte, but it may also be used by a method of charging with an end voltage of 4.3 V or more, which is higher than the above. Even if the battery is charged in this way to increase the capacity and used at high temperatures, it can exhibit good discharge characteristics and storage characteristics. However, it is preferable that the end voltage during charging of the all-solid-state secondary battery is 4.6 V or less.

[0074] The all-solid-state secondary battery of the present invention can be used for the same applications as conventionally known secondary batteries, but since it has a solid electrolyte instead of an organic electrolyte, it has excellent heat resistance and can be preferably used for applications in which it is exposed to high temperatures. EXAMPLES

[0075] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.

[0076] Example 1 <Preparation of positive electrode> LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface 0.98 Al 0.01 Mg 0.01O2 (positive electrode active material), a sulfide-based solid electrolyte (Li6PS5Cl) having an argyrodite structure with an average particle size of 4 μm, and acetylene black (conductive assistant) were mixed in a mass ratio of 60:35:5 and thoroughly kneaded to prepare a positive electrode mixture. Next, 15 mg of the positive electrode mixture was placed in a powder molding die with a diameter of 10 mm and pressure-molded using a press machine to produce a positive electrode consisting of a cylindrical positive electrode mixture compact. Note that LiCo 0.98 Al 0.01 Mg 0.01 The amount of LiNbO3 layer on the surface of O2 is 0.98 Al 0.01 Mg 0.01 O2: 0.5 parts by mass per 100 parts by mass.

[0077] <Formation of solid electrolyte layer> Next, 80 mg of the same sulfide-based solid electrolyte as that used for producing the positive electrode was placed on the positive electrode mixture compact in the powder molding die, and pressure molding was performed using a press to form a solid electrolyte layer on the positive electrode mixture compact.

[0078] <Formation of laminated electrode body> The counter electrode was made by stacking Li and In metals formed into a cylindrical shape, and the counter electrode was placed on the surface of the solid electrolyte layer in the powder molding die opposite to the positive electrode, and pressure molding was performed using a press to produce a laminated electrode body.

[0079] <Assembly of model cell> Using the laminated electrode body, a model cell of a planar structure similar to that shown in Fig. 2 was produced. A positive electrode current collector foil (SUS foil) and a counter electrode current collector foil (SUS foil) were attached side by side with a certain amount of space between them on the inner surface of the aluminum laminate film constituting the laminated film exterior body. Each of the current collector foils was cut into a shape that had a main body portion facing the positive electrode side surface or the counter electrode side surface of the laminated electrode body, and a portion that protrudes from the main body portion toward the outside of the cell to become the positive electrode external terminal 300 and the counter electrode external terminal 400.

[0080] The laminated electrode body was placed on the counter electrode current collector foil of the laminated film exterior body, and the laminated electrode body was wrapped in the laminated film exterior body so that the positive electrode current collector foil was positioned on the positive electrode of the laminated electrode body. The remaining three sides of the laminated film exterior body were then sealed by heat fusion under vacuum to obtain a model cell.

[0081] Example 2 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.9798 Al 0.01 Mg 0.01 Ti 0.0002 O2(LiCo 0.9798 Al 0.01 Mg 0.01 Ti 0.0002 The amount of LiNbO3 layer on the surface of O2 is 0.9798 Al 0.01 Mg 0.01 Ti 0.0002 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0082] Example 3 The positive electrode active material was LiCo with an average particle size of 8 μm and a layer of LiNbO3 on the surface. 0.98 Al 0.01 Mg 0.01 O2(LiCo 0.98 Al 0.01 Mg 0.01 The amount of LiNbO3 layer on the surface of O2 is LiCo 0.98 Al 0.01 Mg 0.01 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0083] Comparative Example 1 A model cell was prepared in the same manner as in Example 1, except that the positive electrode active material was changed to LiCoO2 having an average particle diameter of 5 μm and a layer of LiNbO3 on the surface (the amount of the layer of LiNbO3 on the surface of LiCoO2 was 0.5 parts by mass per 100 parts by mass of LiCoO2).

[0084] Comparative Example 2 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.99 Mg 0.01 O2(LiCo 0.99 Mg 0.01 The amount of LiNbO3 layer on the surface of O2 is 0.99 Mg 0.01 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0085] Comparative Example 3 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.989 Mg 0.01 Ti 0.001 O2(LiCo 0.989 Mg 0.01 Ti 0.001 The amount of LiNbO3 layer on the surface of O2 is 0.989 Mg 0.01 Ti 0.001 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0086] Comparative Example 4 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.99 Al 0.01 O2(LiCo 0.99 Al 0.01 The amount of LiNbO3 layer on the surface of O2 is 0.99 Al 0.01 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0087] Comparative Example 5 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.9 Al 0.05 Mg 0.05 O2(LiCo 0.9 Al 0.05 Mg 0.05 The amount of LiNbO3 layer on the surface of O2 is0.9 Al 0.05 Mg 0.05 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0088] Comparative Example 6 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.9 Al 0.1 O2(LiCo 0.9 Al 0.1 The amount of LiNbO3 layer on the surface of O2 is 0.9 Al 0.1 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0089] Comparative Example 7 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.89 Al 0.1 Mg 0.01 O2(LiCo 0.89 Al 0.1 Mg 0.01 The amount of LiNbO3 layer on the surface of O2 is 0.89 Al 0.1 Mg 0.01 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0090] Comparative Example 8 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.9 Mg 0.1 O2(LiCo 0.9 Mg 0.1 The amount of LiNbO3 layer on the surface of O2 is 0.9 Mg 0.1 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0091] Comparative Example 9 The positive electrode active material was LiCo with an average particle size of 5 μm and a layer of LiNbO3 on the surface. 0.89 Al 0.01 Mg 0.1 O2(LiCo 0.89 Al 0.01 Mg 0.1 The amount of LiNbO3 layer on the surface of O2 is 0.89 Al 0.01 Mg 0.1 A model cell was produced in the same manner as in Example 1, except that the amount of O2 was changed to 0.5 parts by mass per 100 parts by mass of O2.

