Electricity storage device and method for manufacturing the same

By employing an annular roughened tab electrode terminal and thermoplastic insulating resin holder, the challenge of forming stable chemical conversion layers is overcome, achieving cost-effective and airtight power storage devices.

JP7576813B2Active Publication Date: 2024-11-01PRIME PLANET ENERGY & SOLUTIONS INC +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022147303
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-11-01
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

The challenge of forming a stable chemical conversion layer on a large number of tab electrode terminals in laminated power storage devices is difficult and costly, affecting the airtightness and overall cost of the devices.

Method used

The use of a tab electrode terminal with an annular roughened surface and a thermoplastic insulating resin tab holder, which is directly and airtightly thermally welded without a chemical conversion treatment layer, such as a chromate treatment, to enhance adhesion and airtightness.

Benefits of technology

This approach stabilizes the adhesion and airtightness of the tab electrode terminals, reducing costs and maintaining the integrity of the power storage device without the need for expensive chemical treatments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576813000001
    Figure 0007576813000001
  • Figure 0007576813000002
    Figure 0007576813000002
  • Figure 0007576813000003
    Figure 0007576813000003
Patent Text Reader

Abstract

To provide an inexpensive power storage device with excellent airtightness, and a manufacturing method for an inexpensive power storage device with excellent airtightness.SOLUTION: A power storage device 1 includes an electrode body, a pair of case members 21, a tab electrode terminal 30 electrically connected to a current collector part of the electrode body inside the pair of case members, extending between the case members, and exposed out of the case members, the tab electrode terminal 30 having an annular band shaped roughened surface that is roughened in a band shape along the entire periphery in a tab peripheral direction RH1 in the middle of a tab extension direction EH1, a tab holding body 50 that is thermally welded airtightly to the annular band shaped roughened surface directly, is also thermally welded airtightly to a tab peripheral part 21ETP of outer peripheral parts 21E and 22E of the case members that exists in the periphery of a tab electrode terminal, and causes the tab peripheral part to hold the tab electrode terminal. The tab holding body is formed by injecting and solidifying molten resin including a thermoplastic insulating resin in a tab peripheral gap between a surrounded part of the tab electrode terminal and the tab peripheral part of the case member.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electricity storage device and a method for manufacturing an electricity storage device. [Background technology]

[0002] In manufacturing an electricity storage device such as a secondary battery, a so-called laminate type electricity storage device is known in which an electrode body is housed in a pair of case members made of laminate films, the peripheral parts of the case members are heat-sealed together, and the positive electrode potential and the negative electrode potential of the electrode body are taken out from the joint part between the laminate films to the outside by a tab electrode terminal. In such a laminate type electricity storage device, in order to increase the adhesion between the heat-sealable resin layer forming the inner surface of the laminate film and the tab electrode terminal (metal terminal) made of metal, a tab adhesive film having a multilayer structure having a layer of metal-adhesive resin on its surface that has been made metal-adhesive by a modification treatment such as maleic acid modification is interposed between the laminate film and the tab electrode terminal, and the laminate film and the tab adhesive film and the tab adhesive film and the tab electrode terminal are hermetically heat-sealed (for example, see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2022-95833 A [Patent Document 2] JP 2007-95654 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, it is not easy to stably perform the treatment for forming a chemical conversion layer such as the above-mentioned chromate treatment layer on the surfaces of a large number of tab electrode terminals, and the cost tends to be high.

[0005] The present invention has been made in view of the above-mentioned current situation, and provides an inexpensive electricity storage device with good airtightness, and a method for manufacturing an inexpensive electricity storage device with good airtightness. [Means for solving the problem]

[0006] (1) One aspect of the present invention for solving the above problem includes an electrode body having a current collecting portion, a pair of case members made of a laminate film and surrounding the electrode body, a tab electrode terminal made of metal, a connection end portion conductively connected to the current collecting portion of the electrode body within the pair of case members, extending between the pair of case members, and an external terminal portion exposed to the outside of the pair of case members, the tab electrode terminal having, midway in a tab extension direction extending from the connection end portion toward the external terminal portion, an annular band-shaped roughened surface that is roughened in a band-shaped manner around the entire circumference in a tab circumferential direction surrounding the tab extension direction, and a tab electrode terminal made of a thermoplastic insulating resin, and a tab holder that covers an enclosed portion of the terminal, which is a band-shaped region that includes at least a portion of the annular roughened surface in the tab extension direction and extends around the entire circumference of the tab in the tab circumferential direction, and is hermetically heat-welded directly to the annular roughened surface and also to tab peripheral portions of the outer circumferential edge portions of each of the pair of case members that are positioned around the tab electrode terminal, and holds the tab electrode terminal in the tab peripheral portion. The tab holder is an electricity storage device formed by injecting molten resin made of the thermoplastic insulating resin into a tab peripheral gap between the enclosed portion of the tab electrode terminal and the tab peripheral portions of the pair of case members and solidifying it.

[0007] In this electricity storage device, a tab electrode terminal including an annular roughened surface is used in the surrounded portion, and the tab holder covers the surrounded portion and is directly and airtightly heat-welded to the annular roughened surface. In other words, since the tab electrode terminal is provided with a roughened annular surface, the tab holder made of a thermoplastic insulating resin can be stably heat-welded directly and airtightly to the tab electrode terminal by the roughened annular surface without providing a chemical conversion treatment layer such as a chromate treatment layer, and an inexpensive electricity storage device can be obtained. Moreover, since the tab holder is injected into the gap around the tab and solidified, an inexpensive electricity storage device can be obtained.

[0008] Examples of the "electricity storage device" include secondary batteries such as lithium ion secondary batteries, and capacitors such as lithium ion capacitors. In addition to electricity storage devices in which an electrode body is impregnated with an electrolyte, the term also includes electricity storage devices that do not require an electrolyte, such as solid electrolyte batteries. The "electrode body" may be a cylindrical or flat wound electrode body, or a laminated electrode body. In the wound electrode body, the current collector is provided on one side in the axial direction or on both sides. On the other hand, in the laminated electrode body, the current collector is provided in an appropriate direction among the directions perpendicular to the lamination direction.

[0009] The pair of "case members" is made of a laminate film. The pair of case members includes a so-called double-drawing type case member in which both case members are provided with a storage recess that stores and surrounds the electrode body, and a so-called single-drawing type case member in which only one case member is provided with a storage recess and the other case member is flat. The pair of case members may be independent case members, or may be a pair of integrated case members made of a single sheet or cylindrical laminate film, connected to each other via a connecting portion, and used by folding the connecting portion to face each other. The "laminate film" forming the case member is a film in which multiple resin films are laminated. In order to improve gas barrier properties and moisture resistance, a metal foil laminate film in which a metal foil such as aluminum foil or stainless steel foil is arranged as an inner layer can also be used. Among them, it is preferable to use aluminum foil from the viewpoints of cost, light weight, and ease of deformation.

[0010] The "tab electrode terminal" may be selected taking into consideration the material, potential, etc. of the current collector of the electrode body to be connected, and is made of a metal such as aluminum, copper, or nickel-plated copper, and has a connection end and an external terminal portion, and has an annular roughened surface in the middle of these. The tab electrode terminal may be in the form of a rectangular plate or the like that extends linearly from the connection end to the external terminal portion, but may also be bent or have a variable width dimension on the way from the connection end to the external terminal portion.

[0011] The "annular roughened surface" is a roughened surface to which a resin material made of a thermoplastic insulating resin can be stably and directly and airtightly heat-welded without providing a chemical conversion layer such as a chromate treatment layer. For example, a roughened surface having an arithmetic mean height Sa of 0.1 μm to 30 μm can be preferably used. With such a roughened surface, the strength and conductivity of the tab electrode terminal are not impaired, and the surface area of ​​the resin constituting the tab holder that is directly heat-welded can be preferably increased, so that the resin can be well fixed and airtight. The arithmetic mean height Sa of the roughened surface can be measured, for example, by observation with a laser microscope. For example, a VK-X1000 manufactured by Keyence Corporation can be used as the laser microscope.

[0012] The thermoplastic insulating resin constituting the "tab holder" may be a molten resin, and may be a resin capable of being directly and airtightly heat-welded to the annular roughened surface of the tab electrode terminal, and may or may not have metal adhesion. Examples of thermoplastic insulating resins having metal adhesion include metal-adhesive polyolefins such as metal-adhesive polyethylene (PE) and metal-adhesive polypropylene (PP) that have been given metal adhesion by modification such as acid modification such as maleic anhydride modification, or functional group introduction into the resin. On the other hand, examples of thermoplastic insulating resins that do not have metal adhesion include unmodified resins that are thermoplastic and insulating and have not been modified by acid modification or functional group introduction. Specific examples of such resins include unmodified polyolefins such as unmodified polyethylene (PE) and unmodified polypropylene (PP), unmodified polyesters such as unmodified polyethylene terephthalate (PET), unmodified polystyrene, and unmodified polyvinyl chloride (PVC).

[0013] The thermoplastic insulating resin to be melted and injected to form the tab holder preferably has a melting point of 120 to 200° C. By making the thermoplastic insulating resin to have a melting point of 120° C. or higher, the tab holder can be held in the tab peripheral portion of the case member while stably holding the tab electrode terminal without softening under normal use conditions of the electricity storage device. On the other hand, by making the thermoplastic insulating resin to have a melting point of 200° C. or lower, no high temperature is required when injecting the molten resin to form the tab holder, and the tab holder can be easily formed.

