Road petroleum asphalt-based hard and soft carbon composite material as well as preparation method and application thereof

Through the cross-linking treatment of road petroleum asphalt with light-component small-molecule stabilizers and heavy-component small-molecule oxidants, hard and soft carbon composite materials are formed, which solves the problems of high price of hard carbon precursors and high cost of oxidants, and achieves low cost and Anode material for sodium-ion batteries with excellent electrochemical properties.

CN118851174AActive Publication Date: 2024-10-29CHONGQING JIAOTONG UNIV +1

Patent Information

Application Number
CN202410672390.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-10-29
Estimated Expiration
2044-05-28

AI Technical Summary

Technical Problem

The hard carbon precursors of existing sodium-ion battery anode materials are expensive or have low carbon production rates, and the oxidant costs are high, resulting in high preparation costs and complicated processes.

Method used

Road petroleum asphalt is used as the precursor of hard and soft carbon composite materials. Through the cross-linking treatment of light component small molecule stabilizers and heavy component small molecule oxidants, hard and soft carbon composite materials are formed, simplifying the formula and reducing costs.

Benefits of technology

A low-cost hard-soft carbon composite material with excellent electrochemical properties has been realized, which improves sodium storage capacity, reversible specific capacity and first charge and discharge efficiency, simplifies the process flow, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004863063390000111
    Figure BDA0004863063390000111
Patent Text Reader

Abstract

The invention provides a road petroleum asphalt-based hard and soft carbon composite material. The road petroleum asphalt-based hard and soft carbon composite material is prepared from the following raw materials: road petroleum asphalt, a light-component small-molecule stabilizer, a heavy-component small-molecule oxidant, an activating agent and a solvent, according to g / mL / g / g / g, the ratio of the road petroleum asphalt to the solvent to the light-component small-molecule stabilizer to the heavy-component small-molecule oxidant to the activating agent is 1: (15-25): (0.05-0.2): (0.05-0.2): (2-5). On the other hand, the invention also provides a preparation method of the hard and soft carbon composite material, and the preparation method comprises the following steps: crosslinking treatment of light components, crosslinking treatment of heavy components, activation and carbonization. The hard and soft carbon composite material solves the problem that in the prior art, a hard carbon precursor is high in price or low in carbon production rate, an oxidizing agent is high in cost or the overall formula is complex, so that the prepared asphalt-based sodium ion battery negative electrode carbon material is high in cost, and the hard and soft carbon composite material is low in cost, integrates the advantages of hard carbon and soft carbon and has a good application prospect. The material has the advantages of high sodium storage capacity, high reversible specific capacity, high first charge-discharge efficiency and good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a road petroleum asphalt-based hard-soft carbon composite material and a preparation method and application thereof. Background Art

[0002] With the rapid development of new energy technologies, higher requirements are placed on energy conversion and storage devices. Sodium-ion batteries show great potential in large-scale energy storage systems due to their abundant, readily available, and low-cost sodium resources. Sodium ions have a large radius, so suitable sodium storage positive and negative electrode materials are one of the key issues in realizing the practical application of sodium-ion batteries, and sodium storage negative electrode materials are an important component, playing an important role in loading and releasing sodium ions (i.e., inserting and extracting sodium ions). At present, the negative electrode materials of sodium-ion batteries are mainly divided into five types: carbon-based materials, titanium-based materials, alloy materials, organic compounds, and other systems. Among them, carbon-based materials have the highest technical maturity and abundant resources, and are expected to be the first to achieve industrialization.

[0003] According to the microstructure of carbon atoms, carbon-based negative electrode materials are divided into graphite materials, amorphous carbon materials and nano-carbon materials; among them, amorphous carbon materials have a higher sodium storage capacity and are currently the negative electrode materials closest to industrialization. According to the difficulty of graphitization by heat treatment, they are divided into soft carbon and hard carbon; soft carbon can be graphitized at high temperatures above 2500°C, while hard carbon is difficult to graphitize, and is generally obtained by heat treatment in the range of 800-1400°C. The difference between soft and hard carbon lies in the cross-linking interaction of the carbon layer in the microstructure, which fundamentally depends on the structure and shape of the carbonization precursor used. Generally speaking, thermoplastic precursors (petrochemical raw materials and by-products, such as coal tar or high-temperature asphalt, which are commonly used soft carbon precursors) are easy to form soft carbon, and thermosetting precursors (biomass, organic polymers, high molecular materials, etc.) are easy to form hard carbon.

[0004] The microstructure of hard carbon is composed of short-range ordered microdomains stacked by curved graphite-like sheets. The microdomains are randomly and disorderly stacked to leave many nanopores. It has a large carbon layer spacing (usually greater than 0.37nm), rich pore structure and more defect sites, so it can store more sodium ions and has a higher charge and discharge specific capacity. At the same time, due to its large carbon layer spacing, its volume expansion is small when inserting and extracting sodium ions, coupled with its own lattice stability, so it can maintain good structural stability during high-temperature carbonization and battery use, and good structural stability also ensures that it has a certain cycle stability. However, the initial charge and discharge efficiency of hard carbon is low, and its performance depends on the precursor used and the treatment process. Although its precursor is widely available, it has the disadvantages of low carbon yield or high price, which increases the cost of hard carbon and hinders its application in large-scale energy storage.

