A high-strength spray-formed cold-rolled work roll blank and a preparation method thereof
By adding carbon and chromium to the injection molded cold rolling working roll roll blank and combining dual frequency induction heating technology, the problem of insufficient mechanical properties in the existing technology is solved, and the rolling performance of high strength and high hardness is achieved, satisfying the ultra-high Performance requirements of high-strength steel products.
Patent Information
- Application Number
- CN202410412722.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-04-08
AI Technical Summary
The mechanical properties of existing jet-formed cold-rolled working rollers are insufficient and cannot meet the performance requirements of ultra-high strength steel products for high temperature resistance, corrosion resistance, wear resistance, fatigue resistance, etc.
The preparation method of high-strength jet forming cold rolling working roll roll blank is adopted, including jet forming, hot press sintering, forging and quenching treatment. By adding appropriate amounts of carbon and chromium to the raw materials, and using dual-frequency induction heating to form high hardness diffuse carbides , and the density and structure homogenization of the rolls are improved by injection molding and quenching treatment.
The yield strength, tensile strength and density of the roll are significantly improved, forming a high-hard hardened layer, meeting the mechanical properties requirements of ultra-high strength steel products.
Smart Images

Figure BDA0004779772080000061 
Figure BDA0004779772080000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cold rolling, and in particular to a high-strength spray-formed cold-rolled working roll blank and a preparation method thereof. Background Art
[0002] In order to meet the needs of ultra-high-strength steel products and processes, the rollers used to prepare ultra-high-strength steel must have excellent mechanical properties, that is, the surface of the roller must have extremely high hardness and meet the requirements of high temperature resistance, corrosion resistance, wear resistance, and fatigue resistance, while the core must have high toughness and meet the requirements of torque, bending moment, impact, and fatigue. With the development of the mechanical properties of high-strength steel products, small-diameter continuous rolling mills or 20-roller rolling mills have been gradually promoted, which has put forward new requirements for the mechanical properties of rollers. High-speed steel roller production lines conventionally use electroslag remelting to manufacture high-speed steel working rollers, which have the advantages of low cost and relatively low manufacturing difficulty.
[0003] As a new type of rapid solidification technology, spray forming is a process in which molten metal or alloy liquid flow is atomized into fine liquid particles under the impact of high-speed argon or nitrogen and other inert gases, and then sprayed onto the metal depositor and welded together to quickly form a preformed roll blank with high density. Since the fine particles quickly release heat during flight and are in a semi-solid or supercooled liquid state during deposition, the shape and size of the blank can be accurately controlled by controlling the movement of the substrate. Therefore, spray forming is a comprehensive process of rapid solidification, semi-solid processing and near-net shape processing. Compared with traditional metallurgical processes, spray forming integrates alloy smelting and forming into one step, significantly reducing the possibility of material oxidation, and the grains are relatively fine, but there are disadvantages such as uneven primary carbides, relatively insufficient mechanical properties, and prone to accidents, which can no longer meet the needs of rolling. Therefore, the present invention studies and prepares a high-strength spray-formed cold-rolled work roll blank with excellent mechanical properties. Summary of the invention
[0004] The object of the present invention is to provide a high-strength spray-formed cold-rolled work roll blank and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a high-strength spray-formed cold-rolled working roll blank, the chemical components and contents of the high-strength spray-formed cold-rolled working roll blank are: C: 0.82-1.08wt%, Si: 0.6-1.2wt%, Mn: 0.4-0.6wt%, P: 0.01-0.03wt%, S: 0.003-0.009wt%, Cr: 2.8-4.5wt%, Ni: 0.8-1.2wt%, Mo: 1.0-1.4wt%, Co: 1.2-1.8wt%, V: 0.05-0.08wt%, and the rest is Fe.
[0006] Preferably, the yield strength of the high-strength spray-formed cold-rolled work roll blank is ≥752MPa, the tensile strength is ≥982MPa, the density is ≥99.8%, and the grain size is ≤14μm.
