Method for manufacturing liquid-repellent article
A PTFE-based liquid-repellent article with a textured surface layer efficiently repels water and high viscosity foods, addressing contamination and residue issues while reducing manufacturing costs through a single-step drying process.
Patent Information
- Application Number
- JP2018085627
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2018-04-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2038-04-26
AI Technical Summary
Existing liquid-repellent articles face challenges in achieving effective repellency against high viscosity foods like sauces and honey, leading to contamination and residue issues, and current methods are costly and require multiple steps.
A liquid-repellent article with a surface layer composed of polytetrafluoroethylene (PTFE) particles and a fluororesin coating, formed by dispersing first and second fluororesin particles in a suspension and drying, achieving a textured surface with air pockets for enhanced repellency.
The method reduces manufacturing costs and effectively repels water and high viscosity foods, minimizing adhesion and residue on containers.
Smart Images

Figure 0007576904000002 
Figure 0007576904000003 
Figure 0007576904000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid-repellent article and a method for producing the same. [Background technology]
[0002] Various liquid-repellent articles having a liquid-repellent surface layer are known. For example, a liquid-repellent article described in Patent Document 1 has a liquid-repellent surface layer formed on a substrate surface, and the liquid-repellent surface layer is composed of first fluororesin particles, second fluororesin particles, a first fluororesin coating that covers the substrate surface and the first fluororesin particles and fixes the first fluororesin particles to the substrate surface, and a second fluororesin coating that covers the first fluororesin coating and the second fluororesin particles and fixes the second fluororesin particles to the first fluororesin coating. According to Patent Document 1, this liquid-repellent surface layer is formed by a first step of covering the substrate surface with a first suspension in which the first fluororesin particles are dispersed in a first fluororesin solution and drying the first suspension, and a second step of covering the surface formed by the first step with a second suspension in which the second fluororesin particles are dispersed in a second fluororesin solution and drying the second suspension. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-166308 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, if a liquid-repellent surface layer can be formed by only one step of drying the suspension, it is advantageous in terms of manufacturing costs. In addition, it is more difficult to obtain liquid repellency against foods such as sauce, soy sauce, honey, noodle soup, mirin, etc. than to obtain liquid repellency against water. However, if a resin surface capable of exhibiting liquid repellency against such foods can be obtained, for example, by applying the resin surface to a container that can store food so that it can be discharged, it becomes possible to advantageously solve the problem of the adhesion of the contents to the discharge part of such a container and the large amount of contents remaining in the container. In particular, it is generally known that the adhesion of the contents to the discharge part and the large amount of contents remaining in the container are common problems with sauces and honey, which have relatively high viscosities, and it is a problem that is desired to be solved as advantageously as possible.
[0005] The present invention has been made in view of the above circumstances, and has an object to provide a liquid-repellent article that advantageously achieves liquid repellency against water and / or food, and a method for producing the same. [Means for solving the problem]
[0013] A method for producing a liquid repellent article according to one aspect of the present invention includes the steps of: Formed from synthetic resin A liquid-repellent surface layer is formed on the surface of the substrate. , as a container or container component for food A method for producing a liquid repellent article, comprising the steps of: Each is made of polytetrafluoroethylene (PTFE), One or more first fluororesin particles having an average particle size of 3 to 33 μm; , made of polytetrafluoroethylene (PTFE), and second fluororesin particles having an average particle size of 1 μm or less. , formed by a polymer having a perfluoroalkyl group A preparation step of preparing a suspension in which the fluorine-based resin is dispersed; a coating step of coating at least a portion of the surface of the substrate with the suspension; a drying step of drying the suspension to form the liquid-repellent surface layer by the one or more first fluororesin particles, the second fluororesin particles, and the fluororesin coating formed by drying the fluororesin solution, A concentration of the fluororesin particles, which is a sum of all of the one or more first fluororesin particles and the second fluororesin particles contained in the suspension, is 13 to 30% by weight, and a concentration of the second fluororesin particles contained in the suspension is 5% by weight or more. the law of nature, a weight ratio of all of the one or more first fluororesin particles to the second fluororesin