[0005] Relatively speaking, soft carbon has a higher degree of graphitization and a highly ordered carbon layer structure, which is not conducive to the storage of sodium ions, so its charge and discharge specific capacity is lower; but it has higher electronic conductivity, and its specific surface area and surface defect level are lower, which can reduce the formation of solid electrolyte interface film (SEI film) (that is, soft carbon has better electrolyte compatibility), which helps to improve the initial charge and discharge efficiency; and the manufacturing cost of soft carbon is also low, and the process is easy to control.

[0006] From the above analysis, it can be seen that both soft and hard carbon have certain deficiencies in the practical application of negative electrode materials for sodium ion batteries. The prior art usually mixes an oxidant into a soft carbon precursor to pre-oxidize the soft carbon precursor to increase the disorder of the carbon layer of the soft carbon, thereby increasing its sodium storage capacity; or mixes the soft and hard carbon precursors to prepare a soft carbon and hard carbon composite material, thereby combining the advantages of both to improve material performance, for example:

[0007] Patent CN116314773A discloses a pre-oxidized asphalt-based sodium ion battery negative electrode material, which uses graphene oxide as a modifier to improve the conductivity of the prepared asphalt-based negative electrode material. Specifically, graphene oxide is reduced to graphene after carbonization, and the high conductivity and uniform distribution of graphene can form a high-speed conductive network between the negative electrode of the sodium ion battery and the negative electrode and the current collector, thereby effectively improving the conductivity of the material; the asphalt comes from coal tar, petroleum asphalt and synthetic asphalt. Although the patent formula is simple and only requires a precursor and an oxidizing modifier, the use of graphene oxide as the oxidizing modifier will greatly increase the cost.

[0008] Patent CN116675215A discloses a soft carbon and hard carbon composite material, whose raw materials are a soft carbon precursor (selected from coal tar pitch, petroleum pitch, ethylene tar pitch and heavy aromatic hydrocarbon pitch), an organic oxidation promoter, a catalyst and a hard carbon precursor (selected from sucrose, glucose, starch, cellulose, lignin, phenolic resin, epoxy resin and polyfurfuryl alcohol); the soft carbon precursor is first pre-oxidized by an organic oxidation promoter, and then the catalyst and the hard carbon precursor are mixed with the pre-oxidized soft carbon precursor for polymerization reaction, and then coking and carbonization are carried out in sequence to obtain a composite carbon material. Although the composite carbon material combines the advantages of soft carbon and hard carbon, its soft carbon and hard carbon come from two different substances, which makes the formula complicated, and as mentioned above, the hard carbon precursor is not only expensive, but also has a low carbon yield, which further increases the cost of hard carbon, resulting in a complex overall process and increased costs.

[0009] It can be seen that the existing technology usually uses asphalt as a soft carbon precursor, and adds an oxidant to oxidatively modify the asphalt or mixes it with a hard carbon precursor to combine the advantages of soft and hard carbon, thereby improving the performance of asphalt-based carbon materials as negative electrode materials for sodium ion batteries; although asphalt as a soft carbon precursor is cheap, easy to obtain and has a high carbon content, hard carbon precursors are often expensive or have low carbon yields. In addition, the asphalt-based carbon materials prepared in this way often have the disadvantages of high oxidant costs or complex formulas, which need to be improved. Summary of the invention

[0010] In view of the deficiencies in the prior art, the present invention provides a road petroleum asphalt-based hard-soft carbon composite material, which solves the problem in the prior art that the hard carbon precursor is high in price or has a low carbon yield, the oxidant cost is also high or the overall formula is complex, resulting in a high cost of the prepared asphalt-based sodium ion battery negative electrode carbon material.

[0011] According to an embodiment of the present invention, a road petroleum asphalt-based hard-soft carbon composite material, the raw materials used in which include road petroleum asphalt, a light component small molecule stabilizer, a heavy component small molecule oxidant, an activator and a solvent; and in terms of g / mL / g / g / g, the road petroleum asphalt: solvent: light component small molecule stabilizer: heavy component small molecule oxidant: activator is 1:15-25:0.05-0.2:0.05-0.2:2-5.

[0012] On the other hand, according to an embodiment of the present invention, a method for preparing a road petroleum asphalt-based hard-soft carbon composite material comprises the following steps:

[0013] S1, preparing a composite slurry: mixing road petroleum asphalt, a solvent, a light component small molecule stabilizer and a heavy component small molecule oxidant in proportion, and then ultrasonically treating for 20-40 minutes to obtain a composite slurry;

[0014] S2, cross-linking treatment of the light component: in an inert gas atmosphere, the composite slurry is heated to 160-180° C., and then stirred at a constant temperature for 1-2 hours to obtain a first modified asphalt composite;

[0015] S3, cross-linking treatment of the heavy component: heating the first modified asphalt composite to 300-500° C. in an inert gas atmosphere, and then keeping the temperature constant for 1-2 hours to obtain a second modified asphalt composite;

[0016] S4, activation: adding an activator to the second modified asphalt composite, and then heating to 800°C in an inert gas atmosphere, and then maintaining the temperature for 1-2 hours for activation treatment;

[0017] S5, carbonization: in an inert gas atmosphere, the activated second modified asphalt composite is heated to 1000-1400°C, and then carbonized at a constant temperature for 2-3 hours to obtain a road petroleum asphalt-based hard-soft carbon composite material.

