Multilayer Ceramic Capacitors
The multilayer ceramic capacitor addresses reliability issues by using specific roughness and particle size controls in the internal electrode layers to maintain continuity and prevent liquid phase aggregation, enhancing performance.
Patent Information
- Application Number
- JP2023014149
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-01
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2038-02-26
AI Technical Summary
The continuity rate of the internal electrode layer in multilayer ceramic capacitors decreases due to differences in sintering start temperatures between the metal and ceramic layers, leading to surface roughness deterioration and thickness variations, which affect reliability.
A multilayer ceramic capacitor design with internal electrode layers having an arithmetic mean roughness Ra of 28 nm or less and a maximum height Rz of 357 nm or less, using ceramic particles with a size of 15 nm or less and a standard deviation of 5 or less, and a metal component of nickel, with a thickness of 0.5 μm or less, to suppress the discharge of common materials and maintain electrode continuity.
This design enhances the reliability of the multilayer ceramic capacitor by reducing thickness variations and preventing liquid phase aggregation, ensuring predetermined characteristics are maintained.
Smart Images

Figure 0007576640000001 
Figure 0007576640000002 
Figure 0007576640000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic capacitor. [Background technology]
[0002] In recent years, as electronic devices such as smartphones and mobile phones become smaller, the electronic components mounted on them are also rapidly becoming smaller. For example, in multilayer ceramic capacitors, there is a demand for thinner dielectric layers and internal electrode layers in order to reduce chip size while maintaining prescribed characteristics (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-57098 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, due to the difference in sintering start temperature between the metal of the internal electrode layer and the ceramic of the dielectric layer, the continuity rate of the internal electrode layer after sintering decreases. For this reason, it is known to add a ceramic common material to the internal electrode layer to bring about a shrinkage retardation effect. However, when the internal electrode layer is thinned, the common material is easily extruded to the dielectric layer side. This deteriorates the surface roughness of the internal electrode layer, and the thickness of the internal electrode layer varies in the lamination direction of the dielectric layer and the internal electrode layer. When the thickness of the internal electrode layer varies, the liquid phase is easily condensed at the interface between the internal electrode layer and the dielectric layer in the part where the internal electrode layer is thin, and the reliability is easily deteriorated.
[0005] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a multilayer ceramic capacitor capable of suppressing deterioration in reliability. [Means for solving the problem]
[0006] The multilayer ceramic capacitor according to the present invention has a laminated structure in which dielectric layers mainly made of ceramic and internal electrode layers mainly made of metal are alternately laminated, and in at least a portion of the internal electrode layers, the arithmetic mean roughness Ra of the internal electrode layers is 28 nm or less, and in at least a portion of the internal electrode layers, the maximum height Rz of the internal electrode layers is 357 nm or less. the law of nature , The internal electrode layers contain ceramic particles having an average particle size of 15 nm or less and a standard deviation of particle size of 5 or less. It is characterized by:
[0007] In the multilayer ceramic capacitor, at least a portion of the internal electrode layers may have an arithmetic mean roughness Ra of 25 nm or less, and at least a portion of the internal electrode layers may have a maximum height Rz of 150 nm or less.
[0008] In the multilayer ceramic capacitor, the main metal component of the internal electrode layers may be nickel.
[0009] In the above multilayer ceramic capacitor, the main component ceramic of the dielectric layers may be barium titanate.