[0007] Preferably, the method for preparing the high-strength spray-formed cold-rolled working roll blank comprises the following specific steps: spray-forming, hot-pressing sintering, forging, and quenching the raw materials to obtain the high-strength spray-formed cold-rolled working roll blank.
[0008] Preferably, during the injection molding, the raw material is melted and then atomized at a rate of 3 to 5 kg / min through an induction heated liquid guide tube under the action of atomizing gas nitrogen to form a molten droplet jet. The atomization pressure is 0.8 to 1.2 MPa, the angle is 30 to 60°, and the molten droplet jet is sprayed onto a deposition substrate with a rotation speed of 8 to 12 r / min. The deposition substrate is preheated to 550 to 650°C and the spraying temperature is 800 to 840°C.
[0009] Preferably, during the induction heating, the inductor has a frequency of 50 to 70 Hz and a power of 220 to 320 kW.
[0010] Preferably, during the hot pressing sintering, the temperature is raised to 550-650°C, 850-950°C and 1400-1500°C in sequence, and kept warm for 4-6 minutes, 8-10 minutes and 5-10 minutes respectively, and when cooled to 950-1050°C with the furnace, it is kept warm for 5-8 hours and cooled with the furnace.
[0011] Preferably, during the forging, the temperature is maintained at 1150-1250° C., the forging ratio is 4-6, and the die pressing rate is 0.04-0.06 mm / s.
[0012] Preferably, the quenching treatment is carried out in sequence: preheating, dual-frequency induction heating, cooling, and low-temperature tempering.
[0013] Preferably, during the dual-frequency induction heating, the frequency of inductor 1 is 80-100 Hz, the time is 4-10 min, and the power is 280-420 kW; the frequency of inductor 2 is 200-240 Hz, the time is 6-9 min, and the power is 50-140 kW.
[0014] Preferably, the preheating temperature is 260-350°C, and the low-temperature tempering temperature is 120-180°C.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0016] When the high-strength spray-molding cold-rolled work roll blank is produced, the process is sequentially spray-molding, hot-pressing sintering, forging, and quenching.
[0017] Adding a small amount of carbon to the raw material components of the cold-rolled work roll blank can increase the carbon content in the high-speed steel austenite during quenching treatment, strengthen the dispersion hardening effect, and then form high-hardness dispersed carbides with a small amount of chromium and vanadium. The addition of vanadium also strengthens the refinement of the roll blank grain structure, thereby improving the strength of the roll blank;
[0018] In the process of spray forming, the raw materials are melted, atomized under the action of atomizing gas to form a molten droplet jet, and then sprayed directly on the deposition substrate to form a roller blank. The liquid guide tube is induction heated during atomization. The roller blank formed in this way has a finer structure and better mechanical properties. The quenching treatment is preheating, dual-frequency induction heating, cooling and low-temperature tempering. The quenching adopts the method of double-induction heating. The heat is concentrated on the surface of the roller blank, so that a temperature field with a certain gradient is formed from the surface to the core. The structure transformation occurs within a certain depth range of the surface, and a hardened layer of a certain depth is produced, so that the roller has a high surface hardness. Spray forming combined with dual-frequency induction heating can further increase the density, make the structure more homogeneous, and further improve the strength. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] The chemical composition and content are: C: 0.82wt%, Si: 0.6wt%, Mn: 0.4wt%, P: 0.01wt%, S: 0.003wt%, Cr: 2.8wt%, Ni: 0.8wt%, Mo: 1.0wt%, Co: 1.2wt%, V: 0.05wt%, the rest is Fe
[0022] (1) Spray molding: After the raw material is melted, it is passed through an induction heating liquid guide tube at a rate of 3 kg / min. The inductor is 50 Hz and the power is 220 kW. It is atomized to form a molten droplet jet under the action of atomizing gas nitrogen. The atomizing pressure is 0.8 MPa and the angle is 30°. It is sprayed on the deposition substrate at a rotation speed of 8 r / min. The deposition substrate is preheated to 550°C and the spraying temperature is 800°C.