[0018] On the other hand, according to an embodiment of the present invention, there is also provided a sodium ion battery negative electrode plate, which includes the above-mentioned road petroleum asphalt-based hard-soft carbon composite material.

[0019] Finally, according to an embodiment of the present invention, a sodium ion battery is provided, which includes the sodium ion battery negative electrode plate.

[0020] The technical principle of the present invention is:

[0021] The road petroleum asphalt used in the present invention is different from coal asphalt and other high-temperature asphalts. It has a lower softening point and contains more light components (about 65%), and the remaining components are heavy components (about 35%), wherein the light components are saturated components and aromatic components, and the heavy components are colloids and asphaltenes; the carbon content in the light components and the heavy components is as high as 87%, and the light components are generally considered to derive hard carbon, and the heavy components are generally considered to derive soft carbon; but due to its lower molecular weight, the light components have weaker intermolecular forces and lower polarity, so they have poor thermal stability during high-temperature carbonization and are more volatile, resulting in lower carbon production of the asphalt, and after high-temperature carbonization, they show more soft carbon properties and poor sodium storage capacity; the base Here, the main idea of ​​the present invention is: using a light component small molecule stabilizer to improve the high temperature stability of the light component in road petroleum asphalt to avoid its volatilization, so that the road petroleum asphalt is used as a soft carbon and hard carbon precursor, and then using a heavy component small molecule oxidant to oxidatively modify the heavy component, so that the sodium storage capacity of the soft carbon derived from the heavy component is increased, and at the same time, the prepared soft carbon and hard carbon are cross-linked to form a hard-soft carbon composite material, so that the soft carbon derived from the heavy component can further combine the advantages of high sodium storage capacity and good cycle stability of hard carbon, and at the same time, the good conductivity and good electrolyte compatibility of the soft carbon in the composite material also greatly improve the initial charge and discharge efficiency of the material, specifically:

[0022] The light component small molecule stabilizer is cross-linked with the light component, and the heavy component small molecule oxidant has a functional group with strong oxidizing property, which is cross-linked with the heavy component; in this way, the light component and the heavy component in the road petroleum asphalt are each targeted components, and the light component small molecule stabilizer and the heavy component small molecule oxidant play a bridging role, which promotes the reconstruction and modification of the light / heavy components, and establishes a covalently cross-linked network structure inside the modified asphalt, enhances their respective intermolecular forces and mutual forces, thereby avoiding the volatilization of the light component and the heavy component in the subsequent carbonization process, and then promotes the interface bonding force between the hard carbon derived from the light component in the subsequent high-temperature carbonization process and the soft carbon derived from the heavy component to enhance and generate a hard-soft carbon composite material. The hard-soft carbon composite material combines the advantages of hard carbon and soft carbon, so that it has both the high sodium storage capacity and structural stability of hard carbon itself, and the high conductivity and good electrolyte compatibility of soft carbon itself, thereby improving the overall performance of the material.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. Low cost. First of all, the present invention uses road petroleum asphalt as a hard carbon and soft carbon precursor. On the one hand, road petroleum asphalt itself is cheap, easy to obtain, and has a high carbon content. It also avoids the introduction of other hard carbon precursors with high prices and low carbon yields, greatly reducing costs. On the other hand, under the action of light component small molecule stabilizers and heavy component small molecule oxidants, the light / heavy components are not easy to volatilize during the high-temperature carbonization process, especially the light component with a higher content has a lower volatility, which not only greatly improves the carbon yield of the light component part as a hard carbon precursor, but also improves the carbon yield of the heavy component part as a soft carbon precursor, thereby greatly improving the utilization rate of carbon in road petroleum asphalt and greatly reducing costs. Secondly, the hard carbon and soft carbon precursors of the present invention come from the same substance, which simplifies the formula, lays the foundation for the simplification of the process, and then reduces costs. Finally, the light component small molecule stabilizer and the heavy component small molecule oxidant of the present invention can use common chemical reagents according to the characteristics of the light / heavy components, and are easy to purchase, stable in quality, and controllable in price, which increases the cost reduction space of the hard and soft carbon composite material of the present invention.

[0025] 2. Good electrochemical performance. The present invention cross-links the light component with a small molecule modifier of the light component and the heavy component with a small molecule oxidant of the heavy component, so that the hard-soft carbon composite material prepared by the present invention combines the advantages of hard carbon and soft carbon at the same time, wherein the hard carbon provides a higher charge-discharge specific capacity and better structural stability, and the soft carbon ensures high conductivity and good electrolyte compatibility, thereby bringing about high sodium storage capacity, high reversible specific capacity, high first charge-discharge efficiency and better cycle performance.

