Optical Components

The optical component with a cyclic olefin ring-opening polymer maintains high refractive index stability under high temperatures, addressing refractive index changes in camera lenses.

JP7576494B2Active Publication Date: 2024-10-31MITSUI CHEMICALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021043615
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-10-31
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Cyclic olefin copolymers used in optical components like camera lenses suffer from refractive index changes under high-temperature environments, affecting optical performance over time.

Method used

An optical component comprising a cyclic olefin ring-opening polymer with specific structural units (a and b) having a glass transition temperature of 140°C or higher and a refractive index of 1.5340 or more, maintaining a refractive index change of 0.0020 or less after heating at 125°C for 168 hours.

Benefits of technology

The optical component maintains a high refractive index and excellent long-term reliability under high-temperature conditions, suitable for automotive and mobile device camera lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576494000001
    Figure 0007576494000001
  • Figure 0007576494000002
    Figure 0007576494000002
  • Figure 0007576494000003
    Figure 0007576494000003
Patent Text Reader

Abstract

To provide an optical component having a high refractive index, and excellent long-term reliability of optical performance under high temperature environment.SOLUTION: The optical component including a cyclic olefin-based ring-opened polymer (A) is provided, the cyclic olefin-based ring-opened polymer (A) has one structural unit (a) represented by a specific general formula (I), and at least one structural unit (b) represented by a specific general formula (II), the content of the structural unit (a) is 20 mol% or more and 90 mol% or less when the total content of the structural unit (a) and the structural unit (b) is 100 mol%, the glass transition point (Tg) of the cyclic olefin-based ring-opened polymer (A) measured by a differential scanning calorimeter is 140°C or higher, the refractive index (nd) of the cyclic olefin-based ring-opened polymer (A) at a wave length of 589 nm is 1.5340 or more, and when the cyclic olefin-based ring-opened polymer (A) is heated at 125°C for 168 hours, the difference (Δnd) of the refractive indexes before and after being heated, is 0.0020 or smaller.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical component. [Background technology]

[0002] Cyclic olefin copolymers have excellent optical performance and are therefore used as optical components such as optical lenses, etc. Examples of techniques relating to cyclic olefin resin compositions used for optical components include those described in Patent Documents 1 and 2.

[0003] Patent Document 1 discloses a resin composition containing a cyclic olefin resin having a repeating unit containing an alicyclic structure in the molecule, with a weight average molecular weight (Mw) of more than 15,000 and not more than 150,000, and with a ratio of the number of carbon atoms to the number of hydrogen atoms in the repeating unit having a ring structure (number of carbon atoms / number of hydrogen atoms) of 0.60 to 0.70, and a ring-structure-containing hydrocarbon oligomer obtained by cationic polymerization of a cyclic olefin monomer, with a weight average molecular weight (Mw) of more than 500 and not more than 15,000, in a weight ratio (cyclic olefin resin:ring-structure-containing hydrocarbon oligomer) in the range of 99:1 to 30:70.

[0004] Furthermore, Patent Document 2 discloses a cyclic olefin copolymer having an aromatic ring, which contains a specific structural unit (A). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-69448 A [Patent Document 2] JP 2020-105323 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, the demand for in-vehicle camera lenses and camera lenses for mobile devices (mobile phones, smartphones, tablets, etc.) has been increasing. High heat resistance is required for in-vehicle camera lenses and camera lenses for mobile devices. Cyclic olefin copolymers are widely used in optical components such as camera lenses due to their excellent optical and mechanical properties. However, according to the investigations of the present inventors, it has been found that when an optical component containing a cyclic olefin-based copolymer is exposed to a high-temperature environment for a long period of time, the refractive index may change, which may affect the optical performance.

[0007] The present invention has been made in view of the above circumstances, and provides an optical component that has a high refractive index and is excellent in long-term reliability of optical performance even in a high-temperature environment. [Means for solving the problem]

[0008] According to the present invention, there is provided the following optical component.