[0023] (2) Hot pressing sintering: heat up to 550°C, 850°C and 1400°C in sequence, keep them at that temperature for 4 min, 8 min and 5 min respectively, cool down with the furnace to 950°C, keep them at that temperature for 5 h, and cool down with the furnace;
[0024] (3) Forging: The temperature during forging is maintained at 1150°C, the forging ratio is 4, and the die pressing rate is 0.04 mm / s
[0025] (4) Quenching treatment: preheating, dual-frequency induction heating, cooling, and low-temperature tempering are performed in sequence; the preheating temperature is 260°C, and during dual-frequency induction heating, inductor 1 is 80 Hz, the time is 4 min, and the power is 280 kW, inductor 2 is 200 Hz, the time is 6 min, the power is 50 kW, and the cooling and low-temperature tempering temperature is 120°C.
[0026] Example 2
[0027] The chemical composition and content are: C: 0.95wt%, Si: 0.9wt%, Mn: 0.5wt%, P: 0.02wt%, S: 0.006wt%, Cr: 3.7wt%, Ni: 1.0wt%, Mo: 1.2wt%, Co: 1.6wt%, V: 0.06wt%, the rest is Fe
[0028] (1) Spray molding: After the raw material is melted, it is passed through an induction heating liquid guide tube at a rate of 4 kg / min. The inductor is 60 Hz and the power is 270 kW. It is atomized to form a molten droplet jet under the action of atomizing gas nitrogen. The atomizing pressure is 1.0 MPa and the angle is 45°. It is sprayed on a deposition substrate with a rotation speed of 10 r / min. The deposition substrate is preheated to 600°C and the spraying temperature is 820°C.
[0029] (2) Hot pressing sintering: heat up to 600°C, 900°C and 1450°C in sequence, keep warm for 5 min, 9 min and 8 min respectively, cool down to 1000°C, keep warm for 6 h, and cool down;
[0030] (3) Forging: The temperature during forging is maintained at 1200°C, the forging ratio is 5, and the die pressing rate is 0.05 mm / s
[0031] (4) Quenching treatment: preheating, dual-frequency induction heating, cooling, and low-temperature tempering are performed in sequence; the preheating temperature is 305°C, and during dual-frequency induction heating, inductor 1 is 90 Hz, the time is 7 min, and the power is 340 kW, and inductor 2 is 220 Hz, the time is 8 min, the power is 95 kW, and the cooling and low-temperature tempering temperature is 150°C.
[0032] Example 3
[0033] The chemical composition and content are: C: 1.08wt%, Si: 1.2wt%, Mn: 0.6wt%, P: 0.03wt%, S: 0.009wt%, Cr: 4.5wt%, Ni: 1.2wt%, Mo: 1.4wt%, Co: 1.8wt%, V: 0.08wt%, the rest is Fe
[0034] (1) Spray molding: After the raw material is melted, it is passed through an induction heating liquid guide tube at a rate of 5 kg / min. The inductor is 70 Hz and the power is 320 kW. It is atomized to form a molten droplet jet under the action of atomizing gas nitrogen. The atomizing pressure is 1.2 MPa and the angle is 60°. It is sprayed on the deposition substrate at a rotation speed of 12 r / min. The deposition substrate is preheated to 650°C and the spraying temperature is 840°C.
[0035] (2) Hot pressing sintering: heat up to 650°C, 950°C and 1500°C in sequence, keep them at this temperature for 6 min, 10 min and 10 min respectively, cool down with the furnace to 1050°C, keep them at this temperature for 8 h, and cool down with the furnace;
[0036] (3) Forging: The temperature during forging is maintained at 1250°C, the forging ratio is 6, and the die pressing rate is 0.06 mm / s
[0037] (4) Quenching treatment: preheating, dual-frequency induction heating, cooling, and low-temperature tempering are performed in sequence; the preheating temperature is 350°C, and during dual-frequency induction heating, the inductor 1 is 100 Hz, the time is 10 min, and the power is 420 kW, and the inductor 2 is 240 Hz, the time is 9 min, the power is 140 kW, and the cooling and low-temperature tempering temperature is 180°C.