[0026] 3. Environmentally friendly. The present invention uses low softening point road petroleum asphalt as the precursor of the hard-soft carbon composite material, and fixes a large number of light components that are easily volatile during high-temperature carbonization and derives a hard carbon structure, which not only avoids the pollution of the environment caused by the volatilization of light components, but also provides a new idea and direction for the application of low softening point road petroleum asphalt in the field of new energy.

[0027] 4. The process is simple, easy to implement, and has good effects, which is worth promoting. The formula adopted in this process is simple, which makes the process flow simple and easy to implement; the method of modifying the light and heavy components in turn makes the modification more sufficient and the effect is better; the reaction temperature and reaction time of the cross-linking treatment are appropriate. It is understandable that if the reaction temperature is too low or the time is too short, the two components of the asphalt cannot be fully cross-linked, which will affect the final sample carbon layer spacing and disorder, and reduce the sodium storage capacity. If the reaction temperature is too high or the time is too long, it will lead to a decrease in yield and an increase in cost; the carbonization temperature and time are appropriate. It is understandable that if the carbonization temperature is too low or the time is too short, the volatile matter and heteroatoms cannot be effectively removed, resulting in an increase in defects and an increase in irreversible capacity. If the carbonization temperature is too high or the time is too long, the carbon layer spacing will decrease, the disorder will decrease, and the sodium storage capacity will decrease.

[0028] 5. Good application prospects. The invention has a simple formula, low cost, simple and easy-to-implement process, and the prepared hard-soft carbon composite material has good electrochemical properties and can be used as an ideal electrode material for sodium batteries, with potential application prospects.

[0029] Preferably, the light component small molecule stabilizer includes one of phosphoric acid, polyphosphoric acid and resorcinol.

[0030] Beneficial effects: These three small molecule stabilizers are all common chemical substances, which are easily available, of stable quality and inexpensive. They contain highly active functional groups (such as phenolic hydroxyl groups and phosphate groups), which can easily cross-link with the light components of road petroleum asphalt. In addition, phosphoric acid and polyphosphoric acid also provide phosphorus atoms, which can form P=O, PC and other bond types during the reaction and embed into the carbon layer, thereby further expanding the distance between the carbon layers and enhancing the absorption capacity of sodium ions.

[0031] Preferably, the heavy component small molecule oxidant includes one of terephthalic acid alcohol, benzaldehyde and terephthaloyl chloride.

[0032] Beneficial effects: These three small molecule oxidants are all common chemical substances, easily available, of stable quality and inexpensive; they contain highly active functional groups (such as alcohol hydroxyl, aldehyde, and acyl), which can easily cross-link with heavy components of road petroleum asphalt.

[0033] Preferably, the activator includes one of potassium hydroxide, sodium hydroxide and phosphoric acid.

[0034] Beneficial effects: They are all commonly used chemical activators in the preparation of porous carbon materials, and the selection is relatively flexible.

[0035] Preferably, the solvent is trichloroethylene.

[0036] Preferably, the road petroleum asphalt includes one of AH-90 base asphalt, AH-70 base asphalt and AH-50 base asphalt.

[0037] Preferably, the inert gas includes one of nitrogen and argon.

[0038] Beneficial effects: They are all commonly used inert gases and the selection is relatively flexible. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is further described below in conjunction with embodiments.

[0040] 1. Description of the three types of road petroleum asphalt used in Examples 1 to 13 and Comparative Examples 1 to 5 of the present application:

[0041] (1) Their softening points are:

[0042] AH-90 base asphalt: 42~55℃

[0043] AH-70 base asphalt: 44~57℃

[0044] AH-50 base asphalt: 45~58℃

[0045] The softening point data above comes from: GB / T 15180-2010 Heavy Traffic Road Petroleum Asphalt

[0046] (2) The road petroleum asphalt is fresh base asphalt and has not been subjected to any modification treatment.

[0047] (3) Classification of asphalt grades: The asphalt grade is also known as the grade of asphalt. There are many grading methods in the world. my country adopts the penetration grading method. The asphalt grade is determined according to the penetration obtained by the asphalt penetration test and the grading range. For example, the penetration range of No. 90 asphalt is approximately between 80 and 100. The asphalt grade is related to the performance of the asphalt. It is very important to choose the appropriate asphalt grade according to the regional climate, transportation and other factors.

[0048] (4) The definition of road petroleum asphalt and the reasons for selecting the above three types of asphalt in the examples and comparative examples of the present application are as follows:

[0049] Petroleum asphalt is a by-product generated by extracting gasoline, kerosene, diesel and other heavy oils from crude oil in petrochemical plants. It is then processed or formulated into a building material. It is the main material for paving modern highways and urban roads. It is also used to make waterproof layers and caulking materials for houses, underground structures, hydraulic structures, etc. Petroleum asphalt used for highways and urban roads is called road petroleum asphalt. According to the provisions of the industry standard of the People's Republic of China "JTG F40-2004 Technical Specifications for Highway Asphalt Pavement Construction", there are seven grades of asphalt according to the needle penetration, namely 160, 130, 110, 90, 70, 50, and 30.

