Tantalum Carbide Powder

Tantalum carbide powder with tailored particle size distribution and intensity ratios addresses miscibility issues with tungsten carbide, enhancing tool performance through improved mixing and reactivity.

JP7576588B2Active Publication Date: 2024-10-31MITSUI MINING & SMELTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022074184
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-04-28
Publication Date
2024-10-31
Estimated Expiration
2042-04-28

AI Technical Summary

Technical Problem

Tantalum carbide powder with poor miscibility with tungsten carbide results in poor performance of carbide tools, despite having properties like fine and uniform particles and low oxygen content.

Method used

Tantalum carbide powder with specific volume-based particle size distribution and intensity ratios, determined by laser diffraction/scattering method, ensuring coexistence of large and small particle diameters for improved miscibility with tungsten carbide.

Benefits of technology

Enhances the miscibility and reactivity of tantalum carbide with tungsten carbide, resulting in improved properties such as chipping resistance, plastic deformation resistance, and wear resistance in cemented carbide tools.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576588000001
    Figure 0007576588000001
  • Figure 0007576588000002
    Figure 0007576588000002
  • Figure 0007576588000003
    Figure 0007576588000003
Patent Text Reader

Abstract

To provide a tantalum carbide powder having high miscibility with tungsten carbide as a raw material for a cemented carbide tool, and excellent subsequent reactivity.SOLUTION: The tantalum carbide powder of the present invention is the tantalum carbide powder containing a tantalum carbide particle in which a volume-based particle size distribution of the tantalum carbide particles has two peaks within a range of 0.02 to 10 μm as determined by laser diffraction / scattering method particle size distribution measurement, an intensity ratio Y2 / Y1 of a maximum intensity Y2 of a second peak to a maximum intensity Y1 of a first peak is 0.5 or more and 2 or less, where the peak with larger particle size is the first peak and the peak with smaller particle size is the second peak, of the two peaks, and a particle size ratio X2 / X1 of a particle size X1 corresponding to the maximum intensity Y1 of the first peak to a particle size X2 corresponding to the maximum intensity Y2 of the second peak is 0.18 or more and 0.5 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to tantalum carbide powder. [Background technology]

[0002] Tantalum carbide is widely used as an additive to tungsten carbide, which is the raw material for cemented carbide cutting tools such as cutting tools, tips, cutters, drills, and dies, and good mixing performance with tungsten carbide is required for manufacturing high-quality cemented carbide cutting tools. Patent Document 1 discloses, as tantalum carbide used as an additive, a tantalum carbide powder that has little powder aggregation, is fine and uniform in size, and has a low oxygen content that is stoichiometrically sufficiently bonded to carbon. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-31016 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, even if the tantalum carbide powder has the physical properties disclosed in Patent Document 1, if it does not mix well with the raw materials for cemented carbide cutting tools, such as tungsten carbide, it will not become a homogeneous cemented carbide material, and the performance of cemented carbide tools produced from such raw materials will be inferior.

[0005] In view of the above problems, the present invention provides a tantalum carbide powder that has high mixability with tungsten carbide, a raw material for cemented carbide tools, and also has excellent subsequent reactivity. [Means for solving the problem]

[0006] The tantalum carbide powder of the present invention, which has been made to solve the above-mentioned problems, is a tantalum carbide powder containing tantalum carbide particles, wherein the volume-based particle size distribution of the tantalum carbide particles has two peaks within a particle size range of 0.02 to 10 μm as measured by laser diffraction / scattering particle size distribution measurement, the larger of the two peaks being a first peak and the smaller of the two peaks being a second peak, an intensity ratio Y2 / Y1 of a maximum intensity Y2 of the second peak to a maximum intensity Y1 of the first peak being 0.5 or more and 2 or less, and a particle size ratio X2 / X1 of a particle size X2 corresponding to the maximum intensity Y2 of the second peak to a particle size X1 corresponding to the maximum intensity Y1 of the first peak being 0.18 or more and 0.5 or less. The tantalum carbide powder of the present invention contains tantalum carbide particles. The volumetric particle size distribution of the tantalum carbide particles has two peaks within a particle size range of 0.02 to 10 μm as measured by a laser diffraction / scattering particle size distribution method. Here, the position of the peak (particle size) is defined as the point where the differential coefficient of the volumetric particle size distribution curve of the tantalum carbide particles is zero. Of these two peaks, the peak with the larger particle size is defined as the first peak, and the peak with the smaller particle size is defined as the second peak.

