Etching method and plasma processing apparatus

The etching method enhances selectivity and reduces damage by using a plasma-generated gas mixture to deposit substances at etch stop layers, improving etching efficiency and reducing distortion in silicon oxide films.

JP7576484B2Active Publication Date: 2024-10-31TOKYO ELECTRON LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021022434
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-16
Publication Date
2024-10-31
Estimated Expiration
2041-02-16

AI Technical Summary

Technical Problem

Existing etching methods struggle to achieve high selectivity when forming recesses in silicon oxide films due to the lack of effective control over the etching process, particularly when interacting with etch stop layers like tungsten and molybdenum.

Method used

An etching method involving the use of a processing gas containing tungsten or molybdenum, carbon and fluorine, and oxygen gases, which generates plasma to form recesses in a silicon oxide film, depositing substances at the etch stop layer bottoms to reduce etching rates and enhance selectivity.

Benefits of technology

The method improves etching selectivity of silicon oxide films to etch stop layers by up to 65-70% and reduces etching damage, while increasing the etching rate of the silicon oxide film by up to 8.8%, with reduced distortion and resistance changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576484000001
    Figure 0007576484000001
  • Figure 0007576484000002
    Figure 0007576484000002
  • Figure 0007576484000003
    Figure 0007576484000003
Patent Text Reader

Abstract

To provide a technique for improving the etching selectivity of a silicon oxide film to an etching stop layer.SOLUTION: An etching method includes a step (a) of providing a substrate having a silicon oxide film in a chamber. The substrate includes a plurality of etch stop layers disposed within a silicon oxide layer. The positions of the plurality of etching stop layers in the thickness direction of the silicon oxide film are different from each other. Each of the plurality of etch stop layers includes at least one of tungsten and molybdenum. The etching method further includes a step (b) of supplying, into the chamber, a process gas including a gas containing at least one of tungsten and molybdenum, a gas containing carbon and fluorine, and a gas containing oxygen, and a step (c) of forming a plurality of recesses that respectively reach the plurality of etch stop layers in the silicon oxide film by etching the silicon oxide film by generating a plasma from the process gas.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Exemplary embodiments of the present disclosure relate to an etching method and a plasma processing apparatus. [Background technology]

[0002] Patent Document 1 discloses a plasma processing method for forming a plurality of holes with different depths in a multilayer film. The multilayer film has an oxide layer and a plurality of etching stop layers made of tungsten that are arranged below the upper surface of the oxide layer in the stacking direction and at different positions in the stacking direction. A plasma is generated from a processing gas, and etching is performed from the upper surface of the oxide layer to the plurality of etching stop layers, thereby forming a plurality of holes. The processing gas contains a fluorocarbon gas, a noble gas, and nitrogen. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-90022 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides a technique for improving the etching selectivity of a silicon oxide film to an etching stop layer when forming a recess in the silicon oxide film by etching. [Means for solving the problem]

[0005] In one exemplary embodiment, an etching method includes: (a) preparing a substrate having a silicon oxide film in a chamber, the substrate including a plurality of etching stop layers disposed in the silicon oxide film, the positions of the plurality of etching stop layers in a thickness direction of the silicon oxide film being different from each other, and each of the plurality of etching stop layers including at least one of tungsten and molybdenum; (b) supplying a process gas into the chamber, the process gas including a gas including at least one of tungsten and molybdenum, a gas including carbon and fluorine, and an oxygen-containing gas; and (c) generating a plasma from the process gas to etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, the recesses reaching the plurality of etching stop layers, respectively. Effect of the Invention

[0006] According to one exemplary embodiment, a technique is provided for improving the etch selectivity of a silicon oxide film relative to an etch stop layer when etching a silicon oxide film to form a recess. [Brief description of the drawings]

[0007] [Figure 1] 1 is a flow diagram of an etching method according to an exemplary embodiment. [Diagram 2] FIG. 2 is a partially enlarged cross-sectional view of an example substrate. [Diagram 3] FIG. 2 is a partial enlarged cross-sectional view of an example substrate after etching. [Figure 4] 4 is an example of a timing chart showing the change over time of an electric bias applied to a lower electrode and an electric bias applied to an upper electrode. [Diagram 5] 1 is a schematic diagram of a plasma processing apparatus according to an exemplary embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Various exemplary embodiments are described below.

[0009] In one exemplary embodiment, an etching method includes: (a) preparing a substrate having a silicon oxide film in a chamber, the substrate including a plurality of etching stop layers disposed in the silicon oxide film, the positions of the plurality of etching stop layers in a thickness direction of the silicon oxide film being different from each other, and each of the plurality of etching stop layers including at least one of tungsten and molybdenum; (b) supplying a process gas into the chamber, the process gas including a gas including at least one of tungsten and molybdenum, a gas including carbon and fluorine, and an oxygen-containing gas; and (c) generating a plasma from the process gas to etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, the recesses reaching the plurality of etching stop layers, respectively.

