Composite Polymer Film
The composite film with a POP resin and tackifier layer addresses weak seals on non-polar substrates by providing strong and consistent heat sealing across a broad temperature range, enhancing packaging efficiency.
Patent Information
- Application Number
- JP2020517851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-09-27
- Filing Date
- 2018-09-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2038-09-26
AI Technical Summary
Existing heat-sealing adhesives for non-polar substrates like polypropylene (PP) and high-density polyethylene (HDPE) suffer from weak seals, narrow temperature range, and low solubility in organic solvents, limiting their applicability in packaging applications.
A composite film with a heat-sealing layer comprising a polyolefin plastomer (POP) resin, tackifier, and optional primer layer, such as PVdC, applied via solvent coating to enhance adhesion and provide a wide temperature range for effective sealing.
The composite film achieves superior heat seal strength to non-polar substrates with a consistent peel strength across a wide temperature range, reducing process time and improving efficiency.
Smart Images

Figure 0007576979000009 
Figure 0007576979000010 
Figure 0007576979000001
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority to U.S. Provisional Application No. 62 / 563,695, filed Sep. 27, 2017, and entitled COMPOSITE POLYESTER FILMS FOR HEAT SEALING TO NON-POLAR SUBSTRATES, the contents of which are incorporated herein by reference in their entirety for all purposes. [Background technology]
[0002] Polymeric films that are heat sealable to non-polar substrates are becoming increasingly important as more and more food manufacturers are switching to polypropylene (PP) trays to reduce costs. Also, the market for liners of induction seal caps for high density polyethylene (HDPE) and PP containers in the pharmaceutical and food industries is steadily growing. Traditionally, ethylene vinyl acetate (EVA) resins have been used for such applications, but tend to produce relatively weak seals with PP and HDPE, which has limited their applicability in many applications. Alternative heat seal adhesives employing traditional low density polyethylene have been introduced, but these tend to have a fairly narrow serviceable temperature range for the heat sealing process and are not applicable to all polymeric substrates by solvent coating (e.g., not applicable to polyester substrates) due to their extremely low solubility in common organic solvents. Thus, a polymeric film (e.g., polyester film) with a heat seal layer that addresses these issues would represent a welcome advancement in packaging technology. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US 4542199 [Patent Document 2] US4752597 [Patent Document 3] US4808561 [Patent Document 4] US5189192 [Patent Document 5] US5349100 [Patent Document 6] WO 93 / 17060 [Non-patent literature]
[0004] [Non-Patent Document 1] "Determination of Number-Average and Weight-Average Molecular Weights of Polymer Sample from Diffusion and Sedimentation Velocity Measurements in Theta Solvent", Okabe and Matsuda, Vol. 28, pp. 2325-23339, Journal of Applied Polymer Science [Non-Patent Document 2] Pure Appl. Chem., Vol. 68, No. 12, pp. 2287-2311, 1996 Summary of the Invention [Means for solving the problem]
[0005] In general, one aspect of the invention is a method for producing a cellular membrane comprising: a) a free-standing layer of polymer film, which may optionally be a polymer film comprising a polar polymer and / or a polyolefin polymer, and which may further optionally be oriented in at least one direction; b) an optional primer layer on the polymer film and between the polymer film and the heat seal layer (c), the optional primer layer comprising a halopolyvinylidene polymer, an acrylic resin and / or a vinyl resin; A composite film comprising: a heat seal layer comprising a heat seal composition is disposed on the optional primer layer, if present, or directly on the surface of the polymer film, if the optional primer layer (b) is not present; the heat seal composition comprises a polyolefin plastomer (POP) resin and a tackifier; (i) the tackifier is present in an amount of at least 20% by weight of the heat seal composition, where the total weight of the heat seal composition is 100%; (ii) the POP resin is present in an amount of 80% by mass or less of the heat seal composition, where the total mass of the heat seal composition is 100%; (iii) the optional primer layer is absent only if the polymer film comprises a polyolefin, and if the optional primer layer (b) is absent, the surface of the polymer film in contact with the heat seal layer (c) is corona treated; A composite film is provided.
[0006] The composite film may include a heat seal composition further comprising an acrylic resin and / or a vinyl resin.
[0007] The composite film may comprise in the optional primer layer (b) a halopolyvinylidene polymer, i.e. a PVdX resin where X is halo (e.g., X is chloro), more preferably a PVdC resin, most preferably a PVdC resin.
[0008] The composite film may include an acrylic resin and / or a vinyl resin present in the optional primer layer (b) and / or the heat seal layer (c), the acrylic resin and / or the vinyl resin being C 1~4 Alkyl vinyl acetate resin and C 1~4 From the group consisting of (meth)acrylic resins, it is preferably selected from the group consisting of ethyl acrylate (EA), ethylene vinyl acetate (EVA), ethyl acrylic acid (EAA) and ethyl methacrylic acid (EMA).
[0009] The composite film may comprise a POP resin in the heat seal layer (c), suitable POP resins being further defined herein.
[0010] The POP resin may have a DSC melting point below 100°C.
[0011] The molecular weights (e.g., weight average (M w ) and number average (M n )) can be determined by any suitable method known to those skilled in the art, such as by experiment (e.g., GPC, SEC, etc.) and / or theoretical calculation. w and M n A method for measuring velocity is described in “Determination of Number-Average and Weight-Average Molecular Weights of Polymer Sample from Diffusion and Sedimentation Velocity Measurements in Theta Solvent”, Okabe and Matsuda, Vol. 28, pp. 2325-2339, Journal of Applied Polymer Science, which is incorporated herein by reference.
[0012] The amount of α (alpha)-olefin comonomer in the POP resin may be from 5 to 85 mol %, relative to the total amount of the POP resin, which is 100 mol %.
[0013] The composite film may comprise a POP resin present in an amount of up to 75% by weight, based on the total weight of the heat seal composition being 100%.
[0014] The composite film may also include a tackifier resin, preferably comprising at least 25% by weight of the heat seal composition, with the total weight of the heat seal composition being 100%.
[0015] The composite film may comprise at least one polyester selected from the group consisting of polyethylene terephthalate (PET), polylactic acid (PLA), polyhydroxybutyrate (PHB), polyethylene furanoate (PEF), and polyethylene naphthalate (PEN).
[0016] Another aspect of the invention is a method for making a composite film of the invention, comprising the steps of: (i) applying a coating composition comprising a heat seal composition in a solvent to a primer layer overlying a polymeric film (e.g., to a polar film, such as a polyester film) or, if the optional primer layer is not present, directly to the corona-treated surface of the polymeric film; and then (ii) evaporating the solvent; Including, The heat seal composition comprises: Polyolefin plastomer (POP) resin, a tackifying resin present in an amount of at least 20% by weight, based on 100% of the heat seal composition; and Optionally, acrylic and / or vinyl resins, preferably EVA resins; A method is provided.
[0017] A further aspect of the present invention provides a method of adhering a polymeric film to a container or free-standing film, comprising the step of heat-sealing a composite film of the present invention as described herein to a surface of the container or free-standing film. The surface may be a polyolefin surface, such as a polypropylene (PP) and / or high density polyethylene (HDPE) surface. The heat-sealable composite film of the present invention may be an unprimed polyolefin film or a primed polar film (e.g. a primed polyester film) comprising thereon a heat-seal layer as described herein. [Brief description of the drawings]
[0018] [Figure 1]1 is a graph showing peel strength as a function of the temperature at which heat sealing was performed for a composite film comprising a primed polyester film coated with a heat seal composition in accordance with the present invention heat sealed to an HDPE substrate, compared to a prior art film having an extrusion coated EVA heat seal layer. [Diagram 2] 2 is a graph showing peel strength results for trials similar to that depicted in FIG. 1, but using a polypropylene substrate instead of the HDPE substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention provides a composite film that achieves excellent heat seal strength to a variety of substrates, including non-polar substrates, such as polyolefin substrates, such as PP and HDPE. The composite film has the advantage of being able to be applied by solvent coating, with a very wide temperature range for heat sealing to substrates. The composite film advantageously has a low heat seal initiation temperature and achieves a relatively constant peel strength as a function of heat seal temperature, as compared to films using conventional heat seal compositions. This reduces the residence time in the heat seal process, which favors process efficiency.
[0020] As used herein, the term "heat seal initiation temperature" is the temperature at which a seal at 80 psi (about 552 kPa) for 1 second produces a peel strength of at least 350 g force / inch (about 135 N / m) to the HDPE substrate. The heat seal initiation temperature is the minimum temperature at which the sealing polymer melts and flows sufficiently to melt bond to the adjacent layers in the seal. Below this temperature, the coating will have insufficient bond strength to the substrate. In many packaging line applications, sealing temperatures well above the heat seal initiation temperature are commonly used to ensure sufficient seal strength.
[0021] Heat seal initiation temperatures for composite film compositions useful in the present invention are typically no greater than 265°F (about 129°C) or 275°F (about 141°C). Additionally, composite film compositions according to various embodiments of the present invention provide surprisingly little change in peel strength over a wide range of seal temperatures compared to typical extrusion coated products. Peel strengths for heat seals produced at 275°F (about 141°C) are typically at least 70%, or at least 75%, or 80% or more, or 85% or more, or 90% or more than that of heat seals produced at 400°F (about 204°C).
[0022] Composite films according to the present invention typically achieve a peel strength of at least 350 gf / in (about 135 N / m), or at least 500 gf / in, or 700 gf / in or more, or 900 gf / in or more, or 925 gf / in or more, or 950 gf / in or more, or 975 gf / in or more, or 1000 gf / in or more, or 1025 gf / in or more (about 193 N / m or more, about 270 N / m or more, about 347 N / m or more, about 357 N / m or more, about 367 N / m or more, about 376 N / m or more, about 386 N / m or more, and about 396 N / m or more, respectively) when applied to an HDPE substrate at 300° F. (about 149° C.) and 80 psi (about 552 kPa) for 1 second.
[0023] The inventors have found that due to the high tackifier content of the heat seal compositions of the present invention, these heat seal compositions have poor chill roll release and typically cannot be applied by extrusion coating. The inventors solve this problem by solvent coating the heat seal composition onto a primed substrate, where the primed substrate comprises a primer layer on a polar polymer film (e.g., polyester, etc.). The heat seal composition can also be coated onto an unprimed substrate, where the unprimed substrate comprises a polyolefin polymer film, which may optionally be corona treated as an alternative to the use of a primer coating, but the use of a primer is still preferred to achieve improved adhesion of the heat seal layer to the polymer film, as it may prevent delamination of the composite film under a wider range of conditions. The present invention also addresses the thermal stability issue that prevents certain types of tackifier resins from being used in extrusion coating. For example, tackifiers with low softening points (e.g., Piccolyte® C85 resin, softening point 82-88°C) may cause fuming under typical extrusion coating conditions.