[0009] [1] An optical component comprising a cyclic olefin ring-opening polymer (A), The cyclic olefin ring-opening polymer (A) is At least one structural unit (a) represented by the following general formula (I), At least one structural unit (b) represented by the following general formula (II), having When the total content of the structural unit (a) and the structural unit (b) is taken as 100 mol %, the content of the structural unit (a) is 20 mol % or more and 90 mol % or less, the glass transition temperature (Tg) of the cyclic olefin ring-opening polymer (A) is 140° C. or higher as measured by a differential scanning calorimeter (DSC); The refractive index (n d ) is greater than or equal to 1.5340, The cyclic olefin ring-opening polymer (A) was heated at 125° C. for 168 hours, and the difference in refractive index of the optical component before and after heating (Δn d) is 0.0020 or less. [ka] (In the above formula (I), R 7 ~R 10 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 ~R 10 may be bonded to each other to form a monocyclic or polycyclic ring, the monocyclic or polycyclic ring may have a double bond, or the monocyclic or polycyclic ring may be an aromatic ring. [ka] (In the above formula (II), R 1 ~R 6 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 1 ~R 6 may be bonded to each other to form a monocyclic or polycyclic ring, the monocyclic or polycyclic ring may have a double bond, or the monocyclic or polycyclic ring may be an aromatic ring. [2] The optical component according to the above [1], The structural unit (a) is tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-Dodecene derived optical component. [3] The optical component according to the above [1] or [2], An optical component, wherein the structural unit (b) is derived from at least one compound selected from the group consisting of indene norbornene and dicyclopentadiene. [4] The optical component according to any one of the above [1] to [3], The optical component is an fθ lens, an imaging lens, a sensor lens, a prism, or a light guide plate. [5] The optical component according to any one of the above [1] to [4], An optical component which is a vehicle mounted camera lens or a camera lens for a mobile device. Effect of the Invention

[0010] According to the present invention, there is provided an optical component which has a high refractive index and excellent long-term reliability of optical performance even in a high-temperature environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the present invention will be described based on the embodiments. In the present embodiments, "A to B" indicating a numerical range means A or more and B or less unless otherwise specified.

[0012] <Optical components> First, the optical component according to this embodiment will be described. The optical component according to the present embodiment is an optical component containing a cyclic olefin ring-opening polymer (A), The cyclic olefin ring-opening polymer (A) is At least one structural unit (a) represented by the following general formula (I), At least one structural unit (b) represented by the following general formula (II), having When the total content of the structural unit (a) and the structural unit (b) is taken as 100 mol %, the content of the structural unit (a) is 20 mol % or more and 90 mol % or less, the glass transition temperature (Tg) of the cyclic olefin ring-opening polymer (A) is 140° C. or higher as measured by a differential scanning calorimeter (DSC); The refractive index (n d ) is greater than or equal to 1.5340, The ring-opening polymer (A) was heated at 125° C. for 168 hours, and the difference in refractive index of the optical component before and after heating (Δn d) is 0.0020 or less.

[0013] [ka]

[0014] In the above formula (I), R 7 ~R 10 R may be the same or different and are a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 ~R 10 may be bonded to each other to form a monocycle or polycycle, and the monocycle or polycycle may have a double bond, or the monocycle or polycycle may be an aromatic ring.

[0015] [ka]

[0016] In the above formula (II), R 1 ~R 6 R may be the same or different and are a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 1 ~R 6 may be bonded to each other to form a monocycle or polycycle, and the monocycle or polycycle may have a double bond, or the monocycle or polycycle may be an aromatic ring.

[0017] According to the studies of the present inventors, it has been found that when an optical component containing a cyclic olefin-based ring-opening polymer is exposed to a high-temperature environment for a long period of time, the refractive index may change, which may affect the optical performance. The present inventors have conducted extensive research to solve the above problems. As a result, it has been discovered that a ring-opening polymer (A) has at least one structural unit (a) represented by the above general formula (I) and at least one structural unit (b) represented by the above general formula (II), and when the total content of the structural unit (a) and the structural unit (b) is taken as 100 mol%, the content of the structural unit (a) is 20 mol% or more and 90 mol% or less, the glass transition temperature (Tg) of the ring-opening polymer (A) is 140° C. or more as measured by a differential scanning calorimeter (DSC), and the refractive index (n d ) is 1.5340 or more, and when the ring-opening polymer (A) is heated at 125° C. for 168 hours, the difference in refractive index of the optical component before and after heating (Δn d It has been discovered that optical components having a refractive index of 0.0020 or less have a high refractive index, are resistant to a decrease in the refractive index even when exposed to a high-temperature environment for a long period of time, and have excellent long-term reliability of optical performance.