[0010] In the above multilayer ceramic capacitor, the internal electrode layers may have a thickness of 0.5 μm or less. Effect of the Invention
[0011] According to the present invention, it is possible to provide a multilayer ceramic capacitor capable of suppressing deterioration in reliability. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor. [Diagram 2] FIG. 2 is a diagram illustrating a flow of a method for manufacturing a multilayer ceramic capacitor. [Diagram 3]FIG. 3 is a diagram showing the average particle size, standard deviation, and cumulative particle size distribution slope of the main component metals and common materials of the conductive pastes for forming internal electrodes in the examples and comparative examples, and the amount of the common materials added. [Figure 4] 4(a) to 4(d) are SEM photographs of a cross section in the lamination direction of the dielectric layers and the internal electrode layers. [Diagram 5] FIG. 5 is a diagram showing the arithmetic mean roughness Ra and maximum height Rz of the internal electrode layers in the examples and comparative examples, and the capacitance, breakdown voltage (BDV), and high temperature accelerated life (HALT) of the multilayer ceramic capacitors. [Figure 6] 6(a) to 6(d) are diagrams showing the states of the dielectric layers and internal electrode layers in Comparative Example 8 from after the binder removal treatment to after densification. [Figure 7] 7(a) to 7(d) are diagrams showing the states of the dielectric layers and internal electrode layers from after the binder removal treatment to after densification in Comparative Example 3. FIG. [Figure 8] 8(a) to 8(d) are diagrams showing the states of the dielectric layers and internal electrode layers from after the binder removal treatment to after densification in Example 3. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment will be described with reference to the drawings.
[0014] (Embodiment) Fig. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to an embodiment. As illustrated in Fig. 1, the multilayer ceramic capacitor 100 includes a laminated chip 10 having a rectangular parallelepiped shape, and external electrodes 20a, 20b provided on any two opposing end faces of the laminated chip 10. Of the four faces of the laminated chip 10 other than the two end faces, the two faces other than the top and bottom faces in the stacking direction are referred to as side faces. The external electrodes 20a, 20b extend on the top, bottom and two side faces in the stacking direction of the laminated chip 10. However, the external electrodes 20a, 20b are spaced apart from each other.
[0015] The laminated chip 10 has a configuration in which dielectric layers 11 mainly made of a ceramic material that functions as a dielectric and internal electrode layers 12 mainly made of a metal material such as a base metal material are alternately laminated. The edges of the internal electrode layers 12 are alternately exposed to the end face on which the external electrode 20a of the laminated chip 10 is provided and the end face on which the external electrode 20b is provided. As a result, each internal electrode layer 12 is alternately conductive to the external electrode 20a and the external electrode 20b. As a result, the laminated ceramic capacitor 100 has a configuration in which a plurality of dielectric layers 11 are laminated via the internal electrode layers 12. In addition, in the laminate of the dielectric layers 11 and the internal electrode layers 12, the internal electrode layers 12 are arranged on the outermost layer in the lamination direction, and the upper and lower surfaces of the laminate are covered by the cover layers 13. The cover layers 13 are mainly made of a ceramic material. For example, the material of the cover layers 13 is the same as that of the dielectric layers 11 and the ceramic material.
[0016] The size of the multilayer ceramic capacitor 100 is, for example, 0.2 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 1.6 mm in length, 0.8 mm in width, and 0.8 mm in height, or 2.0 mm in length, 1.25 mm in width, and 1.25 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height, but is not limited to these sizes.
[0017] The internal electrode layers 12 are mainly composed of base metals such as Ni (nickel), Cu (copper), and Sn (tin). The internal electrode layers 12 may be mainly composed of precious metals such as Pt (platinum), Pd (palladium), Ag (silver), and Au (gold), or alloys containing these. The average thickness of the internal electrode layers 12 is, for example, 0.5 μm or less, and preferably 0.3 μm or less. The dielectric layers 11 are mainly composed of a ceramic material having a perovskite structure represented by the general formula ABO3. The perovskite structure is an ABO that deviates from the stoichiometric composition. 3-αFor example, the ceramic material includes BaTiO3 (barium titanate), CaZrO3 (calcium zirconate), CaTiO3 (calcium titanate), SrTiO3 (strontium titanate), BaTiO3 (strontium titanate) which forms a perovskite structure, 1-x-y Ca x Sr y Ti 1-z Zr z O3 (0≦x≦1, 0≦y≦1, 0≦z≦1) can be used. The thickness of the dielectric layer 11 is, for example, 0.8 μm or less.