[0010] According to the above etching method, in (c), when each recess reaches each etching stop layer, a substance generated from a gas containing at least one of tungsten and molybdenum in the plasma is deposited on the bottom of each recess. As a result, the etching rate of the etching stop layer is reduced, and the etching selectivity of the silicon oxide film to the etching stop layer can be improved.

[0011] In one exemplary embodiment, the gas containing at least one of tungsten and molybdenum may include at least one of tungsten hexafluoride gas and molybdenum hexafluoride gas.

[0012] In one exemplary embodiment, the pressure in the chamber in (c) may be set to 2.0 Pa or more and 3.3 Pa or less.

[0013] In one exemplary embodiment, a ratio of a flow rate of the gas containing at least one of tungsten and molybdenum in the processing gas to a flow rate of the processing gas may be 5% by volume or less.

[0014] In one exemplary embodiment, in (c), a temperature of a substrate support that supports the substrate may be set to a temperature of 0° C. or more and 120° C. or less.

[0015] In one exemplary embodiment, the process gas may include a fluorocarbon gas as the gas containing carbon and fluorine.

[0016] In one exemplary embodiment, (c) may include periodically applying a negative pulse voltage to a substrate support that supports the substrate.

[0017] In one exemplary embodiment, the absolute value of the pulse voltage applied to the substrate support in (c) may be 150V or more and 1000V or less.

[0018] In one exemplary embodiment, the pulse voltage periodically applied to the substrate support in (c) may have a duty ratio of 50% or more and 100% or less.

[0019] In one exemplary embodiment, a frequency that defines a period during which the pulse voltage is applied to the substrate support in (c) may be 100 kHz or more and 1 MHz or less.

[0020] In one exemplary embodiment, a plasma processing apparatus includes a chamber, a substrate support for supporting a substrate in the chamber, the substrate having a silicon oxide film, the substrate having a plurality of etching stop layers disposed in the silicon oxide film, the positions of the plurality of etching stop layers in a thickness direction of the silicon oxide film being different from each other, and each of the plurality of etching stop layers includes at least one of tungsten and molybdenum; a gas supply unit configured to supply a process gas including a gas containing at least one of tungsten and molybdenum, a gas containing carbon and fluorine, and an oxygen-containing gas into the chamber; a plasma generation unit configured to generate plasma from the process gas in the chamber; and a control unit, the control unit being configured to control the gas supply unit and the plasma generation unit to generate the plasma and etch the silicon oxide film to form a plurality of recesses in the silicon oxide film, the recesses reaching the plurality of etching stop layers, respectively.

[0021] Various exemplary embodiments will now be described in detail with reference to the drawings, in which the same or corresponding parts are designated by the same reference numerals.

[0022] 1 is a flow diagram of an etching method according to an exemplary embodiment. The etching method shown in FIG. 1 (hereinafter referred to as "method MT") is performed to etch a silicon oxide film of a substrate to form a recess in the silicon oxide film.

[0023] FIG. 2 is a partially enlarged cross-sectional view of an example substrate. The method MT can be applied to the substrate W shown in FIG. 2. The substrate W is, for example, a substrate for forming a three-dimensional NAND device. As shown in FIG. 2, the substrate W has a silicon oxide film SF. The substrate W may further have a mask MK and an underlayer region UR. The silicon oxide film SF is provided on the underlayer region UR. The mask MK is provided on the silicon oxide film SF. The mask MK is made of an organic material such as polycrystalline silicon or amorphous carbon. The mask MK has a pattern that is transferred to the silicon oxide film SF by etching. The mask MK has a plurality of openings OP1 to OP8. Each of the openings OP1 to OP8 has, for example, a hole pattern. In the example of FIG. 2, the diameters of the openings OP1 to OP8 are different from each other, but the diameters of the openings OP1 to OP8 may be the same as each other.

[0024] The silicon oxide film SF is made of at least one material including silicon and oxygen. The silicon oxide film SF may be made of a single layer of silicon oxide film. The substrate W includes a plurality of etching stop layers ES1 to ES8 disposed in the silicon oxide film SF. The positions of the plurality of etching stop layers ES1 to ES8 in the thickness direction of the silicon oxide film SF are different from one another, and the etching stop layers ES1 to ES8 are deeper in this order. The etching stop layer ES1 is closest to the mask MK. The silicon oxide film SF is disposed between the etching stop layer ES1 and the mask MK. The etching stop layer ES8 is closest to the underlying region UR. The silicon oxide film SF is disposed between the etching stop layer ES8 and the underlying region UR. The silicon oxide film SF is disposed between the etching stop layers (e.g., the etching stop layer ES1 and the etching stop layer ES2) adjacent to each other in the thickness direction of the silicon oxide film SF. The plurality of etching stop layers ES1 to ES8 have ends located between the corresponding plurality of openings OP1 to OP8 of the mask MK and the underlying region UR. Each of the etching stop layers ES1 to ES8 includes at least one of tungsten and molybdenum, and may be a tungsten layer or a molybdenum layer.