[0024] The composite film of the present invention can be heat sealed to a container or a self-supporting film using the heat seal layer as the contact layer with the container or the self-supporting film. The container may be preformed, and the surface of the container that is bonded to the composite film may be made of any material. Suitable exemplary materials include glass, metal, and polymers. Exemplary polymers include nylon and polyester, including polyesters that are not heat-sealable themselves, such as polyethylene terephthalate (PET) homopolymers. In particular, the material may be HDPE or PP. In contrast, when the composite film is heat sealed to a self-supporting film, the surface of the self-supporting film to which the composite film is heat-sealed may be made of any of these same materials.
[0025] The composite film of the present invention comprises a free-standing layer of polymeric film, an optional primer layer on the polymeric film (optionally present if the polymeric film is a corona-treated polyolefin film), and a heat seal layer on the primer layer or directly on the non-primed corona-treated polymeric film if the optional primer layer is not present. Typically, all of these layers are coextensive.
[0026] The heat seal layer comprises a heat seal composition comprising one or more acrylic and / or vinyl resins, preferably EVA, EAA or EMA, more preferably EVA resin, one or more tackifiers (e.g., tackifying resins), and one or more polyolefin plastomer (POP) resins. Each of the components of the composite film is discussed in detail herein, including a description of the components of the heat seal layer.
[0027] A still further aspect of the present invention provides the use of the inventive films described herein as a heat-sealable component of a packaging article (e.g., an ovenable food container) and / or as a liner for a cap for the packaging article.
[0028] Yet another aspect of the present invention provides a packaging article comprising the composite film of the present invention as described herein, including, for example, an ovenable food container, which may optionally comprise an HDPE or PP tray, as described herein, and / or a cap for the packaging article lined with the composite film of the present invention.
[0029] Acrylic and / or vinyl resin Acrylic and / or vinyl resins refer to a subset of resins that are, or may be, derived from at least one polymeric precursor (i.e., which itself may be a polymer, e.g., an oligomer or monomer) that contains activated unsaturation.
[0030] The term "activated unsaturated moiety" is used herein to denote a species that contains at least one unsaturated carbon-carbon double bond in chemical proximity to at least one activated moiety. Preferably, the activated moiety comprises any group that activates an ethylenically unsaturated double bond for addition thereto by a suitable electrophilic group. Conveniently, the activated moiety comprises an oxy, thio, (optionally organically substituted) amino, thiocarbonyl and / or carbonyl group (the latter two groups may be optionally substituted by thio, oxy or (optionally organically substituted) amino). More conveniently, the activated moiety is a (thio)ether, (thio)ester and / or (thio)amide moiety. Most conveniently, the "activated unsaturated moiety" comprises an "unsaturated ester moiety" which represents an organic species containing one or more "hydrocarbylidenyl(thio)carbonyl(thio)oxy" and / or one or more "hydrocarbylidenyl(thio)-carbonyl(organo)amino" groups and / or similar and / or derived moieties, such as moieties containing (meth)acrylate functional groups and / or derivatives thereof. The "unsaturated ester moiety" may optionally comprise optionally substituted common α,β-unsaturated acids, esters and / or other derivatives thereof, including thio derivatives and analogues thereof.
[0031] Acrylic and / or vinyl polymer precursors (e.g., acrylic and / or vinyl oligomers or monomers) suitable for preparing the acrylic and / or vinyl resins that can be used in the present invention may contain one or more hydrophobic, hydrophilic and / or partially hydrophilic polymer precursors as components thereof that can be polymerized to form the acrylic and / or vinyl polymer.
[0032] The hydrophobic polymer precursor may comprise, and may advantageously consist essentially of, at least one hydrophobic polymer precursor comprising at least one activated unsaturated moiety, advantageously at least one hydrophobic (meth)acrylate monomer, and / or an aryl alkylene polymer precursor. As used herein, (meth)acrylate refers to acrylate and / or methacrylate moieties, and similarly, as used herein, (meth)acrylic refers to acrylic and / or methacrylic moieties.
[0033] Hydrophobic (meth)acrylates are C >4 Hydrocarb(meth)acrylates, conveniently C >4 The hydrocarbyl part is C 4~20 Hydrocarbyl, more conveniently C 4~14 Alkyl, most conveniently C 4~10 Alkyl, e.g. C 4~8 The hydrophobic (meth)acrylate may be selected from isooctyl acrylate, 4-methyl-2-pentyl acrylate, 2-methylbutyl acrylate, isoamyl acrylate, sec-butyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, isodecyl methacrylate, isononyl acrylate, isodecyl acrylate, and / or mixtures thereof.
[0034] The aryl alkylene monomer may include an (optionally hydrocarbyl-substituted) styrene, the optional hydrocarbyl being C 1~10 Hydrocarbyl, more preferably C 1~4 The aryl alkylene monomer may be selected from styrene, alpha-methyl styrene, vinyl toluene, t-butyl styrene, dimethyl styrene, and / or mixtures thereof.
[0035] The hydrophilic polymer precursor may be copolymerizable with the hydrophobic polymer precursor and is water-soluble. At least one hydrophobic polymer precursor may contain at least one activated unsaturated moiety. The hydrophilic monomer comprises, advantageously consists essentially of, at least one ethylenically unsaturated carboxylic acid (e.g., an acid having one ethylene group and one or two carboxy groups). The acid may be selected from the group consisting of acrylic acid (and its oligomers), beta-carboxyethyl acrylate, citraconic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, methacrylic acid, and mixtures thereof.
[0036] The partially hydrophilic polymer precursor may be referred to as a partially water-soluble monomer and may advantageously contain at least one activated unsaturated moiety. Preferred partially hydrophilic monomers include at least one C 1~2 More preferred partially hydrophilic monomers comprising, and advantageously consisting essentially of, alkyl (meth)acrylates are selected from the group consisting of methyl acrylate (MA), methyl methacrylate (MMA), ethyl acrylate (EA), and mixtures thereof.
[0037] An example of a suitable ethyl acrylate (EA) resin is available from DuPont under the trade name Bynel® 2000 series.
[0038] Ethylene-vinyl acetate (EVA) resin, also known as poly(ethylene-vinyl acetate) (PEVA), represents a class of copolymers formed from ethylene and vinyl acetate monomers. Vinyl acetate (VA) has the following structure:
[0039] [ka]
[0040] Ethylene-acrylic acid (EAA) resins represent a class of copolymers formed from ethylene and acrylic acid (AA) monomers, which have the following structure:
[0041] [ka]
[0042] Ethylene-methacrylic acid (EMA) resins represent a class of copolymers formed from ethylene and methacrylic acid (MAA) monomers, which have the following structure:
[0043] [ka]
[0044] Typically, the total amount of one or more acrylic and / or vinyl resins (e.g., EA, EAA, EVA and / or EMA resins) in the heat seal composition of the heat seal layer is at least 15%, or at least 18%, or at least 20%, or at least 25%, or 30% by weight of the heat seal composition is acrylic and / or vinyl resin. Typically, no more than 60%, or no more than 55%, 50%, 45%, or 40% of acrylic and / or vinyl resins are present in the heat seal composition, all of the weights of the acrylic and / or vinyl resins being based on the total weight of the respective heat seal composition being 100% (depending on the composition of which the acrylic and / or vinyl resins form part). EVA resin is the preferred vinyl resin, and is more preferably used in the amount described above. The total amount of acrylic and / or vinyl resins present in the heat seal composition may be 15%-60% by weight of the heat seal composition, preferably 18%-55%, more preferably 20%-50%, even more preferably 25%-45%, most preferably 30%-40%, or such as 18%, 23%, 30%, 34%, 36%, 54% or 60%. All weights of acrylic and / or vinyl resins mentioned herein are relative to the total weight of the respective heat seal composition which is 100%.
[0045] Of course, if any acrylic and / or vinyl resins are also present as components of the optional primer layer, the amount of any such acrylic and / or vinyl resin primer layer components is calculated separately and does not form part of the amounts set forth herein for the acrylic and / or vinyl resins that may form part of the heat seal layer.
[0046] Ethylene vinyl acetate (EVA) polymers useful in the present invention contain 15-50 wt.%, or 18-40 wt.%, or 25-40 wt.% vinyl acetate. Such EVA resins are commercially available from DuPont under the trademarks Elvax® (250, 420, 3180, 3185, 4031, 4260), from Celanese under the trademarks Ateva® (2810A, 2821A, 3325AC, 4031AC), and from Arkema under the trademarks Evatane® (28-05, 28-25, 28-40, 28-150, 33-25, 33-45, 40-55, 42-60).
[0047] The EVA resin can also be an EVA terpolymer. These are terpolymers of ethylene, vinyl acetate, and acrylic or methacrylic acid. Examples include Elvax® 4260, 4310, and 4320.
[0048] Tackifier To achieve a relatively constant heat seal peel strength as a function of heat seal temperature as well as an adequately low heat seal initiation temperature, the heat seal composition comprises a total amount of one or more tackifiers in an amount such that at least 20% of the heat seal composition by weight, or at least 22%, 25%, 27%, or 30% of the heat seal composition by total weight, is tackifier. The tackifier may be a tackifying resin. However, there may be disadvantages when a total amount of tackifier is included in the heat seal composition for typical applications that is more than 60% by weight, since tackifiers tend to be relatively expensive compared to other components in the heat seal composition and tend to cause coating blocking problems. Typically, the total amount of tackifier to be present in the heat seal composition is 60% or less, or 55%, 50%, or 45% or less of tackifier by weight of the heat seal composition. The total amount of tackifier present in the heat seal composition may be 20% to 60% by weight of the heat seal composition, preferably 22% to 60%, more preferably 25% to 55%, even more preferably 27% to 50%, most preferably 30% to 45%, or such as 6%, 18%, 24%, 25%, 30% or 60%. All weights of tackifier described herein are relative to the total weight of the heat seal composition which is 100%.
[0049] Tackifiers (which may include tackifying resins) suitable for the present invention include, but are not limited to, synthetic and natural polyterpenes, hydrocarbon resins, rosin and rosin ester resins, and combinations thereof. The tackifying resin may have a Ring and Ball softening point of from 20° C. to 160° C., preferably from 90° C. to 125° C. The number average molecular weight of the tackifying resin is typically at least 200 or 500 Daltons, typically no more than 5000 Daltons, 2000 Daltons, or 1000 Daltons, and thus typically has an M of from 200 to 5000 Daltons, preferably from 500 to 1000 Daltons, and more preferably from 500 to 1000 Daltons. n
[0043]
[0050] Natural polyterpene tackifying resins are based on natural renewable feedstocks, including alpha-pinene, beta-pinene, and d-limonene. Examples include: 1) Piccolyte® C resins (C85, C105, C115, C125, C135), Piccolyte® F resins (F105, F115), Piccolyte® A resins (A25, A115, A125, A135), Piccolyte® S resins (525, 585, 5115, 5125, 5135); all available from Pinova. 2) Sylvares® TR resins (A25L, 90, 105, 7115, 7125); all available from Arizona Chemical Company.