[0014] (2) In the electricity storage device according to (1), the tab holder may be made of an unmodified thermoplastic insulating resin.

[0015] In this electricity storage device, the thermoplastic insulating resin forming the tab holder is an unmodified thermoplastic insulating resin, and therefore, compared to a case in which a relatively expensive thermoplastic insulating resin having metal adhesion that has been modified with maleic acid or the like is used, it is possible to obtain an inexpensive electricity storage device having an inexpensive tab holder.

[0016] (3) The energy storage device according to (1) or (2) may further include a direct welding portion formed by directly and airtightly heat welding peripheral opposing portions of the outer peripheral edges of the pair of case members that face each other except around the tab.

[0017] In this energy storage device, as in the conventional case, the peripheral edge portions of a pair of case members made of laminate film that face each other except around the tab are directly and airtightly heat-welded to form a direct weld portion, so that the case can be easily formed.

[0018] (4) The energy storage device according to (1) or (2) may further include a resin interposition portion, in which peripheral opposing portions of the outer peripheral edges of the pair of case members that face each other except around the tab, are made of the thermoplastic insulating resin and hermetically heat-welded to the tab holder via a resin interposition body that is hermetically integrated with the tab holder.

[0019] In this power storage device, peripheral facing parts of the outer peripheries of the pair of case members that face each other except for the tab periphery are not directly heat-welded, but are hermetically heat-welded via the resin interposer. Therefore, compared to when the peripheral facing parts are directly heat-welded, the peripheral facing parts that face each other via the resin interposer can be reliably connected in an airtight manner. In addition, the resin interposer is also airtightly integrated with the tab holder, so that the space between the resin interposer and the tab holder can be reliably kept airtight.

[0020] (5) Another aspect includes a tab electrode terminal including an electrode body having a current collecting portion, a pair of case members made of a laminate film and surrounding the electrode body, the pair of case members having a connection end conductively connected to the current collecting portion of the electrode body within the pair of case members, extending between the pair of case members, and an external terminal portion exposed to the outside of the pair of case members, the tab electrode terminal having, midway in a tab extension direction extending from the connection end toward the external terminal portion, an annular roughened surface that is roughened in a band-like shape over the entire circumference in a tab circumferential direction surrounding the tab extension direction, and a tab surrounding portion made of a thermoplastic insulating resin, the tab electrode terminal including at least a part of the tab extension direction of the annular roughened surface, covering an enclosed portion that is a band-shaped region over the entire circumference in the tab circumferential direction, and being directly heat-welded in an airtight manner to the annular roughened surface, and the tab surrounding portion being a part of an outer circumferential edge portion of each of the pair of case members that is located around the tab electrode terminal. and a tab holder for holding the tab electrode terminal in the tab peripheral portion, the tab holder including: a connecting step of connecting the connection end of the tab electrode terminal to the current collecting portion of the electrode body; an accommodating step of accommodating the electrode body within the pair of case members in a posture in which the annular roughened surface of the tab electrode terminal overlaps with the tab peripheral portion of each of the pair of case members in a tab thickness direction of the tab electrode terminal, the tab electrode terminal extends in the tab extension direction through between the tab peripheral portions, and the tab electrode terminal is spaced from the tab peripheral portion of each of the pair of case members; and a holder forming step of injecting molten resin made of the thermoplastic insulating resin into the surrounded portion of the tab electrode terminal and into a tab peripheral gap of the tab peripheral portions of the pair of case members and solidifying it, thereby forming the tab holder.

[0021] In this method for manufacturing an electricity storage device, in the holder formation step, a molten resin is injected into the tab peripheral gap between the surrounded portion of the tab electrode terminal and the tab peripheral portions of the pair of case members and solidified to form a tab holder. Therefore, even if the tab electrode terminal does not have a chemical conversion treatment layer such as a chromate treatment layer, the tab holder can be stably and directly hermetically heat-welded to the annular roughened surface in the surrounded portion of the tab electrode terminal and also hermetically heat-welded to the tab peripheral portions of the case members, thereby manufacturing an inexpensive electricity storage device. In addition, since the tab holder is made of an injected and solidified thermoplastic insulating resin, there is no need to use the tab adhesive film with the multilayer structure described above, and an electricity storage device can be manufactured inexpensively.

[0022] (6) A method for manufacturing an electric storage device as set forth in (5), wherein the electric storage device further comprises a direct welded portion formed by directly and airtightly heat-welding peripheral opposing portions of the outer circumferential edges of the pair of case members that face each other except around the tab, and the method for manufacturing an electric storage device may further include a peripheral heat-welding process for directly and airtightly heat-welding the peripheral opposing portions of the outer circumferential edges of the pair of case members to form the direct welded portion after the accommodation process and prior to the holder formation process.

[0023] In this manufacturing method, in a peripheral heat welding process that follows the accommodation process and precedes the holder forming process, peripheral facing portions of the outer peripheries of the pair of case members are heat welded to each other to form a direct weld portion. As a result, before the holder forming process, the peripheral facing portions of the outer peripheries of the pair of case members are directly welded to each other and fixed to each other, so that the remaining tab peripheral portions of the outer peripheries are also generally fixed. Therefore, when molten resin is injected into the tab peripheral gap in the holder forming process, it is possible to easily inject the molten resin by suppressing the occurrence of misalignment or deformation of the tab peripheral portion.

[0024] In addition, when the peripheral facing parts are airtightly heat-welded to form a direct welded part, this includes a case where the peripheral facing parts are airtightly heat-welded over the entire area, as well as a case where a predetermined part of the peripheral facing parts other than the tab periphery is left unwelded in order to perform a process of injecting an electrolyte into a case formed by a pair of case members after the peripheral facing parts are heat-welded. In this case, the remaining unwelded parts of the peripheral facing parts are heat-welded after the electrolyte is injected.

[0025] In a manufacturing method for an electric storage device according to (7) or (5), the electric storage device may further include a resin interposition portion formed by hermetically heat-welding peripheral opposing portions of the outer peripheral edges of the pair of case members that face each other except around the tab, the peripheral opposing portions being made of the thermoplastic insulating resin and hermetically integrated with the tab holder, and the holder forming step may be a holder interposition forming step of injecting molten thermoplastic insulating resin into a gap between the peripheral opposing portions that are held with a predetermined opposing gap between them, in parallel with or before or after the formation of the tab holder, to form the resin interposition that is interposed between the peripheral opposing portions and that is also hermetically heat-welded to each of the peripheral opposing portions.

[0026] In this manufacturing method, in the holder interposition forming step, molten resin is injected not only into the gaps around the tabs but also into the gaps between the opposing peripheral portions held by the opposing portion gap to form resin interpositions that are interposed between the opposing peripheral portions and are hermetically heat-welded to the opposing peripheral portions and are hermetically integrated with the tab holder, thereby making it easy to form an electricity storage device having a tab holder and a resin interposition.

[0027] In the holder intermediate forming step, when forming the tab holder and the resin intermediate body airtightly integrated therewith, the tab holding portion and the resin intermediate body may be formed in parallel at the same time, or the tab holding portion may be formed first and then the resin intermediate body may be formed while being airtightly integrated with the tab holder. Conversely, the resin intermediate body may be formed first and then the tab holding portion may be formed while being airtightly integrated with the resin intermediate body. The holder intermediate formation step includes a case where a resin intermediate is formed over the entire gap between the opposing peripheral portions, as well as a case where a resin intermediate is not formed in a predetermined portion of the gap between the opposing peripheral portions in order to enable a subsequent step of injecting an electrolyte into a case formed by a pair of case members, a tab holder, and a holding member. In this case, after the injection of the electrolyte is completed, resin is injected into the predetermined portion to seal it. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a perspective view showing the appearance of a battery according to a first embodiment. [Diagram 2] FIG. 2 is a vertical cross-sectional view of the battery according to the first and second embodiments. [Diagram 3] 2 is a cross-sectional view taken along the line AA' in FIG. 1, illustrating the structure of an extracted portion of a tab electrode terminal in the battery according to Embodiment 1. FIG. [Figure 4] FIG. 11 is a perspective view of a roughened tab electrode terminal in the first and second embodiments. [Diagram 5] 4 is a flowchart showing a procedure for manufacturing the tab electrode terminal and the battery in the first and second embodiments. [Figure 6] FIG. 4 is a plan view of an electrode body to which a tab electrode terminal is connected in the first and second embodiments. [Figure 7] FIG. 11 is an explanatory diagram illustrating a state in which the electrode body is housed in a pair of case members in the first and second embodiments. [Figure 8] 10A and 10B are explanatory views illustrating a state in which a resin is injected into the tab peripheral portion to form a tab holder in the first and second embodiments. [Figure 9] 5A to 5C are explanatory views showing a procedure for injecting a resin into the periphery of the tab when forming the tab holder in the first embodiment. [Figure 10] FIG. 11 is a perspective view showing the appearance of a battery according to a second embodiment. [Figure 11] 11 is a cross-sectional view taken along the line BB' in FIG. 10, illustrating the structure of an extracted portion of a tab electrode terminal in the battery according to Embodiment 2. FIG. [Figure 12]13A and 13B are explanatory views illustrating a procedure for injecting resin into the tab surrounding portion and the peripheral edge opposing portion when forming the tab holder and the resin interposing body according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Preferred embodiments of the disclosed technology will be described below with reference to the drawings as appropriate. Matters other than those specifically mentioned in this specification that are necessary for implementation can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the relevant field. In addition, in the following drawings, components and parts that perform the same function are given the same reference numerals, and duplicated explanations may be omitted or simplified.