[0025] As shown in Fig. 1, the method MT starts with step STa. Steps STa, STb, and STc are performed in order. When step STc is completed, the method MT ends. Steps STb and STc may be performed simultaneously.

[0026] In step STa, a substrate W is prepared in a chamber of the plasma processing apparatus. The substrate W is placed on a substrate support in the chamber.

[0027] In step STb, a processing gas is supplied into a chamber of a plasma processing apparatus. The processing gas includes a gas containing at least one of tungsten and molybdenum (hereinafter referred to as a "W / Mo-containing gas"), a gas containing carbon and fluorine, and an oxygen-containing gas. The processing gas may further include an inert gas such as a noble gas.

[0028] The W / Mo-containing gas may include at least one of tungsten hexafluoride gas (WF6 gas) and molybdenum hexafluoride gas (MoF6 gas). The W / Mo-containing gas may include the same metal as that included in the etching stop layers ES1 to ES8. For example, when the etching stop layers ES1 to ES8 include tungsten, the W / Mo-containing gas may include tungsten. When the etching stop layers ES1 to ES8 include molybdenum, the W / Mo-containing gas may include molybdenum. The ratio of the flow rate of the W / Mo-containing gas to the flow rate of the process gas supplied into the chamber may be 5 vol.% or less, or may be 0.5 vol.% or more and 2.0 vol.% or less. The gas containing carbon and fluorine may include a fluorocarbon gas. The fluorocarbon gas may include one or more of C4F6 gas, C4F8 gas, C3F8 gas, and CF4 gas. The oxygen-containing gas may include one or more of O2 gas, CO gas, and CO2 gas.

[0029] In step STc, plasma is generated from a processing gas to etch the silicon oxide film SF. As a result, as shown in FIG. 3, a plurality of recesses RC1 to RC8 reaching the plurality of etching stop layers ES1 to ES8, respectively, are formed in the silicon oxide film SF. FIG. 3 is a partially enlarged cross-sectional view of the substrate W in FIG. 2 after etching. Each of the recesses RC1 to RC8 is, for example, a contact hole. Each of the recesses RC1 to RC8 has, for example, a circular shape in a cross section perpendicular to the thickness direction of the silicon oxide film SF. The diameters of the recesses RC1 to RC8 are different from one another and increase in the order of the recesses RC1 to RC8. The diameters of the recesses RC1 to RC8 are the same as the diameters of the openings OP1 to OP8 of the mask MK, respectively.

[0030] Step STc is performed while the processing gas is being supplied into the chamber in step STb. During the period in which step STc is being performed, the pressure in the chamber may be set to a pressure of 2.0 Pa or more and 3.3 Pa or less (15 mTorr or more and 25 mTorr or less). During the period in which step STc is being performed, the temperature of the substrate support may be set to a temperature of 0° C. or more and 120° C. or less. If the temperature of the substrate support in step STc is lower than 0° C., the adhesion coefficient of the deposits to the mask MK is high, so clogging due to the deposits on the mask MK may occur, which may result in poor etching. Also, if the temperature of the substrate support in step STc is higher than 120° C., the adhesion coefficient of the deposits to the mask MK is low, so the amount of deposits in the recesses RC1 to RC8 becomes excessive, which may result in poor etching.

[0031] The etching of the silicon oxide film SF in the step STc may be stopped at the etching stop layers ES1 to ES8. In the step STc, when the recesses RC1 to RC8 reach the etching stop layers ES1 to ES8, respectively, a substance generated from the W / Mo-containing gas in the plasma is deposited on the bottom of the recesses RC1 to RC8. As a result, it is estimated that a deposition film DP is formed. The substance generated from the W / Mo-containing gas in the plasma is, for example, a radical containing tungsten or a radical containing molybdenum. It is estimated that the deposition film DP is also formed on the side walls of the recesses RC1 to RC8 near the bottom of the recesses RC1 to RC8. It is estimated that the deposition film DP is also formed on the upper surface of the mask MK and the side walls of the openings OP1 to OP8.