[0051] Hydrocarbon tackifying resins are made from petroleum-based feedstocks, either aliphatic (C5), aromatic (C9), DCPD (dicyclopentadiene), or mixtures thereof. Examples include: 1) Piccotac™ 1020, 1095, 1100, 1115, 6095-E, 8095; Picco™ 5120, 5140, 6100, 2215; Regalite™ 51100, 7125; Regalite™ R1010, 1100, 9100, Regalrez™ 1018, 1094, 3102, 6108; all available from Eastman Corporation; 2) Quintone® A100, B170, K100, M100, N295, U190, 5100, D100, U185; all available from Nippon Zeon of Japan; 3) Escorez™ 1102, 1304, 1315, 2203, 5300, 5320, 5340, 5400, 5415, 5600, 5615, 5690; all available from ExxonMobil; 4) Wingtack® 86, 95, 98; Norsolene® W85, 90, 100, 110, 120, 130, 140; all available from Cray Valley.
[0052] Rosin ester tackifying resins are prepared by the reaction of rosin acids with alcohols. The rosin acids may be modified by hydrogenation or disproportionation. Typical commercial products are esters of methyl, triethylene glycol, glycerol, and pentaerythritol. Examples include: 1) Foral® 85, 105; 3085; Pentalyn® A, H, Pentalyn® 9085, 9100; Staybelite® Esters 3, 5, 10; all available from Pinova; 2) Sylvalite® RE8OHP, RE85GB, RE100XL, RE100L, 105L, 110L, RE25, 85, 98; all available from Arizona Chemical Company; 3) Foralyn™ 90, 110, 50201; Permalyn™ 2085, 5095, 3100, 5110, 6110; all available from Eastman.
[0053] Polyolefin Plastomer (POP) Resin Typically, the heat seal composition comprises at least 10% by weight of one or more polyolefin plastomer (POP) resins in total, or at least 15% or 20% by weight of the heat seal composition by weight of POP resin. Typically, there is no more than 60% by weight of the heat seal composition, or no more than 50%, no more than 40%, or no more than 30% by weight of POP resin. The total amount of POP resin present in the heat seal composition may be 10% to 60%, preferably 10% to 50%, more preferably 15% to 40%, and most preferably 20% to 30% by weight of the heat seal composition. All weights of POP resins described herein are relative to the total weight of the heat seal composition, which is 100%.
[0054] Polyolefin plastomer (POP) resins are polymers that combine the properties of elastomers and plastics, providing rubber-like properties with the processability of thermoplastic resins. POP resins suitable for use in the present invention are made from ethylene and at least one C3-C6 polyolefin polymerized using a metallocene catalyst. 20 The resins include α-olefins, preferably C4-C8 α-olefins. Examples of such resins and methods for making them are disclosed in US 4542199, US 4752597, US 4808561, US 5189192 and US 5349100, all of which are incorporated herein by reference for all purposes. Suitable plastomers are commercially available under the trademarks Affinity™, Versify™ and Engage™ (Dow Chemicals), Queo™ (Borealis), Exact™ and VistaMaxx™ (ExxonMobil).
[0055] The POP resin used in the present invention is Formula 1 below: CH2=CHR Equation 1 (Wherein, R is H or C 1~10 (It is alkyl) (Preferably, formula 1 represents an ethylene monomer) and at least one monomer of Below I to V: I. At least one different polymer precursor having the same formula 1 II. At least one polymer precursor represented by formula 2 C 4~20 α (alpha), ω (omega)-diolefin - formula 2 III. At least one polymer precursor represented by formula 3 C 3~20 α-Olefins - Formula 3 IV. At least one polymer precursor represented by formula 4 C ≧18 Diolefins - Formula 4, and V. At least one polymer precursor represented by formula 5 C 4~18 Cyclic Olefins (including Norborene) - Formula 5 and at least one other different polymer precursor selected from any one of is obtained or derivable from
[0056] The POP resins useful in the present invention include at least one C 2~4 Copolymers of alkylene and at least one polymer precursor of any of formulas 2-5 may also be useful.
[0057] The preferred POP resin is a POP resin made of ethylene and / or propylene and at least one C 5~20 More preferably, it is a copolymer of ethylene and at least one C 6~15 and even more preferably a copolymer of ethylene and at least one C 6~12 and most preferably a copolymer of ethylene and at least one linear monounsaturated C 6~10 Copolymers with alkylenes, for example, copolymers of ethylene and 1-octene.
[0058] Advantageously, the POP resins used in the present invention are prepared using a suitable catalyst, more advantageously other than a Ziegler-Natta catalyst or a free radical initiator, and most advantageously the catalyst is selected from the group consisting of metallocenes (e.g. complexes with zirconium, hafnium and / or vanadium), alumoxanes, anionic, non-ionic ligand systems containing Group 4-8 metals, and / or chiral organometallic complexes.
[0059] The polyolefin plastomer resins used in the present invention may combine the properties of elastomers and plastics, for example by exhibiting rubber-like properties with the processability of plastics. Currently commercially available POP resins are copolymers of ethylene and other olefins, typically produced using metallocene catalysts. In contrast, typical low density olefin polymers (e.g., linear low density polyethylene (LLDPE); low density polyethylene (LDPE) and very linear low density polyethylene (VLDPE)) are produced by conventional Ziegler-Natta catalysts or free radical initiators. Without wishing to be bound by any theory, the applicant believes that POP resins may be particularly suitable for the requirements of heat sealable coatings, since they contain a large amount of other olefin units and may have a very low melting point and low crystallinity, yet still exhibit a relatively high molecular weight.
[0060] The molecular weight, e.g., the weight average molecular weight (M w (also referred to as number average molecular weight (M n The molecular weight distribution (also referred to as the molecular weight distribution) may be calculated by theory and / or measured by any suitable conventional method as known to the skilled artisan, for example by gel permeation chromatography (GPC); gas chromatography-mass spectrometry (GC-MS) and / or size exclusion chromatography (SEC). The GPC method using polystyrene standards is preferred.
[0061] The mass average molecular weight (M w ) is typically at least 3 kilodaltons, or at least 5 kilodaltons, or at least 12 kilodaltons, or at least 15 kilodaltons, and not more than 60 kilodaltons, or not more than 50 kilodaltons, or not more than 40 kilodaltons, or not more than 30 kilodaltons; M wis preferably determined by GPC using polystyrene standards. Usefully, the POP plastomer has an M of 3 to 60 kilodaltons, or 5 to 50 kilodaltons, or 12 to 40 kilodaltons, or 15 to 30 kilodaltons. w has.
[0062] The number average molecular weight s(M n ) is typically at least 5 kilodaltons, or at least 15 kilodaltons, and not more than 50 kilodaltons, or not more than 30 kilodaltons; n is preferably determined by GPC using polystyrene standards. Usefully, the POP plastomer has an M of 5 to 50 kilodaltons, or 15 to 30 kilodaltons. n has.
[0063] The amount of α-olefin comonomer in the plastomer is 5-85 mol%, preferably 10-25 mol%, more preferably 10-30 mol%. The DSC melting point of the plastomer is typically less than 100° C., or 70° C. or less. The DSC melting point is typically at least 40° C., or at least 45° C. or 50° C. The tensile strength of the plastomer is generally 1.0-20 MPa, preferably 5-10 MPa [20 in / min (about 50.8 cm / min), ASTM D369].
[0064] Typically, POP resins suitable for use with the present invention are soluble in at least one of toluene, xylene, dichlorobenzene, trichlorobenzene, or mixtures of any of these with THF or ethyl acetate, in each case at a solids concentration of at least 10% at 65° C. Typically, the resulting solution is clear.
[0065] Other Ingredients Slip additives are used to reduce the resistance of the composite film as it slides over itself or over parts of a converting device. The most common slip additives in the coatings industry are long chain fatty acid amides such as erucamide and oleamide.
[0066] One or more slip agents, such as calcium stearate or fatty acid amides (e.g., Kemamide® EZ and Kemamide® OR, available from Chemtura, Inc.), are typically included in the heat seal composition. If included, the slip agents, in total, typically comprise at least 0.15% by weight of the heat seal composition, or at least 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, or 3.5% of the heat seal composition by weight.
[0067] The slip agents, in total, typically constitute no more than 7 wt% of the composition, or no more than 6.5%, 6%, 5.5%, 5%, or 4.5% of the heat seal composition. The total amount of slip agents present in the heat seal composition may be 0.15% to 7% by weight of the heat seal composition, preferably 0.2% to 6.5%, more preferably 0.5% to 6.5%, even more preferably 1% to 6.5%, and most preferably 1.5% to 6.5%, or 2% to 6%, or 2.5% to 5.5%, or 3% to 5%, or 3.5% to 4.5%, or such as 1.5%, 1.7%, or 2.5%. All weights of slip agents described herein are relative to the total weight of the heat seal composition, which is 100%.
[0068] Optional raw materials for the heat seal layer may include, inter alia, one or more of the following: antiblock additives and / or matte feel agents, such as silica, e.g., Syloid 244 or Syloid 620 available from Grace Davison (optionally present in an amount of 1% to 3%, preferably 1.5% to 2.5%, e.g., 1.5%; 2.2% or 2.5% by weight of the heat seal composition), anti-fog agents, such as sorbitan esters, e.g., ATMER™ 100 available from Croda Polymer Additives; antistatic agents, such as glycerol esters, e.g., Atmer™ 129 available from Croda Polymer Additives; UV absorbers, such as Tinuvin™ 477DW and Tinuvin™ 1130 available from Ciba; and pigments, such as titanium dioxide, e.g., Ti-Pure™ R-101 available from Chemours.
[0069] The heat seal composition forms the heat seal layer of the composite film of the present invention, and so the same weight percent of acrylic resin, vinyl resin, POP resin tackifier, slip agent and / or any other components thereof in the heat seal composition given herein also corresponds to the total weight of these components by weight that may be present in the heat seal layer, where the total weight of the heat seal layer is 100%.
[0070] Polymer Film The polymeric films used in the present invention may be any suitable polymer capable of forming a film, prior to the deposition of any coatings or layers, and may thus include polyolefins [e.g., polypropylene (PP) and / or polyethylene (PE)], polyurethanes, polyvinyl halides [e.g., polyvinyl chloride (PVC)], polar polymers, polyesters [e.g., polyethylene terephthalate (PET)] or other polyesters as described herein, polyamides [e.g., nylon], polyaryletherketones, and / or non-hydrocarbon polymers; suitable combinations and / or mixtures thereof.
[0071] Preferably, the polymer film comprises a homopolymer, a crystalline polymer and / or a polymer with randomly oriented amorphous, non-crystalline polymer chains.
[0072] Advantageously, the polyolefin film to be used as the polymer film in the present invention may comprise one or more polyolefins, such as polypropylene homopolymer, polyethylene homopolymer (e.g., linear low density polyethylene (LLDPE)) and / or polypropylene / polyethylene copolymer, optionally in one or more layers. The constituent polymers and / or layers of the polymer film of the present invention may be oriented, blown, shrunk, stretched, cast, extruded, coextruded, and / or may comprise any suitable mixture and / or combination thereof. The polymer film may optionally be crosslinked by any suitable means, such as electron beam (EB) or UV crosslinking, if necessary by the use of suitable additives in the polymer film.