[0018] That is, the optical component of this embodiment has a high refractive index and is excellent in long-term reliability of optical performance even in a high-temperature environment.

[0019] The lower limit of the content of the cyclic olefin ring-opening polymer (A) in the optical component according to this embodiment is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, still more preferably 90% by mass or more, and particularly preferably 95% by mass or more, when the entire optical component is taken as 100% by mass. By having the content of the cyclic olefin ring-opening polymer (A) in the optical component according to this embodiment be equal to or more than the above lower limit, the optical performance can be further improved. The upper limit of the content of the cyclic olefin ring-opening polymer (A) in the optical component according to this embodiment is not particularly limited, but is, for example, 100 mass % or less.

[0020] The optical component according to this embodiment contains the cyclic olefin ring-opening polymer (A), and therefore has excellent optical performance. Therefore, it can be suitably used as an optical component in an optical system that requires highly accurate recognition of an image. The optical component is a component used in optical equipment, and specifically includes a sensor lens, which is a lens used in various sensors, a pickup lens, a projector lens, a prism lens, an fθ lens, an imaging lens, a light guide plate, and the like. From the viewpoint of the effect according to this embodiment, it can be suitably used in an fθ lens, an imaging lens, a sensor lens, a prism, or a light guide plate.

[0021] The cyclic olefin ring-opening polymer (A) according to the present embodiment has a glass transition point of 140° C. or higher as measured by differential scanning calorimetry (DSC). The upper limit of the glass transition temperature is not particularly limited, but is preferably 180° C. or lower. When the glass transition temperature is in such a range, the cyclic olefin ring-opening polymer (A) has high heat resistance while satisfying moist heat resistance. Therefore, optical parts containing the cyclic olefin ring-opening polymer (A) can be particularly suitably used for optical parts that require heat resistance, such as in-vehicle camera lenses and camera lenses for mobile devices (mobile phones, smartphones, tablets, etc.). Examples of in-vehicle camera lenses and camera lenses for mobile devices include view cameras, sensing camera lenses, light converging lenses for head-up displays, and light diffusing lenses for head-up displays.

[0022] The optical component according to this embodiment may be combined with a second optical component different from the above optical component. The second optical component is not particularly limited, but for example, an optical component made of at least one type of resin selected from polycarbonate resin and polyester resin can be used.

[0023] The surface of the optical component according to this embodiment may be provided with a coating layer such as an anti-reflection layer or a hard coat layer as necessary. The anti-reflection layer may be a single layer or a multilayer, and may be an organic or inorganic material, preferably an inorganic material. Specific examples include oxides or fluorides such as silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, cerium oxide, tantalum oxide, magnesium oxide, and magnesium fluoride. The film formation method is not particularly limited, but the anti-reflection layer can be formed on the surface of the optical lens by a method such as vacuum deposition or sputtering. A water-repellent layer or other functional layers may or may not be provided on the antireflection layer. If necessary, a buffer layer may be formed between the lens surface and the antireflection layer to prevent cracks in the antireflection layer due to thermal expansion. The buffer layer may be coated with amorphous silica, acrylic resin, or the like. The coating method is not particularly limited, but examples of the coating method include a method in which a coating liquid is formed by dispersing or dissolving the substance to be coated in a solvent in which the substance can be dissolved or dissolved, and then applying the coating liquid by a method such as spin coating, or a method using vapor deposition. The coating layer and the buffer layer may be formed before or after the annealing treatment.

[0024] Each component will be specifically described below.

[0025] [Cyclic olefin ring-opening polymer (A)] The cyclic olefin ring-opening polymer (A) has at least one structural unit (a) represented by the above general formula (I) and at least one structural unit (b) represented by the above general formula (II). When the total content of the structural units (a) and (b) is taken as 100 mol%, the content of the structural unit (a) is 20 mol% or more and 90 mol% or less. If the content of the structural unit (a) is within the above range, the refractive index of the obtained optical component can be 1.5340 or more, and the change in the refractive index before and after a heating test can be suppressed to 0.0020 or less.

[0026] (Structural unit (a)) At least one structural unit (a) represented by the above general formula (I) is a ring-opening polymer derived from the following general formula (III). The ring-opening polymer can be obtained by ring-opening metathesis polymerization. The ring-opening metathesis polymerization can be carried out by a known method such as that described in JP-A-2016-69448.