[0032] According to the method MT, the etching of the etching stop layers ES1 to ES8 is suppressed. This is presumed to be because the deposition film DP is formed on the bottom of the recesses RC1 to RC8. As a result, the etching rate of the etching stop layers ES1 to ES8 is reduced, and the etching selectivity of the silicon oxide film SF to the etching stop layers ES1 to ES8 can be improved. In one example, when WF6 gas is used, the etching selectivity of the silicon oxide film to the etching stop layers is increased by 65% ​​compared to when WF6 gas is not used. Also, the etching of the mask MK is suppressed. This is presumed to be because the deposition film DP is formed on the surface of the mask MK. As a result, the etching rate of the mask MK is reduced, and the etching selectivity of the silicon oxide film SF to the mask MK can be improved. In one example, when WF6 gas is used, the etching selectivity of the silicon oxide film to the mask is increased by 70% compared to when WF6 gas is not used. Therefore, the etching rate of the silicon oxide film SF can be increased while keeping the reduction amount of the mask MK and the etching stop layers ES1 to ES8 due to etching small. Furthermore, when the W / Mo-containing gas contains fluorine, fluorine radicals generated in the plasma promote the etching of the silicon oxide film SF. Therefore, the etching rate of the silicon oxide film SF can be increased. In one example, when WF6 gas is used, the etching rate of the silicon oxide film increases by 8.8% compared to when WF6 gas is not used. Furthermore, when the W / Mo-containing gas is used, the distortion of the shape of the bottom of the recesses RC1 to RC8 can be reduced. In one example, when WF6 gas is used, an index indicating the smallness of distortion increases by 87% compared to when WF6 gas is not used. The index indicating the smallness of distortion is a value obtained by dividing the minimum diameter of the bottom of a circular recess by the maximum diameter.

[0033] When the W / Mo-containing gas contains the same metal as that contained in the etching stop layers ES1-ES8, the change in the resistance value of the etching stop layers ES1-ES8 due to the metal (e.g., the deposited film DP) is small. Therefore, when the conductor portion filled in the recesses RC1-RC8 contains the same metal as that contained in the etching stop layers ES1-ES8, the resistance value between the conductor portion and the etching stop layers ES1-ES8 can be reduced. Also, etching damage to the etching stop layers ES1-ES8 is repaired by the metal (e.g., the deposited film DP).

[0034] FIG. 4 is an example of a timing chart showing the time change of the electric bias applied to the lower electrode and the electric bias applied to the upper electrode. This timing chart is related to step STc in the method MT. Step STc may include periodically generating a negative potential on the substrate W by applying an electric bias EB (negative pulse voltage) to a substrate support supporting the substrate W. In one example, as shown in FIG. 4, a negative DC voltage is periodically applied to the lower electrode of the substrate support with a period CY as the electric bias EB. The period CY includes a period PA and a period PB. The negative DC voltage is applied to the lower electrode of the substrate support in the period PA. In the period PB, the application of the negative DC voltage to the lower electrode of the substrate support is stopped. The absolute value of the negative DC voltage applied to the lower electrode of the substrate support in the period PA may be 150V or more and 1000V or less. The ratio of the period PA in the cycle CY, i.e., the duty ratio of the negative DC voltage periodically applied to the lower electrode in the step STc, may be 50% or more and 100% or less. The duty ratio may be 60% or more and 80% or less. The frequency defining the cycle CY may be 100 kHz or more and 1 MHz or less. The frequency defining the cycle CY may be 300 kHz or more and 800 kHz or less. The time length of the cycle CY is the reciprocal of the frequency defining the cycle CY. Although the electric bias EB is depicted as a rectangular wave in FIG. 4, it may be depicted as a triangular wave or an impulse.

[0035] In one embodiment, the plasma processing apparatus used in the method MT may be a capacitively coupled plasma processing apparatus. That is, the plasma processing apparatus may further include an upper electrode. The upper electrode is provided above the substrate support. In the step STc, another electric bias DCS may be applied to the upper electrode. Specifically, as shown in FIG. 4, in the step STc, a negative DC voltage is applied to the upper electrode as the electric bias DCS in a period PB in a cycle CY. Note that, in the period PA, the application of the negative DC voltage to the upper electrode may be stopped. Alternatively, the absolute value of the negative DC voltage applied to the upper electrode in the period PA may be smaller than the absolute value of the negative DC voltage applied to the upper electrode in the period PB.

[0036] A plasma processing apparatus that can be used to perform the method MT will be described below. Fig. 5 is a diagram that shows a schematic diagram of a plasma processing apparatus according to an exemplary embodiment. The plasma processing apparatus 1 shown in Fig. 5 can be used in the method MT. The plasma processing apparatus 1 is a capacitively coupled plasma processing apparatus.

[0037] The plasma processing apparatus 1 includes a chamber 10. The chamber 10 provides an internal space 10s therein. The central axis of the chamber 10 is an axis AX extending in the vertical direction. In one embodiment, the chamber 10 includes a chamber body 12. The chamber body 12 has a substantially cylindrical shape. The internal space 10s is provided in the chamber body 12. The chamber body 12 is made of, for example, aluminum. The chamber body 12 is electrically grounded. A corrosion-resistant film is provided on the inner wall surface of the chamber body 12. The corrosion-resistant film may be a film made of a ceramic such as aluminum oxide or yttrium oxide.

