Freshness Preserving Film
A biaxially oriented polypropylene resin film with a propylene random copolymer and polyethylene resin sealing layer, combined with a crystalline polypropylene base layer and zinc oxide deodorant, addresses issues of breakage and sealing strength, ensuring effective freshness preservation for fruits and vegetables.
Patent Information
- Application Number
- JP2021016282
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-02-04
AI Technical Summary
Existing packaging films for fruits and vegetables, particularly bean sprouts, face issues such as breakage and collapse due to excessive force, inadequate sealing strength, and variability in deodorizing and anti-fog properties, leading to spoilage and reduced freshness.
A biaxially oriented polypropylene resin film with a sealing layer composed of propylene random copolymer and polyethylene resin, and a base material layer of crystalline polypropylene resin, incorporating a deodorant nanofiller like zinc oxide, ensuring thinness, flexibility, and effective sealing while maintaining freshness.
The film effectively prevents bean sprouts from breaking, maintains freshness through anti-fogging and deodorizing properties, and ensures sufficient sealing strength, even with a thin design, thus enhancing the preservation of fruits and vegetables.
Smart Images

Figure 0007576992000001 
Figure 0007576992000002
Abstract
Description
[Technical field]
[0001] The present invention belongs to the technical field of biaxially oriented polypropylene-based resin films. The present invention relates to a freshness-preserving film or packaging bag for fruits and vegetables, which is made of such a resin film. The present invention also relates to a package in which fruits and vegetables, particularly bean sprouts, are enclosed in such a packaging bag. [Background technology]
[0002] To maintain freshness and protect fruits and vegetables such as raw vegetables, fruits, potatoes, and mushrooms from damage caused by contact with the outside, fresh produce is packaged in bags made of resin film such as polyethylene film or polypropylene film after harvesting and then distributed. As a device for automatically packaging fresh produce such as raw vegetables by processing the resin film into bags, for example, an automatic vertical pillow packaging machine is used.
[0003] Among fruits and vegetables, bean sprouts are prone to deterioration, so they are packaged in plastic film bags and distributed and sold at low temperatures. Patent Document 1 discloses an invention related to a packaging film that extends the shelf life of bean sprouts and other foods that are prone to deterioration. When packaging bean sprouts and other foods in plastic film bags, the air inside the bag is usually removed. This deaeration suppresses the respiration of the bean sprouts and gives the entire bag a firm feel, improving the bag's handling and displayability. However, when the deaeration bags are put on display in stores, they may contain air and become slightly swollen (deaeration return). Patent Document 2 discloses an invention related to a plastic film that suppresses such deaeration return.
[0004] In addition, since ethylene gas and the like emitted by fruits and vegetables have an adverse effect on freshness retention, gas adsorbents such as activated carbon and zeolite are sometimes enclosed in the resin film bag. However, it is troublesome and time-consuming to encapsulate a gas adsorbent in each of the divided packages. Patent Document 3 solves this problem by incorporating fine particles made of zinc oxide into the thermoplastic transparent resin that forms the packaging material.
[0005] Meanwhile, in addition to simply maintaining the freshness of fruits and vegetables for a long period of time, there has been a recent trend toward thinner plastic films for packaging due to the trend toward resource conservation. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-025524 A (Patent No. 4854881 A) [Patent Document 2] JP 2020-100431 A [Patent Document 3] JP 2003-268242 A Summary of the Invention [Problem to be solved by the invention]
[0007] In vacuum packaging of bean sprouts using an automatic vertical pillow packaging machine, if a thick and stiff film is used, more force than necessary is applied to the bean sprouts, causing the sprouts to break or be crushed, which results in the generation of moisture, which allows bacteria to grow and makes the sprouts more likely to spoil. Therefore, a film with excellent content tracking ability and low stiffness is desired for such vacuum packaging.
[0008] On the other hand, thin and stiff films have excellent content tracking during vacuum packaging, but when packaged using an automatic packaging machine, they do not provide sufficient seal strength at normal packaging speeds. In particular, when a deodorant is added to the sealing layer, the seal strength is further reduced. If the seal strength is not sufficient, the bag may break at the back seal during automatic packaging. Furthermore, anti-fog properties are usually imparted to prevent loss of freshness due to condensation, but if an anti-fog agent is added to a thin film in an amount sufficient to obtain an anti-fog effect, whitening due to bleeding of the anti-fog agent is likely to occur. Furthermore, in order to suppress the odor when opened, deodorizing properties are imparted to the film, but if the film does not adhere sufficiently to the bean sprouts, the deodorizing effect cannot be fully exerted, and there is large variation in the deodorizing properties.