[0027] [ka]

[0028] In the above formula (III), R 7 ~R 10 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 ~R 10 may be bonded to each other to form a monocycle or polycycle, and the monocycle or polycycle may have a double bond, or the monocycle or polycycle may be an aromatic ring.

[0029] In this embodiment, the structural unit (a) is tetracyclo[4.4.0.1 2,5 .1 7,10 It is preferable that the structural unit (a) is derived from ]-3-dodecene. Specifically, it means a structural unit represented by the following formula (a-1). That is, the structural unit (a) according to the present embodiment preferably contains a structural unit represented by the following general formula (a-1). This makes it possible to obtain a cyclic olefin-based ring-opening polymer having an excellent balance of transparency, heat resistance, and density.

[0030] [ka]

[0031] (Structural unit (b)) At least one structural unit (b) represented by the above general formula (II) is a ring-opening polymer derived from the following general formula (IV). The ring-opening polymer can be obtained by ring-opening metathesis polymerization. The ring-opening metathesis polymerization can be carried out by a known method.

[0032] [ka]

[0033] In the above formula (IV), R 1 ~R 6 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 1 ~R 6 may be bonded to each other to form a monocycle or polycycle, and the monocycle or polycycle may have a double bond, or the monocycle or polycycle may be an aromatic ring.

[0034] In this embodiment, the structural unit (b) is preferably derived from at least one compound selected from indene norbornene and dicyclopentadiene, which allows a cyclic olefin ring-opening polymer having a more excellent refractive index to be obtained.

[0035] When the total content of the structural unit (a) and the structural unit (b) is taken as 100 mol%, the content of the structural unit (a) is 20 mol% or more and 90 mol% or less, preferably 30 mol% or more and 80 mol% or less, more preferably 35 mol% or more and 75 mol% or less. 13 It can be measured by C-NMR.

[0036] The cyclic olefin ring-opening polymer (A) has a refractive index at a wavelength of 589 nm (n d) is 1.5340 or more. The upper limit of the refractive index of the cyclic olefin ring-opening polymer (A) is not particularly limited, but is preferably 1.5540 or less. When the refractive index is within the above range, the cyclic olefin ring-opening polymer (A) exhibits a high refractive index. A sodium lamp can be used as the light source with a wavelength of 589 nm. Specifically, the measurement can be performed in accordance with ASTM D542.

[0037] In addition, when the cyclic olefin-based ring-opening polymer (A) was heated at 125°C for 168 hours, the difference in refractive index of the optical component before and after heating (Δn d ) is 0.0020 or less. When heating at 125°C, it can be performed in a low-oxygen atmosphere or a nitrogen atmosphere. For example, such heating can be performed in an oven into which nitrogen can be introduced (inert oven). When an inert oven is used, heating can be performed under low-oxygen conditions by introducing nitrogen.

[0038] (Other ingredients) The optical component according to this embodiment may contain known additives as optional components in addition to the cyclic olefin ring-opening polymer (A) within the range that does not impair the excellent physical properties of the optical component. Examples of additives include hydrophilic stabilizers, hydrophilic agents, antioxidants, secondary antioxidants, lubricants, antifogging agents, weather resistance stabilizers, light resistance stabilizers, ultraviolet absorbers, antistatic agents, metal deactivators, phenolic stabilizers, higher fatty acid metal salts, hindered amine light stabilizers, hydrochloric acid absorbers, slip agents, nucleating agents, plasticizers, flame retardants, and phosphorus-based stabilizers. It is more preferable to contain a hydrophilic stabilizer, since this can suppress deterioration of optical performance under high temperature and high humidity conditions. The hydrophilic stabilizer is preferably a fatty acid ester of a fatty acid and a polyhydric alcohol, more preferably a fatty acid ester of a fatty acid and a polyhydric alcohol having one or more ether groups.

[0039] <Manufacturing methods for optical components> The optical component according to this embodiment can be produced by molding a cyclic olefin resin composition containing the cyclic olefin ring-opening polymer (A) into a predetermined shape. The method of molding the cyclic olefin resin composition to obtain an optical part is not particularly limited, and a known method can be used. Depending on the application and shape, for example, extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, vacuum molding, powder slush molding, calendar molding, foam molding, etc. can be applied. Among these, injection molding is preferred from the viewpoint of moldability and productivity. In addition, molding conditions are appropriately selected depending on the purpose of use or molding method. For example, the resin temperature in injection molding is appropriately selected within the range of usually 150°C to 400°C, preferably 200°C to 350°C, more preferably 230°C to 330°C.