[0038] The chamber body 12 provides a passage 12p in its sidewall. The substrate W passes through the passage 12p when being transferred between the internal space 10s and the outside of the chamber 10. The passage 12p can be opened and closed by a gate valve 12g. The gate valve 12g is provided along the sidewall of the chamber body 12.

[0039] The plasma processing apparatus 1 further includes a substrate support 16. The substrate support 16 is configured to support a substrate W in the chamber 10. The substrate W may have a substantially disk-like shape. The substrate support 16 may be supported by a support 15. The support 15 extends upward from the bottom of the chamber body 12. The support 15 has a substantially cylindrical shape. The support 15 is made of an insulating material such as quartz.

[0040] The substrate support 16 includes a lower electrode 18. The substrate support 16 may further include an electrostatic chuck 20. The substrate support 16 may further include an electrode plate 19. The electrode plate 19 is made of a conductive material such as aluminum. The electrode plate 19 has a substantially disk-like shape, and its central axis is an axis line AX. The lower electrode 18 is provided on the electrode plate 19. The lower electrode 18 is made of a conductive material such as aluminum. The lower electrode 18 has a substantially disk-like shape, and its central axis is an axis line AX. The lower electrode 18 is electrically connected to the electrode plate 19.

[0041] The lower electrode 18 provides a flow path 18f therein. The flow path 18f is a flow path for a heat exchange medium (e.g., a coolant). The flow path 18f receives the heat exchange medium from a supply device (e.g., a chiller unit) via a pipe 23a. This supply device is provided outside the chamber 10. The heat exchange medium supplied to the flow path 18f flows through the flow path 18f and is returned to the supply device via a pipe 23b. The supply device for the heat exchange medium constitutes a temperature adjustment mechanism of the plasma processing device 1.

[0042] The electrostatic chuck 20 is provided on the lower electrode 18. The substrate W is placed on the upper surface of the electrostatic chuck 20. The electrostatic chuck 20 has a body and an electrode (chuck electrode). The body of the electrostatic chuck 20 is formed from a dielectric material. The electrostatic chuck 20 and its body each have a substantially disk shape, and their central axes are axis lines AX. The chuck electrode of the electrostatic chuck 20 is a film-like electrode and is provided in the body of the electrostatic chuck 20. The chuck electrode of the electrostatic chuck 20 is connected to a DC power supply via a switch. When a voltage from the DC power supply is applied to the electrode of the electrostatic chuck 20, an electrostatic attractive force is generated between the electrostatic chuck 20 and the substrate W. The generated electrostatic attractive force attracts the substrate W to the electrostatic chuck 20 and the substrate W is held by the electrostatic chuck 20. As described below, when a bias electrode is provided in the electrostatic chuck 20, a chuck electrode may be provided on the front surface side of the electrostatic chuck 20 (the surface on which the substrate W is placed), and a bias electrode may be provided on the back surface side of the electrostatic chuck 20 (the surface facing the lower electrode 18).

[0043] The substrate support 16 may further support an edge ring ER disposed thereon. The edge ring ER may be made of silicon, silicon carbide, or quartz. The substrate W is disposed on the electrostatic chuck 20 and within a region surrounded by the edge ring ER.

[0044] The plasma processing apparatus 1 may further include a gas supply line 25. The gas supply line 25 supplies a heat transfer gas (e.g., He gas) from a gas supply mechanism to the gap between the upper surface of the electrostatic chuck 20 and the rear surface (lower surface) of the substrate W.

[0045] The plasma processing apparatus 1 may further include a cylindrical portion 28 and an insulating portion 29. The cylindrical portion 28 extends upward from the bottom of the chamber body 12. The cylindrical portion 28 extends along the outer periphery of the support 15. The cylindrical portion 28 is made of a conductive material and has a substantially cylindrical shape. The cylindrical portion 28 is electrically grounded. The insulating portion 29 is provided on the cylindrical portion 28. The insulating portion 29 is made of a material having insulating properties. The insulating portion 29 is made of a ceramic such as quartz. The insulating portion 29 has a substantially cylindrical shape. The insulating portion 29 extends along the outer periphery of the electrode plate 19, the outer periphery of the lower electrode 18, and the outer periphery of the electrostatic chuck 20.

[0046] The plasma processing apparatus 1 further includes an upper electrode 30. The upper electrode 30 is provided above the substrate support 16. The upper electrode 30 is supported on the upper part of the chamber body 12 via a member 32. The member 32 is made of an insulating material. The upper electrode 30 and the member 32 close the upper opening of the chamber body 12.