[0050] The asphalt grade used for asphalt pavement should be determined carefully after technical demonstration according to the highway grade, climate conditions, traffic conditions, pavement type, layer position in the pavement structure, construction method, etc., combined with local usage experience. For expressways, first-class highways, high summer temperatures, long-lasting high temperatures, heavy traffic, steep slopes and sharp bends in mountainous or hilly areas, parking lots or sections with slow driving speeds, it is advisable to use asphalt with high viscosity, such as No. 70, No. 50, etc. For areas with cold winters or low traffic volume, light loads, and tourist roads, it is advisable to use asphalt with low viscosity and high low-temperature ductility. When high temperature requirements conflict with low temperature requirements, high temperature performance requirements should be given priority.

[0051] It can be seen that when a large area of ​​road is constructed, the amount of asphalt with a higher viscosity is generally selected based on comprehensive conditions. Based on this, and taking into account the subsequent recycling of large amounts of asphalt (such as being used as a carbon material precursor), in the embodiments of the present application and the comparative examples, road petroleum asphalts with higher viscosities of No. 90, No. 70 and No. 50 are selected as carbon material precursors.

[0052] 2. Description of other raw materials in Examples 1 to 13 and Comparative Examples 1 to 5 of the present application:

[0053] Trichloroethylene: McLean, AR, 99.0%, containing 40 ppm diisopropylamine (stabilizer), 131.39 (MW);

[0054] Phosphoric acid: MacLean, density is 1.69 g / mL;

[0055] Polyphosphoric acid (H n+2 P n O 3n+1 ): McLean, content (H3PO4) ≥ 115%;

[0056] Resorcinol: Aladdin, AR, 99.0%;

[0057] p-Terephthalate: McLean, AR, 98.0%;

[0058] Benzaldehyde: Aladdin, AR, ≥98%;

[0059] Terephthaloyl chloride: Aladdin, AR, 99%;

[0060] Potassium hydroxide: Aladdin, AR, 85%;

[0061] Sodium hydroxide: Aladdin, AR, 96%.

[0062] 3. Explanation of terms related to electrochemical performance involved in this application:

[0063] (1) Sodium storage capacity (here for sodium ion half-cell; also called sodium storage capacity): the capacity of sodium ions embedded in the anode carbon material during discharge.

[0064] (2) Reversible capacity: The sodium ion capacity that can be recovered under given discharge / charge conditions (current density, temperature, voltage, etc.) after a full charge / discharge process under certain charge / discharge conditions (current density, temperature, voltage, etc.).

[0065] (3) Reversible specific capacity: reversible capacity per unit mass.

[0066] (4) 30mA / g reversible specific capacity: refers to the sodium capacity that can be recovered per unit mass of sodium battery during the charge and discharge cycle at a current density of 30mA / g.

[0067] (5) Charge and discharge efficiency (here for sodium ion half-cell): the ratio of the charge specific capacity (corresponding to sodium removal) to the discharge specific capacity (corresponding to sodium insertion).

[0068] (6) First charge and discharge efficiency (here for sodium ion half-cell; also called first coulombic efficiency): refers to the ratio of the first charge specific capacity (corresponding to the first sodium removal) to the first discharge specific capacity (corresponding to the first sodium insertion).

[0069] (7) Irreversible capacity: The sodium ion capacity of a sodium battery that cannot be released (recovered) under given discharge conditions (charge rate, temperature, discharge voltage, etc.) after a full charge process under certain discharge conditions (charge rate, temperature, discharge voltage, etc.).

[0070] Example 1

[0071] A method for preparing a road petroleum asphalt-based hard-soft carbon composite material comprises the following steps:

[0072] S1, preparing a composite slurry: 5 g of AH-70 road petroleum asphalt, 100 mL of trichloroethylene, 0.25 g of phosphoric acid and 0.25 g of terephthalic acid were added into a 500 mL three-necked flask, and the composite slurry was obtained after ultrasonic treatment for 30 min;

[0073] S2, cross-linking treatment of light components: transfer the composite slurry to an oil bath pot, and carry out subsequent operations under N2 protection: heat to 160°C, then stir at a constant temperature for 1 hour until the solvent evaporates, carry out modification and cross-linking reaction of the light components, and finally obtain a uniformly mixed first modified asphalt composite;

[0074] S3, cross-linking treatment of heavy components: the first modified asphalt composite is transferred to a tubular furnace and subjected to subsequent operations under N2 protection: after heating to 300°C, the temperature is kept for 2 hours to carry out the modification and cross-linking reaction of the heavy components, and then the second modified asphalt composite is obtained;

[0075] S4, activation: weigh 10g potassium hydroxide and add it to a beaker, then add 50g deionized water, stir evenly and prepare a potassium hydroxide aqueous solution; take out the obtained second modified asphalt composite, let it stand and cool, then add it to the newly prepared potassium hydroxide aqueous solution, stir evenly and let it stand for 12h, then put the mixed solution back into the tube furnace, and perform activation treatment under N2 protection: heat to 800℃, and then keep the temperature constant for 1h;

[0076] S5, carbonization: the activated second modified asphalt composite is further subjected to subsequent operations under N2 protection: after heating to 1200°C, the composite is kept at this temperature for 2 hours for carbonization treatment, and finally a road petroleum asphalt-based hard-soft carbon composite material is obtained.