[0018] In order to miniaturize and increase the capacity of the multilayer ceramic capacitor 100, it is required to make the dielectric layers 11 and the internal electrode layers 12 thinner. Due to the difference in the sintering start temperature between the metal of the internal electrode layer 12 and the ceramic of the dielectric layer 11, there is a problem that the continuity rate of the internal electrode layer after sintering decreases. For this reason, it is known to add a ceramic co-material to the internal electrode layer 12 to bring about a shrinkage delay effect. However, when the internal electrode layer 12 becomes thinner, the co-material is easily released to the dielectric layer 11 side, and the surface roughness of the internal electrode layer 12 deteriorates. As a result, the thickness of the internal electrode layer 12 varies in the lamination direction of the dielectric layer 11 and the internal electrode layer 12. When the thickness of the internal electrode layer 12 varies, a liquid phase is easily coagulated at the interface between the internal electrode layer 12 and the dielectric layer 11 in the part where the internal electrode layer 12 is thin, and the reliability is easily deteriorated.
[0019] Therefore, in this embodiment, the surface roughness of the internal electrode layer 12 is reduced. Specifically, the arithmetic mean roughness Ra of the internal electrode layer 12 is set to 30 nm or less, and the maximum height Rz of the internal electrode layer 12 is set to 360 nm or less. Here, the arithmetic mean roughness Ra and the maximum height Rz are those specified in JIS B 0601:2013. The arithmetic mean roughness Ra is preferably set to 25 nm or less. The maximum height Rz is preferably set to 150 nm or less. In this configuration, the variation in the thickness of the internal electrode layer 12 is reduced, and further, the continuity rate of the internal electrode layer 12 is increased. As a result, the liquid phase is suppressed from coagulating at the interface between the dielectric layer 11 and the internal electrode layer 12, so that the deterioration of reliability is suppressed and it is possible to obtain a predetermined characteristic. If the average thickness of the internal electrode layer 12 is 0.5 μm or less, the common material is easily discharged to the dielectric layer 11, so this configuration is effective when the average thickness of the internal electrode layer 12 is 0.5 μm or less.
[0020] Next, a description will be given of a method for manufacturing the multilayer ceramic capacitor 100. FIG.
[0021] (Raw powder production process) First, as illustrated in FIG. 2, a dielectric material for forming the dielectric layer 11 is prepared. The A-site elements and B-site elements contained in the dielectric layer 11 are usually contained in the dielectric layer 11 in the form of a sintered body of ABO3 particles. For example, BaTiO3 is a tetragonal compound having a perovskite structure and exhibits a high dielectric constant. This BaTiO3 can generally be obtained by synthesizing barium titanate by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. Various methods have been known so far as a method for synthesizing the ceramics constituting the dielectric layer 11, such as a solid-phase method, a sol-gel method, a hydrothermal method, and the like. In this embodiment, any of these methods can be adopted.
[0022] The obtained ceramic powder is added with a specific additive compound according to the purpose, such as oxides of Mn (manganese), V (vanadium), Cr (chromium), rare earth elements (Y (yttrium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium) and Yb (ytterbium)), as well as oxides or glasses of Co (cobalt), Ni (nickel), Li (lithium), B (boron), Na (sodium), K (potassium) and Si (silicon).
[0023] In this embodiment, preferably, first, a compound containing an additive compound is mixed with the ceramic particles constituting the dielectric layer 11, and calcined at 820 to 1150°C. Then, the obtained ceramic particles are wet-mixed with the additive compound, and then dried and pulverized to prepare a ceramic powder. For example, the average particle size of the ceramic powder is preferably 50 to 300 nm from the viewpoint of thinning the dielectric layer 11. For example, the ceramic powder obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size.
[0024] (Lamination process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained dielectric material and wet mixed. The obtained slurry is used to coat a strip-shaped dielectric green sheet, for example, with a thickness of 0.8 μm or less, on a substrate by, for example, a die coater method or a doctor blade method, and then dried.