[0030] (Embodiment 1) Hereinafter, a first embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a perspective view showing the appearance of a battery (electricity storage device) 1 according to this embodiment, and Fig. 2 is a vertical cross-sectional view of the battery 1. This battery 1 is a so-called laminated lithium ion secondary battery that is mounted in vehicles such as hybrid cars, plug-in hybrid cars, and electric cars, drones, and various devices.

[0031] This battery 1 comprises a case 20, an electrode assembly 10 contained and surrounded within a container 20S of the case 20, a tab positive electrode terminal 30 connected to the positive electrode current collecting portion 12 of the electrode assembly 10 and extending to the outside through a positive electrode peripheral portion 20P of the case 20, a tab negative electrode terminal 40 connected to the negative electrode current collecting portion 13 and extending to the outside through a negative electrode peripheral portion 20N of the case 20, and tab holders 50, 60 interposed between the positive electrode peripheral portion 20P and the tab positive electrode terminal 30 or between the negative electrode peripheral portion 20N and the tab negative electrode terminal 40.

[0032] Of these, the case 20 is formed by thermally welding together the outer peripheral edge portions 21E, 22E of a pair of case members 21, 22 made of laminate film (see Figs. 1, 2, and 7). Specifically, each of the case members 21, 22 is made of a metal foil laminate film in which a resin layer is laminated on the inside and outside of an aluminum foil, and rectangular recessed accommodation recesses 21S, 22S constituting the accommodation portion 20S for accommodating the electrode body 10 are provided in the central portion in the planar direction surrounded by the outer peripheral edge portions 21E, 22E by a press process performed in advance. In addition, in the outer peripheral edge portions 21E, 22E surrounding the periphery of the accommodating recesses 21S, 22S, the positive electrode tab peripheral portions 21ETP, 22ETP constituting the positive electrode peripheral portion 20P and the negative electrode tab peripheral portions 21ETN, 22ETN constituting the negative electrode peripheral portion 20N are provided in the form of grooves extending outward from the accommodating recesses 21S, 22S (left-right direction in Figs. 1, 2, and 7). Of the multilayered metal foil laminate film constituting the case members 21, 22, the opposing layers 21IL, 22IL opposed to each other are made of unmodified polypropylene that has insulating properties, a relatively low melting point (melting point is 120 to 200°C, 160°C in this embodiment) that can be heat-welded to each other, and does not have metal adhesiveness. For this reason, the peripheral opposing portions 21EM, 22EM of the outer peripheral edge portions 21E, 22E of the case members 21, 22 can be directly, airtightly and easily heat-welded to each other by melting and heat-welding their opposing layers 21IL, 22IL to form a direct weld portion 20DM.

[0033] However, since the opposing layers 21IL, 22IL are made of polypropylene which does not have the aforementioned metal adhesiveness, it is difficult to hermetically join the case members 21, 22 (specifically, the positive electrode tab peripheral portions 21ETP, 22ETP and the negative electrode tab peripheral portions 21ETN, 22ETN) to an unprocessed metal plate (specifically, one that does not have a roughened surface 33, etc.) via the opposing layers 21IL, 22IL by only heat welding.

[0034] The electrode body 10 can be an electrode body in a known battery, and is not particularly limited. In this embodiment, the electrode body 10 (see Figs. 2 and 7) is a so-called laminated type electrode body having an electrode body main body part 11 in which a large number of rectangular plate-shaped positive electrode plates 15 and negative electrode plates 16 are alternately laminated with separators 17 between, a positive electrode current collector part 12 in which the positive electrode foil lead part 15L of the positive electrode plate 15 is overlapped, and a negative electrode current collector part 13 in which the negative electrode foil lead part 16L of the negative electrode plate 16 is overlapped. The case 20 that houses the electrode body 10 contains an electrolyte 19 impregnated in the electrode body 10. Note that, as the electrode body 10, a so-called wound type electrode body in which a strip-shaped positive electrode plate and a strip-shaped negative electrode plate are wound with a strip-shaped separator between them may be used, and further, a flat wound type electrode body may be used. In addition, a solid electrolyte type electrode body using a solid electrolyte instead of the electrolyte 19 may be used.

[0035] The tab positive electrode terminal 30 (see FIG. 4) is a rectangular plate made of aluminum. The tab positive electrode terminal 30 has a positive electrode connection end 31 located on one side (upper right side in FIG. 4) and a positive electrode external terminal portion 32 located on the other side (lower left side in FIG. 4). In addition, in the middle of the positive electrode extension direction EH1 (lower left direction in FIG. 4) from the positive electrode connection end 31 toward the positive electrode external terminal portion 32, there is a roughened surface (annular band-shaped roughened surface) 33 (shown by a thick line in FIG. 2 and FIG. 7) that is roughened in a ring shape around the entire circumference in the positive electrode circumferential direction RH1 surrounding the positive electrode extension direction EH1, specifically, in a ring shape around four faces connected to the positive electrode circumferential direction RH1.

[0036] The roughened surface 33 has unevenness formed by the roughening treatment, and the surface roughness is higher than that of the other untreated portions (positive electrode connection end 31, positive electrode external terminal portion 32). Therefore, the roughened surface 33 can be directly and airtightly heat-welded to the tab holder 50 by contacting not only a metal adhesive resin but also a molten resin MR made of an unmodified thermoplastic insulating resin (specifically, unmodified polypropylene in the present embodiment 1) that does not have metal adhesiveness. The arithmetic mean height Sa of the roughened surface 33 is not particularly limited, but is preferably 0.1 μm or more and 30 μm or less. Within this range, the surface area to which the tab holder 50 is heat-welded can be suitably increased without impairing the strength and conductivity of the tab positive terminal 30, and the molten resin MR that becomes the tab holder 50 can be heat-welded to the roughened surface 33 firmly and airtightly. In the present embodiment, specifically, the arithmetic mean height Sa is about 1.0 μm.

[0037] The positive electrode connection end 31 of the tab positive electrode terminal 30 is connected by ultrasonic welding to the positive electrode current collector 12 of the electrode body 10, on which a large number of positive electrode foil lead portions 15L made of aluminum foil overlap. The positive electrode external terminal portion 32 is exposed to the outside (the outside on the right side in Figs. 1 and 2) of the case 20 (case members 21, 22). A part of the annular roughened surface 33 in the positive electrode extension direction EH1 shown by a dashed line in Fig. 4 forms an annular surrounded portion 34. This surrounded portion 34 is an area to which the tab holder 50 is directly and airtightly heat-welded in a band-like shape over the entire circumference of the positive electrode circumferential direction RH1 so as to surround the surrounded portion 34, as described later (see Fig. 2).

[0038] In this embodiment, as described above, a narrow band-shaped region including only a part of the width direction (corresponding to the positive electrode extending direction EH1) of the band-shaped roughened surface 33 is set as the surrounded portion 34, and a band-shaped tab holder 50 narrower than the band-shaped roughened surface 33 is heat-welded to cover the surrounded portion 34. However, a wide band-shaped region including the entire width direction of the band-shaped roughened surface 33 may be set as the surrounded portion 34, and a band-shaped tab holder 50 wider than the band-shaped roughened surface 33 may be formed on the surrounded portion 34. In addition, the band-shaped surrounded portion 34 may be set so that a part of the surrounded portion 34 includes a part of the width direction of the band-shaped roughened surface 33, and the band-shaped tab holder 50 may be formed on the surrounded portion 34. The relationship between the surrounded portion 44 of the tab negative electrode terminal 40 and the tab holder 60 described later can be the same.

[0039] As described below, the resin that constitutes the tab holder 50 is also hermetically heat-welded to the positive electrode peripheral portion 20P of the case 20 (the positive electrode tab peripheral portions 21ETP, 22ETP of the case members 21, 22), so that the tab positive terminal 30 is hermetically held to the positive electrode peripheral portion 20P of the case 20 via the tab holder 50.

[0040] On the other hand, the tab negative electrode terminal 40 (see FIG. 4) is a rectangular plate made of nickel-plated copper. This tab negative electrode terminal 40 has a negative electrode connection end 41 located on one side (upper right side in FIG. 4) and a negative electrode external terminal portion 42 located on the other side (lower left side in FIG. 4) like the above-mentioned tab positive electrode terminal 30. In addition, in the middle of the negative electrode extension direction EH2 (lower left direction in FIG. 4) from the negative electrode connection end 41 toward the negative electrode external terminal portion 42, there is a roughened surface (annular band-shaped roughened surface) 43 (shown by a thick line in FIG. 2 and FIG. 7) that is roughened in a ring shape around the entire circumference in the negative electrode circumferential direction RH2 surrounding the negative electrode extension direction EH2, specifically, in a ring shape around four faces connected to the negative electrode circumferential direction RH2.