[0073] The definition of polyolefin intended herein is a polymer assembled from a significant percentage, preferably 50% by weight or more, of one or more olefin monomers. A copolymer is a polymer assembled from two or more monomers. The polyolefin film may include, but is not limited to, polyethylene homopolymer, ethylene-α-olefin copolymer, polypropylene-α-olefin copolymer, polypropylene homopolymer, ethylene-vinyl acetate copolymer, ethylene-methacrylic acid copolymer and their salts, ethylene-styrene polymer and / or blends of such polymers.
[0074] The polymeric resins used in the manufacture of the polymeric films of the present invention are generally commercially available in pellet form and may be melt blended or mechanically mixed by well-known methods known in the art using commercially available equipment including tumblers, mixers and / or blenders. The resins may have other additional resins blended with well-known additives such as processing aids and / or colorants. Methods of manufacturing polymeric films are well-known and include techniques in which the film is cast as a thin sheet through a narrow slit die and blown film techniques in which an extruded tube of molten polymer is expanded to a desired cell size and / or film thickness. For example, to manufacture a polymeric film, the resin and additives may be introduced into an extruder where the resin is melt plasticized by heating and then transferred to an extrusion die for formation into a film tube. Extrusion and die temperatures generally depend on the particular resin being processed, with suitable temperature ranges generally known in the art or described in technical bulletins available from the resin manufacturers. Processing temperatures may vary depending on the process parameters selected.
[0075] The polymer film of the present invention may be unoriented (cast film), preferably oriented in at least one direction (uniaxial orientation), and more preferably oriented in two directions (biaxial orientation).
[0076] Orientation of the polymer film of the present invention can be achieved by stretching the polymer film at a temperature above the glass transition temperature (Tg) of its constituent polymers. The resulting oriented polymer film can exhibit significant improvements in tensile and stiffness properties. Orientation can be along one axis, if the polymer film is stretched in only one direction, or biaxially oriented, if the polymer film is stretched in each of two mutually perpendicular directions in the plane of the film. Biaxially oriented polymer films can be balanced or unbalanced, with unbalanced films having a higher degree of orientation in the preferred direction, usually the transverse direction. Traditionally, the longitudinal direction (LD) is the direction in which the film passes through the machine (also known as the machine direction or MD), and the transverse direction (TD) is perpendicular to the MD. Preferred polymer films are oriented in both MD and TD. Orientation of the polymer film can be achieved by any suitable technique. For example, flat polymer films can be oriented by stretching in each of two mutually perpendicular directions simultaneously or sequentially by a tenter, or by a combination of a take-up roll and a tenter. In the cellular process, a polymer film is extruded in the form of a composite tube, which is subsequently quenched, reheated, and then expanded by internal gas pressure to become oriented in the TD, and drawn out at a speed faster than the extrusion speed to become stretched and oriented in the MD.
[0077] The polymer film of the composite film is preferably a self-supporting, biaxially oriented film, optionally a polar polymer or polyolefin. The polymer film may optionally contain slip and / or antiblock additives.
[0078] As used herein, the term "polar polymer" refers to a polymer obtained and / or obtainable from at least one polymer precursor that itself contains a polar moiety, and / or a polymer obtained and / or obtainable when the polymer contains a repeat unit that contains a polar moiety. An example of such a polar moiety is a carbonyloxy moiety. The term polar polymer therefore does not necessarily imply any general properties in the resulting polymer or film produced therefrom. Usefully, polar polymers include polyester polymers and / or polyaryletherketone polymers.
[0079] Examples of polar polymers include polyaryletherketones; polyesters including polyethylene terephthalate (PET), polylactate (PLA), polyhydroxybutyrate (PHB), polyfuranoate (PEF) and / or polyethylene naphthalate (PEN); copolyesters including repeat units for any of the above (or any other polyesters described herein), such as copolyesters including or consisting of terephthalic acid, lactic acid, hydroxybutyric acid, furanoic acid, naphthalic acid and / or aliphatic dicarboxylic acids and diols; such as copolyesters of terephthalic acid, naphthalic acid and / or aliphatic dicarboxylic acids and diols. Further examples of suitable polar polymers are described herein. Polyesters are particularly preferred for forming the free-standing layers of the polymeric films described herein.
[0080] The polymeric film may have a shrinkage of less than 5% in length and / or width when exposed to boiling water for 5 seconds. The polymeric film may be a single layer of polymer with no other layers comprising any polymer (same or different) or layers of metal on the surface opposite the surface carrying the primer and heat seal composition.
[0081] Polyolefins suitable for forming free-standing layers of the polymeric film used in the present invention can include any of the polyolefins described herein that can be formed into a film, either alone (i.e., as a substantially pure polymer) and / or in blends and / or copolymers with other polymers (e.g., any described herein). Preferred polyolefin films are polypropylene (PP) and / or polyethylene (PE), with biaxially oriented polypropylene (BOPP) films being more preferred.
[0082] Polyesters suitable for forming free-standing layers of the polymeric films used in the present invention can include any of the following that can be formed into films, alone and / or in blends and / or copolymers with other polymers (e.g., any other polymer described herein, e.g., polyesters):
[0083] Aliphatic polyester homopolymers, such as polyglycolide or polyglycolic acid (PGA), polylactic acid (PLA), polycaprolactone (PCL), polyhydroxyalkanoates (PHA) and / or polyhydroxybutyrates (PHB).
[0084] Aliphatic polyester copolymers, such as polyethylene adipate (PEA), polybutylene succinate (PBS) and / or poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV).
[0085] Semi-aromatic polyester copolymers, such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN) and / or polyethylene furanoate (PEF).
[0086] Aromatic polyester copolymers, for example polymers obtained and / or obtainable by polycondensation of 4-hydroxybenzoic acid and 6-hydroxynaphthalene-2-carboxylic acid, sold under the trade name Vectran (trademark) by Kuraray.
[0087] Also suitable for use in the present invention are filmable polar polymers such as polyaryletherketones (PAEK), for example polyetheretherketones (PEEK) available from Victrex Plc under the registered trademark Victrex®.
[0088] The polyesters and / or polyaryletherketones suitable for use as the polar polymer film in the present invention may include at least one polymer selected from the group consisting of aliphatic polyester homopolymers (e.g., PGA, PLA, PCL, PHA and / or PHB); aliphatic polyester copolymers (e.g., PEA, PBS and / or PHBV); semi-aromatic polyester copolymers (e.g., PET, PBT, PTT, PEN and / or PEF); aromatic polyester copolymers (e.g., Vectran™), PEEK polymers (e.g., those commercially available under the registered trademark Victrex®), any suitable mixtures, combinations and copolymers thereof.
[0089] Preferred polymers suitable for use as polar polymer films in the present invention include at least one polymer selected from the group consisting of PGA, PLA, PCL, PHA, PHB, PEA, PBS, PHBV, PET, PBT, PTT, PEN, PEF, Vectran®, PEEK, and / or any suitable mixtures, combinations, and copolymers thereof.
[0090] More preferred polyesters suitable for use as the polymeric film in the present invention include at least one polyester selected from the group consisting of PLA, PHB, PET, PEN, PEF, any suitable mixtures, combinations, and copolymers thereof.
[0091] Even more preferred polyesters suitable for use as polymeric films in the present invention include at least one polymer selected from the group consisting of PET, PEN, and PEF.
[0092] The most preferred polyesters suitable for use as the polymeric film in the present invention include at least one polymer selected from the group consisting of PET and PEN.
[0093] For example, polyesters suitable for use as polymeric films in the present invention include at least one PET polymer.
[0094] Primer layer The optional primer layer, if present, may comprise a halo polyvinylidene polymer (e.g., a PVdX polymer, where X is halo), preferably a polyvinylidene chloride polymer (e.g., where X is chloro, i.e., PVdC) and / or an acrylic and / or vinyl polymer (preferably an EVA polymer). Acrylic and / or vinyl polymers useful for inclusion in the primer layer are those described herein for inclusion in the heat seal layer such that the heat seal layer adheres sufficiently to the primer layer to resist delamination. Ethylene-acrylic acid (EAA) and / or ethylene-methacrylic acid (EMA) primers may also be used. Alternatively, a primer layer may not be present if the free-standing layer of the polymer film is a corona-treated polyolefin film, thus sufficiently activated in its surface so that the heat sealable composition can be applied directly to the unprimed polyolefin film and strongly adhere thereto.
[0095] The primer composition may be applied to the free-standing layer of the polymeric film used in preparing the composite film of the present invention, the primer composition comprising a suitable amount of halopolyvinylidene, acrylic and / or vinyl resin. Thus, the optional primer layer may also comprise any suitable proportion or amount of any halopolyvinylidene polymer, acrylic and / or vinyl resin in any suitable mixture thereof.
[0096] The total amount of acrylic and / or vinyl resin that may be present in the primer layer may be the same as that described herein for the acrylic and / or vinyl resin present in the heat seal layer, with the remainder of the primer layer being the PVdX component. Preferably, the primer layer comprises, more preferably consists of, a halopolyvinylidene polymer (e.g., a PVdC polymer), an acrylic and / or vinyl resin (e.g., EVA), even more preferably PVdC and / or EVA, and most preferably PVdC.
[0097] When the primer composition comprises an acrylic resin and / or a vinyl resin, the amounts of these components (expressed as percentages by weight relative to the total weight of the primer composition or layer being 100%) may correspond to the total weight of the acrylic resin and / or vinyl resin given by weight herein for the amount present in the heat seal composition or layer, although it will be understood that the amount of acrylic resin and / or vinyl resin that may be present in each of the primer layer and / or heat seal layer is calculated separately and independently.
[0098] Coating (Heat Seal and / or Primer) Compositions and Methods The above components may be applied to a polymeric film, such as a polyester substrate, from a solution in an organic solvent or a mixture thereof. Any conventional coating method may be used to apply the coating composition, such as spray coating, roll coating, slot coating, meniscus coating, dip coating, wire bar coating, air knife coating, curtain coating, doctor knife coating, direct and reverse gravure coating, etc. The coating is then dried.
[0099] Yet another aspect of the present invention provides a packaging article that is a cap for a packaging article, lined with a composite film of the present invention as described herein.
[0100] Yet another aspect of the present invention provides a filled packaging article sealed with a cap of the present invention as described herein.
[0101] Yet another aspect of the present invention is a method for filling a packaging article with a food product or a liquid for human and / or animal consumption, comprising the steps of: a) filling the article with a foodstuff or liquid suitable for human and / or animal consumption; b) applying a cap of the present invention to the filled article to reversibly seal the article; The present invention provides a method comprising:
[0102] Unless the context clearly indicates otherwise, as used herein, plural forms of the terms herein are to be construed as including the singular and vice versa.
[0103] The term "comprising", as used herein, is understood to mean that the list which follows is not exhaustive but may or may not include any other additional suitable items as appropriate, such as one or more further features, components, ingredients and / or substituents.
[0104] The terms "consisting," "consisting of," and / or "is," as used herein, are understood to mean that the list that follows is substantially exhaustive, and thus includes the recited components generally as its major components, and thus may, for example, exclude other additional items.