[0025] Next, a metal conductive paste for forming an internal electrode containing an organic binder is printed on the surface of the dielectric green sheet by screen printing, gravure printing, or the like to arrange an internal electrode layer pattern that is alternately drawn to a pair of external electrodes with different polarities. For example, a metal material of the metal conductive paste is used that has an average particle size of 100 nm or less. In addition, the standard deviation of the particle size is set to 15 or less. This allows a sharp particle size distribution to be obtained. The average particle size is preferably 100 nm or less, more preferably 70 nm or less. In addition, the maximum particle size is preferably 140 nm or less. This is because if a metal material having a particle size larger than 140 nm is mixed in, the surface roughness of the internal electrode layer 12 will deteriorate due to the large particle size. The standard deviation of the particle size is preferably 15 or less, more preferably 12 or less. In addition, the slope of the cumulative particle size distribution is preferably 8 or more. The slope of the cumulative particle size distribution can be defined as the slope between D20 and D80 (=1 / (logD80-logD20)) when the cumulative particle size distribution is logarithmically plotted.
[0026] Ceramic particles are added to the metal conductive paste as a co-material. The main component ceramic of the ceramic particles is not particularly limited, but is preferably the same as the main component ceramic of the dielectric layer 11. For example, barium titanate may be uniformly dispersed. The co-material has an average particle size of 10 nm or less. The standard deviation of the particle size is 5 or less. This allows a sharp particle size distribution to be obtained. The average particle size is preferably 15 nm or less, more preferably 10 nm or less. The standard deviation of the particle size is preferably 5 or less, more preferably 3 or less. The slope of the cumulative particle size distribution is preferably 7 or more. The slope of the cumulative particle size distribution can be defined as the slope between D20 and D80 (=1 / (logD80-logD20)) when the cumulative particle size distribution is logarithmically plotted. Furthermore, the amount of the co-material added is preferably 2.5 to 25 parts by weight, more preferably 5 to 20 parts by weight, relative to 100 parts by weight of the metal material. If the amount of the common material added is less than 5 parts, the continuity rate of the internal electrode layer 12 decreases due to the insufficient amount of the common material, and the arithmetic mean roughness Ra and the maximum height Rz deteriorate. Conversely, if the amount of the common material added is more than 20 parts, the amount of the common material is too large, and the continuity rate of the internal electrode layer 12 decreases, and the arithmetic mean roughness Ra and the maximum height Rz deteriorate.
[0027] Then, the dielectric green sheet on which the internal electrode layer pattern is printed is punched out to a predetermined size, and the punched dielectric green sheet is laminated by a predetermined number of layers (for example, 100 to 500 layers) so that the internal electrode layer 12 and the dielectric layer 11 are alternated and the internal electrode layer 12 is alternately drawn out to a pair of external electrodes 20a, 20b with different polarities with the end edges alternately exposed on both end faces in the length direction of the dielectric layer 11. Cover sheets that become the cover layer 13 are pressed on the top and bottom of the laminated dielectric green sheet, and the laminated dielectric green sheet is cut to a predetermined chip size (for example, 1.0 mm x 0.5 mm), and then a metal conductive paste that becomes the base layer of the external electrodes 20a, 20b is applied to both end faces of the cut laminate by a dipping method or the like and dried. As a result, a molded body of the multilayer ceramic capacitor 100 is obtained.
[0028] (Firing process) The molded body thus obtained was subjected to binder removal treatment in a N2 atmosphere at 250 to 500°C, and then subjected to a 10 -5 ~10 -8 By firing at 1100 to 1300°C for 10 minutes to 2 hours in a reducing atmosphere of atm, each compound is sintered and grains grow (densification). In this way, a multilayer ceramic capacitor 100 is obtained. The amount of the common material remaining in the internal electrode layer 12 can be adjusted by adjusting the firing conditions. Specifically, by increasing the temperature rise rate in the firing process, the main component metal is sintered before the common material is discharged from the metal conductive paste, so that the common material is more likely to remain in the internal electrode layer 12. For example, from the viewpoint of increasing the amount of the common material remaining in the internal electrode layer 12, the average temperature rise rate from room temperature to the maximum temperature in the firing process is preferably 30°C / min or more, more preferably 45°C / min or more. If the average temperature rise rate is too high, the organic components remaining in the molded body are not sufficiently discharged, and problems such as cracks occurring during the firing process may occur. Alternatively, there is a risk of problems such as insufficient densification due to the occurrence of an internal and external difference in sintering of the molded body, resulting in a decrease in capacitance. Therefore, the average temperature rise rate is preferably 80° C. / min or less, and more preferably 65° C. / min or less.