[0041] Like the roughened surface 33 described above, the roughened surface 43 is roughened to form irregularities, and the surface roughness is higher than that of the other untreated portions (negative electrode connection end 41, negative electrode external terminal portion 42). Therefore, the tab holder 60 can be directly and airtightly heat-welded to the roughened surface 43 by contacting not only the metal adhesive resin but also the molten resin MR made of unmodified polypropylene that does not have metal adhesiveness. The arithmetic mean height Sa of the roughened surface 43 is not particularly limited, but is preferably 0.1 μm or more and 30 μm or less. Within this range, the surface area to which the tab holder 60 is heat-welded can be suitably increased without impairing the strength or conductivity of the tab negative electrode terminal 40, and the tab holder 60 can be heat-welded to the roughened surface 43 firmly and airtightly. In this embodiment, the arithmetic mean height Sa is specifically set to about 1.0 μm.

[0042] The negative electrode connection end 41 of the tab negative electrode terminal 40 is connected by ultrasonic welding to the negative electrode current collecting portion 13 of the electrode body 10, on which a large number of negative electrode foil lead portions 16L made of copper foil overlap. The negative electrode external terminal portion 42 is exposed to the outside (the outside on the left side in Figs. 1 and 2) of the case 20 (case members 21, 22). A band-shaped tab holder 60 is directly and airtightly heat-welded to a ring-shaped surrounded portion 44 of the ring-shaped roughened surface 43, which constitutes a part of the negative electrode extending direction EH2 shown by a dashed line in Fig. 4, over the entire circumference in the negative electrode circumferential direction RH2 so as to surround the ring-shaped surrounded portion 44 (see Fig. 2).

[0043] Furthermore, as described below, the resin that constitutes this tab retainer 60 is also hermetically heat-welded to the negative electrode surrounding portion 20N of the case 20 (negative electrode tab surrounding portions 21ETN, 22ETN of case members 21, 22), so that the tab negative electrode terminal 40 is airtightly held to the negative electrode surrounding portion 20N of the case 20 via the tab retainer 60.

[0044] Unlike the tab adhesive film described above, which has a multi-layer structure and metal adhesiveness, the tab holders 50 and 60 are made of a single resin material and are made of unmodified polypropylene that is heat-sealable and insulating but does not have metal adhesiveness. The melting point of the polypropylene used for the tab holders 50 and 60 is preferably 120 to 160°C. The melting point of the polypropylene used for the facing layers 21IL and 22IL of the laminate film that constitutes the case members 21 and 22 described above and the melting point of the polypropylene used for the tab holders 50 and 60 should be approximately the same, and in this embodiment, polypropylene with a melting point of 160°C is used.

[0045] As described later, the tab holders 50, 60 are formed by injecting molten resin MR between the surrounded portions 34, 44 of the tab positive terminal 30 and the tab negative terminal 40 and the positive electrode tab peripheral portions 21ETP, 22ETP or the negative electrode tab peripheral portions 21ETN, 22ETN of the case members 21, 22.

[0046] In the battery 1 of the present embodiment 1, even if a chemical conversion treatment layer such as a chromate treatment layer is not provided on the tab positive terminal 30 and the tab negative terminal 40, the tab holders 50, 60 made of a thermoplastic insulating resin can be stably and directly and airtightly heat-welded to the tab positive terminal 30 or the tab negative terminal 40 via the roughened surfaces 33, 43, resulting in an inexpensive battery 1. Moreover, since the tab holders 50, 60 are formed by injecting and solidifying molten resin MR, the battery 1 is inexpensive. Moreover, since the tab holders 50, 60 of the battery 1 of the present embodiment 1 are made of inexpensive unmodified polypropylene, the battery 1 is even more inexpensive.

[0047] In this battery 1, the melting point of the polypropylene constituting the tab holders 50, 60 is set to 160°C, which is higher than 120°C, so that when the battery 1 is in use, the tab positive terminal 30 and the tab negative terminal 40 can be stably held without softening and can be held by the positive electrode tab peripheral portions 21ETP, 22ETP and the negative electrode tab peripheral portions 21ETN, 22ETN of the case members 21, 22, respectively. Meanwhile, since the melting point of polypropylene is set to 160°C or lower, no high temperature is required when injecting molten resin MR to form the tab holders 50, 60, and the tab holders 50, 60 can be easily formed.

[0048] In addition, in this battery 1, as in the conventional battery, the peripheral opposing portions 21EM, 22EM of the pair of case members 21, 22 made of laminate film, which face each other except for the positive electrode tab peripheral portions 21ETP, 22ETP and the negative electrode tab peripheral portions 21ETN, 22ETN, are directly and airtightly heat-welded to form the direct weld portion 20DM, so that the case 20 can be easily formed.

[0049] In the battery 1 of the first embodiment, as shown in Fig. 1 and Fig. 2, the tab holder 50 surrounds the surrounded portion 34 of the tab positive terminal 30 and has a sandwiched portion 51 sandwiched between the positive tab peripheral portions 21ETP, 22ETP of the case members 21, 22. In addition, in the present embodiment, the tab holder 50 has an extended surrounding portion 52 that is formed in the positive extension direction EH1 (right side in Fig. 1 and Fig. 2) wider than the sandwiched portion 51, i.e., wider than the positive tab peripheral portion edges 21ETPE, 22ETPE of the positive tab peripheral portions 21ETP, 22ETP in the positive extension direction EH1, and covers the tab positive terminal 30 in a band-like shape over the entire circumference in the positive circumferential direction RH1. As a result, the creeping distance SL1 from the positive tab peripheral portion edges 21ETPE, 22ETPE to the tab positive terminal 30 is extended as shown by the dashed line in Fig. 1.

[0050] Similarly, the tab holder 60 surrounds the surrounded portion 44 of the tab negative electrode terminal 40 and has a sandwiched portion 61 that is sandwiched between the negative electrode tab peripheral portions 21ETN, 22ETN of the case members 21, 22. In addition, the tab holder 60 has an extended surrounding portion 62 that is formed in the negative electrode extending direction EH2 (left side in Figs. 1 and 2) wider than the sandwiched portion 61, i.e., wider than the negative electrode tab peripheral portion edges 21ETNE, 22ETNE of the negative electrode tab peripheral portions 21ETN, 22ETN in the negative electrode extending direction EH2, and covers the tab negative electrode terminal 40 in a band-like shape over the entire circumference in the negative electrode circumferential direction RH2. As a result, the creeping distance SL2 from the negative electrode tab peripheral portion edges 21ETNE, 22ETNE to the tab negative electrode terminal 40 is extended as shown by the dashed line in Fig. 1.

[0051] As described above, the case members 21 and 22 are made of a metal foil laminate film containing aluminum foil. Therefore, when the laminate film is cut during the manufacture of the case members 21 and 22, burrs of the aluminum foil may occur at the edges of the outer peripheral edges 21E and 22E of the case members 21 and 22. In particular, if burrs are generated at the positive electrode tab peripheral edge 21ETPE and 22ETPE of the positive electrode tab peripheral portion 21ETP and 22ETP or the negative electrode tab peripheral edge 21ETNE and 22ETNE of the negative electrode tab peripheral portion 21ETN and 22ETN, the burrs may come into contact with the tab positive electrode terminal 30 or the tab negative electrode terminal 40, and the aluminum foil may be electrically connected to the tab positive electrode terminal 30 or the tab negative electrode terminal 40. In this case, if the edges of the outer peripheral portions 21E, 22E of the case members 21, 22 come into contact with another member not shown, there is a risk that the other member will become electrically connected to the tab positive terminal 30 or the tab negative terminal 40 via the aluminum foil and burrs.

[0052] In contrast, in the battery 1 of this embodiment 1, the tab holders 50, 60 have extended surrounding portions 52, 62, so that even if burrs occur on the positive electrode tab peripheral edge 21ETPE, 22ETPE or the negative electrode tab peripheral edge 21ETNE, 22ETNE, it is possible to prevent the burrs from coming into contact with the tab positive electrode terminal 30 or the tab negative electrode terminal 40, and thus prevent the aluminum foil from becoming conductive with the tab positive electrode terminal 30 or the tab negative electrode terminal 40. It is advisable to ensure the creepage distances SL1, SL2 of the extending surrounding portions 52, 62 to be, for example, 2 to 10 mm, and in this embodiment, for example, the creepage distances SL1=SL2=5 mm.

[0053] The sandwiched portion 51 of the tab holder 50 is formed so as to surround the entire circumference of the surrounded portion 34 of the tab positive terminal 30, and has two flat plate portions 51P1, 51P2 formed on the two main surfaces 34P1, 34P2, and two side portions 51S1, 51S2 formed on the outer side WHO1 in the positive electrode width direction WH1 of the two side surfaces 34S1, 34S2. Similarly, the sandwiched portion 61 of the tab holder 60 is also formed so as to surround the entire circumference of the surrounded portion 44, and has two flat plate portions 61P1, 61P2 formed on the two main surfaces 44P1, 44P2, and two side portions 61S1, 61S2 formed on the outer side WHO2 in the negative electrode width direction WH2 of the two side surfaces 44S1, 44S2 (see FIGS. 1 to 3). The positive electrode width direction WH1 is a direction perpendicular to the positive electrode extension direction EH1 and the positive electrode thickness direction TH1, and the negative electrode width direction WH2 is a direction perpendicular to the negative electrode extension direction EH2 and the negative electrode thickness direction TH2.