[0007] Furthermore, the maximum intensity of the first peak is defined as Y1, and the particle size corresponding to the maximum intensity Y1 of the first peak is defined as X1. Furthermore, the maximum intensity of the second peak is defined as Y2, and the particle size corresponding to the maximum intensity Y2 of the second peak is defined as X2. Furthermore, the intensity ratio of the maximum intensity Y2 of the second peak to the maximum intensity Y1 of the first peak is defined as the intensity ratio Y2 / Y1, and the particle size ratio of the particle size X2 corresponding to the maximum intensity Y2 of the second peak to the particle size X1 corresponding to the maximum intensity Y1 of the first peak is defined as the particle size ratio X2 / X1.

[0008] In the tantalum carbide powder of the present invention, when the intensity ratio Y2 / Y1 is 0.5 or more and 2 or less, and the particle size ratio X2 / X1 is 0.18 or more and 0.5 or less, particles with large and small particle sizes are mixed, and if the proportion of the smaller particle sizes is large, this is preferable in terms of improving the mixability with tungsten carbide.

[0009] Furthermore, the intensity ratio Y2 / Y1 is more preferably equal to or greater than 1, and even more preferably equal to or greater than 1.1. The particle size ratio X2 / X1 is more preferably equal to or greater than 0.22, and even more preferably equal to or greater than 0.25.

[0010] Here, the volume-based particle size distribution of the tantalum carbide particles of the present invention can be measured by a dynamic light scattering method in accordance with JIS Z 8828:2019 "Particle size analysis-Dynamic light scattering method" using a laser diffraction / scattering particle size distribution measuring device (MT3300EXII manufactured by Microtrack Bell Co., Ltd.). In addition, filtering is not performed, and a dispersion treatment using ultrasonic waves as follows is performed.

[0011] The procedure for ultrasonic dispersion is as follows. First, as a pretreatment for ultrasonic dispersion, 1 mg of sample powder, pure water 20 mL of the solution is placed in a 50 mL wide-mouth PP bottle, which is then placed in an ultrasonic cleaner (VS-100III, manufactured by AS ONE Corp.). The inside of the cleaner is then filled with pure water up to 5 cm above the floor, and ultrasonic dispersion treatment is carried out for 60 minutes at a frequency of 28 kHz and an output of 100 W.

[0012] The volume-based particle size distribution curve of the tantalum carbide particles of the present invention measured after carrying out the above-mentioned ultrasonic dispersion treatment has two peaks within a particle size range of 0.02 to 10 μm as measured by laser diffraction / scattering particle size distribution measurement, where the horizontal axis represents particle size (μm) and the vertical axis represents frequency (%).

[0013] The tantalum carbide powder of the present invention is characterized in that the relationship between the median diameter D50(N) of the tantalum carbide particles and the median diameter D50(U) obtained by irradiating the tantalum carbide particles with ultrasonic waves satisfies the following formula (1):

[0014]

number

[0015] In the tantalum carbide powder of the present invention, when the relationship between the median diameter D50(N) of the tantalum carbide particles and the median diameter D50(U) obtained by irradiating the tantalum carbide particles with ultrasonic waves satisfies formula (1), the particle diameter after ultrasonic waves is smaller than the particle diameter before ultrasonic waves, and the pulverization by ultrasonic waves is easy, which is preferable in terms of improving the mixability with tungsten carbide. In addition, the relationship between the median diameter D50(N) of the tantalum carbide particles and the median diameter D50(U) obtained by irradiating the tantalum carbide particles with ultrasonic waves is more preferably 0.65 or less, even more preferably 0.63 or less, particularly preferably 0.61 or less, even more particularly preferably 0.60 or less, and also particularly preferably 0.59 or less.