[0029] (Reoxidation treatment process) After that, a re-oxidation treatment may be performed at 600°C to 1000°C in an N2 gas atmosphere. (Plating process) Thereafter, the undercoat layers of the external electrodes 20a, 20b are coated with a metal such as Cu, Ni, Sn, etc. by plating.
[0030] According to the manufacturing method of the multilayer ceramic capacitor of this embodiment, a highly dispersed metal conductive paste is produced by using small-diameter materials with sharp particle size distribution as the main component metal and common material constituting the internal electrode layer 12. Also, the mixing of large materials partially is suppressed. By using such a metal conductive paste, the diffusion of the common material into the dielectric layer 11 during the sintering process is suppressed, and the deterioration of the arithmetic mean roughness Ra and maximum height Rz of the internal electrode layer 12 is suppressed. Specifically, a metal powder having an average particle size of 100 nm or less and a standard deviation of the particle size distribution of 1.5 or less is used as the main component metal, and a ceramic powder having an average particle size of less than 10 nm and a standard deviation of the particle size distribution of 5 or less is used as the common material. Furthermore, the number of parts of the common material per 100 parts by weight of the metal powder is 2.5 to 25.
[0031] Suppressing the deterioration of the arithmetic mean roughness Ra and maximum height Rz of the internal electrode layers 12 suppresses the diffusion of the common material into the dielectric layers 11, resulting in a multilayer ceramic capacitor 100 having a high continuity rate of the internal electrode layers 12 and less variation in thickness of the internal electrode layers 12. This suppresses the aggregation of the liquid phase at the interface between the dielectric layers 11 and the internal electrode layers 12, suppressing the deterioration of reliability and making it possible to obtain predetermined characteristics. EXAMPLES
[0032] The multilayer ceramic capacitor according to the embodiment was fabricated and its characteristics were examined.
[0033] (Examples 1 to 5) Average particle size is 100 nm (specific surface area 10 m 2 The necessary additives were added to barium titanate powder (1.0 g / g), which was then thoroughly wet mixed and pulverized in a ball mill to obtain a dielectric material. An organic binder and solvent were added to the dielectric material, and a dielectric green sheet was produced using the doctor blade method. The coating thickness of the dielectric green sheet was set to 0.8 μm, and polyvinyl butyral (PVB) or the like was used as the organic binder, with ethanol, toluene acid, etc. added as the solvent. Other additives such as plasticizers were also added.
[0034] Next, a conductive paste for forming an internal electrode containing powder of the main component metal (Ni) of the internal electrode layer 12 (50 wt% Ni solid content), a co-material (barium titanate), 5 parts of a binder (ethyl cellulose), a solvent, and other auxiliary agents as necessary was prepared using a planetary ball mill. As shown in FIG. 3, the powder of the main component metal had an average particle size of 70 nm (specific surface area of 10 m 2 / g), a standard deviation of particle size of 12, and a slope of cumulative particle size distribution of 8. The co-material used had an average particle size of 8.6 nm, a standard deviation of particle size of 2.7, and a slope of cumulative particle size distribution of 7. The amounts of the co-material added, in parts per 100 parts by weight of the main component metal, were 2.5 parts in Example 1, 5 parts in Example 2, 10 parts in Example 3, 20 parts in Example 4, and 25 parts in Example 5.
[0035] A conductive paste for forming internal electrodes was screen-printed on a dielectric sheet. 250 sheets with the conductive paste for forming internal electrodes printed on them were stacked, and a cover sheet was laminated on the top and bottom of each. After that, a ceramic laminate was obtained by thermocompression bonding, and cut into a specified shape.