[0054] In addition, the two flat plate portions 51P1, 51P2 of the sandwiched portion 51 of the tab holder 50 are also hermetically heat-welded to the flat portions 21ETPP, 22ETPP of the groove-shaped positive electrode tab peripheral portions 21ETP, 22ETP formed in advance in the case members 21, 22. The two side portions 51S1, 51S2 are also hermetically heat-welded to the two pairs of inclined surface portions 21ETPS, 22ETPS of the positive electrode tab peripheral portions 21ETP, 22ETP. Similarly, the two flat plate portions 61P1, 61P2 of the sandwiched portion 61 of the tab holder 60 are also hermetically heat-welded to the flat portions 21ETNP, 22ETNP of the groove-shaped negative electrode tab peripheral portions 21ETN, 22ETN of the case members 21, 22. The two side portions 61S1, 61S2 are also hermetically heat-welded to the two pairs of inclined surface portions 21ETNS, 22ETNS of the negative electrode tab surrounding portions 21ETN, 22ETN, respectively.

[0055] In the first embodiment, the positive electrode tab surrounding parts 21ETP, 22ETP of the case members 21, 22 are provided with the inclined parts 21ETPS, 22ETPS extending at an inclination of 30 to 70 degrees (approximately 45 degrees in the first embodiment) at both ends of the outer WHO1 in the positive electrode width direction WH1. Therefore, the side parts 51S1, 51S2 of the sandwiched part 51 have a tapered shape toward the outer WHO1, specifically, a triangular prism shape narrowing toward the outer WHO1 (see FIG. 3). By providing the above-mentioned inclined parts 21ETPS, 22ETPS, when the molten resin MR is injected to form the tab holder 50 as described later, the molten resin MR is easily injected toward the outer WHO1 along the inclined parts 21ETPS, 22ETPS, and the side parts 50S1, 50S2 airtightly heat-welded to the inclined parts 21ETPS, 22ETPS are easily formed.

[0056] Similarly, in the negative electrode tab surrounding parts 21ETN, 22ETN of the case members 21, 22, both ends of the outer WHO2 in the negative electrode width direction WH2 are provided with inclined parts 21ETNS, 22ETNS extending at an inclination of about 45 degrees within a range of 30 to 70 degrees. Therefore, the side parts 61S1, 61S2 of the sandwiched part 61 also have a triangular prism shape tapered toward the outer WHO2 and narrowing toward the outer WHO1. By providing these inclined parts 21ETNS, 22ETNS, when the molten resin MR is injected to form the tab holder 60 as described later, the molten resin MR is easily injected toward the outer WHO2 along the inclined parts 21ETNS, 22ETNS, and the side parts 60S1, 60S2 airtightly heat-welded to the inclined parts 21ETNS, 22ETNS are easily formed.

[0057] Next, the roughened tab positive electrode terminal 30 and tab negative electrode terminal 40 used in the manufacture of the battery 1 of the present embodiment 1, and the manufacturing method of the battery 1 will be described with reference to Figs. 4 to 9. First, an unroughened tab positive electrode terminal 30BR is prepared, and in a roughening step S1, a known roughening treatment is applied to the surface of a middle portion in the positive electrode extending direction EH1 to form a roughened surface 33 over the entire circumference in the positive electrode circumferential direction RH1 (see Fig. 4). Similarly, an unroughened tab negative electrode terminal 40BR is prepared, and a roughened surface 43 is formed by the roughening step S1. The arithmetic mean height Sa of the roughened surfaces 33, 43 is set to a range of 0.1 to 30 µm, specifically 0.1 µm. As the roughening method, known methods such as laser irradiation, etching, plating (e.g., roughened nickel plating, roughened copper plating, roughened silver plating, etc.), frame treatment, corona treatment, plasma treatment, surface polishing, etc. can be used. In this embodiment, a laser irradiation process similar to that described in JP 2022-28587 A was performed.

[0058] In addition to the above-mentioned tab positive electrode terminal 30 and tab negative electrode terminal 40 (see FIG. 4), an electrode body 10 manufactured by a known method and a pair of case members 21, 22 are prepared (see FIGS. 6 and 7). Then, in a connection step S11, the positive electrode connection end 31 of the tab positive electrode terminal 30 is connected to the positive electrode current collecting part 12 of the electrode body 10 by ultrasonic welding. Similarly, the negative electrode connection end 41 of the tab negative electrode terminal 40 is connected to the negative electrode current collecting part 13 of the electrode body 10 by ultrasonic welding.

[0059] In the subsequent accommodating step S12, the electrode body 10 is accommodated in a pair of case members 21, 22. Specifically, the electrode body main body 11 of the electrode body 10 is positioned between the accommodating recesses 21S, 22S provided in the case members 21, 22, and the peripheral opposing portions 21EM, 22EM of the case members 21, 22 are brought close to each other. At the same time, the electrode body 10 is accommodated in the case members 21, 22 so that the roughened surface 33 of the tab positive terminal 30 overlaps with the positive electrode tab peripheral portions 21ETP, 22ETP of each of the case members 21, 22 in the positive electrode thickness direction TH1 (up and down direction in Figures 7 and 8) of the tab positive terminal 30, the tab positive terminal 30 extends in the positive electrode extension direction EH1 (rightward in Figures 7 and 8) between the positive electrode tab peripheral portions 21ETP, 22ETP, and the tab positive terminal 30 is positioned away from the positive electrode tab peripheral portions 21ETP, 22ETP. In addition, the electrode body 10 is accommodated in the case members 21, 22 such that the roughened surface 43 of the tab negative electrode terminal 40 overlaps with the negative electrode tab peripheral portions 21ETN, 22ETN of each of the case members 21, 22 in the negative electrode thickness direction TH2 (up and down direction in Figures 7 and 8) of the tab negative electrode terminal 40, the tab negative electrode terminal 40 extends in the negative electrode extension direction EH2 (leftward in Figures 7 and 8) between the negative electrode tab peripheral portions 21ETN, 22ETNN, and the tab negative electrode terminal 40 is positioned away from the negative electrode tab peripheral portions 21ETN, 22ETN.

[0060] Furthermore, in the peripheral heat welding process S13, peripheral opposing portions 21EM, 22EM, which are portions of the outer peripheral portions 21E, 22E of the pair of case members 21, 22 other than the positive electrode tab peripheral portions 21ETP, 22ETP and the negative electrode tab peripheral portions 21ETN, 22ETN, are directly and airtightly heat-welded to each other by a known heat sealing method to form a direct weld portion 20DM (see FIGS. 1 and 3). As a result, the electrode body 10 is accommodated in the accommodation portion 20S of the case 20 consisting of the pair of case members 21, 22. On the other hand, the positive electrode tab peripheral portions 21ETP, 22ETP and the tab positive electrode terminal 30, and the negative electrode tab peripheral portions 21ETN, 22ETN and the tab negative electrode terminal 40 are spaced apart from each other with a tab peripheral gap ST formed therebetween.

[0061] Thereafter, proceeding to the holder formation process S14, molten resin MR obtained by heating and melting unmodified polypropylene is injected into the tab surrounding gaps ST between the positive electrode tab surrounding portions 21ETP, 22ETP and the surrounded portion 34 of the tab positive electrode terminal 30, and between the negative electrode tab surrounding portions 21ETN, 22ETN and the surrounded portion 44 of the tab negative electrode terminal 40, and solidified to form the tab holders 50, 60 described above.

[0062] In this embodiment 1, the molten resin MR is generated by heating and pressurized to be pumped, and the molten resin MR is injected into the tab surrounding gap ST using four resin injection devices J1a, J1b, J2a, and J2b that eject the molten resin MR from the tips of ejection nozzles J1aZ, J1bZ, J2aZ, and J2bZ (see Figures 8 and 9).

[0063] Specifically, as shown in Fig. 8, the molten resin MR is discharged from the tips of the discharge nozzles J1aZ, J1bZ inserted into the tab surrounding gap ST, and the molten resin MR is injected and filled into the tab surrounding gap ST between the positive electrode tab surrounding parts 21ETP, 22ETP and the tab positive electrode terminal 30, to form the clamped part 51 of the tab holder 50 airtight between the positive electrode tab surrounding parts 21ETP, 22ETP and the surrounded part 34 including the roughened surface 33 of the tab positive electrode terminal 30. The molten resin MR is also discharged so as to extend in the positive electrode extension direction EH1 (rightward in Fig. 8) beyond the positive electrode tab surrounding parts 21ETP, 22ETP on the tab positive electrode terminal 30, to form the extended surrounded part 52 of the tab holder 50. In this way, the tab holder 50 is formed on the surrounded part 34 of the tab positive electrode terminal 30.

[0064] Similarly, for the negative electrode, the molten resin MR is discharged from the tips of the discharge nozzles J2aZ, J2bZ inserted into the tab surrounding gap ST, while the molten resin MR is injected and filled into the tab surrounding gap ST between the negative electrode tab surrounding parts 21ETN, 22ETN and the tab negative electrode terminal 40, and the clamped part 61 of the tab holder 60 is airtightly formed between the negative electrode tab surrounding parts 21ETN, 22ETN and the surrounded part 44 including the roughened surface 43 of the tab negative electrode terminal 40. The molten resin MR is also discharged so as to extend in the negative electrode extending direction EH2 (leftward in FIG. 8) beyond the negative electrode tab surrounding parts 21ETN, 22ETN on the tab negative electrode terminal 40, and the extended surrounded part 62 of the tab holder 60 is formed. In this way, the tab holder 60 is formed on the surrounded part 44 of the tab negative electrode terminal 40.