[0047] The upper electrode 30 may include a top plate 34 and a support 36. The bottom surface of the top plate 34 is the bottom surface on the side of the internal space 10s and defines the internal space 10s. The top plate 34 may be made of a low-resistance conductor or semiconductor with little Joule heat. In one embodiment, the top plate 34 is made of silicon. The top plate 34 provides a plurality of gas holes 34a. The plurality of gas holes 34a penetrate the top plate 34 in the plate thickness direction.

[0048] The support 36 detachably supports the top plate 34. The support 36 is made of a conductive material such as aluminum. The support 36 provides a gas diffusion chamber 36a therein. The support 36 further provides a plurality of gas holes 36b. The plurality of gas holes 36b extend downward from the gas diffusion chamber 36a. The plurality of gas holes 36b communicate with the plurality of gas holes 34a, respectively. The support 36 further provides a gas inlet 36c. The gas inlet 36c is connected to the gas diffusion chamber 36a. A gas supply pipe 38 is connected to the gas inlet 36c.

[0049] A gas source group 40 is connected to the gas supply pipe 38 via a valve group 41, a flow rate controller group 42, and a valve group 43. The gas source group 40, the valve group 41, the flow rate controller group 42, and the valve group 43 constitute a gas supply unit GS. The gas source group 40 includes a plurality of gas sources. The gas sources of the gas source group 40 include a plurality of gas sources used in the method MT. Each of the valve group 41 and the valve group 43 includes a plurality of opening and closing valves. The flow rate controller group 42 includes a plurality of flow rate controllers. Each of the plurality of flow rate controllers of the flow rate controller group 42 is a mass flow controller or a pressure control type flow rate controller. Each of the plurality of gas sources of the gas source group 40 is connected to the gas supply pipe 38 via a corresponding opening and closing valve of the valve group 41, a corresponding flow rate controller of the flow rate controller group 42, and a corresponding opening and closing valve of the valve group 43.

[0050] The plasma processing apparatus 1 may further include a shield 46. The shield 46 is detachably provided along the inner wall surface of the chamber body 12. The shield 46 prevents by-products of the plasma processing from adhering to the chamber body 12. The shield 46 is configured by forming a corrosion-resistant film on the surface of a member made of, for example, aluminum. The corrosion-resistant film may be a film made of a ceramic such as yttrium oxide.

[0051] The plasma processing apparatus 1 may further include a baffle member 48. The baffle member 48 is provided between a member (e.g., the cylindrical portion 28) surrounding the substrate support 16 and the shield 46. The baffle member 48 is formed by forming a corrosion-resistant film on the surface of a member made of, for example, aluminum. The corrosion-resistant film may be a film made of ceramic such as yttrium oxide. The baffle member 48 has a plurality of through holes. An exhaust port is provided below the baffle member 48 and at the bottom of the chamber body 12. An exhaust device 50 is connected to the exhaust port via an exhaust pipe 52. The exhaust device 50 has a pressure adjustment valve and a vacuum pump such as a turbo molecular pump.

[0052] The plasma processing apparatus 1 further includes a high-frequency power supply 61 and a pulse power supply 62. The high-frequency power supply 61 is configured to generate high-frequency power (hereinafter, referred to as "high-frequency power HF"). The high-frequency power HF has a frequency suitable for generating plasma. The frequency of the high-frequency power HF is, for example, 27 MHz or more and 100 MHz or less. The high-frequency power supply 61 is connected to the lower electrode 18 via a matching device 61m. The matching device 61m has a circuit for matching the impedance of the load side (lower electrode 18 side) of the high-frequency power supply 61 to the output impedance of the high-frequency power supply 61. In one embodiment, the high-frequency power supply 61 constitutes a plasma generating unit. The high-frequency power supply 61 may be connected to the upper electrode 30 via the matching device 61m.

[0053] The pulsed power supply 62 is configured to apply the above-mentioned electric bias EB to the lower electrode 18. That is, the pulsed power supply 62 is configured to generate a negative potential on the substrate W as the electric bias EB in step STc of the method MT. The pulsed power supply 62 may be configured to periodically apply the electric bias EB to the lower electrode 18 by itself, or may be configured to include a device for pulsing the electric bias EB downstream of the pulsed power supply 62. As described above, the electric bias EB from the pulsed power supply 62 is applied to the lower electrode 18 during the period PA in the cycle CY. During the period PB in the cycle CY, the application of the electric bias EB from the pulsed power supply 62 to the lower electrode 18 is stopped. Note that the pulsed power supply 62 may be configured to apply the electric bias EB to a bias electrode provided in the electrostatic chuck 20 instead of the lower electrode 18.