particles is 3:20 to 25:5; The liquid-repellent surface layer is The one or more first fluorine-based resin particles; The second fluorine-based resin particles; the fluororesin coating at least partially covers the substrate surface, the one or more first fluororesin particles and the second fluororesin particles, and fixes the one or more first fluororesin particles and the second fluororesin particles to the substrate surface, The liquid-repellent surface layer is one or more first surfaces formed in an uneven shape by overlapping each of the one or more first fluororesin particles and the second fluororesin particles; and a second surface formed in an uneven shape by aggregation of the second fluororesin particles, A plurality of air pockets are formed by the first surface and the second surface. It is something. Effect of the Invention
[0020] According to the present invention, it is possible to provide a liquid-repellent article that advantageously achieves liquid repellency against water and / or food, and a method for producing the same. [Brief description of the drawings]
[0021] [Figure 1] 1 is a schematic diagram showing a liquid-repellent surface layer of a liquid-repellent article according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a state in which the surface of a substrate is covered with a suspension in order to form the liquid-repellent surface layer shown in FIG. [Diagram 3] 1 is a flowchart showing manufacturing steps in a method for manufacturing a liquid repellent article according to one embodiment of the present invention. [Figure 4] 2 is an SEM image showing an example of a liquid repellent surface layer of a liquid repellent article according to one embodiment of the present invention. [Diagram 5] FIG. 13 is a schematic diagram for explaining the procedure of a liquid repellency confirmation test carried out on the cap according to the embodiment of the present invention. [Figure 6] 6 is a photograph of the cap shown in FIG. 5, showing the state before and after a liquid repellency confirmation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] A liquid repellent article according to one embodiment of the present invention will be described in detail below with reference to the drawings.
[0023] As shown in FIG. 1, a liquid-repellent article 1 according to this embodiment has a liquid-repellent surface layer 3 formed on a surface (substrate surface) 2a of a substrate 2. The substrate 2 is preferably formed of a synthetic resin such as polypropylene (PP) or polyethylene (PE). However, the substrate 2 may be formed of a material other than synthetic resin. The liquid-repellent surface layer 3 is composed of one or more first fluororesin particles 4 having an average particle size of 3 to 33 μm, second fluororesin particles 5 having an average particle size of 1 μm or less, and a fluororesin coating 6.
[0024] Although only one first fluororesin particle 4 is shown in FIG. 1, the liquid-repellent surface layer 3 is composed of two or more first fluororesin particles 4. For example, the liquid-repellent surface layer 3 may be composed of four first fluororesin particles 4, such as sample 25 described later, which includes a first fluororesin particle 4 having an average particle size of 33 μm, a first fluororesin particle 4 having an average particle size of 10 μm, a first fluororesin particle 4 having an average particle size of 6.2 μm, and a first fluororesin particle 4 having an average particle size of 3 μm. The liquid-repellent surface layer 3 may also be composed of one first fluororesin particle 4. In this specification, the average particle size means a 50% particle size d50 measured by a laser diffraction scattering method.
[0025] In order to obtain excellent liquid repellency, it is preferable that each of the one or more first fluororesin particles 4 is made of polytetrafluoroethylene (PTFE). However, each of the one or more fluororesins may be made of a fluororesin other than PTFE.
[0026] In order to obtain excellent liquid repellency, it is preferable that the second fluororesin particles 5 have a maximum particle size of 1 μm or less. In order to obtain excellent liquid repellency, it is preferable that the liquid repellent surface layer 3 has one second fluororesin particle 5. However, the liquid repellent surface layer 3 may have one or more second fluororesin particles 5.
[0027] In order to obtain excellent liquid repellency, it is preferable that the second fluororesin particles 5 are made of PTFE, but the second fluororesin particles 5 may be made of a fluororesin other than PTFE.
[0028] The fluororesin coating 6 at least partially covers the substrate surface 2a, one or more first fluororesin particles 4, and the second fluororesin particles 5. The fluororesin coating 6 also fixes one or more first fluororesin particles 4 and the second fluororesin particles 5 to the substrate surface 2a. As a result, in this embodiment, the liquid-repellent surface layer 3 has one or more first surfaces 7 formed in an uneven shape by overlapping one or more first fluororesin particles 4 with the second fluororesin particles 5, and a second surface 8 formed in an uneven shape by aggregation of the second fluororesin particles 5. A scanning electron microscope (SEM) image showing an example of such a liquid-repellent surface layer 3 is shown in FIG. 4. From this image, it can be visually confirmed that a large number of air pockets are formed by the first surface 7 and the second surface 8.