[0040] The cyclic olefin resin composition according to the present embodiment can be obtained, for example, by a method of melt-kneading the cyclic olefin ring-opening polymer (A) and other components added as required using a known kneading device such as an extruder or a Banbury mixer; a method of dissolving the cyclic olefin ring-opening polymer (A) and other components added as required in a common solvent and then evaporating the solvent; or a method of adding the cyclic olefin copolymer (A) and other components added as required to a solution in a poor solvent to cause precipitation.

[0041] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0042] Hereinafter, the present embodiment will be described in detail with reference to examples, etc. However, the present embodiment is not limited to the description of these examples.

[0043] (Production Example 1) Into a polymerization reactor whose inside had been substituted with nitrogen, 7 parts of a monomer mixture (36 mol% of structural units derived from tetracyclododecene, 64 mol% of structural units derived from indenenorbornene), 1600 parts of dehydrated cyclohexane, 0.6 parts of 1-hexene, 1.3 parts of diisopropyl ether, 0.33 parts of isobutyl alcohol, 0.84 parts of triisobutylaluminum, and 30 parts of a cyclohexane solution of tungsten hexachloride (concentration: 0.66%) were placed, and the entire content was stirred at 55° C. for 10 minutes. Next, while continuing stirring, 693 parts of the monomer mixture and 72 parts of a cyclohexane solution of tungsten hexachloride (concentration: 0.77%) were continuously added dropwise over 150 minutes at 55°C. After completion of the dropwise addition, stirring was continued for another 30 minutes, and then 1.0 part of isopropyl alcohol was added to terminate the polymerization reaction. When the polymerization reaction solution was measured by gas chromatography, the conversion rate of the monomer to polymer was 100%.

[0044] Next, 300 parts of the polymerization reaction solution containing the polymer was transferred to an autoclave equipped with a stirrer, and 100 parts of cyclohexane and 2.0 parts of a diatomaceous earth supported nickel catalyst (manufactured by JGC Chemical Industries, Ltd., product name: T8400RL, nickel support rate 58%) were added. After replacing the atmosphere in the autoclave with hydrogen, a hydrogenation reaction was carried out at 180°C under a hydrogen pressure of 4.5 MPa for 6 hours. After completion of the hydrogenation reaction, the solution was filtered at a pressure of 0.25 MPa using a pressure filter (manufactured by Ishikawajima-Harima Heavy Industries Co., Ltd., product name: Funda Filter) with diatomaceous earth (manufactured by Showa Chemical Industry Co., Ltd., product name: Radiolite (registered trademark) #500) as a filter bed to obtain a colorless, transparent solution.

[0045] Next, the solvent (cyclohexane) and other volatile components were removed from the colorless, transparent solution at a temperature of 260°C and a pressure of 1 kPa or less using a cylindrical concentrating dryer (Hitachi), and the melt was extruded in the form of strands from a die directly connected to the concentrating dryer. After cooling with water, the melt was cut with a pelletizer (Osada Manufacturing, product name: OSP-2) to obtain pellets of the cyclic olefin ring-opening polymer resin.

[0046] (Production Example 2) Production was carried out in the same manner as in Production Example 1, except that the monomer mixture consisted of 76 mol % of structural units derived from tetracyclododecene, 12 mol % of structural units derived from indenenorbornene, and 12 mol % of structural units derived from dicyclopentadiene.

[0047] (Production Example 3) Production was carried out in the same manner as in Production Example 1, except that the monomer mixture contained 100% structural units derived from indene norbornene.

[0048] Example 1 The pellets produced in Production Example 1 were used to obtain a resin molded product using an injection molding machine. Each evaluation was carried out using this product.

[0049] Example 2 A resin molded product was obtained in the same manner as in Example 1, except that the pellets produced in Production Example 2 were used. Using this product, various evaluations were carried out.

[0050] (Comparative Example) The pellets produced in Production Example 3 were used to obtain a resin molded product using an injection molding machine. Each evaluation was carried out using this product.