[0009] The main object of the present invention is to provide a new freshness-preserving film or a packaging bag or the like formed from said film that can solve the above-mentioned problems. [Means for solving the problem]
[0010] As a result of extensive research, the inventors have discovered a freshness-preserving film that can solve the above problems, and have completed the present invention.
[0011] The present invention can include, for example, the following. [1] A biaxially oriented polypropylene-based resin film including at least a seal layer and a base layer, the seal layer being mainly composed of a propylene-based random copolymer and a polyethylene-based resin, the base layer being mainly composed of a crystalline polypropylene-based resin having a mesopentad fraction of 95% or more, the total thickness being less than 25 μm, and the seal layer having a primary particle diameter in the range of 10 to 29 nm and a specific surface area of 35 to 60 m. 2 % by weight of a deodorant nanofiller having an oil absorption in the range of 20 to 90 g / 100 g. [2] The freshness-preserving film according to [1] above, wherein the deodorant nanofiller is zinc oxide nanofiller. [3] A freshness-preserving film as described in [1] or [2] above, wherein the loop stiffness of the film is 2.0 mN or less in the MD direction and 4.0 mN or less in the TD direction. [4] A freshness-preserving film according to any one of [1] to [3] above, which is formed into a sealable packaging bag, and when the contents are sealed and the air inside is removed, the film comes into close contact with the contents.
[0012] [5] A packaging bag formed from the freshness-preserving film described in any one of [1] to [4] above. [6] The packaging bag described in [5] above, which is for fresh produce or bean sprouts. [7] A package in which fresh produce or bean sprouts are vacuum-sealed in the packaging bag described in [5] or [6] above. Effect of the Invention
[0013] The freshness-preserving film of the present invention is thin and therefore can contribute to resource saving. When the freshness-preserving film of the present invention is used for degassing packaging, the excellent conformity to the contents makes it difficult for the stems of bean sprouts to break or collapse, and even though it is thin, it can be degassed sufficiently without causing degassing back. Therefore, a better freshness-preserving effect can be expected, and since the film adheres closely to the bean sprouts, it also has an excellent deodorizing effect. In the freshness-preserving film of the present invention, the antifogging agent easily migrates to the sealing layer, so that even a small amount of the antifogging agent can provide an antifogging effect and suppress whitening due to bleeding. Also, deterioration of freshness due to condensation is unlikely to occur. The freshness-preserving film of the present invention is thin and a deodorizing agent is added to the sealing layer, but a packaging bag formed from the freshness-preserving film of the present invention can have sufficient sealing strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The freshness-preserving film of the present invention (hereinafter referred to as the "film of the present invention") is a biaxially oriented polypropylene-based resin film including at least a seal layer and a base layer, the seal layer being mainly composed of a propylene-based random copolymer and a polyethylene-based resin, the base layer being mainly composed of a crystalline polypropylene-based resin having a mesopentad fraction of 95% or more, the total thickness being 25 μm or less, and the seal layer having a primary particle diameter in the range of 10 to 29 nm and a specific surface area of 35 to 60 m. 2 / g and an oil absorption rate of 20 to 90 g / 100 g in the range of 0.3 to 2 wt % of a deodorant nanofiller.
[0015] Here, "mainly composed of" means that other components are permitted to be contained within a range that does not impair the effects of the present invention, and does not limit the content of the components, but generally means that the content of the essential component relative to the total components of the layer accounts for 50% by weight or more. Preferably, the content accounts for 70% by weight or more, and more preferably, the content accounts for 80% by weight or more to 90% by weight or more. The content may be 100% by weight. The present invention will be described in detail below.
[0016] 1. About the film of the present invention The film of the present invention comprises a seal layer and a substrate layer. The "sealing layer" of the film of the present invention is the layer (innermost layer) that becomes the inside of the tube that comes into contact with the contents when the film of the present invention is formed into a cylindrical shape, and the sealing layers are bonded to each other when heat is applied. The "substrate layer" of the film of the present invention is the layer that faces the sealing layer directly or with an intermediate layer in between, and becomes the outside of the tube when the film of the present invention is formed into a cylindrical shape, and is the layer (outermost layer) that comes into contact with the outside world.