[0038] Comparative Example 1
[0039] The prescription composition of comparative example 1 is the same as that of example 2. The method for manufacturing a high-strength spray-formed cold-rolled work roll blank is different from that of example 2 only in that the chemical composition and content are: C: 0.95wt%, Si: 0.9wt%, Mn: 0.5wt%, P: 0.02wt%, S: 0.006wt%, Cr: 3.7wt%, Ni: 1.0wt%, Mo: 1.2wt%, Co: 1.6wt%, and the rest is Fe.
[0040] Comparative Example 2
[0041] The prescription composition of comparative example 2 is the same as that of example 2. The method for making a high-strength spray-formed cold-rolled work roll blank is different from that of example 2 only in that the chemical composition and content are: C: 0.95wt%, Si: 0.9wt%, Mn: 0.5wt%, P: 0.02wt%, S: 0.006wt%, Ni: 1.0wt%, Mo: 1.2wt%, Co: 1.6wt%, V: 0.06wt%, and the rest is Fe.
[0042] Comparative Example 3
[0043] The prescription composition of comparative example 3 is the same as that of example 2. The method for manufacturing a high-strength spray-molded cold-rolled work roll blank is different from that of example 2 only in that after the raw material is melted in spray molding, it is atomized under the action of an atomizing gas to form a molten droplet jet, which is directly sprayed on a deposition substrate to form a roll blank.
[0044] Comparative Example 4
[0045] The prescription composition of comparative example 4 is the same as that of example 2. The method for manufacturing the high-strength spray-molded cold-rolled work roll blank is different from that of example 2 only in that the high-strength spray-molded cold-rolled work roll blank is subjected to spray molding, hot pressing sintering, forging, and annealing treatment at 800° C. for 6 hours in sequence.
[0046] Effect example
[0047] Table 1 below shows the performance analysis results of the high-strength spray-formed cold-rolled work roll blanks of Examples 1 to 3 of the present invention and Comparative Examples 1 to 4:
[0048] 752MPa, tensile strength ≥982MPa, density ≥99.8%, grain size ≤14μ
[0049] Table 1
[0050]
[0051]
[0052] By comparing the experimental data of the embodiments and the comparative examples in Table 1, it can be clearly found that the high-strength spray-formed cold-rolled work roll blanks prepared in Examples 1, 2, and 3 have excellent mechanical properties.
[0053] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, Comparative Example 3, it can be found that adding a small amount of carbon to the raw material components of the cold-rolled work roll blank can increase the carbon content in the austenite of the high-speed steel during the quenching treatment, strengthen the dispersion hardening effect, and then form high-hardness dispersed carbides with a small amount of chromium and vanadium. The addition of vanadium also strengthens the refinement of the roll blank grain structure, thereby improving the strength and wear resistance of the roll blank;
[0054] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 3, Comparative Example 4, it can be found that after the raw material is melted, it is atomized to form a molten droplet jet under the action of the atomizing gas, and is directly sprayed on the deposition substrate to form a roller blank. The liquid guide tube is induction heated during atomization. The roller blank formed by this injection molding method has a finer structure and better mechanical properties. The quenching treatment is preheating, dual-frequency induction heating, cooling and low-temperature tempering. The quenching adopts a double-splicing induction heating method. The heat is concentrated on the surface of the roller blank, so that a temperature field with a certain gradient is formed from the surface to the core. A structural transformation occurs within a certain depth range of the surface, and a hardened layer of a certain depth is produced, so that the roller has a high surface hardness. Injection molding is combined with dual-frequency induction heating to further increase the density, make the structure more homogenous, and further improve the strength and wear resistance.