[0105] "Major component" (or its synonyms), as used herein, is understood to mean the proportion where any additional elements or additives present have no substantial effect on the properties of the component, and thus the major component may be present in an amount of at least 50%, preferably at least 60%, more preferably at least 70%, most preferably at least 80%, especially at least 90%, and especially about 99% of the relevant total.
[0106] The terms "effective", "acceptable", "active" and / or "suitable" (e.g., with respect to any process, use, method, application, preparation, product, material, formulation, compound, monomer, oligomer, polymer precursor, and / or polymer of the present invention and / or as appropriate described herein) are understood to refer to features of the present invention and / or features used for the present invention, which, when used in the correct manner, provide the necessary properties to render what they are added to and / or introduced into a utility as described herein. Such utility can be direct, for example, if the material has the properties required for said use, and / or indirect, for example, if the material has use as a synthetic intermediate and / or diagnostic tool in preparing other materials that have a direct utility. As used herein, these terms also refer to the compatibility of a functional group with the production of an effective, acceptable, active and / or suitable end product.
[0107] Preferred utilities of the present invention include one or more of the use of the film as a heat-sealable component (e.g., a lid) of a packaging article, such as an ovenable tray for food, and / or as a liner for a cap for the packaging article.
[0108] In the discussion of the invention herein, unless otherwise indicated, when alternative values for the upper and lower limits of a parameter's acceptable range are disclosed with the indication that one of said values is more preferred than the other, this should be construed as a statement that implies that each intermediate value of said parameter between the more preferred and less preferred alternative values is itself preferred over the less preferred value and is also preferred over each less preferred value and the intermediate value.
[0109] For all upper and / or lower bounds of any parameter given herein, the bounds are included in the values for each parameter. It should also be understood that all combinations of preferred and / or intermediate minimum and maximum bounds of parameters described herein in various embodiments of the invention may also be used to define alternative ranges for each parameter with respect to various other embodiments and / or preferences of the invention, whether or not such value combinations are specifically disclosed herein.
[0110] Thus, for example, a substance described herein as being present in an amount of 0 to "x" (e.g., in units of mass and / or mass %) is meant to encompass both of two options (unless the context clearly indicates otherwise): first, the broader option that the substance may optionally be absent (where the amount is zero) or present in a very small amount below detectable amounts. The second preferred option (represented by a small amount of zero in the range for the amount of the substance) indicates that the substance is present, with zero indicating that the small amount is a very small amount, e.g., any amount sufficient to be detected by suitable conventional analytical techniques, and more preferably, zero indicating that the lower limit of the amount of the substance is 0.001 mass % (calculated as described herein) or greater.
[0111] Of course, the total of any amount expressed as a percentage herein cannot exceed 100% (even allowing for rounding errors). For example, the sum of all components that make up the composition (or a portion thereof) of the present invention, when expressed as a mass (or other) percentage of the composition (or the same portion thereof), may total 100%, allowing for rounding errors. However, if the list of components is not exhaustive, the total of the percentages for each of these components may be less than 100%, allowing for some percentage of the additional amount of any additional component not specified herein.
[0112] The term "substantially" as used herein refers to an amount or entity and may mean that it is a large amount or a majority. "Substantially", when relevant in the context in which it is used, can be understood to mean that it quantitatively (with respect to any amount or entity to which it refers in the context of the description) constitutes at least 80%, preferably at least 85%, more preferably at least 90%, most preferably at least 95%, especially at least 98%, for example about 100% of the relevant total. By analogy, the term "substantially free" can similarly denote that the amount or entity to which it refers constitutes 20% or less, preferably 15% or less, more preferably 10% or less, most preferably 5% or less, especially 2% or less, for example about 0%, of the relevant total.
[0113] The terms "optional substituents" and / or "optionally substituted", as used herein (unless followed by a list of other substituents), refer to one or more of the following groups (or substitution with these groups): carboxy, sulfo, formyl, hydroxy, haloamino, imino, nitrilo, mercapto, cyano, nitro, methyl, methoxy, and / or combinations thereof. These optional groups include all chemically possible combinations of more than one (preferably two) of the aforementioned groups on the same moiety (e.g., amino and sulfonyl, when directly bonded to each other, represent a sulfamoyl group). Preferred optional substituents include carboxy, sulfo, hydroxy, amino, mercapto, cyano, methyl, chloro, fluoro, trihalomethyl, and / or methoxy.
[0114] As used herein, the synonyms "organic substituent" and "organic group" (also abbreviated herein as "organo") refer to any monovalent or polyvalent moiety containing one or more carbon atoms and, optionally, one or more other heteroatoms (optionally bonded to one or more other moieties). Organic groups may also include organoheteryl groups (also known as organoelement groups) that contain a monovalent group containing carbon, and thus are organic, but have a free valence at an atom other than carbon (e.g., organothio groups). Organic groups may alternatively or additionally include organyl groups that contain any organic substituent having one free valence at a carbon atom, regardless of the type of functional group. Organic groups may also include heterocyclyl groups that contain a monovalent group formed by removing a hydrogen atom from any ring atom of a heterocyclic compound (a cyclic compound having atoms of at least two different elements as ring members, in this case one being carbon). Preferably, the non-carbon atoms in the organic group may be selected from hydrogen, halo, phosphorus, nitrogen, oxygen, silicon and / or sulfur, more preferably from hydrogen, nitrogen, oxygen, phosphorus and / or sulfur.
[0115] The most preferred organic groups include one or more of the following carbon-containing moieties: alkyl, alkoxy, alkanoyl, carboxy, carbonyl, formyl, and / or combinations thereof, optionally in combination with one or more of the following heteroatom-containing moieties: oxy, thio, sulfinyl, sulfonyl, amino, imino, nitrilo, and / or combinations thereof. The organic groups include all chemically possible combinations of multiple (preferably two) of the aforementioned carbon-containing and / or heteroatom moieties in the same moiety (e.g., alkoxy and carbonyl, when directly bonded to each other, represent an alkoxycarbonyl group).
[0116] The term "hydrocarbolite" as used herein is a subset of organic radicals and represents any monovalent or polyvalent moiety (optionally bonded to one or more other moieties) consisting of one or more hydrogen atoms and one or more carbon atoms, and may include one or more saturated, unsaturated and / or aromatic moieties. Hydrocarbolite may include one or more of the following groups: Hydrocarbyl groups include monovalent groups formed by removing a hydrogen atom from a hydrocarbon (e.g., alkyl). Hydrocarbylene groups include divalent groups formed by removing two hydrogen atoms from a hydrocarbon, the free valence of which is not involved in a double bond (e.g., alkylene). Hydrocarbylidene groups include divalent groups (which may be represented as "RC=") formed by removing two hydrogen atoms from the same carbon atom of a hydrocarbon, the free valence of which is involved in a double bond (e.g., alkylidene). Hydrocarbylidine groups include trivalent groups (which can be represented as "RC≡") formed by removing three hydrogen atoms from the same carbon atom of a hydrocarbon, the free valence of which participates in a triple bond (e.g., alkylidynes). Hydrocarbyl groups may also include saturated carbon-carbon single bonds (e.g., in alkyl groups); unsaturated double and / or triple carbon-carbon bonds (e.g., in alkenyl and alkynyl groups, respectively); aromatic groups (e.g., in aryl groups) and / or combinations thereof in the same moiety, which may be substituted with other functional groups, if specified.
[0117] The term "alkyl" or its equivalents (e.g., "alk") as used herein may be readily replaced, where appropriate, unless the context clearly indicates otherwise, by any other hydrocarbyl-inclusive term, such as those described herein, including double bonds, triple bonds, aromatic moieties (e.g., alkenyl, alkynyl, and / or aryl, respectively), and / or combinations thereof (e.g., aralkyl), and any polyvalent hydrocarbyl species linking two or more moieties (e.g., a divalent hydrocarbylene radical, e.g., alkylene).
[0118] Any radical, substituent, group or moiety referred to herein may be a polyvalent or monovalent species, but is preferably a monovalent species (e.g., a divalent hydrocarbylene moiety (e.g., alkylene moiety) linking two other moieties), unless otherwise stated or the context clearly indicates otherwise. However, such monovalent or polyvalent species may still include optional substituents, where specified herein. A group containing a chain of three or more atoms means that the chain may be wholly or partially linear, branched, and / or may form rings (including spiro and / or fused rings). Certain total numbers of atoms are specified for certain substituents, e.g., C 1~N Organo means an organo moiety containing 1 to N carbon atoms. In any of the formulas herein, if one or more substituents are not shown as attached to any particular atom in a moiety (e.g., at a particular position along a chain and / or ring), the substituents may replace any H and / or be located at any available position of the moiety that is chemically suitable and / or effective.
[0119] Preferably, any organo group recited herein contains 1 to 36 carbon atoms, more preferably 1 to 18. Even more preferably, the number of carbon atoms in the organo group is 1 to 12, most preferably 1 to 10, even most preferably 1 to 6, for example 1 to 4 carbon atoms.
[0120] As used herein, chemical terms (other than the IUAPC name of a specifically identified compound) that include features set forth in parentheses, e.g., (alkyl)acrylate, (meth)acrylate and / or (co)polymer, represent that the moieties within the parentheses are optional, as the context indicates, so that, for example, the term (meth)acrylate represents both methacrylate and acrylate.
[0121] The substituents on the repeat units of the polymers and / or oligomers may be selected to improve compatibility with the polymers and / or resins into which they may be formulated and / or incorporated for use as described herein, and thus the size and length of the substituents may be selected to optimize physical entanglement or mutual arrangement with the resin, which may or may not include other reactive materials capable of chemical reaction and / or crosslinking with such other resins, as appropriate.
[0122] Certain moieties, species, groups, repeat units, compounds, oligomers, polymers, materials, mixtures, compositions and / or formulations constituting and / or used in any or all of the present invention as described herein may exist in one or more different forms (e.g., isomers and / or physical forms), including any of the following non-exhaustive list: Stereoisomers (e.g., enantiomers (e.g., E and / or Z), diastereoisomers and / or geometric isomers); tautomers (e.g., keto and / or enol forms), conformers, salts, zwitterions, complexes (e.g., chelates, clathrates, crown compounds, cryptands / cryptates, inclusion compounds, intercalation compounds, ligand complexes, organometallic complexes, non-stoichiometric complexes, π-adducts, solvates and / or hydrates); isotopic substitution forms, macromolecular architectures [e.g., homo- or copolymers, random, graft and / or block polymers, linear and / or branched polymers (e.g., star and / or side-chain branched), multibranched polymers (e.g., WO 93 / 17060), crosslinked and / or networked polymers, polymers obtainable from divalent and / or trivalent repeating units, dendritic macromolecules (e.g. dendrimers), polymers with different stereoregularities (e.g. isotactic, syndiotactic or atactic polymers)]; polymorphs (e.g. interstitial, crystalline and / or amorphous forms), heterophases, solid solutions; and / or combinations and / or mixtures thereof, where possible. The present invention includes and / or uses all such forms that are effective (e.g. as defined herein).