[0065] In the peripheral heat welding step S13 of the first embodiment, parts (not shown) of the peripheral opposing portions 21EM, 22EM are not heat-welded to each other in order to later inject electrolyte 19 into the storage portion 20S of the case 20. Then, after the holder formation step S14, electrolyte 19 is injected from this unwelded portion, and then the unwelded portion is heat-welded to seal it, and other known steps are performed to manufacture the battery 1.

[0066] In the manufacturing method of the battery 1, in the holder formation step, molten resin MR is injected into the tab peripheral gap ST between the surrounded portion 34, 44 of the tab positive terminal 30 or the tab negative terminal 40 and the positive electrode tab peripheral portion 21ETP, 22ETP or the negative electrode tab peripheral portion 21ETN, 22ETN of the pair of case members 21, 22, and solidified to form the tab holder 50, 60. Therefore, even if the tab positive terminal 30 or the tab negative terminal 40 does not have a chemical conversion treatment layer such as a chromate treatment layer, the tab holder 50, 60 can be stably and directly hermetically heat-welded to the roughened surface 33, 43 in the surrounded portion 34, 44, and can also be hermetically heat-welded to the positive electrode tab peripheral portion 21ETP, 22ETP or the negative electrode tab peripheral portion 21ETN, 22ETN, thereby manufacturing an inexpensive battery 1. Furthermore, since the tab holders 50, 60 are made of injected and solidified thermoplastic insulating resin (polypropylene in this first embodiment), there is no need to use the multi-layered tab adhesive film described above, and the battery 1 can be manufactured at low cost.

[0067] Moreover, in the manufacturing method of the battery 1, the direct welded portion 20DM is formed in the peripheral heat welding step S13 that is performed after the accommodation step S12 and prior to the holder formation step S14. As a result, the peripheral facing portions 21EM, 22EM of the outer peripheral portions 21E, 22E of the pair of case members 21, 22 are fixed to each other as the direct welded portion 20DM before the holder formation step S14. Therefore, the remaining positive electrode tab peripheral portions 21ETP, 22ETP and negative electrode tab peripheral portions 21ETN, 22ETN of the outer peripheral portions 21E, 22E are also generally fixed. Therefore, when the molten resin MR is injected into the tab peripheral gap ST in the holder formation step S14, the occurrence of positional deviation or deformation of the positive electrode tab peripheral portions 21ETP, 22ETP or the negative electrode tab peripheral portions 21ETN, 22ETN can be suppressed, and the molten resin MR can be easily injected.

[0068] In addition, when forming the tab holders 50, 60 by injecting and solidifying the above-mentioned molten resin MR, taking into consideration the ease of thermal welding of the tab holders 50, 60 to the positive electrode tab peripheral portions 21ETP, 22ETP and negative electrode tab peripheral portions 21ETN, 22ETN of the case members 21, 22, it is advisable to heat the positive electrode tab peripheral portions 21ETP, 22ETP and negative electrode tab peripheral portions 21ETN, 22ETN to a temperature lower than the melting point of the resin constituting the tab holders 50, 60 (for example, 60 to 100°C) in order to reduce the temperature difference with the molten resin MR. Similarly, in consideration of the ease of thermal welding of the tab holders 50, 60 to the surrounded portions 34, 44 of the tab positive terminal 30 and the tab negative terminal 40, it is advisable to heat the surrounded portions 34, 44 of the tab positive terminal 30 and the tab negative terminal 40 to a temperature (e.g., 60 to 100°C) lower than the melting point of the resin constituting the tab holders 50, 60.

[0069] Furthermore, in order to sufficiently inject and airtightly fill the tab-periphery gap ST with molten resin MR in the positive electrode extension direction EH1 or the negative electrode extension direction EH2 to form the clamped portions 51, 61 and further to form the extension surrounding portions 52, 62, it is advisable to inject and fill the molten resin MR while moving the discharge nozzles J1aZ, J1bZ, J2aZ, J2bZ in the positive electrode extension direction EH1 or the negative electrode extension direction EH2, as shown by dashed lines on the left side of FIG. 8.

[0070] 9, the discharge nozzle J1aZ may be advanced along the travel path Z1a indicated by the dashed arrow, and the discharge nozzle J1bZ may be advanced synchronously along the travel path Z1b indicated by the dashed arrow to inject and fill the molten resin MR into the tab surrounding gap ST to form the tab holder 50. That is, first, the two discharge nozzles J1aZ and J1bZ are inserted into a side gap STS1 located on the outer side WHO1 (right side in FIG. 9) in the positive electrode width direction WH1 of the tab surrounding gap ST from the side surface 34S1 of the surrounded portion 34 of the tab positive terminal 30, and the molten resin MR is discharged to inject and fill the side gap STS1. As a result, the molten resin MR is hermetically heat-welded to the side surface 34S1 of the surrounded portion 34 of the tab positive terminal 30, and is also hermetically heat-welded to the inclined surfaces 21ETPS, 22ETPS of the positive tab peripheral portions 21ETP, 22ETP of the case members 21, 22. It is more preferable to move the discharge nozzles J1aZ, J1bZ within the side gap STS1 so that the molten resin MR reaches each portion within the side gap STS1.

[0071] Then, one of the discharge nozzles J1aZ is advanced along the advancement path Z1a indicated by the dashed arrow, and the molten resin MR is injected and filled into the flat plate gap STP1 between the main surface 34P1 of the surrounded portion 34 and the flat portion 21ETPP of the positive electrode tab surrounding portion 21ETP of the case member 21, among the tab surrounding gap ST. Then, the discharge nozzle J1aZ passes through this flat plate gap STP1 and reaches the side gap STS2 located on the outer side WHO1 (left side in FIG. 9) in the positive electrode width direction WH1 of the tab surrounding gap ST, beyond the side surface 34S2 of the surrounded portion 34. As a result, the molten resin MR is hermetically heat-sealed to the main surface 34P1 of the surrounded portion 34 of the tab positive terminal 30, and is also hermetically heat-sealed to the flat portion 21ETPP of the positive electrode tab surrounding portion 21ETP of the case member 21. Furthermore, in synchronization with the movement of the discharge nozzle J1aZ, the other discharge nozzle J1bZ is caused to move along the movement path Z1a indicated by the dashed arrow, and the molten resin MR is injected and filled into the flat plate gap STP2 between the main surface 34P1 of the surrounded portion 34 and the flat portion 22ETPP of the positive electrode tab surrounding portion 22ETP of the case member 22, among the tab surrounding gap ST. Then, the discharge nozzle J1bZ passes through this flat plate gap STP2 and reaches the side gap STS2. As a result, the molten resin MR is hermetically heat-sealed to the main surface 34P2 of the surrounded portion 34, and is also hermetically heat-sealed to the flat portion 22ETPP of the positive electrode tab surrounding portion 22ETP.

[0072] Thereafter, the two discharge nozzles J1aZ and J1bZ inject and fill the molten resin MR into the side gap STS2. This causes the molten resin MR to be airtightly heat-sealed to the side surface 34S2 of the tab positive terminal 30, and also to be airtightly heat-sealed to the inclined surfaces 21ETPS and 22ETPS of the positive tab peripheral portions 21ETP and 22ETP of the case members 21 and 22. In this manner, the tab holder 50 is formed. In addition, in the formation of the tab holder 60, the discharge nozzles J2aZ and J2bZ are advanced along the similar advancement paths Z2a and Z2b, and the molten resin MR is injected and filled into the entire tab peripheral gap ST.

[0073] In this way, the molten resin MR can be injected evenly into the side gaps STS1 and STS2 to fill them airtight. Also, since the molten resin MR can be injected and filled in parallel into the flat plate gap STP1 and the flat plate gap STP2, the flat parts 21ETPP and 22ETPP of the positive electrode tab surrounding parts 21ETP and 22ETP of the case members 21 and 22 due to the injection of the molten resin MR move in a biased manner in the positive electrode thickness direction TH1, and it is possible to suppress uneven thickness between the flat plate parts 51P1 and 51P2 of the sandwiched part 51 of the tab holder, such as one of which becomes thick and the other becomes thin.

[0074] In addition, the suction surface SU1F shown by the two-dot chain line in Fig. 9 is a flat suction plate SU1 that sucks the flat parts 21ETPP, 22ETPP of the positive electrode tab peripheral parts 21ETP, 22ETP of the case members 21, 22, and fixes the positions of the flat parts 21ETPP, 22ETPP in the positive electrode thickness direction TH1 (the vertical direction in Fig. 9). In this state, it is also preferable to use the discharge nozzles J1aZ, J1bZ as described above to inject and fill the molten resin MR into the tab peripheral gap ST, and solidify it to form the tab holder 50. Furthermore, it is more preferable to incorporate a heater for heating the suction surface SU1F of the suction plate SU1 in the suction plate SU1 or provide it separately so that the flat parts 21ETPP, 22ETPP can be fixed and heated at the same time. The same can be done in forming the tab holder 60.