[0092] The model cells prepared in the examples and comparative examples were subjected to direct current resistance (DCR) measurement by the following method. Each model cell was charged at a constant current of 0.05 C until the voltage reached 3.68 V, then charged at a constant voltage of 0.01 C, and then discharged at a current of 0.02 C until the voltage reached 1.88 V, and the discharge capacity (initial capacity) was measured.

[0093] After the initial capacity measurement, each model cell was charged at a constant current and a constant voltage under the same conditions as the initial capacity measurement, and then discharged at a current value of 0.1 C until the depth of charge (SOC) reached 50%, after which it was left to rest for 1 hour. After that, each battery was pulse discharged at a current value of 0.1 C for 10 seconds, after which the voltage was measured, and the voltage difference before and after the pulse discharge was subtracted by the voltage drop attributable to the solid electrolyte layer and the counter electrode to determine the voltage, and the DCR was calculated from this value.

[0094] It can be said that the smaller the DCR determined by this method, the lower the internal resistance of the positive electrode used in the model cell, and the more likely it is that an all-solid-state secondary battery with excellent load characteristics can be constructed.

[0095] The composition of the lithium cobalt oxide used in the positive electrode of each model cell is shown in Table 1, and the evaluation results are shown in Table 2. 1 (Element M 1 ) column and M 2 (Element M 2The numerical values ​​in the "a+b" column respectively represent the values ​​of a, b, and c in the general formula (1), and the numerical value in the "a+b" column represents the total value of a and b.

[0096] [Table 1]

[0097] [Table 2]

[0098] As shown in Tables 1 and 2, the model cells prepared in Examples 1 to 3 had a positive electrode containing lithium cobalt oxide (A) of appropriate composition as a positive electrode active material, and had a low DCR. Therefore, with these positive electrodes, an all-solid-state secondary battery with excellent load characteristics can be constructed.

[0099] In contrast, the model cells prepared in Comparative Examples 1 to 10 had a positive electrode using lithium cobalt oxide as the positive electrode active material, the amount of the constituent elements of which did not satisfy the general formula (1), and had a higher DCR than the model cells prepared in the Examples. [Explanation of symbols]

[0100] 1,100 All-solid-state secondary battery 10 positive electrode 20 negative electrode 30 Solid electrolyte layer 40 Outer can 50 sealed cans 60 Gasket 200 Electrode body 300 Positive external terminal 400 Negative external terminal 500 Laminated film exterior

Claims

1. A positive electrode for an all-solid-state secondary battery having a molded body of a positive electrode mixture containing a positive electrode active material, a conductive assistant, and a solid electrolyte, The positive electrode active material is represented by the following general formula (1): Love 1-a-b-c Al a M 1 b M 2 c O 2 (1) [In the general formula (1), M 1 represents at least one element selected from the group consisting of Mg, Ni and Na; M 2 is at least one element selected from the group consisting of Mn, Fe, Cu, Zr, Ti, Bi, Ca, F, P, Sr, W, Ba, Nb, Si, Zn, Mo, V, Sn, Sb, Ta, Ge, Cr, K, S, and Er, and 0<a<0.1, 0<b<0.1, a+b<0.1, 0≦c≦0.05; and the lithium cobalt oxide contains a lithium cobalt oxide in which at least a part of the Co sites is substituted with the Al; The positive electrode for an all-solid-state secondary battery is characterized in that the solid electrolyte contains a sulfide-based solid electrolyte.

2. 2. The positive electrode for an all-solid-state secondary battery according to claim 1, further comprising a reaction suppression layer formed on a surface of the positive electrode active material for suppressing a reaction between the positive electrode active material and the solid electrolyte.

3. An all-solid-state secondary battery having a positive electrode, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode, An all-solid-state secondary battery comprising the positive electrode for an all-solid-state secondary battery according to claim 1 or 2 as the positive electrode.

Citation Information

Patent Citations

  • Material for positive electrode active material

    JP2010170715A

  • Lithium ion secondary battery

    JP2016062683A

  • Measurement method of water amount in sulfide solid state electrolyte

    JP2017040531A

  • Inorganic solid electrolyte material, solid electrolyte sheet, and all-solid type lithium ion battery

    JP2017168387A