[0036] After the obtained ceramic laminate was debindered in a N2 atmosphere, a metal paste containing a metal filler mainly composed of Ni, a co-material, a binder, a solvent, etc. was applied to both end faces and each side of the ceramic laminate, and then dried. The metal paste was then fired simultaneously with the ceramic laminate at 1100°C to 1300°C for 10 minutes to 2 hours in a reducing atmosphere to obtain a sintered body. The average heating rate from room temperature to the maximum temperature was 55°C / min in all of Examples 1 to 5.
[0037] The dimensions of the obtained sintered body were length 1.0 mm, width 0.5 mm, and height 0.5 mm. The sintered body was subjected to a reoxidation treatment under conditions of 800°C in an N2 atmosphere, and then plated to form a Cu plating layer 22, a Ni plating layer 23, and a Sn plating layer 24 on the surface of the underlayer 21, thereby obtaining a multilayer ceramic capacitor 100. The average thickness of the internal electrode layers 12 in the multilayer ceramic capacitor 100 was 0.3 μm.
[0038] (Comparative Examples 1 to 10) In Comparative Examples 1 to 5, as shown in Fig. 3, the powder of the main component metal (Ni) of the conductive paste for forming the internal electrodes had an average particle size of 70 nm, a standard deviation of the particle size of 12, and a slope of the cumulative particle size distribution of 8. The co-material had an average particle size of 29 nm, a standard deviation of the particle size of 8.7, and a slope of the cumulative particle size distribution of 5. The amount of the co-material added was 2.5 parts in Comparative Example 1, 5 parts in Comparative Example 2, 10 parts in Comparative Example 3, 20 parts in Comparative Example 4, and 25 parts in Comparative Example 5.
[0039] In Comparative Examples 6 to 10, as shown in Fig. 3, the powder of the main component metal (Ni) of the conductive paste for forming the internal electrodes had an average particle size of 120 nm, a standard deviation of the particle size of 33, and a slope of the cumulative particle size distribution of 6. The co-material had an average particle size of 29 nm, a standard deviation of the particle size of 8.7, and a slope of the cumulative particle size distribution of 5. The amount of the co-material added was 2.5 parts in Comparative Example 6, 5 parts in Comparative Example 7, 10 parts in Comparative Example 8, 20 parts in Comparative Example 9, and 25 parts in Comparative Example 10. The other conditions were the same as those of Examples 1 to 5.
[0040] (analysis) 4(a) to 4(d) are SEM (scanning electron microscope) photographs of a cross section in the lamination direction of the dielectric layers 11 and the internal electrode layers 12 near the center in the length direction, width direction, and height direction. FIG. 4(a) is an SEM photograph of Comparative Example 3 in which the ceramic laminate was fired at 900°C, and FIG. 4(b) is an SEM photograph of Comparative Example 3 in which the ceramic laminate was fired at 1250°C. FIG. 4(c) is an SEM photograph of Example 3 in which the ceramic laminate was fired at 900°C, and FIG. 4(d) is an SEM photograph of Example 3 in which the ceramic laminate was fired at 1250°C. From the results of FIG. 4(b) and FIG. 4(d), the arithmetic mean roughness Ra and maximum height Rz of the internal electrode layers 12 in the lamination direction of the dielectric layers 11 and the internal electrode layers 12 were measured. At the point 102 where the internal electrode layer 12 is discontinued, the height of the internal electrode layer 12 in the lamination direction is defined as the maximum height Rz.