[0054] In one embodiment, the plasma processing apparatus 1 may further include a DC power supply 70. The DC power supply 70 is configured to apply the above-mentioned electric bias DCS to the upper electrode 30. That is, the DC power supply 70 is configured to periodically apply a negative DC voltage to the upper electrode 30 as the electric bias DCS. As described above, the negative DC voltage from the DC power supply 70 is applied to the upper electrode 30 in the period PB in the cycle CY. In the period PA in the cycle CY, the application of the negative DC voltage from the DC power supply 70 to the upper electrode 30 may be stopped. Alternatively, the absolute value of the negative DC voltage applied to the upper electrode in the period PA may be smaller than the absolute value of the negative DC voltage applied to the upper electrode in the period PB.

[0055] The plasma processing apparatus 1 may further include a control unit 80. The control unit 80 is a computer including a processor, a storage device, an input device, a display device, etc., and controls each part of the plasma processing apparatus 1. Specifically, the control unit 80 executes a control program stored in the storage device, and controls each part of the plasma processing apparatus 1 based on recipe data stored in the storage device. Under the control of the control unit 80, a process specified by the recipe data is executed in the plasma processing apparatus 1. The method MT can be executed in the plasma processing apparatus 1 under the control of the control unit 80 for each part of the plasma processing apparatus 1.

[0056] When the method MT is applied to the substrate W using the plasma processing apparatus 1, in step STa, the substrate W is placed on the substrate support 16. In the subsequent step STb, the control unit 80 controls the gas supply unit GS to supply the above-mentioned processing gas into the chamber 10. In the subsequent step STc, the control unit 80 controls the exhaust unit 50 to set the pressure in the chamber 10 to a designated pressure. In addition, in the step STc, the control unit 80 controls the plasma generation unit to generate plasma from the processing gas in the chamber 10. Specifically, the control unit 80 controls the high-frequency power supply 61 to supply high-frequency power HF. In addition, in the step STc, the control unit 80 may control the pulse power supply 62 to periodically apply a negative DC voltage as the electric bias EB to the lower electrode 18. In the step STc, the control unit 80 may control the DC power supply 70 to periodically apply a negative DC voltage as the above-mentioned electric bias DCS to the upper electrode 30.

[0057] Although various exemplary embodiments have been described above, the present invention is not limited to the above-described exemplary embodiments, and various additions, omissions, substitutions, and modifications may be made. In addition, elements in different embodiments can be combined to form other embodiments.

[0058] For example, the plasma processing apparatus used in the method MT may be a type of plasma processing apparatus other than the capacitively coupled type, such as an inductively coupled plasma processing apparatus, an electron cyclotron resonance (ECR) plasma processing apparatus, or a plasma processing apparatus that generates plasma using surface waves such as microwaves.

[0059] From the foregoing, it will be understood that various embodiments of the present disclosure have been described herein for purposes of illustration, and that various modifications may be made without departing from the scope and spirit of the present disclosure. Accordingly, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims. [Explanation of symbols]

[0060] 1...plasma processing apparatus, 10...chamber, 16...substrate support, 61...high frequency power supply, 80...control unit, ES1 to ES8...etching stop layer, GS...gas supply unit, RC1 to RC8...recess, SF...silicon oxide film, W...substrate.

Claims

1. (a) preparing a substrate having a silicon oxide film in a chamber, the substrate including a plurality of etch stop layers disposed in the silicon oxide film, the positions of the plurality of etch stop layers in a thickness direction of the silicon oxide film being different from each other, and each of the plurality of etch stop layers including at least one of tungsten and molybdenum; (b) supplying a process gas into the chamber, the process gas comprising a molybdenum-containing gas, a carbon- and fluorine-containing gas, and an oxygen-containing gas; (c) generating a plasma from the processing gas to etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, each of which reaches the plurality of etching stop layers; An etching method comprising:

2. A method of manufacturing a semiconductor device comprising the steps of: (a) preparing a substrate having a silicon oxide film in a chamber, the substrate comprising a plurality of etch stop layers disposed in the silicon oxide film, the positions of the plurality of etch stop layers in a thickness direction of the silicon oxide film being different from one another, and each of the plurality of etch stop layers including at least one of tungsten and molybdenum; (b) supplying a process gas into the chamber, the process gas including a gas containing at least one of tungsten and molybdenum, a gas containing carbon and fluorine, and an oxygen-containing gas; (c) generating a plasma from the processing gas to etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, each of which reaches the plurality of etching stop layers; Including, The etching method, wherein the step (c) includes periodically applying a negative pulse voltage to a substrate support that supports the substrate.