[0029] In order to obtain excellent liquid repellency, it is preferable that the fluororesin coating 6 is formed of a polymer having a perfluoroalkyl group, but the fluororesin coating 6 may be formed of a fluororesin other than such a polymer having a perfluoroalkyl group.
[0030] In order to obtain excellent liquid repellency, it is preferable that the weight ratio of all of the one or more first fluororesin particles 4 to the second fluororesin particles 5 is 3:20 to 25:5, however, this weight ratio may be outside this range.
[0031] The liquid-repellent article 1 may be a container or a container component (e.g., a cap) for water and / or food. However, the liquid-repellent article 1 may be an article other than a container or a container component. When the liquid-repellent surface layer 3 is provided on the inside of a container, the remaining amount of the contents (unused contents) that cannot be used due to adhesion to the inner surface of the container can be reduced. Furthermore, when the liquid-repellent surface layer 3 is provided on the outside of the container, the occurrence of stains due to adhesion of the contents to the outer surface of the container can be suppressed. The container may include a container body having a cylindrical mouth, a body part connected below the mouth, and a bottom part closing the lower end of the body, and a cap having, for example, a cylindrical discharge part that is attached to the mouth of the container body and can discharge the contents. The liquid-repellent article 1 may be such a cap, and the liquid-repellent surface layer 3 may be provided on the discharge part of such a cap. If a liquid-repellent surface layer 3 is provided on the discharge portion of such a cap, when the body of the container body is squeezed (pressed) to discharge the contents such as sauce, soy sauce, honey, noodle soup, mirin, etc. to the outside through the discharge portion of the cap, the liquid in the contents is drained off easily at the discharge portion and adhesion of liquid to the discharge portion can be suppressed, thereby suppressing the occurrence of dirt at the discharge portion.
[0032] The liquid repellent article 1 can be obtained by a liquid repellent article manufacturing method according to one embodiment of the present invention described below, however, the liquid repellent article 1 may be obtained by other manufacturing methods.
[0033] In this embodiment, the liquid-repellent surface layer 3 is composed of one or more first fluororesin particles 4, second fluororesin particles 5, and a fluororesin coating 6 that at least partially covers the substrate surface 2a, the one or more first fluororesin particles 4, and the second fluororesin particles 5 and fixes the one or more first fluororesin particles 4 and the second fluororesin particles 5 to the substrate surface 2a. Therefore, according to the liquid-repellent article 1 according to this embodiment, the liquid-repellent surface layer 3 can be formed by simply going through a step of drying a suspension 10 in which one or more first fluororesin particles 4 and second fluororesin particles 5 are dispersed in a fluororesin solution 9 (see FIG. 2), thereby reducing the manufacturing cost.
[0034] Moreover, in this embodiment, the liquid-repellent surface layer 3 has one or more first surfaces 7 and a second surface 8. Therefore, the liquid-repellent article 1 according to this embodiment can exhibit excellent liquid repellency not only to water but also to food.
[0035] Next, a method for manufacturing a liquid-repellent article according to one embodiment of the present invention will be described in detail with reference to the drawings. In the following, the manufacturing method for a liquid-repellent article according to one embodiment of the present invention will be described as an example, but the manufacturing method for a liquid-repellent article according to one embodiment of the present invention can be appropriately applied to the manufacturing of liquid-repellent articles of other configurations.
[0036] As shown in FIG. 3, in the method for manufacturing a liquid-repellent article according to this embodiment, the liquid-repellent article 1 according to one embodiment of the present invention described above is manufactured by going through a preparation step p1, a coating step p2, and a drying step p3 in this order.
[0037] The preparation step p1 is a step of preparing a suspension 10 in which one or more first fluororesin particles 4 and one or more second fluororesin particles 5 are dispersed in a fluororesin solution 9. The fluororesin solute of the fluororesin solution 9 is preferably formed of a polymer having a perfluoroalkyl group in order to obtain excellent liquid repellency. However, the fluororesin solute of the fluororesin solution 9 may be formed of a fluororesin other than such a polymer having a perfluoroalkyl group. In the preparation step p1, for example, ultrasonic waves are applied to the fluororesin solution 9 containing one or more first fluororesin particles 4 and one or more second fluororesin particles 5 for 5 to 10 minutes to obtain a suspension 10 in which one or more first fluororesin particles 4 and one or more second fluororesin particles 5 are well dispersed.