[0041] As shown in FIG. 5, the arithmetic mean roughness Ra and maximum height Rz were confirmed to be 28 [nm] and 357 [nm], respectively, in Example 1, 25 [nm] and 148 [nm], respectively, in Example 2, 22 [nm] and 134 [nm], respectively, in Example 4, 21 [nm] and 122 [nm], respectively, and in Example 5, 27 [nm] and 327 [nm], respectively. In addition, it was confirmed that the arithmetic mean roughness Ra and maximum height Rz were 37 [nm] and 612 [nm], respectively, in Comparative Example 1, 32 [nm] and 554 [nm], respectively, in Comparative Example 2, 32 [nm] and 542 [nm], respectively, in Comparative Example 4, 31 [nm] and 533 [nm], respectively, in Comparative Example 5, 36 [nm] and 587 [nm], respectively, in Comparative Example 6, 46 [nm] and 775 [nm], respectively, in Comparative Example 7, 42 [nm] and 712 [nm], respectively, in Comparative Example 8, 41 [nm] and 720 [nm], respectively, in Comparative Example 9, 41 [nm] and 713 [nm], respectively, and in Comparative Example 10, 43 [nm] and 743 [nm], respectively.
[0042] The reason why the arithmetic mean roughness Ra and maximum height Rz of the internal electrode layer 12 are better in Comparative Examples 1 to 5 than in Comparative Examples 6 to 10, and the arithmetic mean roughness Ra and maximum height Rz of the internal electrode layer 12 are better in Examples 1 to 5 than in Comparative Examples 1 to 5, is thought to be as follows.
[0043] For example, in Comparative Example 8, since the average particle diameter of the main component metal (Ni) is 120 nm, after the binder removal process, as shown in FIG. 6(a), the common material CM1 is likely to exist in the gaps between the particles P12 of the main component metal, and a part of the common material CM1 is aggregated. When the temperature reaches about 800°C in the firing process, as shown in FIG. 6(b), the common material CM1 diffuses from between the particles P12 of the main component metal to the dielectric layer 11 side, and the surface roughness of the internal electrode layer 12 deteriorates. In this case, during liquid phase diffusion at a temperature of 900°C to 1000°C, as shown in FIG. 6(c), the liquid phase 101 is likely to accumulate in the parts (gaps) of the internal electrode layer 12 with poor surface roughness. Then, when the temperature further rises to the maximum temperature (for example, 1250°C), it is considered that liquid phase aggregation further occurs, as shown in FIG. 6(d), and the surface roughness of the internal electrode layer 12 further deteriorates.
[0044] Also, for example, in Comparative Example 3, since the average particle diameter of the main component metal (Ni) is smaller (70 nm) than that of Comparative Example 8, as shown in FIG. 7(a), the voids are small, but the common material CM1 still exists in the voids and some of them aggregate. Then, when the temperature reaches about 800°C in the firing process, although the gaps between the particles P12 of the main component metal are small because the average particle diameter of the main component metal is small, the aggregated common material CM1 diffuses as shown in FIG. 7(b), and the surface roughness of the internal electrode layer 12 deteriorates. Then, during liquid phase diffusion at a temperature of 900°C to 1000°C, as shown in FIG. 7(c), the liquid phase 101 tends to accumulate in the parts (voids) of the internal electrode layer 12 with poor surface roughness. Then, when the firing temperature is further increased to the maximum temperature (for example, 1250°C), it is considered that liquid phase aggregation occurs further as shown in FIG. 7(d), and the surface roughness of the internal electrode layer 12 deteriorates further.
[0045] On the other hand, for example, in Example 3, a highly dispersed metal conductive paste is prepared by using small-diameter materials with sharp particle size distribution as the main component metal and the common material, so that the common material CM1 is uniformly present between the particles P12 of the main component metal as shown in FIG. 8(a). Since the common material CM1 is highly dispersed and small-diameter, it has a strong interaction with the main component metal, and even if the temperature reaches about 800°C in the firing process, the diffusion of the common material is suppressed as shown in FIG. 8(b), and the deterioration of the surface roughness of the internal electrode layer 12 is suppressed. Furthermore, at a temperature of 900°C to 1000°C, the liquid phase 101 is relatively uniformly aggregated inside the dielectric layer 11 and at the interface between the dielectric layer 11 and the internal electrode layer 12 as shown in FIG. 8(c). Therefore, it is considered that the internal electrode layer 12 can maintain its surface roughness even after the temperature reaches the maximum temperature as shown in FIG. 8(d).