3. A method of manufacturing a semiconductor device comprising the steps of: (a) preparing a substrate having a silicon oxide film in a chamber, the substrate comprising a plurality of etch stop layers disposed in the silicon oxide film, the positions of the plurality of etch stop layers in a thickness direction of the silicon oxide film being different from one another, and each of the plurality of etch stop layers including at least one of tungsten and molybdenum; (b) supplying a process gas into the chamber, the process gas including a gas containing at least one of tungsten and molybdenum, a gas containing carbon and fluorine, and an oxygen-containing gas; (c) generating a plasma from the processing gas to etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, the recesses each reaching the plurality of etching stop layers, the diameters of the recesses differing depending on the depths of the recesses; An etching method comprising:

4. 4. The etching method according to claim 2, wherein the gas containing at least one of tungsten and molybdenum includes at least one of tungsten hexafluoride gas and molybdenum hexafluoride gas.

5. 5. The etching method according to claim 1, wherein the pressure inside the chamber in step (c) is set to 2.0 Pa or more and 3.3 Pa or less.

6. 5. The etching method according to claim 2, wherein a ratio of a flow rate of the gas containing at least one of tungsten and molybdenum in the processing gas to a flow rate of the processing gas is 5 volume % or less.

7. 7. The etching method according to claim 1, wherein in (c), a temperature of a substrate support that supports the substrate is set to a temperature of 0° C. or more and 120° C. or less.

8. 8. The etching method according to claim 1, wherein the process gas contains a fluorocarbon gas as the gas containing carbon and fluorine.

9. 4. The etching method according to claim 1, wherein the step (c) includes periodically applying a negative pulse voltage to a substrate support that supports the substrate.

10. 10. The etching method according to claim 2, wherein an absolute value of the pulse voltage applied to the substrate support in (c) is 150 V or more and 1000 V or less.

11. 11. The etching method according to claim 2, wherein the pulse voltage periodically applied to the substrate support in (c) has a duty ratio of 50% or more and 100% or less.

12. 12. The etching method according to claim 2, wherein in (c), a frequency that defines a period during which the pulse voltage is applied to the substrate support is 100 kHz or more and 1 MHz or less.

13. A chamber; a substrate support for supporting a substrate in the chamber, the substrate having a silicon oxide film, the substrate including a plurality of etch stop layers disposed in the silicon oxide film, the positions of the plurality of etch stop layers in a thickness direction of the silicon oxide film being different from each other, and each of the plurality of etch stop layers including at least one of tungsten and molybdenum; a gas supply configured to supply a process gas into the chamber, the process gas comprising a molybdenum-containing gas, a carbon- and fluorine-containing gas, and an oxygen-containing gas; a plasma generating unit configured to generate a plasma from the process gas in the chamber; A control unit; Equipped with the control unit is configured to control the gas supply unit and the plasma generation unit so as to generate the plasma and etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, each of which reaches the plurality of etching stop layers.

14. A chamber; a substrate support for supporting a substrate in the chamber, the substrate having a silicon oxide film, the substrate including a plurality of etch stop layers disposed in the silicon oxide film, the positions of the plurality of etch stop layers in a thickness direction of the silicon oxide film being different from each other, and each of the plurality of etch stop layers including at least one of tungsten and molybdenum; a gas supply configured to supply a process gas into the chamber, the process gas including a gas containing at least one of tungsten and molybdenum, a gas containing carbon and fluorine, and an oxygen-containing gas; a plasma generating unit configured to generate a plasma from the process gas in the chamber; A control unit; Equipped with the control unit is configured to control the gas supply unit and the plasma generation unit so as to periodically apply a negative pulse voltage to the substrate support, generate the plasma, and etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, each of which reaches the plurality of etching stop layers.

15. A chamber, a substrate support for supporting a substrate in the chamber, the substrate having a silicon oxide film, the substrate including a plurality of etch stop layers disposed in the silicon oxide film, the positions of the plurality of etch stop layers in a thickness direction of the silicon oxide film being different from each other, and each of the plurality of etch stop layers including at least one of tungsten and molybdenum; a gas supply configured to supply a process gas into the chamber, the process gas including a gas containing at least one of tungsten and molybdenum, a gas containing carbon and fluorine, and an oxygen-containing gas; a plasma generating unit configured to generate a plasma from the process gas in the chamber; A control unit; Equipped with the control unit is configured to control the gas supply unit and the plasma generation unit so as to generate the plasma and etch the silicon oxide film, thereby forming a plurality of recesses in the silicon oxide film, each of which reaches a plurality of etching stop layers, and diameters of the plurality of recesses vary depending on depths of the plurality of recesses.

Citation Information

Patent Citations

  • Dry etching

    JP1988148637A

  • Dry etching method and manufacture of semiconductor device using it

    JP1992032228A

  • Plasma processing method and apparatus

    JP2014090022A

  • Dry etching method and manufacturing method of semiconductor device

    JP2018085389A

  • Control method and plasma processing apparatus

    JP2020025083A