[0038] 2, the coating step p2 is a step of coating at least a part of the substrate surface 2a with the suspension 10. At least a part of the substrate surface 2a with the suspension 10 can be coated by, for example, coating or immersion. In this case, it is not necessary to apply a primer or perform a surface treatment on the substrate surface 2a.
[0039] The drying step p3 is a step of drying the suspension 10 to form a liquid-repellent surface layer 3 (see FIG. 1) made of one or more first fluororesin particles 4, second fluororesin particles 5, and a fluororesin coating 6 formed by drying the fluororesin solution 9. In the drying step p3, the suspension 10 can be dried by leaving it at 80° C. for 5 to 10 minutes, for example, but may also be left at room temperature.
[0040] In this embodiment, in the preparation step p1, the concentration of the fluororesin particles, which is the total concentration of all the one or more first fluororesin particles 4 and the second fluororesin particles 5 contained in the suspension 10, is 13 to 30% by weight, and the concentration of the second fluororesin particles contained in the suspension 10 is 5% by weight or more. By setting the concentration of each component contained in the suspension 10 within such a range, it is possible to stably obtain the liquid-repellent surface layer 3 having one or more first surfaces 7 and second surfaces 8 as described above. It is preferable that the concentration of the fluororesin solute in the fluororesin solution 9 contained in the suspension 10 is about 5% by weight.
[0041] According to the method for producing a liquid repellent article according to this embodiment, the liquid repellent surface layer 3 can be formed in a single drying step, which allows for a reduction in production costs.
[0042] The above-described embodiment is merely one example of the embodiment of the present invention, and it goes without saying that various modifications are possible without departing from the gist of the invention. EXAMPLES
[0043] The inventors formed a liquid-repellent surface layer on a resin plate using fluororesin particles having various average particle sizes, and evaluated the liquid repellency. The results are shown in Table 1. As a comparative example, sample 1 was a resin plate alone. As a comparative example, sample 2 was a resin plate on which a liquid-repellent surface layer was formed only by a fluororesin coating made of a polymer having a perfluoroalkyl group. Samples 3 to 27, 34, 35, 38 to 41, and 46 to 64 are examples produced according to the method for producing a liquid-repellent article according to the embodiment described above. Samples 28 to 33, 36, 37, and 42 to 45 are comparative examples produced according to the method for producing a liquid-repellent article according to the embodiment described above, except that they do not contain the second fluororesin particles.
[0044] The liquid repellency was evaluated not only for water, but also for sauces (Bulldog Sauce's "Chuno Sauce" and "Worcestershire Sauce"), soy sauce (Kikkoman's "Specially Selected Whole Soy Sauce"), honey (Kato Bee Garden's "Sakura Brand Pure Honey"), noodle soup (Yamasa Soy Sauce's "Kombu Tsuyu"), and mirin (Mizkan's "Hon Mirin"). The sliding angles for each of the water, sauce, soy sauce, honey, noodle soup, and mirin were measured, and Table 1 shows that all of these sliding angles were within 30° and are marked with an O, and any one of them exceeded 30° and is marked with an X. The sliding angles were measured by applying a drop of each liquid to each sample, tilting the sample, and measuring the angle at which each liquid began to slide down.
[0045] As the first fluororesin particles, KTL-400M (average particle size 33 μm), KTL-450A (average particle size 17.5 μm), KTL-620 (average particle size 11.5 μm), KTL-10S (average particle size 10 μm), KTL-9S (average particle size 6.2 μm), and KTL-4N (average particle size 3 μm) manufactured by Kitamura Co., Ltd. were used. As the second fluororesin particles, KTL-500F (average particle size 1 μm or less) manufactured by Kitamura Co., Ltd. was used. The concentrations of the particles used in Samples 3 to 47 are shown in Table 1. In the preparation process, the fluororesin solution contained in the suspension was "SF Coat" manufactured by AGC Seimi Chemical Co., Ltd. The concentration of the fluororesin solute in this fluororesin solution was about 5% by weight. [Table 1]
[0046] In the results shown in Table 1, among the Examples, only Samples 3 to 27 and 48 to 64, in which the weight ratio of all of the one or more first fluororesin particles to the second fluororesin particles was 3:20 to 25:5, exhibited good liquid repellency against food. In addition, focusing on the concentration, it is found that in Samples 3 to 27 and 48 to 64, the concentration of the fluororesin particles, which is the total concentration of all of the one or more first fluororesin particles and the second fluororesin particles contained in the suspension, was 13 to 30% by weight, and the concentration of the second fluororesin particles contained in the suspension was 5% by weight or more.