[0123] Other conventional terms from polymer science (e.g., polymer, monomer, oligomer, etc.) used herein have the meanings as recommended by IUPAC and defined in Pure Appl. Chem., Vol. 68, No. 12, pp. 2287-2311, 1996, the contents of which are incorporated herein by reference. The terms "resin" and "polymer" are used interchangeably herein unless the context clearly indicates otherwise, so that, for example, the terms acrylic resin and vinyl resin also refer to acrylic polymer and vinyl polymer, respectively, and vice versa.
[0124] The formulas herein may represent polymer mixtures or a series of individual compounds. When the formulas herein represent species (e.g., compounds) that are monodisperse, the values of any numerical variables shown therein (e.g., "n" representing the number of repeat units, etc.) are independently integers within a particular range (or zero, where the context permits). When the formulas represent the average structure of multiple individual species present in a polydisperse oligomer and / or polymer mixture, the values of any variables shown in the formula may be real, non-integer numbers having a particular range.
[0125] It will be understood that certain features of the invention, which are, for clarity, described in the context of separate embodiments, can also be implemented in combination in a single embodiment. Conversely, various features of the invention, which are, for brevity, described in the context of a single embodiment, can also be implemented separately or in any suitable subcombination. Many other variations of the invention will be apparent to those skilled in the art, and such variations are intended to be included within the broad scope of the invention.
[0126] Further aspects of the invention and preferred features thereof are set out in the claims hereinafter. EXAMPLES
[0127] The present invention will now be described in detail with reference to the following non-limiting examples, which are provided to further illustrate the process and composition of the present invention. These examples are merely illustrative and are not intended to limit the scope of the present invention in any way. Unless otherwise specified, all parts, percentages, and ratios are by weight. The prefix C or COMP before an example indicates that it is a comparative example and does not form part of the present invention.
[0128] Various trademarks, other names and / or abbreviations are used herein to represent some of the raw materials used in the preparation of the polymers and compositions of the present invention. These are identified below by chemical name and / or trade name, and optionally by the manufacturer or supplier who markets them. However, if the chemical name and / or supplier of a material described herein is not given, it can be readily found, for example, in references well known to those skilled in the art.
[0129] Unless otherwise indicated, all composition percentages and ratios described herein are by weight and all coating weights refer to the weight of the dried coating. The following raw materials are further referenced in the examples discussed below.
[0130] Affinity™ GA1950 polymer is an ethylene-octylene triolefin elastomer available from Dow and is produced by metallocene catalyzed polymerization.
[0131] Elvax® 3180 resin is an EVA containing 28% vinyl acetate and 72% ethylene units and is available from DuPont.
[0132] Elvax® 3185 resin is an EVA containing 32% vinyl acetate and 68% ethylene units and is available from DuPont.
[0133] Elvax® 4260 resin is an EVA containing 28% vinyl acetate, 71% ethylene and approximately 1% methacrylic acid units and is available from DuPont.
[0134] Engage™ 8200 polyolefin elastomer is an ethylene-octene copolymer available from Dow and is produced by metallocene catalyzed solution polymerization.
[0135] Exact™ plastomers are ethylene-alpha olefin copolymers available from ExxonMobil and are produced by metallocene catalyzed polymerization.
[0136] Kemamide® EZ is a fatty amide (erucamide) slip agent available from Chemtura.
[0137] Pentalyn® H tackifying resin has a Ring and Ball softening point of 94-102° C. and is available from Pinova Solutions.
[0138] Piccolyte® A115, C115, and F115 tackifying resins have Ring and Ball softening points of 112-118° C. and are available from Pinova Solutions.
[0139] Queo™ 7007LA polymer is an ethylene-based octene-1 plastomer with a melting point of 62° C., produced by metallocene catalyzed solution polymerization and available from Borealis.
[0140] Queo™ 8201 polymer is an ethylene-based octene-1 plastomer produced by metallocene catalyzed solution polymerization and is available from Borealis.
[0141] Syloid® 620 mattifying agent is an amorphous synthetic silica available from Grace.
[0142] Vistamaxx™ 5102 polymer is composed primarily of isotactic propylene repeat units with random ethylene distribution, is available from ExxonMobil, and is produced by metallocene catalyzed polymerization.
[0143] Vistamaxx™ 6202 polymer is an ethylene-propylene elastomer available from ExxonMobil and is produced by metallocene catalyzed polymerization.
[0144] The heat seal strength (also referred to herein as peel strength) of the coatings to high density polyethylene (HDPE) or polypropylene (PP) was evaluated as follows: The coated polymeric films, i.e., composite films, were sealed to HDPE or PP using a Sentinel heat sealer (Model 12 by Packaging Industries Group Inc.). Unless otherwise stated, the heat sealer parameters were 350°F (upper jaw), 100°F (lower jaw) / 1 sec / 80 psi. Even when the upper jaw was at a different temperature, the lower jaw was still at about 100°F with minor variations. The sealed samples were marked and cut into 25 mm wide strips and the heat seal strength was determined by a peel strength test on an INSTRON® Model 4464 testing machine. The jaws were set at 50 mm intervals. The upper jaw gripped the sealed sample film strip and rose at a rate of 250 mm / min, while the lower jaw gripped the sealed sample HDPE or PP strip and remained stationary. The average force required to separate the two pieces of film was recorded. Five sealed sample strips were measured for each coated sample.
[0145] In the examples herein, when an example is described as being repeated and / or prepared in the same manner as another example described herein, it is prepared in the same manner, using the same ingredients in the same amounts as used in the preceding example, unless otherwise indicated.
[0146] Example C1 and Examples 2, 3 and 4 (Example C1) (Comparative Example, Heat Seal Composition Not Containing POP Resin) This heat seal composition did not contain POP resin.A heat seal coating solution was prepared by dissolving Elvax® 3180 (9.0 g, DuPont, 28% vinyl acetate by weight of the heat seal composition, approximately 60 wt% EVA resin), Piccolyte® C115 tackifier resin (5.4 g, Pinova, approximately 36 wt% tackifier resin by weight of the heat seal composition), Syloid 620 (0.375 g, Grace, approximately 2.5 wt% matte feel agent by weight of the heat seal composition) and Kemamide® EZ (0.225 g, Chemtura, approximately 1.5 wt% slip agent by weight of the heat seal composition) in 100 ml toluene at 65°C. The heat seal coating solution was coated onto 23 μm (micron) PET polymer film primed with Elvax® 4260 EVA resin using a Mayer coating rod (coating weight, 5.5 g / m 2 The coated film, i.e., the composite film, was dried for 2 minutes in a forced air oven preset at 115°C. The composite film was sealed to HDPE and PP substrates [300°F (about 149°C) / 1 second] with seal strengths of 892 gf / in (about 344 N / m) (HDPE) and 615 gf / in (about 237 N / m) (PP).
[0147] Example 2 (6wt% POP) Comparative Example C1 was repeated, except that a composite film of the invention was prepared by replacing 0.9 g of Elvax® 3180 resin with Queo™ 7007LA polymer. The amounts of other raw materials were unchanged, so that the heat seal composition of Example 2 contained 8.1 g (about 54 wt%) EVA resin and 0.9 g POP resin (about 6 wt%). The resulting composite film was tested as described in Example C1 and had a seal strength of 1105 gf / in (about 427 N / m) (HDPE) and 756 gf / in (about 292 N / m) (PP).
[0148] Example 3 (30wt% POP) Comparative Example 1 was repeated, except that a composite film of the invention was prepared by replacing 4.5 g of Elvax® 3180 resin with Queo™ 7007LA polymer. The amounts of other raw materials were unchanged, so that the heat seal composition of Example 3 contained 4.5 g (about 30 wt%) of EVA resin and 4.5 g of POP resin (about 30 wt%). The resulting composite film was tested as described in Example C1 and had a seal strength of 1447 gf / in (about 559 N / m) (HDPE) and 761 gf / in (about 294 N / m) (PP).
[0149] Example 4 (60wt% POP) Comparative Example 1 was repeated, except that a composite film of the invention was prepared by completely replacing 9.0 g of Elvax® 3180 resin with the same amount of Queo™ 7007LA polymer. The amounts of other raw materials were not changed, so that the heat seal composition of Example 3 contained no EVA resin and 9.0 g of POP resin (about 60 wt%). The resulting composite film was tested as described in Example C1 and had a seal strength of 1415 gf / in (about 546 N / m) (HDPE) and 743 gf / in (about 287 N / m) (PP).
[0150] Example C5 and Examples 6, 7 and 8 Heat Seal Coating of Example 3 (Elvax® 3180 / Queo™ 7007LA / Piccolyte®) Effect of primer on PET (Example C5) (Comparative Example - Non-primed PET polymer film) The PET polymer film of Example C1 was not primed (nor corona treated) and was used to provide a comparative example. The coating weight on the unprimed PET polymer film was 6.5 g / m 2Example 3 was repeated, except that the seal strength was 744 gf / in (about 287 N / m) (HDPE) and 775 gf / in (about 299 N / m) (PP). After sample testing, a significant amount of the heat seal coating remained on the HDPE and PP, indicating poor adhesion between the heat seal coating on the non-corona treated PET film and the PET polymer film without the primer layer.
[0151] Example 6 (PET polymer film treated with PVdC primer) Example C5 was repeated, except the PET polymer film was primed with PVdC. The seal strength was 1454 gf / in (about 561 N / m) (HDPE) and 815 gf / in (about 315 N / m) (PP).
[0152] Example 7 (PET polymer film treated with EVA primer) Example 5 was repeated, except that a PET polymer film primed with Elvax® 4260 EVA resin was used. The seal strengths were 1564 gf / in (approximately 604 N / m) (HDPE) and 791 gf / in (approximately 305 N / m) (PP).
[0153] Example 8 (PET polymer film treated with EAA primer) Example 5 was repeated, except that an EAA-primed PET polymer film was used. The seal strengths were 712 gf / in (about 275 N / m) (HDPE) and 894 gf / in (about 345 N / m) (PP). The clean peeling of the composite film from the HDPE indicates that the heat-sealable topcoat is particularly effective at adhering to the EAA-primed PET polymer film and therefore resists delamination when the composite film is peeled from the HDPE surface.
[0154] Other POP and EVA resins (Examples 9-16) Example 9 Elvax® 3185 (2.7 g, DuPont, 32% by weight vinyl acetate, approximately 18% by weight EVA resin of the heat seal composition), Elvax® 4260 (2.7 g, DuPont, 28% by weight vinyl acetate, approximately 18% by weight EVA resin of the heat seal composition), Affinity™ GA1950 (3.6 g, DOW Chemical A heat seal coating solution was prepared by dissolving 100 mL of toluene at 65° C. with 100 mL of toluene. The heat seal coating solution was coated onto a 23 μm (micron) PET polymer film primed with Elvax® 4260 EVA resin using a Mayer coating rod (coating weight, 6.5 g / m2). 2 The coated film was dried for 2 minutes in a forced air oven preset at 115°C. The coated film, i.e., composite film, was sealed to HDPE and PP substrates at 300°F (149°C) / 1 sec with seal strengths of 1200 gf / in (HDPE) and 895 gf / in (PP).