[0046] The reason why the arithmetic mean roughness Ra and maximum height Rz of the internal electrode layer 12 are better in Examples 2 to 4 than in Examples 1 and 5 is considered as follows. If the amount of the common material added is less than 5 parts, the continuity rate of the internal electrode layer 12 decreases due to the insufficient amount of the common material, and the arithmetic mean roughness Ra and maximum height Rz deteriorate. On the other hand, if the amount of the common material added is more than 20 parts, the amount of the common material is too large, and the continuity rate of the internal electrode layer 12 decreases, and the arithmetic mean roughness Ra and maximum height Rz deteriorate.
[0047] Next, the capacitance, dielectric breakdown voltage (BDV), and high temperature accelerated life (HALT) of the multilayer ceramic capacitor 100 according to the examples and comparative examples were evaluated. FIG. 5 shows the evaluation results of the capacitance, dielectric breakdown voltage (BDV), and high temperature accelerated life (HALT). The BDV was measured by applying a DC voltage at a rate of 10V / sec. The HALT was measured at 125°C-10V.
[0048] 5, assuming that the capacity is 19 [μF] or more, the BDV is 38 [V] or more, and the HALT is 300 [min] or more as the pass criteria, it can be seen that all of Examples 1 to 5 meet the pass criteria, but Comparative Examples 1 to 10 do not meet the pass criteria. This is because, in Examples 1 to 5, the arithmetic mean roughness Ra of the internal electrode layer 12 is 30 nm or less and the maximum height Rz is 360 nm or less, while in Comparative Examples 1 to 10, the arithmetic mean roughness Ra of the internal electrode layer 12 is not 30 nm or less and the maximum height Rz is not 360 nm or less.
[0049] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0050] 10 Stacked Chip 11 Dielectric layer 12 Internal electrode layer 13 Cover Layer 20a,20b external electrode 100 Multilayer ceramic capacitors
Claims
1. The capacitor has a laminated structure in which dielectric layers mainly made of ceramic and internal electrode layers mainly made of metal are alternately laminated, In at least a portion of the internal electrode layer, the arithmetic mean roughness Ra of the internal electrode layer is 28 nm or less, In at least a portion of the internal electrode layer, the maximum height Rz of the internal electrode layer is 357 nm or less; The internal electrode layers contain ceramic particles having an average particle size of 15 nm or less and a standard deviation of particle size of 5 or less.
1. A multilayer ceramic capacitor comprising:
2. In at least a part of the internal electrode layer, the arithmetic mean roughness Ra of the internal electrode layer is 25 nm or less, In at least a portion of the internal electrode layer, the maximum height Rz of the internal electrode layer is 150 nm or less.
2. The multilayer ceramic capacitor according to claim 1.
3. 3. The multilayer ceramic capacitor according to claim 1, wherein the main component metal of the internal electrode layers is nickel.
4. 4. The multilayer ceramic capacitor according to claim 1, wherein the main component ceramic of the dielectric layers is barium titanate.
5. 5. The multilayer ceramic capacitor according to claim 1, wherein the internal electrode layers have a thickness of 0.5 μm or less.
6. The internal electrode layer includes ceramic particles having an average particle size of 10 nm or less and a standard deviation of particle size of 3 or less. The multilayer ceramic capacitor according to any one of claims 1 to 5.
7. The internal electrode layer includes ceramic particles having an average particle size of 8.6 nm or less and a standard deviation of particle size of 2.7 or less. The multilayer ceramic capacitor according to any one of claims 1 to 5.
Citation Information
Patent Citations
Conductive paste and its manufacturing method
JP2002245874A
Conductive paste, and dried film and laminated ceramic capacitor using conductive paste
JP2010087434A
Multilayer ceramic electronic component and manufacturing method therefor
JP2013058718A
Multilayer ceramic electronic component
JP2014007187A
Multilayer ceramic capacitor
JP2014057098A