[0055] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A high-strength spray-formed cold-rolled work roll blank, It is characterized in that The chemical composition and content of the high-strength spray-formed cold-rolled work roll blank are: C: 0.82-1.08wt%, Si: 0.6-1.2wt%, Mn: 0.4-0.6wt%, P: 0.01-0.03wt%, S: 0.003-0.009wt%, Cr: 2.8-4.5wt%, Ni: 0.8-1.2wt%, Mo: 1.0-1.4wt%, Co: 1.2-1.8wt%, V: 0.05-0.08wt%, and the rest is Fe; The method for preparing a high-strength spray-formed cold-rolled work roll blank comprises the following specific steps: spray-forming, hot-pressing sintering, forging, and quenching the raw materials to obtain a high-strength spray-formed cold-rolled work roll blank; During the injection molding, the raw material is melted and then atomized at a rate of 3-5 kg / min through an induction-heated liquid guide tube under the action of atomizing gas nitrogen to form a molten droplet jet, the atomizing pressure is 0.8-1.2 MPa, the angle is 30-60°, and the molten droplet jet is sprayed on a deposition substrate at a rotation speed of 8-12 r / min, the deposition substrate is preheated at 550-650°C, and the spraying temperature is 800-840°C; The quenching treatment is performed in sequence: preheating, dual-frequency induction heating, cooling, and low-temperature tempering.
2. A high-strength spray-formed cold-rolled work roll blank according to claim 1, It is characterized in that The high-strength spray-formed cold-rolled work roll blank has a yield strength of ≥752MPa, a tensile strength of ≥982MPa, a density of ≥99.8%, and a grain size of ≤14μm.
3. The method for preparing a high-strength spray-formed cold-rolled work roll blank according to claim 1, It is characterized in that The method for preparing a high-strength spray-formed cold-rolled work roll blank comprises the following specific steps: spray-forming, hot-pressing sintering, forging, and quenching the raw materials to obtain a high-strength spray-formed cold-rolled work roll blank; During the injection molding, the raw material is melted and then atomized at a rate of 3-5 kg / min through an induction-heated liquid guide tube under the action of atomizing gas nitrogen to form a molten droplet jet, the atomizing pressure is 0.8-1.2 MPa, the angle is 30-60°, and the molten droplet jet is sprayed on a deposition substrate at a rotation speed of 8-12 r / min, the deposition substrate is preheated at 550-650°C, and the spraying temperature is 800-840°C; The quenching treatment is performed in sequence: preheating, dual-frequency induction heating, cooling, and low-temperature tempering.
4. The method for preparing a high-strength spray-formed cold-rolled work roll blank according to claim 3, It is characterized in that During the induction heating, the inductor is 50-70 Hz and the power is 220-320 kW.
5. The method for preparing a high-strength spray-formed cold-rolled work roll blank according to claim 3, It is characterized in that During the hot pressing sintering, the temperature is raised to 550-650°C, 850-950°C and 1400-1500°C in sequence, and kept warm for 4-6 minutes, 8-10 minutes and 5-10 minutes respectively. When the temperature is cooled to 950-1050°C, it is kept warm for 5-8 hours and cooled in the furnace.
6. The method for preparing a high-strength spray-formed cold-rolled work roll blank according to claim 3, It is characterized in that During the forging, the temperature is maintained at 1150-1250° C., the forging ratio is 4-6, and the die pressing rate is 0.04-0.06 mm / s.
7. The method for preparing a high-strength spray-formed cold-rolled work roll blank according to claim 3, It is characterized in that During the dual-frequency induction heating, the frequency of inductor 1 is 80-100 Hz, the time is 4-10 minutes, and the power is 280-420 kW; the frequency of inductor 2 is 200-240 Hz, the time is 6-9 minutes, and the power is 50-140 kW.
8. The method for preparing a high-strength spray-formed cold-rolled work roll blank according to claim 3, It is characterized in that The preheating temperature is 260-350°C, and the low-temperature tempering temperature is 120-180°C.