[0155] Example 10 Example 9 was repeated, except that a PVdC-primed PET polymer film was used. The seal strength was 1300 gf / in (about 502 N / m) (HDPE) and 847 gf / in (about 327 N / m) (PP).
[0156] Example 11 Example 10 was repeated, except that the Affinity™ GA1950 POP resin was replaced with an equal weight of Vistamaxx™ 6202 (ExxonMobil) (3.6 g, approximately 24 wt% POP resin by weight of the heat seal composition). The seal strength was 1190 g / in (approximately 459 N / m) (PP).
[0157] Example 12 Example 10 was repeated, except that the Affinity™ GA1950 POP resin was replaced with the same weight of Vistamaxx™ 6102 (ExxonMobil) (3.6 g, about 24 wt% POP resin by weight of the heat seal composition). 5.4 g of Piccolyte® C115 tackifier resin was replaced with the same weight of Pentalyn® H tackifier resin (Pinova) (5.4 g, about 36 wt% tackifier resin by weight of the heat seal composition). The seal strength was 1080 gf / in (about 417 N / m) (PP).
[0158] Example 13 Example 9 was repeated, except that the Affinity™ GA1950 POP resin was replaced with an equal weight of Queo™ 8201 POP polymer (3.6 g, approximately 24 wt% POP resin by weight of the heat seal composition). The seal strengths were 1115 gf / in (approximately 430 N / m) (HDPE) and 714 gf / in (approximately 276 N / m) (PP).
[0159] Example 14 Example 10 was repeated, except that the Affinity™ GA1950 POP resin was replaced with an equal weight of Queo™ 7007 LA POP polymer (3.6 g, approximately 24 wt% POP resin by weight of the heat seal composition). The seal strengths were 1230 gf / in (approximately 475 N / m) (HDPE) and 849 gf / in (approximately 337 N / m) (PP).
[0160] Example 15 Example 14 was repeated, except that both Elvax® 3185 and Elvax® 4260 EVA resins were replaced with the same total amount of low VA EVA resin, Elvax® 420 (5.4 g, approximately 36 wt% EVA resin by weight of the heat seal composition). Seal strengths were 1277 gf / in (approximately 493 N / m) (HDPE) and 923 gf / in (approximately 356 N / m) (PP). Elvax® 420 had very good compatibility with Queo™ 7007 LAPOP polymer, as indicated by better film clarity.
[0161] Example 16 The Affinity™ GA1950 POP resin was replaced with an equal weight of Engage™ 8200 POP resin (DOW Chemical Company) (3.6 g, approximately 24 wt% POP resin by weight of the heat seal composition), resulting in a coating weight of 8.5 g / m 2 Example 9 was repeated except that the seal strength was 1480 gf / in (HDPE) and 1039 gf / in (PP).
[0162] FIG. 1 shows the peel strength as a function of the temperature at which a composite film was heat sealed, the composite film being primed with Elvax® 426 CEVA resin and coated with 6.8 g / m of the heat seal composition described in Example 15. 2 A conventional EVA heat seal composition was heat sealed to an HDPE substrate under the same conditions at approximately 12.5 g / m 2 Corresponding results are also shown for a commercial PET film extrusion coated with
[0163] FIG. 2 shows the peel strength results for a trial similar to that illustrated in FIG. 1, but using a polypropylene substrate instead of the HDPE substrate.
[0164] As can be seen in Figures 1 and 2, the use of the heat seal composition according to the present invention resulted in significantly higher peel strengths and the peel strength was more constant with respect to heat seal temperature.
[0165] Effect of Heat Seal Coating Composition on Seal Strength to HDPE (Example 17 and C18, C19 and C20) (Example 17) A heat seal coating solution was prepared by dissolving EVA (6.12 g, Elvax® 4260 resin, DuPont, approximately 25 wt% EVA resin by weight of the heat seal composition), POP (4.50 g, Queo™ 7007LA polymer, approximately 24 wt% POP resin by weight of the heat seal composition), tackifier (6.66 g, Piccolyte® C115, approximately 37 wt% tackifier resin by weight of the heat seal composition) in 100 mL of toluene at 65° C., followed by addition of Kemamide-EZ (0.17 g, approximately 0.9 wt% slip agent by weight of the heat seal composition), Kemamide W20 (0.15 g, approximately 0.8 wt% slip agent by weight of the heat seal composition), and Syloid 620 (0.40 g, approximately 2.2 wt% matte feel agent by weight of the heat seal composition). The heat seal coating solution was coated onto a PVdC primed 23 μm (micron) PET polymer film using a Mayer coating rod (coating weight, 6.5 g / m 2 The coated films were dried in an oven at 115° C. for 2 minutes. The coated films, i.e., composite films, were sealed to HDPE substrates at various temperatures [80 psi (approximately 552 kPa) / 1 second] and the seal strength was measured on an INSTRON® Model 4464 tester.
[0166] (Examples C18, C19 and C20 (Comparative Examples)) Comparative Examples C18-C20 were made similarly to Example 17 using the heat seal compositions shown in Table 1. Table 1 reports the peel strength in g force / inch (peel strength values in parentheses have been converted to N / m). The examples were prepared as follows:
[0167] (Example C18) (Comparative example, lack of tackifier) Example 17 was repeated except that the mass of the same Piccolyte® C115 tackifier resin was reduced to 1.8 g (about 10 wt% tackifier resin by mass of the heat seal composition) and the mass of the same Elvax® 4260 EVA resin was increased to 10.98 g (about 61 wt% EVA resin by mass of the heat seal composition) and the other ingredients (POP resin, slip agent and matte feel agent) remained the same and were present in the same masses. Comparative Example C18 had a much lower amount of tackifier compared to the amount of tackifier used in the heat seal layer that constitutes the composite film of the present invention.
[0168] (Example C19) (Comparative example, no tackifier) Example 17 was repeated except that the Piccolyte® C115 tackifying resin was omitted and the weight of the same Elvax® 4260 EVA resin was increased to 12.78 g (about 71 wt% EVA resin by weight of the heat seal composition), and the other ingredients (POP resin, slip agent, and matte feel agent) remained the same and were present at the same weights. Comparative Example C19 did not have a tackifier, unlike the heat seal layer that comprises the composite film of the present invention.
[0169] (Example C20) (Comparative example, no POP resin) Example 17 was repeated except that the Queo™ 7007 LA POP resin was omitted and the weight of the same Elvax® 4260 EVA resin was increased to 10.62 g (about 59 wt% EVA resin by weight of the heat seal composition), and the other ingredients (tackifying resin, slip agent, and matte feel agent) remained the same and were present in the same weight amounts. Comparative Example C20 did not have a POP resin, unlike the heat seal layer that comprises the composite film of the present invention.
[0170] The differences in properties between these comparative films C18, C19 and C20 and Example 17 can be seen in Table 1.
[0171] [Table 1]
[0172] As can be seen in comparison with Examples C18-20, the composite film of the present invention (Example 17) produced strong heat seals even at low sealing temperatures, and the seal strength was relatively constant over a wide range of sealing temperatures.
[0173] Heat seal compositions using other tackifiers (Examples 21 to 29) Example 21 Example 21 was prepared similarly to Example 17, except that the Piccolyte® C115 tackifier resin was replaced with an equal weight of Piccolyte® A115 (Pinova Solutions, Ring and Ball softening point 112-118°C) (6.66 g, approximately 37 wt% tackifier resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350°F (approximately 177°C) / 80 psi (approximately 552 kPa) / 1 sec was 1412 gf / in (approximately 542 N / m).
[0174] Example 22 Example 22 was prepared similarly to Example 17, except that the Piccolyte® C115 tackifier resin was replaced with an equal weight of Piccolyte® F115 (Pinova Solutions, Ring and Ball softening point 112-118°C) (6.66 g, approximately 37 wt% tackifier resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350°F (approximately 177°C) / 80 psi (approximately 552 kPa) / 1 sec was 1530 gf / in (approximately 591 N / m).
[0175] (Example 23) Example 23 was prepared similarly to Example 17, except that the Piccolyte® C115 tackifier resin was replaced with an equal weight of Piccolyte® C85 (Pinova Solutions, Ring and Ball softening point 82-88° C.) (6.66 g, about 37 wt % tackifier resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350° F. (about 177° C.) / 80 psi (about 552 kPa) / 1 sec was 1389 gf / in (about 536 N / m).
[0176] Example 24 Example 24 was prepared similarly to Example 17, except that the Piccolyte® C115 tackifier resin was replaced with an equal weight of Foral® 105 (Pinova Solutions, Ring and Ball softening point 95-103° C.) (6.66 g, about 37 wt % tackifier resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350° F. (about 177° C.) / 80 psi (about 552 kPa) / 1 sec was 1240 gf / in.
[0177] (Example 25) Example 25 was prepared similarly to Example 17, except that the Piccolyte® C115 tackifier resin was replaced with the same weight of Pentalyn® H (6.66 g, about 37 wt% tackifier resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350° F. (about 177° C.) / 80 psi (about 552 kPa) / 1 sec was 1286 gf / in (about 497 N / m).
[0178] (Example 26) Example 26 was prepared similarly to Example 17, except that 33% of the mass of Piccolyte® C115 was replaced with Foral® 105 (Pinova Solutions, Ring and Ball softening point 95-103°C) (4.44 g, approximately 12.3 wt% tackifying resin by mass of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350°F (approximately 177°C) / 80 psi (approximately 552 kPa) / 1 sec was 1353 gf / in (approximately 522 N / m).
[0179] Example 27 Example 27 was prepared similarly to Example 17, except that Piccolyte® C115 was replaced with Piccotac™ 6095-E (Eastman, Ring and Ball softening point 98° C.) (6.66 g, about 37 wt % tackifying resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350° F. (about 177° C.) / 80 psi (about 552 kPa) / 1 sec was 1290 gf / in.
[0180] (Example 28) Example 28 was prepared similarly to Example 17, except that Piccolyte® C115 was replaced with Regalite™ S1100 (Eastman, Ring and Ball softening point 100° C.) (6.66 g, about 37 wt % tackifying resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350° F. (about 177° C.) / 80 psi (about 552 kPa) / 1 sec was 1238 gf / in.
[0181] (Example 29) Example 29 was prepared similarly to Example 17, except that Piccolyte® C115 was replaced with Foralyn™ 90-FG (Eastman, Ring and Ball softening point 100° C.) (6.66 g, about 37 wt % tackifying resin by weight of the heat seal composition). The peel strength of the heat seal coating sealed to HDPE at 350° F. (about 177° C.) / 80 psi (about 552 kPa) / 1 sec was 1311 gf / in.
[0182] Heat seal compositions with higher tackifier content (Examples 30 and 31) (Example 30) Example 30 was prepared similarly to Example 17, except that the weight ratio of EVA / POP / tackifier was 23 / 23 / 50 (weights of these ingredients were 4.14g, 4.14g, and 9g, respectively, with the weights of other ingredients unchanged). The tackifier content was 50% by weight of the heat seal composition. The peel strength of the heat seal coating sealed to HDPE at 350°F (about 177°C) / 80 psi (about 552 kPa) / 1 sec was 1560 gf / in (about 602 N / m).