[0075] In the above-mentioned embodiment 1, an example was shown in which four discharge nozzles J1aZ, etc. were used, but when forming the tab holding bodies 50, 60 using the molten resin MR, many patterns can be considered for the number of discharge nozzles J1aZ, etc. used and the manner in which they are moved, and an appropriate method can be adopted that can appropriately form the tab holding bodies 50, 60.

[0076] (Embodiment 2) First, a battery 101 of the second embodiment (see Figs. 10 and 11) will be described. In each drawing of the second embodiment, the same parts as those of the first embodiment are given the same reference numerals. Also, the different parts will be mainly described, and the description of the same parts as those of the first embodiment will be omitted or simplified. In the battery 1 of the first embodiment (see Fig. 1), as described above, the peripheral opposing parts 21EM, 22EM of the case members 21, 22 are directly and airtightly heat-welded to each other to form the direct welded part 20DM. In contrast, the battery 101 of the present embodiment 2 has substantially the same shape as the battery 1, but differs in that a pair of resin intervening portions 120 having a pair of resin intervening bodies 170 airtightly heat-welded to the peripheral opposing portions 21EM, 22EM are provided between the peripheral opposing portions 21EM, 22EM of the case members 21, 22. The pair of resin intervening bodies 170 are formed so as to bridge between the two tab holders 50, 60, and are airtightly integrated with each of the tab holders 50, 60.

[0077] Even in the battery 101 of this embodiment 2, the tab holders 50, 60 can be stably and airtightly heat-welded directly to the roughened surfaces 33, 43 without providing a chemical conversion treatment layer such as a chromate treatment layer on the tab positive terminal 30 and the tab negative terminal 40, resulting in an inexpensive battery 1.

[0078] Additionally, in the battery 101 of the second embodiment, the peripheral facing portions 21EM, 22EM of the case members 21, 22 are not directly heat-welded to each other, but are airtightly heat-welded to each other via the resin interposer 170 to form a resin interposer 120RM. Therefore, compared to the case where the peripheral facing portions 21EM, 22EM are directly heat-welded to each other (first embodiment), the peripheral facing portions 21EM, 22EM that are certainly opposed to each other can be reliably connected airtight via the resin interposer 170. Note that in the battery 101 of the second embodiment, the resin interposer 170 is also made of the same polypropylene as the tab holders 50, 60, so that the battery 101 can be made inexpensive even though it has the resin interposer 170.

[0079] In the manufacture of the battery 1 of the above-described embodiment 1, in a peripheral heat welding step S13 prior to the holder formation step S14, peripheral opposing portions 21EM, 22EM of the outer peripheral portions 21E, 22E of the case members 21, 22 are directly and airtightly heat welded to each other to form a direct weld portion 20DM. Then, in the holder formation step S14, molten resin MR is injected and filled into the tab peripheral gaps ST around the tab positive terminal 30 and the tab negative terminal 40 to form the tab holders 50, 60.

[0080] In contrast, in the manufacture of the battery 101 of the second embodiment, as shown by the broken lines in Fig. 5, instead of the peripheral heat welding step S13 and the holder forming step S14 in the first embodiment, a holder intermediate forming step S23 is included. That is, in parallel with or before or after the formation of the tab holders 50, 60 by injecting the molten resin MR into the tab peripheral gap ST and solidifying it, the molten resin MR is also injected into the facing gap DM between the peripheral facing parts 21EM, 22EM held by forming the facing gap DM, to form a pair of resin intermediates 170 that are interposed between the peripheral facing parts 21EM, 22EM and are hermetically heat-welded to the peripheral facing parts 21EM, 22EM, respectively. In the following, a case will be described in which the holder intermediate forming step S23 employs a procedure in which the tab holders 50, 60 are first formed, and then the resin intermediates 170 are formed. However, in the holder intermediate formation step, a procedure may be adopted in which the resin intermediate body 170 is formed first, and then the tab holders 50, 60 are formed. Also, a procedure may be adopted in which the tab holders 50, 60 and the resin intermediate body 170 are formed in parallel.

[0081] First, similarly to the first embodiment, a tab positive electrode terminal 30 and a tab negative electrode terminal 40 roughened in a roughening step S1 are prepared, and connected to the electrode body 10 in a connection step S11 (see FIG. 6). Thereafter, in a housing step S22, similarly to the housing step S12 of the first embodiment, the electrode body 10 is housed in a pair of case members 21, 22 (see FIGS. 7 and 12). However, unlike the first embodiment (see FIG. 9) in which the peripheral opposing portions 21EM, 22EM of the case members 21, 22 are brought close to each other in the housing step S12, in the second embodiment, as shown in FIG. 12, the peripheral opposing portions 21EM, 22EM of the case members 21, 22 are separated from each other, and the case members 21, 22 are held in a state in which the opposing portion gap DM is opened. As in embodiment 1, a tab surrounding gap ST is provided between the surrounded portion 34 of the tab positive terminal 30 and the positive electrode tab surrounding portions 21ETP, 22ETP of the pair of case members 21, 22, and between the surrounded portion 44 of the tab negative terminal 40 and the negative electrode tab surrounding portions 21ETN, 22ETN of the pair of case members 21, 22.

[0082] As a method for holding the peripheral facing parts 21EM, 22EM of the case members 21, 22 with the facing part gap DM open, for example, there is a method in which the peripheral facing parts 21EM, 22EM of the case members 21, 22 are sucked by a suction plate SU2 having a flat suction surface SU2F shown by a dashed line in Fig. 12, and the facing part gap DM is opened to fix the positions of the peripheral facing parts 21EM, 22EM in the positive electrode thickness direction TH1 (the vertical direction in Fig. 12). Note that it is more preferable to incorporate a heater for heating the suction surface SU2F of the suction plate SU2 in the suction plate SU2 or provide it separately so that the peripheral facing parts 21EM, 22EM can be held and heated at the same time.

[0083] Thereafter, in the holder intermediate forming step S23 of the present embodiment 2, first, in the same manner as in the holder forming step S14 of the embodiment 1, the discharge nozzle J1aZ of the resin injecting device J1a or the like is advanced along the traveling path Z1a, etc., to inject and solidify the molten resin MR obtained by heating and melting the same thermoplastic insulating resin (specifically, unmodified polypropylene) as used in the embodiment 1 into the tab surrounding gap ST between the positive electrode tab surrounding portion 21ETP, 22ETP and the roughened surface 33 of the tab positive electrode terminal 30, and between the negative electrode tab surrounding portion 21ETN, 22ETN and the surrounded portion 34, 44 including the roughened surface 33, 43 of the tab negative electrode terminal 40. Thus, the tab holder 50, 60 airtightly heat-welded to the roughened surface 33, 43 and the positive electrode tab surrounding portion 21ETP, 22ETP or the negative electrode tab surrounding portion 21ETN, 22ETN is formed (see FIG. 8 and FIG. 12).

[0084] In the same manner as in the first embodiment, in the second embodiment, the flat suction plate SU1, which has a suction surface SU1F indicated by a two-dot chain line in FIG. 12, sucks the flat parts 21ETPP, 22ETPP of the positive electrode tab peripheral parts 21ETP, 22ETP, and fixes the positions of the flat parts 21ETPP, 22ETPP in the positive electrode thickness direction TH1. In this state, it is preferable to use the discharge nozzles J1aZ, J1bZ to inject and fill the molten resin MR into the tab peripheral gap ST and solidify it to form the tab holder 50. In addition, it is more preferable to incorporate a heater for heating the suction surface SU1F of the suction plate SU1 in the suction plate SU1 or provide it separately so that the flat parts 21ETPP, 22ETPP can be fixed and heated at the same time. The same can be done for the tab holder 60.

[0085] Following the injection of the molten resin MR into the tab surrounding gap ST described above, the molten resin MR made of the same thermoplastic insulating resin (specifically, unmodified polypropylene) is also injected and filled into the opposing gap DM between the peripheral opposing portions 21EM, 22EM of the case members 21, 22 using an ejection nozzle J1aZ of a resin injection device J1a, etc., to form a pair of resin intermediate bodies 170 that are airtightly integrated with the tab holders 50, 60 and airtightly heat-welded to the peripheral opposing portions 21EM, 22EM, respectively.

[0086] In the manufacturing method of the battery 101, in the holder intermediate forming step S23, molten resin MR is injected into the tab surrounding gap ST and solidified to form the tab holder 50, 60 that is heat-welded to the roughened surface 33, 43 in the surrounded portion 34, 44 and the positive electrode tab surrounding portion 21ETP, 22ETP or the negative electrode tab surrounding portion 21ETN, 22ETN. Therefore, even if the tab positive electrode terminal 30 or the tab negative electrode terminal 40 does not have a chemical conversion treatment layer such as a chromate treatment layer, an inexpensive battery 1 can be manufactured in which the tab holder 50, 60 is stably and directly heat-welded airtightly to the roughened surface 33, 43 in the surrounded portion 34, 44. In addition, since the tab holder 50, 60 is made of an injected and solidified thermoplastic insulating resin (polypropylene in the second embodiment as well), there is no need to use the tab adhesive film with the multilayer structure described above, and the battery 1 can be manufactured inexpensively.