[0047] The inventor also formed a liquid-repellent surface layer on the inner surface of a cap for a bottle-shaped container in the same manner as sample 13, and conducted a test to confirm the liquid repellency against sauce. As shown in FIG. 5, the cap 11 has a disk-shaped top wall 11a and a cylindrical peripheral wall 11b that hangs down from the outer periphery of the top wall 11a. The liquid-repellent surface layer was formed only on half of the entire bottom surface of the top wall 11a. In FIG. 5, the region R where the liquid-repellent surface layer was formed is shown by shading. This cap 11 was attached to the mouth 12a of a bottle-shaped container body 12 containing a sauce, the entire container was inverted, and the sauce was brought into contact with the entire bottom surface of the top wall 11a of the cap 11. The cap 11 was then removed from the container body 12, and the liquid repellency was visually confirmed.
[0048] Photographs of the cap 11 taken before and after it was attached to the container body 12 are shown in Fig. 6. The photograph in Fig. 6 shows the top wall 11a of the cap 11 taken from the bottom side. In Fig. 6, the right half area on the bottom surface of the top wall 11a (area R shown by hatching in Fig. 5) is a liquid-repellent surface layer, and it can be seen that this area is clearly liquid-repellent to the sauce. [Explanation of symbols]
[0049] 1 Liquid repellent articles 2 Base material 2a Base material surface 3 Liquid repellent surface layer 4. First fluorine-based resin particles 5. Second fluorine-based resin particles 6 Fluorine resin coating 7 1st surface 8 Second surface 9. Fluorine-based resin solution 10 Suspension 11 Cap 11a Ceiling wall 11b Surrounding wall 12 Container body 12a Mouth R region
Claims
[Claim 1] A method for producing a liquid-repellent article as a container or container component for food, the article having a liquid-repellent surface layer formed on a surface of a substrate made of a synthetic resin, comprising: a preparation step of preparing a suspension in which one or more first fluororesin particles formed of polytetrafluoroethylene (PTFE) and having an average particle size of 3 to 33 μm and second fluororesin particles formed of polytetrafluoroethylene (PTFE) and having an average particle size of 1 μm or less are dispersed in a fluororesin solution formed of a polymer having a perfluoroalkyl group; a coating step of coating at least a portion of the surface of the substrate with the suspension; a drying step of drying the suspension to form the liquid-repellent surface layer by the one or more first fluororesin particles, the second fluororesin particles, and the fluororesin coating formed by drying the fluororesin solution, a concentration of fluororesin particles, which is a sum of all of the one or more first fluororesin particles and the second fluororesin particles contained in the suspension, is 13 to 30% by weight, and a concentration of the second fluororesin particles contained in the suspension is 5% by weight or more, a weight ratio of all of the one or more first fluororesin particles to the second fluororesin particles is 3:20 to 25:5; The liquid-repellent surface layer is The one or more first fluorine-based resin particles; The second fluorine-based resin particles; the fluororesin coating at least partially covers the substrate surface, the one or more first fluororesin particles and the second fluororesin particles, and fixes the one or more first fluororesin particles and the second fluororesin particles to the substrate surface, The liquid-repellent surface layer is one or more first surfaces formed in an uneven shape by overlapping each of the one or more first fluororesin particles and the second fluororesin particles; and a second surface formed to have an uneven shape by aggregation of the second fluororesin particles, wherein a plurality of air pockets are formed by the first surface and the second surface. A method for producing a liquid-repellent article.
Citation Information
Patent Citations
Water-repellent laminate
JP2013208815A
Water-repellent / oil-repellent coating film and article including the same
JP2014080465A
Super water-repellent surface structure
JP2016166308A
Composition for water-repellent coating
JP2016216585A
Packaging material and packaging container
JP2017100778A