[0183] (Example 31) Example 31 was prepared similarly to Example 17, except that the EVA / POP / tackifier ratio was 18 / 18 / 60 (the weights of these ingredients were 3.24g, 3.24g, and 10.8g, respectively, with the weights of the other ingredients unchanged). The tackifier content was 60% by weight of the heat seal composition. The peel strength of the heat seal coating sealed to HDPE at 350°F (177°C) / 80 psi (552 kPa) / 1 sec was 1343 gf / in (519 N / m).
[0184] Film Blocking and Processability Evaluation of Examples 30 and 31 To evaluate film blocking and processability, roll samples were coated on a pilot coater with the high tackifier heat seal compositions of Examples 30 and 31 onto PVdC primed PET. The heat seal coating solution temperature was 50° C., the drying temperature of the coated film was 120° C.; the chill roll temperature was 25° C. Both coated rolls unwound easily without tearing. As seen in Table 2, the static and kinetic coefficient of friction (COF) values were between 0.30 and about 0.50, which is within the typical COF range of commercial film products with good processability.
[0185] [Table 2]
[0186] Comparison of Two Coatings for Heat Sealing to HDPE and PP (Examples 32 and 33) Example 32 The heat seal coating solution of Example 17 was prepared, except that the Elvax® 4260 EVA resin was replaced with the same weight of Elvax® 420 EVA resin (DuPont, 18% vinyl acetate by weight, 6.12 g, approximately 25 wt% EVA resin by weight of the heat seal composition), and the other ingredients were the same and present in the same weight amounts. This solution was coated onto 23 μm PET film primed with Elvax® 4260 EVA resin using a Mayer coating rod (coating weight, 3.5 g / m2). 2 The coated films were dried in an oven for 2 minutes at 115°C.
[0187] (Example 33) Example 32 was repeated, but with a coating weight of 10 g / m 2 It was decided.
[0188] The coated films, i.e., composite films prepared in Examples 32 and 33, were heat sealed to HDPE and PP substrates at various temperatures with 1 second dwell time at 80 psi (approximately 552 kPa) and the seal strength in grams per inch was measured on an INSTRON® Model 4464 tester. The results for HDPE are shown in Table 3 and for PP in Table 4 (showing peel strength values in grams per inch, converted to N / m in parentheses).
[0189] [Table 3]
[0190] [Table 4]
[0191] As can be seen in Examples 32 and 33, composite films containing a heat seal layer containing Elvax® 420 EVA resin with a vinyl acetate content of 18% demonstrated strong peel strength to both HDPE and PP substrates.
[0192] Comparison of Example 17 and Comparative Example C34 - Composite Film Containing an Extrusion Coated Heat Seal Layer Example 17 was compared with a commercial PET film (Comparative Example C34) with an extrusion coated LDPE (low density polyethylene) heat seal layer, and the results are shown in Table 5 (Table 5 shows peel strength values in g / in, converted to N / m in parentheses).
[0193] [Table 5]
[0194] As seen in Table 5, Example 17 achieved a peelable product with consistent peel strength, while the extruded product (Example C34) showed a dramatic increase in seal strength, resulting in shredding of the film during the peel test and / or an unpeelable welded seal.
[0195] Although the invention has been illustrated and described herein with reference to specific embodiments, it is not intended that the invention be limited to the details shown, but rather various modifications may be made thereto within the scope and range of equivalents of the claims without departing from the invention.
Claims
1. a) a free-standing layer of polymer film; b) a primer layer on the polymer film and between the polymer film and the heat seal layer (c), the primer layer comprising a polyvinylidene chloride polymer or comprising an acrylic resin and / or a vinyl resin, the acrylic resin and / or the vinyl resin being selected from the group consisting of C 1~4 Alkyl vinyl acetate resin and C 1~4 A primer layer selected from the group consisting of (meth)acrylic resins; A composite film comprising: the heat seal layer comprising a heat seal composition is disposed on the primer layer; the heat seal composition comprises a polyolefin plastomer (POP) resin, a tackifier, and an acrylic and / or vinyl resin selected from the group of resins consisting of C 1-4 alkyl vinyl acetate resins and C 1-4 (meth)acrylic acid resins; i. the tackifier is present in an amount of at least 36% and no more than 60% by weight of the heat seal composition, where the total weight of the heat seal composition is 100%; ii. the POP resin is present in an amount of at least 15% and not more than 60% by weight of the heat seal composition, where the total weight of the heat seal composition is 100%; iii. the acrylic and / or vinyl resin is present in an amount of at least 15% and no more than 40% by weight of the heat seal composition, where the total weight of the heat seal composition is 100%; Composite film.
2. 2. The composite film of claim 1, wherein the acrylic and / or vinyl resin is selected from the group consisting of ethylene acrylate (EA), ethylene vinyl acetate (EVA), ethylene acrylic acid (EAA) and ethylene methacrylic acid (EMA).
3. The POP resin in the heat seal layer (c) Formula 1: CH 2 =CHR Formula 1 (Wherein, R is H or C 1~10 (It is alkyl) and at least one monomer of Below are I) to V): I. At least one different polymer precursor also represented by formula 1 II. At least one polymer precursor represented by formula 2 C 4-20 α(alpha),ω(omega)-diolefin Formula 2 III. At least one polymer precursor represented by formula 3 C 3-20 α(Alpha)-Olefin Formula 3 IV. At least one polymer precursor represented by formula 4 C ≧18 Diolefins Formula 4, and V. At least one polymer precursor represented by formula 5 C 4~18 Cyclic olefins (including norborene) Formula 5 and at least one other different polymer precursor selected from any one of 3. The composite film according to claim 1 or 2, wherein the resin is selected from the group consisting of a resin obtained or obtainable from
4. 4. The composite film of claim 3, wherein Formula 1 represents an ethylene monomer.
5. The POP resin is at least one C 2~4 4. The composite film of claim 3, comprising a copolymer of an alkylene and at least one polymer precursor of any of formulas 2-5.
6. The POP resin is a copolymer of ethylene and / or propylene and at least one C 5~20 4. The composite film of claim 3 comprising a copolymer with a hydrocarbylene.
7. The POP resin is a copolymer of ethylene and at least one C 6~15 7. The composite film of claim 6, comprising a copolymer with an alkylene.
8. The POP resin is a copolymer of ethylene and at least one C 6~12 8. The composite film of claim 7, comprising a copolymer with an alkylene.
9. The POP resin is a copolymer of ethylene and at least one linear monounsaturated C 6~10 9. The composite film of claim 8, comprising a copolymer with an alkylene.
10. 10. The composite film of claim 9, wherein the POP resin is a copolymer of ethylene and 1-octene.
11. 11. The composite film according to claim 1, wherein the POP resin has a DSC melting point of less than 100°C.
12. The number average molecular weight (M n 12. The composite film according to claim 1, wherein the molecular weight of the polymer is 5,000 to 50,000 Daltons.
13. 13. The composite film according to claim 1, wherein the amount of α-olefin comonomer in the POP resin is 5 to 85 mol %, based on the total amount of the POP resin being 100 mol %.
14. 10. The composite film of claim 1, wherein the polymeric film layers are formed from polar polymers and / or polyolefin polymers.
15. 10. The composite film of claim 1, wherein the polymer film comprises a polyester or a polyolefin.
16. 16. The composite film of claim 15, wherein the polymer film comprises a biaxially oriented polyester film.
17. 2. The composite film of claim 1, wherein the polymer film comprises at least one polymer selected from the group consisting of polypropylene (PP), polyethylene (PE), polyglycolic acid (PGA), polylactic acid (PLA), polycaprolactone (PCL), polyhydroxyalkanoate (PHA), polyhydroxybutyrate (PHB), polyethylene adipate (PEA), polybutylene succinate (PBS), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polyethylene furanoate (PEF), liquid crystal aromatic polyester, polyether ether ketone (PEEK), and / or combinations and copolymers thereof.
18. 10. The composite film of claim 1, wherein the polymer film comprises at least one polyester selected from the group consisting of PLA, PHB, PET, PEN, PEF, combinations and copolymers thereof.
19. 20. The composite film of claim 18, wherein the polyester is selected from the group consisting of PET, PEN, and PEF.
20. 20. The composite film of claim 19, wherein the polyester is selected from the group consisting of PET and PEN.
21. 21. The composite film of claim 20, wherein the polyester is PET.
22. 22. The composite film of claim 1, wherein the polymeric film layer is biaxially oriented.
23. A method for producing the composite film of claim 1, comprising the steps of: i) applying a coating composition comprising the heat seal composition in a solvent to the primer layer overlying the polymeric film; and then ii) evaporating the solvent; Including, The heat seal composition comprises: a polyolefin plastomer (POP) resin present in an amount of at least 15% and not more than 60% by weight of the heat seal composition, where the total weight of the heat seal composition is 100%; a tackifier present in an amount of at least 36% and not more than 60% by weight of the heat seal composition, where the total weight of the heat seal composition is 100%; and an acrylic and / or vinyl resin selected from the group consisting of C 1-4 alkyl vinyl acetate resins and C 1-4 (meth)acrylic resins, and present in an amount of at least 15% and no more than 40% by weight of the heat seal composition, the total weight of the heat seal composition being 100%; A method comprising:
24. 24. The method of making a composite film of claim 23, wherein the polymer film comprises polyester.
25. 24. The method of producing a composite film according to claim 23, wherein the acrylic and / or vinyl resin is selected from the group consisting of ethylene acrylate (EA), ethylene vinyl acetate (EVA), ethylene acrylic acid (EAA) and ethylene methacrylic acid (EMA).
26. 23. A method for adhering a polymeric film to a container or a free-standing film, comprising the step of heat sealing a composite film according to any one of claims 1 to 22 to a surface of the container or the free-standing film.
27. 27. The method of claim 26, wherein the surface is a polyolefin surface.
28. 28. The method of claim 27, wherein the surface is a polypropylene (PP) or high density polyethylene (HDPE) surface.
29. 23. Use of a composite film according to any one of claims 1 to 22 as a heat-sealable component of a packaging article and / or as a liner for a cap for a packaging article.
30. 30. The use of a composite film according to claim 29, wherein the packaging article is an ovenable food container.
31. 23. A packaging article comprising the composite film of any one of claims 1 to 22.
32. 32. The packaging article of claim 31, which is an ovenable food container.
33. A cap for a packaging article lined with a composite film according to any one of claims 1 to 22.
34. 34. A filled package sealed with a cap as defined in claim 33.
35. 1. A method for filling a packaging article with a food product or liquid, comprising the steps of: a. filling the packaging article with the food product or liquid; b. applying the cap of claim 33 to the filled article to reversibly seal the article; A method comprising:
Citation Information
Patent Citations
Heat / low-temperature resistant food container
JP1999165772A
Cap having heat seal lid, and heat seal lid
JP2002205752A
Ethylene / vinyl acetate copolymer composition for heat-sealable and easily openable packaging
JP2007519814A
Laminate for a packaging material and method for manufacturing the same as well as packaging material
JP2014144570A
Process for the preparation of polyolefins
US4542199A