[0077] Example 2

[0078] A method for preparing a road petroleum asphalt-based hard-soft carbon composite material comprises the following steps:

[0079] S1, preparing a composite slurry: 5 g of AH-70 road petroleum asphalt, 75 mL of trichloroethylene, 0.5 g of polyphosphoric acid and 0.5 g of benzaldehyde were added into a 500 mL three-necked flask, and subjected to ultrasonic treatment for 30 min to obtain a composite slurry;

[0080] S2, cross-linking treatment of light components: the composite slurry is transferred to an oil bath pot, and the subsequent operation is carried out under Ar protection: heating to 170°C, and then stirring at a constant temperature for 1 hour until the solvent is evaporated, and the light component is modified and cross-linked to obtain a uniformly mixed first modified asphalt composite;

[0081] S3, cross-linking treatment of the heavy component: the first modified asphalt composite is transferred to a tubular furnace and subjected to subsequent operations under Ar protection: after heating to 350°C, the temperature is kept at this temperature for 1.5 hours to carry out the modification and cross-linking reaction of the heavy component, and then a second modified asphalt composite is obtained;

[0082] S4, activation: weigh 15g of sodium hydroxide and add it to a beaker, then add 100g of deionized water, stir evenly and prepare a sodium hydroxide aqueous solution; take out the obtained second modified asphalt composite, let it stand and cool, then add it to the newly prepared sodium hydroxide aqueous solution, stir evenly and let it stand for 12h, then put the mixed solution back into the tube furnace, and perform activation treatment under Ar protection: heat to 800℃, and then keep the temperature constant for 1.5h;

[0083] S5, carbonization: the activated second modified asphalt composite is further subjected to subsequent operations under Ar protection: after heating to 1200°C, the composite is kept at this temperature for 2.5 hours for carbonization treatment, and finally a road petroleum asphalt-based hard-soft carbon composite material is obtained.

[0084] Example 3

[0085] A method for preparing a road petroleum asphalt-based hard-soft carbon composite material comprises the following steps:

[0086] S1, preparing a composite slurry: 5 g of AH-70 road petroleum asphalt, 125 mL of trichloroethylene, 0.75 g of resorcinol and 0.75 g of terephthaloyl chloride were added into a 500 mL three-necked flask, and subjected to ultrasonic treatment for 20 min to obtain a composite slurry;

[0087] S2, cross-linking treatment of light components: transfer the composite slurry to an oil bath pot, and carry out subsequent operations under N2 protection: heat to 180°C, then stir at a constant temperature for 2 hours until the solvent evaporates, carry out modification and cross-linking reaction of the light components, and finally obtain a uniformly mixed first modified asphalt composite;

[0088] S3, cross-linking treatment of the heavy component: the first modified asphalt composite is transferred to a tubular furnace and subjected to subsequent operations under N2 protection: after heating to 400°C, the temperature is kept for 2 hours to carry out the modification and cross-linking reaction of the heavy component, and then the second modified asphalt composite is obtained;

[0089] S4, activation: add 40g of deionized water to a beaker, and then weigh 20g of phosphoric acid and add it to the deionized water while stirring to dilute the phosphoric acid solution; then take out the obtained second modified asphalt composite, let it stand and cool, then add it to the newly diluted phosphoric acid solution, stir evenly and let it stand for 12h, then put the mixed solution back into the tube furnace and perform activation treatment under Ar protection: heat it to 800℃ and keep it at a constant temperature for 2h;

[0090] S5, carbonization: the activated second modified asphalt composite is further subjected to subsequent operations under N2 protection: after heating to 1400°C, the composite is kept at this temperature for 3 hours for carbonization treatment, and finally a road petroleum asphalt-based hard-soft carbon composite material is obtained.

[0091] Example 4

[0092] A method for preparing a road petroleum asphalt-based hard-soft carbon composite material comprises the following steps:

[0093] S1, preparing a composite slurry: 5 g of AH-50 road petroleum asphalt, 100 mL of trichloroethylene, 1 g of phosphoric acid and 1 g of terephthalic acid were added into a 500 mL three-necked flask, and subjected to ultrasonic treatment for 40 min to obtain a composite slurry;

[0094] S2, cross-linking treatment of light components: transfer the composite slurry to an oil bath pot, and carry out subsequent operations under N2 protection: heat to 160°C, then stir at a constant temperature for 1.5 hours until the solvent evaporates, carry out modification and cross-linking reaction of the light components, and finally obtain a uniformly mixed first modified asphalt composite;

[0095] S3, cross-linking treatment of the heavy component: the first modified asphalt composite is transferred to a tubular furnace and subjected to subsequent operations under N2 protection: after heating to 450°C, the temperature is kept for 1 hour to carry out the modification and cross-linking reaction of the heavy component, and then the second modified asphalt composite is obtained;

[0096] S4, activation: weigh 25g potassium hydroxide and add it to a beaker, then add 200g deionized water, stir evenly and prepare a potassium hydroxide aqueous solution; take out the obtained second modified asphalt composite, let it stand and cool, then add it to the newly prepared potassium hydroxide aqueous solution, stir evenly and let it stand for 12h, then put the mixed solution back into the tube furnace, and perform activation treatment under N2 protection: heat to 800℃, and then keep the temperature constant for 1.5h;

[0097] S5, carbonization: the activated second modified asphalt composite is continued to be operated under N2 protection: after heating to 1000°C, it is kept warm for 2 hours for carbonization treatment, and finally a petroleum asphalt-based hard-soft carbon composite material is obtained.