[0087] Furthermore, in the manufacturing method of battery 101, in holder intermediate formation step S23, molten resin is injected to form resin intermediate body 170 that is airtightly heat-welded not only to the tab holder but also to peripheral opposing portions 21EM, 22EM, and is airtightly integrated with tab holders 50, 60. Therefore, battery 101 having tab holders 50, 60 and resin intermediate body 170 can be easily formed.

[0088] The present invention has been described above with reference to the first and second embodiments, but these are merely examples of the laminated electricity storage device disclosed herein and are not intended to limit the technology disclosed herein. In other words, the present invention is not limited to the embodiments, and can be modified as appropriate without departing from the spirit of the present invention. For example, in the batteries 1 and 101 of the first and second embodiments, the positive electrode extension direction EH1 of the tab positive electrode terminal 30 and the negative electrode extension direction EH2 of the tab negative electrode terminal 40 are in the left-right reversed direction (see, for example, FIGS. 1, 2, and 10). However, the present invention is not limited to this. For example, the tab positive electrode terminal 30 and the tab negative electrode terminal 40 can be arranged side by side so that the positive electrode extension direction EH1 and the negative electrode extension direction EH2 are in the same direction. The tab positive electrode terminal 30 and the tab negative electrode terminal 40 can also be arranged so that the positive electrode extension direction EH1 and the negative electrode extension direction EH2 form an angle of 90 degrees. [Explanation of symbols]

[0089] 1,101 Batteries (energy storage devices) 10 Electrode body 12 Positive electrode current collector (current collector) 13 Negative electrode current collector (current collector) 20DM Direct weld part 120RM Resin interposed part 21, 22 Case parts 21IL,22IL Opposite layer 21S, 22S Recessed portion 21E, 22E Outer periphery 21ETP, 22ETP Positive electrode tab periphery (tab periphery) 21ETN, 22ETN Negative electrode tab periphery (tab periphery) 21ETPE, 22ETPE Positive electrode tab peripheral edge (tab peripheral edge) 21ETNE, 22ETNE Negative electrode tab peripheral edge (tab peripheral edge) 21EM, 22EM Peripheral facing part (area other than the tab periphery) 30 Tab positive terminal (tab electrode terminal) 30BR Unroughened tab positive terminal 31 Positive connection end (connection end) 32 Positive external terminal part (external terminal part) 40 Tab negative terminal (tab electrode terminal with enclosure) 40BR Unroughened tab negative terminal 41 Negative electrode connection end (connection end) 42 Negative electrode external terminal part (external terminal part) 33,43 Roughened surface (ring-shaped roughened surface) 34,44 Enclosed part EH1 Positive electrode extension direction (tab extension direction) RH1 Positive electrode circumferential direction (tab circumferential direction) TH1 Positive electrode thickness direction (tab thickness direction) WH1 Positive electrode width direction (tab width direction) WHO1 (Positive electrode width direction) Outer EH2 Negative electrode extension direction (tab extension direction) RH2 Negative electrode circumferential direction (tab circumferential direction) TH2 Negative electrode thickness direction (tab thickness direction) WH2 Negative electrode width direction (tab width direction) WHO2 (negative electrode width direction) Outer side (tab width direction) MR Melt Resin ST Tab Surrounding Gap STP1, STP2 (tab perimeter clearance) plate gap STS1, STS2 Side gap (around tab) DM Opposing part gap 50,60,150,160 Tab holder 51,61 Clamped part 52,62 Extension enclosure SL1,SL2 creepage distance 170 Resin inclusion S1 Roughening process S11 Connection process S12, S22 Storage process S13 Edge heat welding process S14 Holding body forming process MR Melt Resin S23 Holding body intervening body forming process (holding body forming process)

Claims

1. An electrode body having a current collecting portion; A pair of case members made of a laminate film and surrounding the electrode body; a tab electrode terminal made of metal, a connection end portion conductively connected to the current collecting portion of the electrode body within the pair of case members, extending between the pair of case members, and an external terminal portion exposed to the outside of the pair of case members, the tab electrode terminal having, midway in a tab extension direction extending from the connection end portion toward the external terminal portion, an annular band-shaped roughened surface that is roughened in a band-shaped manner all around the circumference in a tab circumferential direction surrounding the tab extension direction; a tab holder made of a thermoplastic insulating resin, covering an enclosed portion of the tab electrode terminal which is a band-shaped region including at least a portion of the annular roughened surface in the tab extending direction and extending around the entire circumference of the tab in the tab circumferential direction, and directly heat-welded in an airtight manner to the annular roughened surface, and also heat-welded in an airtight manner to tab peripheral portions of the outer circumferential edges of each of the pair of case members which are positioned around the tab electrode terminal, and holding the tab electrode terminal in the tab peripheral portions; The tab holder is The molten thermoplastic insulating resin is injected into a tab peripheral gap between the surrounded portion of the tab electrode terminal and the tab peripheral portions of the pair of case members and then solidified. Energy storage device.

2. The power storage device according to claim 1 , The tab holder is made of an unmodified thermoplastic insulating resin. Energy storage device.

3. The electricity storage device according to claim 1 or 2, The case further includes a direct welded portion formed by directly and airtightly heat-welding peripheral facing portions of the outer peripheral edges of the pair of case members that face each other except for the tab periphery. Energy storage device.

4. The electricity storage device according to claim 1 or 2, Among the outer peripheral edges of the pair of case members, peripheral facing portions that face each other except the tab periphery portion are made of the thermoplastic insulating resin and further include a resin intervening portion that is airtightly heat-welded via a resin intervening body that is airtightly integrated with the tab holder. Energy storage device.

5. An electrode body having a current collecting portion; A pair of case members made of a laminate film and surrounding the electrode body; a tab electrode terminal made of metal, a connection end portion conductively connected to the current collecting portion of the electrode body within the pair of case members, extending between the pair of case members, and an external terminal portion exposed to the outside of the pair of case members, the tab electrode terminal having, midway in a tab extension direction extending from the connection end portion toward the external terminal portion, an annular band-shaped roughened surface that is roughened in a band-shaped manner all around the circumference in a tab circumferential direction surrounding the tab extension direction; a tab holder made of a thermoplastic insulating resin, covering an enclosed portion of the tab electrode terminal which is a band-shaped region including at least a portion of the annular roughened surface in the tab extending direction and extending around the entire circumference of the tab in the tab circumferential direction, and directly heat-welded in an airtight manner to the annular roughened surface, and also heat-welded in an airtight manner to tab peripheral portions of the outer circumferential edges of each of the pair of case members which are positioned around the tab electrode terminal, and holding the tab electrode terminal in the tab peripheral portions; The tab holder is The molten thermoplastic insulating resin is injected into a tab peripheral gap between the surrounded portion of the tab electrode terminal and the tab peripheral portions of the pair of case members and then solidified. A method for manufacturing an electricity storage device, comprising: a connecting step of connecting the connection end of the tab electrode terminal to the current collecting portion of the electrode body; an accommodating process for accommodating the electrode body in a pair of case members in such a position that the annular roughened surface of the tab electrode terminal overlaps with the tab peripheral portion of each of the pair of case members in a tab thickness direction of the tab electrode terminal, the tab electrode terminal extends in the tab extension direction through between the tab peripheral portions, and the tab electrode terminal is spaced apart from the tab peripheral portion of each of the pair of case members; a holder forming process for forming the tab holder by injecting molten resin made of the thermoplastic insulating resin into the surrounded portion of the tab electrode terminal and into a tab peripheral gap of the tab peripheral portions of the pair of case members and solidifying the molten resin. A method for manufacturing an electricity storage device.

6. A method for producing the electricity storage device according to claim 5, comprising the steps of: The power storage device is The case further includes a direct welding portion formed by directly and airtightly heat welding peripheral facing portions of the outer peripheral edges of the pair of case members that face each other except for the tab surrounding portion, After the housing step and before the holder forming step, a peripheral heat welding step is performed in which the peripheral facing portions of the peripheral edge portions of the pair of case members are directly and airtightly heat-welded to each other to form the directly welded portion. A method for manufacturing an electricity storage device.

7. A method for producing the electricity storage device according to claim 5, comprising the steps of: The power storage device is a resin interposed portion formed by hermetically heat-welding peripheral opposing portions of the outer peripheral edges of the pair of case members, the peripheral opposing portions being made of the thermoplastic insulating resin and airtightly integrated with the tab holder, the resin interposed portion being airtightly heat-welded to the outer peripheral edges of the pair of case members, the resin interposed portion being made of the thermoplastic insulating resin and airtightly integrated with the tab holder; The support forming step includes: In parallel with or before or after the formation of the tab holder, a holder interposer forming process for injecting the molten thermoplastic insulating resin into the gap between the peripheral opposing portions held with a predetermined opposing portion gap to form the resin interposer that is interposed between the peripheral opposing portions and is also hermetically heat-welded to each of the peripheral opposing portions. A method for manufacturing an electricity storage device.

Citation Information

Patent Citations

  • Capacitor and manufacturing method thereof

    JP2006310834A

  • Lithium ion battery

    JP2007095654A

  • Nonaqueous electrolyte battery

    JP2010244725A

  • Method of manufacturing electronic component, and electronic component

    JP2011009516A

  • External packaging material of laminate battery, method of producing external packaging material of laminate battery, method of manufacturing laminate battery, and laminate battery

    JP2012094374A