[0016] Here, D50 indicates the particle diameter that reaches 50% in terms of volume fraction. In the present invention, it is measured by the dynamic light scattering method described above. The median diameter D50(N) of the tantalum carbide particles is the median diameter of the tantalum carbide particles that are not subjected to the above-mentioned ultrasonic dispersion treatment and are subjected to particle size evaluation. The median diameter D50(N) of the tantalum carbide particles also includes the median diameter of the tantalum carbide particles that are subjected to the above-mentioned ultrasonic dispersion treatment for less than the above-mentioned frequency and ultrasonic irradiation time. On the other hand, the median diameter D50(U) of the tantalum carbide particles is the median diameter of the tantalum carbide particles that are subjected to the particle size evaluation immediately after the above-mentioned ultrasonic dispersion treatment.

[0017] Furthermore, it is preferable to measure D10, which is the 10% particle size of the tantalum carbide particles of the present invention, and D90, which is the 90% particle size of the tantalum carbide particles of the present invention, by the dynamic light scattering method described above. That is, D10 indicates the particle size that reaches 10% in terms of volume fraction, D10(N) is the 10% particle size of the tantalum carbide particles that are not subjected to the above-mentioned ultrasonic dispersion treatment and are subjected to particle size evaluation, and D10(U) is the 10% particle size of the tantalum carbide particles that are subjected to the above-mentioned ultrasonic dispersion treatment immediately after the above-mentioned ultrasonic dispersion treatment. Also, D90 indicates the particle size that reaches 90% in terms of volume fraction, D90(N) is the 90% particle size of the tantalum carbide particles that are not subjected to the above-mentioned ultrasonic dispersion treatment and are subjected to particle size evaluation, and D90(U) is the 90% particle size of the tantalum carbide particles that are subjected to the above-mentioned ultrasonic dispersion treatment immediately after the above-mentioned ultrasonic dispersion treatment.

[0018] The tantalum carbide powder of the present invention is a tantalum carbide powder containing tantalum carbide particles, characterized in that the relationship between the median diameter D50(N) of the tantalum carbide particles and the median diameter D50(U) obtained by irradiating the tantalum carbide particles with ultrasound satisfies the following formula (1):

[0019]

number

[0020] The tantalum carbide powder of the present invention is characterized in that the relationship between the median diameter D50(N) of the tantalum carbide particles and the median diameter D50(U) obtained by irradiating the tantalum carbide particles with ultrasonic waves satisfies the following formula (2):

[0021]

number

[0022] In the tantalum carbide powder of the present invention, when the relationship between the median diameter D50(N) of the tantalum carbide particles and the median diameter D50(U) obtained by irradiating the tantalum carbide particles with ultrasonic waves satisfies formula (2), the particle size of the tantalum carbide particles is not too fine, and the mixing property with tungsten carbide is improved, which is preferable. If the particle size of the tantalum carbide particles of the present invention is too fine, the tantalum carbide particles will aggregate with each other.

[0023] The tantalum carbide powder of the present invention is characterized in that the ratio of the BET diameter measured by the BET method to the FSSS diameter measured by the FSSS method is 0.1 or more and 0.5 or less. The tantalum carbide powder of the present invention is preferably such that the ratio of the BET diameter measured by the BET method to the FSSS diameter measured by the FSSS method (hereinafter referred to as BET diameter / FSSS diameter) is 0.1 or more and 0.5 or less, in terms of improving the mixability with tungsten carbide.Moreover, the BET diameter / FSSS diameter is more preferably 0.2 or more and 0.45 or less, even more preferably 0.25 or more and 0.4 or less, and particularly preferably 0.3 or more and 0.35 or less.