[0098] Example 5

[0099] The difference from Example 1 is that 0.25 g of phosphoric acid and 0.5 g of terephthalic acid are added.

[0100] Example 6

[0101] The difference from Example 1 is that 0.25 g of phosphoric acid and 1 g of terephthalic acid are added.

[0102] Example 7

[0103] The difference from Example 1 is that 0.5 g of phosphoric acid and 0.25 g of terephthalic acid are added.

[0104] Example 8

[0105] The difference from Example 1 is that 0.5 g of phosphoric acid and 1 g of terephthalic acid are added.

[0106] Example 9

[0107] The difference from Example 1 is that 1 g of phosphoric acid and 0.25 g of terephthalic acid are added.

[0108] Example 10

[0109] The difference from Example 1 is that 1 g of phosphoric acid and 0.5 g of terephthalic acid are added.

[0110] Embodiment 11

[0111] The difference from Example 1 is that AH-90 road petroleum asphalt is used.

[0112] Example 12

[0113] The difference from Example 3 is that the cross-linking temperature of the heavy component is 500°C.

[0114] Embodiment 13

[0115] The difference from Example 4 is that the carbonization treatment temperature is 1200°C.

[0116] Comparative Example 1

[0117] The difference from Example 1 is that phosphoric acid is not added.

[0118] Comparative Example 2

[0119] The difference from Example 1 is that terephthalic acid alcohol is not added.

[0120] Comparative Example 3

[0121] The difference from Example 1 is that phosphoric acid and terephthalic acid are not added.

[0122] Comparative Example 4

[0123] The difference from Example 1 is that 2 g of phosphoric acid and 2 g of terephthalic acid are added.

[0124] Comparative Example 5

[0125] The difference from Example 1 is that 0.1 g of phosphoric acid and 0.1 g of terephthalic acid are added.

[0126] Performance Testing

[0127] When the prepared hard-soft carbon composite material is used as the negative electrode material of sodium ion battery, the electrode test conditions are:

[0128] The electrode is composed of 80% modified asphalt-based sodium ion battery negative electrode material, 10% by mass Super P and 10% by mass sodium alginate, and the diluent is deionized water. The electrolyte is a solvent in which 1 mol of sodium hexafluorophosphate is dissolved and the volume ratio of DME is 100 Vol%.

[0129] The performance data of the hard and soft carbon composite materials for the negative electrode of sodium ion batteries obtained in Examples 1 to 13 and Comparative Examples 1 to 5 are summarized as shown in Table 1:

[0130] Table 1 Preparation parameters of Examples 1 to 13 and Comparative Examples 1 to 5 and performance test data of the obtained hard and soft carbon composite materials

[0131]

[0132] In Comparative Example 1, no light component small molecule stabilizer was added during the preparation, and its 30mA / g reversible specific capacity and first charge and discharge efficiency (hereinafter referred to as first efficiency) were only 221.8mAh / g and 65%, respectively, and the electrochemical performance was not good, indicating that only under the action of the heavy component small molecule oxidant, the light component in the road petroleum asphalt precursor volatilized and lost a lot during the high-temperature carbonization process, resulting in the prepared carbon material mainly showing soft carbon properties. Since the sodium storage capacity of the soft carbon may be improved after oxidation modification, its electrochemical performance is not too bad, but the improvement effect of the oxidation modification is limited, so the electrochemical performance is not good.

[0133] In Comparative Example 2, no heavy component small molecule oxidant was added during the preparation, and its 30mA / g reversible specific capacity and first efficiency were only 203.1mAh / g and 62%, respectively, and the electrochemical performance was poor, indicating that only under the action of the light component small molecule stabilizer, although the light component in the road petroleum asphalt precursor was fixed, the heavy component part was not oxidatively modified, and it was difficult to organically combine the hard carbon derived from the light component with the soft carbon derived from the heavy component, and it was impossible to achieve the complementary advantages of hard and soft carbon, resulting in poor electrochemical performance.

[0134] In Comparative Example 3, neither of the above two small molecule preparations was added during the preparation, and its 30mA / g reversible specific capacity and first efficiency were only 157.2mAh / g and 54%, respectively, and the electrochemical performance was even worse, indicating that the effects of the two small molecule preparations were lacking. Not only were the light components not retained in the road petroleum asphalt precursor, but the soft carbon derived from the heavy components was not subjected to oxidative modification. In other words, the prepared carbon material could only exhibit soft carbon properties, and the structure of the soft carbon had not been optimized by oxidative modification. Its sodium storage capacity was particularly low, resulting in particularly poor electrochemical performance.