[0051] [evaluation] (glass transition temperature) The values ​​were determined by differential scanning calorimetry under the following conditions. Equipment: SII NanoTechnology, DSC7000 Measurement conditions: Under a nitrogen atmosphere, the temperature was raised from room temperature to 260°C at a rate of 10°C / min and held for 5 minutes. The temperature was then lowered to 30°C at a rate of 10°C / min and held for 5 minutes. The DSC curve was then obtained during the process of raising the temperature to 260°C at a rate of 10°C / min. In the obtained DSC curve, the temperature at the point where a straight line equidistant in the vertical direction from the extended straight line of each baseline intersects with the curve of the stepwise change portion of the glass transition was taken as the glass transition temperature.

[0052] (transparency) The internal haze of a 30 mm×30 mm×2 mm thick square plate specimen obtained from the resin molded article was measured, and the transparency was evaluated according to the following criteria. The internal haze was measured in benzyl alcohol using a haze meter (NDH-20D manufactured by Nippon Denshoku Industries Co., Ltd.). ○: Internal haze is less than 5.0% ×: Internal haze is 5.0% or more

[0053] (Refractive Index) The refractive index (n d ) was measured.

[0054] (Refractive index change: environmental test) The test piece was heated at 125° C. for 168 hours while introducing nitrogen into an inert oven. The refractive index at a wavelength of 589 nm after heating was measured. The change in refractive index between before and after heating (Δn d ) was calculated.

[0055] The compositions and evaluation results of the above Examples 1 and 2 and Comparative Example are shown in Table 1. In Table 1, TD means tetracyclododecene, IndNB means indenenorbornene, and DCPD means dicyclopentadiene.

[0056] [Table 1]

[0057] In Examples 1 and 2, the structural unit (a) and the structural unit (b) are contained, and the content of the structural unit (a) is within a specific range, so that the glass transition temperature (Tg) and the refractive index (n d ) and the small refractive index change (Δn d ) We were also able to keep the internal haze low. On the other hand, the comparative examples showed high glass transition temperatures, low internal haze amounts, and low refractive index changes, but did not achieve a high refractive index.

Claims

1. An optical component comprising a cyclic olefin ring-opening polymer (A), The cyclic olefin ring-opening polymer (A) has a structural unit (a) and a structural unit (b), The structural unit (a) has a structural unit derived from tetracyclo[4.4.0.12,5.17,10]-3-dodecene, The structural unit (b) has a structural unit derived from indene norbornene, When the total content of the structural unit (a) and the structural unit (b) is taken as 100 mol%, the content of the structural unit (a) is 20 mol% or more and 90 mol% or less, The glass transition temperature (Tg) of the cyclic olefin ring-opening polymer (A) is 144° C. or higher as measured by a differential scanning calorimeter (DSC); The refractive index (n d ) is 1.5340 or more, The difference in refractive index (Δn d ) is 0.0020 or less. (Method 1) A square plate test piece of 30 mm x 30 mm x 2 mm thick is prepared from the cyclic olefin ring-opening polymer (A). Next, the refractive index of the square plate test piece at a wavelength of 589 nm is measured according to ASTM D542. The obtained refractive index is defined as the refractive index (n d ) of the cyclic olefin ring-opening polymer (A) at a wavelength of 589 nm. (Method 2) A square plate test piece of 30 mm × 30 mm × 2 mm thick is prepared from the cyclic olefin ring-opening polymer (A). The square plate test piece is then heated at 125°C for 168 hours in a nitrogen atmosphere. The difference in refractive index of the square plate test piece before and after the heating is defined as the difference in refractive index of the cyclic olefin ring-opening polymer (A) before and after the heating (Δn d ).

2. 2. The optical component according to claim 1 , The optical component, wherein the structural unit (b) further has a structural unit derived from dicyclopentadiene.

3. 3. The optical component according to claim 1, The optical component is an fθ lens, an imaging lens, a sensor lens, a prism, or a light guide plate.

4. The optical component according to any one of claims 1 to 3, An optical component which is a vehicle camera lens or a camera lens for a mobile device.

Citation Information

Patent Citations

  • Hydrogenated product of ring-opening copolymer and preparation thereof

    JP1989168725A

  • Hydrogenated tetracyclododecene ring-opened polymer, method for producing the same and optical material

    JP2007137935A

  • Norbornene-based ring-opening polymer hydrogenated material and utilization of the same

    JP2010150443A

  • Resin composition, resin molded article, and optical member

    JP2016069448A

  • Cyclic olefin copolymer, cyclic olefin copolymer composition, and molding

    JP2020105323A