[0024] Here, the FSSS diameter (Fisher diameter) is the average particle diameter measured by the air permeability method using a fully automatic dry particle measuring device (Fisher Sub-Sieve Sizer 2229) in accordance with JIS H 2116: 2002. The BET diameter is the particle diameter calculated from the specific surface area measured by the BET method using a fully automatic specific surface area measuring device (Macsorb HM-1230 type) in accordance with JIS Z8830, assuming that the particles are spherical.

[0025] The present invention also provides a cemented carbide tool, which is characterized by containing the tantalum carbide powder of the present invention. Since the cemented carbide tool of the present invention contains the tantalum carbide powder of the present invention, it has high mixability with tungsten carbide and excellent subsequent reactivity, and has the properties required of a cemented carbide tool, such as chipping resistance, plastic deformation resistance, and wear resistance.

[0026] In addition, the tantalum carbide powder of the present invention may contain components other than tantalum or tantalum carbide-derived components or carbon black-derived components (referred to as "other components") within a range that does not impair the action and effect of the powder. Examples of other components include Li, Mg, Si, Ca, Ti, Mn, Ni, Cu, Zn, Sr, Nb, Zr, Mo, Ba, W, and Bi. However, the other components are not limited to these. The content of other components in the tantalum carbide powder of the present invention is preferably less than 5% by mass, more preferably less than 4% by mass, and even more preferably less than 3% by mass. It is assumed that the tantalum carbide powder of the present invention contains unavoidable impurities, not intentionally. The content of unavoidable impurities is preferably less than 0.01% by mass.

[0027] The method for producing the above-mentioned tantalum carbide powder of the present invention will now be described.

[0028] The method for producing tantalum carbide powder of the present invention includes a weighing step of weighing out predetermined amounts of tantalum oxide and carbon black, a mixing step of mixing the weighed tantalum oxide and the carbon black to obtain a mixed powder, a primary carbonization step of firing the mixed powder using a resistance heating hydrogen furnace to obtain a primary carbide, a secondary carbonization step of firing the obtained primary carbide using a high-frequency induction heating vacuum furnace to obtain a secondary carbide, a coarse crushing step of coarsely crushing the obtained secondary carbide, a fine crushing step of finely crushing the coarsely crushed secondary carbide using a jet mill, and a classification step of classifying the finely crushed secondary carbide using a sieve or the like.

[0029] First, in the weighing step, a predetermined amount of each of the raw materials, tantalum oxide, for example, tantalum pentoxide (Ta2O5) and carbon black (C), is weighed using a platform balance or the like.

[0030] Next, in the mixing step, the weighed tantalum oxide and carbon black are mixed uniformly using a vertical mixer or the like to obtain a mixed powder.

[0031] In the primary carbonization process, the obtained mixed powder is filled into a carbon container, and the carbon container filled with the mixed powder is placed in a resistance heating hydrogen furnace. In a hydrogen reducing atmosphere, the temperature inside the hydrogen furnace is kept at 1,400°C to 1,800°C, and the mixture is fired for 1 to 10 hours, whereby tantalum pentoxide (Ta2O5) reacts with carbon black (C) to obtain a primary carbide. The obtained primary carbide is cooled to room temperature in the hydrogen furnace. If the temperature inside the hydrogen furnace is less than 1,400°C, the primary carbonization is insufficient, and the amount of free carbon and oxygen in the primary carbide increases. Also, if the temperature inside the hydrogen furnace exceeds 1,800°C, it is difficult due to the structure and material of the furnace.

[0032] After the primary carbonization step, it is preferable to average the quality of the primary carbonized product by stirring and mixing the primary carbonized product with a Hensel mixer, etc. In addition, the amount of free carbon and oxygen in the primary carbonized product may be analyzed and measured. If the amount of carbon required for the reaction is insufficient, carbon black may be added to make up for the shortage and stirred.