[0135] In Examples 1 to 13, the electrochemical properties are all good, the 30mA / g reversible specific capacity is all greater than 260mAh / g, and the first efficiency is all greater than 70%; among them, the 30mA / g reversible specific capacity of Examples 1, 4, 5, 7, and 13 is all above 275mAh / g, and the first efficiency is basically around 80% or even exceeds 80%; this indicates that the hard-soft carbon composite material prepared by the present invention has good electrochemical properties when applied to the negative electrode of a sodium ion battery, thereby proving that the road petroleum asphalt used in the present invention has a very good composite effect of hard carbon and soft carbon derived from the light component and the heavy component respectively under the action of the light component small molecule stabilizer and the heavy component small molecule oxidant, and the composite material achieves the complementary effect of the advantages of hard and soft carbon.

[0136] Finally, in Comparative Example 4, an excessive amount of light component small molecule stabilizer and heavy component small molecule oxidant was added. Although its electrochemical test data was also good (slightly lower than the lowest level in Examples 1 to 7), it caused a waste of raw materials; while in Comparative Example 5, too little light component small molecule stabilizer and heavy component small molecule oxidant were added, and its electrochemical test data was even lower than that of Comparative Example 4, indicating that insufficient light component small molecule stabilizer and heavy component small molecule oxidant resulted in incomplete modification of the light / heavy components, which also proved the rationality of the raw material ratio in the present application.

[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A road petroleum asphalt-based hard-soft carbon composite material, characterized in that: The raw materials used for the hard-soft carbon composite materials include road petroleum asphalt, a light component small molecule stabilizer, a heavy component small molecule oxidant, an activator and a solvent; and in terms of g / mL / g / g / g, the road petroleum asphalt: solvent: light component small molecule stabilizer: heavy component small molecule oxidant: activator is 1:15-25:0.05-0.2:0.05-0.2:2-5.

2. A road petroleum asphalt-based hard-soft carbon composite material as claimed in claim 1, characterized in that: The light component small molecule stabilizer includes one of phosphoric acid, polyphosphoric acid and resorcinol.

3. A road petroleum asphalt-based hard-soft carbon composite material as claimed in claim 1, characterized in that: The heavy component small molecule oxidant includes one of terephthalic acid alcohol, benzaldehyde and terephthaloyl chloride.

4. A road petroleum asphalt-based hard-soft carbon composite material as claimed in claim 1, characterized in that: The activator includes one of potassium hydroxide, sodium hydroxide and phosphoric acid.

5. A road petroleum asphalt-based hard-soft carbon composite material as claimed in claim 1, characterized in that: The solvent is trichloroethylene.

6. A road petroleum asphalt-based hard-soft carbon composite material as claimed in claim 1, characterized in that: The road petroleum asphalt includes one of AH-90 base asphalt, AH-70 base asphalt and AH-50 base asphalt.

7. A method for preparing a road petroleum asphalt-based hard-soft carbon composite material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, preparing a composite slurry: mixing road petroleum asphalt, a solvent, a light component small molecule stabilizer and a heavy component small molecule oxidant in proportion, and then ultrasonically treating for 20-40 minutes to obtain a composite slurry; S2, cross-linking treatment of the light component: in an inert gas atmosphere, the composite slurry is heated to 160-180° C., and then stirred at a constant temperature for 1-2 hours to obtain a first modified asphalt composite; S3, cross-linking treatment of the heavy component: heating the first modified asphalt composite to 300-500° C. in an inert gas atmosphere, and then keeping the temperature constant for 1-2 hours to obtain a second modified asphalt composite; S4, activation: adding an activator to the second modified asphalt composite, and then heating to 800°C in an inert gas atmosphere, and then maintaining the temperature for 1-2 hours for activation treatment; S5, carbonization: in an inert gas atmosphere, the activated second modified asphalt composite is heated to 1000-1400°C, and then carbonized at a constant temperature for 2-3 hours to obtain a road petroleum asphalt-based hard-soft carbon composite material.

8. The method for preparing a road petroleum asphalt-based hard-soft carbon composite material according to claim 7, characterized in that: The inert gas includes one of nitrogen and argon.

9. A negative electrode plate for a sodium ion battery, characterized in that: A road petroleum asphalt-based hard-soft carbon composite material comprising the material described in any one of claims 1-6.

10. A sodium ion battery, characterized in that Including the sodium ion battery negative electrode plate as described in claim 9.

Citation Information

Patent Citations

  • Anode material precursor with high carbon residue rate and preparation method and application thereof

    CN111785963A

  • Preparation method of soft carbon-hard carbon composite material with high initial efficiency

    CN114852989A

  • Preparation method of fast-charging negative electrode material

    CN116190647A

  • Heteroatom doped hard carbon-soft carbon composite material and preparation method and application thereof

    CN117059759A

  • Soft carbon-coated phosphorus-doped hard carbon composite material as well as preparation method and application thereof

    CN117894952A

Cited By

  • Method for preparing hard and soft carbon core-shell material based on biomass depolymerization technology and application of hard and soft carbon core-shell material

    CN120039865A

  • Asphalt-based hard carbon negative electrode material for sodium-ion battery and preparation method of asphalt-based hard carbon negative electrode material

    CN120081362A

  • Soft and hard carbon composite material and preparation method and application thereof

    CN122224818A

  • Soft-hard carbon composite material and preparation method and application thereof

    CN122224818B