[0033] In the secondary carbonization process, the primary carbide obtained in the primary carbonization process is filled into a carbon crucible, and the carbon crucible filled with the primary carbide is placed in a high-frequency induction heating vacuum furnace. The temperature inside the vacuum furnace is kept at 1,800°C to 2,000°C under vacuum, and the secondary carbide is obtained by firing for 1 to 10 hours. The secondary carbide obtained is cooled to room temperature in the vacuum furnace. If the temperature inside the vacuum furnace is less than 1,800°C, carbonization is insufficient, and the effect of reducing the free carbon and oxygen remaining in the primary carbonization process is small. In addition, if the temperature inside the vacuum furnace exceeds 2,000°C, the tantalum carbide powder begins to coagulate, which is also a waste of energy.

[0034] In the coarse pulverization step, the obtained secondary carbide is taken out of the carbon crucible and coarsely pulverized by a jaw crusher or the like.

[0035] In the fine pulverization step, the coarsely pulverized secondary carbide is finely pulverized using a jet mill. The jet mill used for fine pulverization is preferably an airflow type pulverizer, which pulverizes secondary carbide particles by collision with each other. Specifically, the coarsely pulverized secondary carbide is finely pulverized using a jet mill set at a feed rate of 2.2 to 10 kg / hr and a wind speed of 2.5 m / min.

[0036] In the classification step, the finely pulverized secondary carbide is classified using a sieve or the like, and the undersieve (fine particle side) obtained is used as the tantalum carbide powder of the present invention. The oversieve (coarse particle side) may be classified by performing a coarse pulverization step again and / or a fine pulverization step. The sieve used for classification is preferably one with an opening of 30 to 1,000 μm.

[0037] In this specification, when "X to Y" (X and Y are any numbers) is expressed, unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the meaning of "preferably greater than X" or "preferably less than Y". Effect of the Invention

[0038] The tantalum carbide powder of the present invention is excellent in mixability with tungsten carbide, which is a raw material for cemented carbide tools, and is also excellent in the subsequent reactivity. BEST MODE FOR CARRYING OUT THEINVENTION

[0039] The tantalum carbide powder according to the embodiment of the present invention will be further described below with reference to the following examples, although the present invention is not limited to these examples.

[0040] Example 1 120 kg of tantalum oxide manufactured by Mitsui Mining & Smelting Co., Ltd. and 22 kg of carbon black were weighed out on a platform balance and mixed by stirring for 5 minutes in a vertical mixer to obtain a mixed powder.

[0041] This mixed powder was filled into a carbon container (2 kg / bottle), fed into a resistance heating hydrogen furnace at a rate of two bottles per three hours, and fired at a temperature of 1,700°C for 14 hours to perform primary carbonization, obtaining a primary carbide.

[0042] This primary carbide was packed into a carbon crucible (100 kg / piece), which was then placed in a high-frequency induction heating vacuum furnace and fired at 1,800°C for 5 hours to obtain a secondary carbide.

[0043] The secondary carbide was cooled to room temperature in the high-frequency induction heating vacuum furnace, removed from the carbon crucible, and coarsely crushed into lumps with a diameter of 2 cm or less using a jaw crusher.

[0044] After the coarse crushing, the coarsely crushed secondary carbide was finely crushed using a jet mill, which is an airflow type crusher. The jet mill used for fine crushing was set at a feed rate of 10 kg / hr and a wind speed of 2.5 m / min.

[0045] The finely pulverized secondary carbide was then classified using a vibrating sieve, and the undersize particles (fine particle side) were collected to obtain the tantalum carbide powder according to Example 1.

[0046] Example 2 In Example 2, the same production method as in Example 1 was carried out, except that the feed rate of the jet mill used for fine pulverization was 5 kg / hr, to obtain tantalum carbide powder according to Example 2.

[0047] Example 3 In Example 3, the same production method as in Example 1 was carried out, except that the feed rate of the jet mill used for fine pulverization was 2.5 kg / hr, to obtain tantalum carbide powder according to Example 3.

[0048] Example 4 In Example 4, the same production method as in Example 1 was carried out, except that the feed rate of the jet mill used for fine pulverization was 2.2 kg / hr, to obtain tantalum carbide powder according to Example 4.

[0049] Comparative Example 1 In Comparative Example 1, the same manufacturing method as in Example 1 was carried out, except that the coarsely pulverized secondary carbide was finely pulverized for 20 hours using a ball mill filled with iron balls having diameters of 20 to 50 mm, thereby obtaining tantalum carbide powder according to Comparative Example 1.

[0050] Comparative Example 2 In Comparative Example 2, the same manufacturing method as in Example 1 was carried out, except that the coarsely pulverized secondary carbide was finely pulverized using a dry fine powder grinder (feed rate: 10 kg / hr, air speed: 2.5 m / min), to obtain tantalum carbide powder according to Comparative Example 2.

[0051] The following physical properties were measured for the tantalum carbide powders according to Examples 1 to 4 and Comparative Examples 1 and 2. The measured physical properties and the methods for measuring the physical properties are shown below, and the measurement results are shown in Table 1.

[0052] <Elemental analysis> If necessary, the sample was appropriately diluted with hydrofluoric acid and nitric acid, and the Ta weight fraction in terms of Ta2O5 was measured by ICP emission spectrometry (Agilent Technologies: AG-5110).

[0053] <Particle size distribution> The particle size distribution was evaluated by a dynamic light scattering method in accordance with JIS Z 8828:2019 using a laser diffraction / scattering particle size distribution measuring device (Microtrack Bell Co., Ltd.: MT3300EXII). In addition, filtering was not performed, and the above-mentioned ultrasonic dispersion treatment was performed, and the volume-based particle size distribution curve of the tantalum carbide particles was measured. The point where the differential coefficient of the measured particle size distribution curve was zero was taken as the peak position (particle size). Furthermore, D10, D50, and D90 indicate the particle sizes at 10%, 50%, and 90% by volume. In addition, D10(N), D50(N), and D90(N) are the volume-integrated particle sizes D10, D50, and D90 measured without performing the above-mentioned ultrasonic dispersion treatment. Furthermore, D10(U), D50(U), and D90(U) are the volume-integrated particle sizes D10, D50, and D90 measured after the above-mentioned dispersion treatment using ultrasonic waves is performed.

[0054] <Fisher diameter (FSSS diameter)> The average particle size was measured by the air permeability method using a fully automatic dry particle size measuring device (Fisher Sub-Sieve Sizer 2229) in accordance with JIS H 2116:2002.

[0055] <BET diameter> Using a fully automatic specific surface area measuring device (Macsorb HM-1230 type), the particle size was calculated from the specific surface area measured by the BET method in accordance with JIS Z8830, assuming that the particles were spherical.

[0056] <Mixed Evaluation> Mixed samples (total 10 g) of tantalum carbide powder and tungsten carbide (manufactured by Nippon Shinkinzoku Co., Ltd., particle size 0.8 μm) according to Examples 1 to 4 and Comparative Examples 1 and 2 were weighed so that the molar ratio of the two was 1:1, and were placed in a 100 ml wide-mouthed PP bottle, and stirred and mixed for 1 minute using a paint shaker (frequency: 50 Hz). Then, five samples of the mixed samples that were stirred and mixed were taken using a medicine spoon, and the Ta weight fraction of each sample was analyzed. Samples in which the difference between the maximum and minimum Ta analysis values ​​of the five points after stirring and mixing for 1 minute was 0.5 mass% or less were evaluated as having excellent mixability and were evaluated as "○", and samples in which the difference between the maximum and minimum Ta analysis values ​​of the five points after stirring and mixing for 1 minute was more than 0.5 mass% were evaluated as having poor mixability and were evaluated as "×".

[0057] [Table 1]

[0058] As shown in Table 1, the tantalum carbide powders according to Examples 1 to 4 had an intensity ratio Y2 / Y1 of 0.5 to 2 and a particle size ratio X2 / X1 of 0.18 to 0.5, and had a mixture of large and small particles with a large proportion of small particles, and had excellent mixability with tungsten carbide. Note that the tantalum carbide powder according to Comparative Example 2 had only one peak in the particle size range of 0.02 to 10 μm, and therefore the intensity ratio Y2 / Y1 and particle size ratio X2 / X1 could not be calculated.

[0059] In the tantalum carbide powders of Examples 1 to 4, when the relationship between the median diameter D50 (N) of the tantalum carbide particles and the median diameter D50 (U) obtained by irradiating the tantalum carbide particles with ultrasound satisfies the above-mentioned formula (1), the particle diameter after ultrasound irradiation is smaller than the particle diameter before ultrasound irradiation, and pulverization by ultrasound irradiation is easy, indicating excellent mixability with tungsten carbide.

[0060] In the tantalum carbide powders of Examples 1 to 4, when the relationship between the median diameter D50 (N) of the tantalum carbide particles and the median diameter D50 (U) obtained by irradiating the tantalum carbide particles with ultrasonic waves satisfies the above-mentioned formula (2), the particle size of the tantalum carbide particles does not become too fine, and the mixability with tungsten carbide is improved.

[0061] The tantalum carbide powders according to Examples 1 to 4 had excellent mixability with tungsten carbide when the ratio of the BET diameter calculated from the specific surface area measured by the BET method to the FSSS diameter measured by the FSSS method was 0.1 or more and 0.5 or less.

[0062] The inventions disclosed in this specification include, in addition to the configurations of each invention or embodiment, those that are specified by changing these partial configurations to other configurations disclosed in this specification, to the extent applicable, or those that are specified by adding other configurations disclosed in this specification to these configurations, or those that are specified as higher-level concepts by deleting these partial configurations to the extent that partial action and effects are obtained. [Industrial Applicability]

[0063] The tantalum carbide according to the present invention has excellent miscibility with tungsten carbide and is therefore suitable as an additive to the raw material of cemented carbide tools.

Claims

1. 1. A tantalum carbide powder comprising tantalum carbide particles, The volume-based particle size distribution of the tantalum carbide particles has two peaks within a particle size range of 0.02 to 10 μm as measured by a laser diffraction / scattering method, Of the two peaks, the peak with the larger particle size is designated as the first peak, and the peak with the smaller particle size is designated as the second peak; The maximum intensity Y of the first peak 1 The maximum intensity Y of the second peak 2 Intensity ratio Y 2 / Y 1 is 0.5 or more and 2 or less, and the maximum intensity Y 1 Particle size X corresponding to 1 The maximum intensity Y of the second peak 2 Particle size X corresponding to 2 Particle size ratio X 2 / X 1 The tantalum carbide powder is characterized in that:

2. The tantalum carbide powder according to claim 1, characterized in that the relationship between the median diameter D50 (N) of the tantalum carbide particles and the median diameter D50 (U) obtained by irradiating the tantalum carbide particles with ultrasound satisfies the following formula (1): [0010]

3. 1. A tantalum carbide powder comprising tantalum carbide particles, A tantalum carbide powder characterized in that the relationship between the median diameter D50 (N) of the tantalum carbide particles and the median diameter D50 (U) obtained by irradiating the tantalum carbide particles with ultrasonic waves satisfies the following formula (1): [0025]

4. The tantalum carbide powder according to claim 2 or 3, characterized in that the relationship between the median diameter D50 (N) of the tantalum carbide particles and the median diameter D50 (U) obtained by irradiating the tantalum carbide particles with ultrasound satisfies the following formula (2): [0030]

5. 4. The tantalum carbide powder according to claim 1, wherein the ratio of the BET diameter measured by the BET method to the FSSS diameter measured by the FSSS method is 0.1 or more and 0.5 or less.

6. A cemented carbide tool comprising the tantalum carbide powder according to claim 1 or 3.

Citation Information

Patent Citations

  • Sintered hard alloy

    JP1987170451A

  • Sintered hard alloy and coated sintered hard alloy for cutting tool

    JP1994220571A

  • Cemented carbide body with improved wear resistance

    JP2000514874A

  • Tantalum carbide powder, tantalum carbide-niobium composite powder and their production method

    JP2008031016A

  • Cutting insert and cutting tool

    WO2018180911A1