[0017] 1.1 Sealing layer 1.1.1 Propylene random copolymer The sealing layer is mainly composed of a propylene-based random copolymer and a polyethylene-based resin. The propylene random copolymer is not particularly limited as long as it is a copolymer of propylene and another α-olefin, and is processed together with a polyethylene resin or the like to form a film layer, and has a sealability that allows the film layers to be bonded together when heat is applied to the layer. Examples of the α-olefin other than propylene include α-olefins having 2 to 20 carbon atoms other than propylene, and specifically include, for example, ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 3-methyl-1-butene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, cyclopentene, cycloheptene, norbornene, 5-ethyl-2-norbornene, tetracyclododecene, 2-ethyl-1,4,5,8-dimethano-1,2,3,4,4a,5,8,8a-octahydronaphthalene, etc. Among these, α-olefins having 2 to 4 carbon atoms, for example, ethylene and butene, are preferred, and ethylene is more preferred. These α-olefins other than propylene may be used alone or in combination of two or more kinds.
[0018] The content of α-olefins other than propylene in the propylene random copolymer is preferably 14% by weight or less, more preferably 10% by weight or less.
[0019] Specific examples of the propylene random copolymer include propylene-ethylene random copolymer, propylene-butene random copolymer, propylene-ethylene-butene random copolymer, etc. Among these, propylene-ethylene-butene random copolymer is preferred.
[0020] Among the propylene random copolymers, those having a melt flow rate (MFR) value in the range of 0.5 to 20 g / 10 min when measured according to ISO1133 (1997) at 230°C and a load of 21.18 N (2.16 kg) are preferred. Also, propylene random copolymers having a melt flow rate value in the range of 2 to 8 g / 10 min are more preferred. The melt flow rate (MFR) value of the polymer can be appropriately adjusted depending on the type and content of α-olefin other than propylene, the molecular weight of the polymer, and the degree of polymerization. Furthermore, the propylene random copolymer has a density of 850 to 950 kg / m when measured in accordance with ISO1183 (1987). 3 Preferably, the range is 860 to 920 kg / m 3 A propylene random copolymer within the range is more preferred.
[0021] 1.1.2 Polyethylene resins The sealing layer contains a polyethylene resin in addition to the propylene random copolymer. The polyethylene resin is a copolymer of ethylene and other α-olefins. Examples of the α-olefins other than ethylene include α-olefins having 3 to 20 carbon atoms, specifically, for example, propylene, 1-butene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, etc. Among them, those having 3 to 8 carbon atoms, such as propylene, 1-hexene, 4-methyl-1-pentene, and 1-octene, are preferred. These α-olefins other than ethylene may be used alone or in combination of two or more.
[0022] The content ratio of ethylene to the other α-olefins in the polyethylene resin is usually 65 to 100 weight % ethylene and 0 to 35 weight % of the other α-olefins, preferably 70 to 99.9 weight % ethylene and 0.1 to 30 weight % of the other α-olefins, more preferably 72 to 99.5 weight % ethylene and 0.5 to 28 weight % of the other α-olefins, and even more preferably 75 to 99 weight % ethylene and 1 to 25 weight % of the other α-olefins.
[0023] Among these polyethylene resins, those having a melt flow rate (MFR) value measured in accordance with ISO1133 (1997) at 190°C under a load of 21.18N (2.16kg) within the range of 0.5 to 20g / 10min are preferred, and those having a melt flow rate value within the range of 2 to 4g / 10min are more preferred. Furthermore, among the polyethylene resins, the density measured according to ISO1183 (1987) is 850 to 900 kg / m 3 Polyethylene resins having a molecular weight of 860 to 890 kg / m are preferred. 3 More preferred is a polyethylene-based resin that is in the range of .
[0024] The content of the propylene-based random copolymer in the resin of the sealing layer varies depending on the specific type of resin, but can be, for example, in the range of 65 to 97% by weight, preferably in the range of 70 to 95% by weight, and more preferably in the range of 72 to 93% by weight. The blending ratio of the propylene-based random copolymer and the polyethylene-based resin in the resin of the sealing layer varies depending on the specific types of resins, but is suitably within a weight ratio range of 1.5 to 10 (propylene-based random copolymer / polyethylene-based resin), preferably within a range of 2 to 8, and more preferably within a range of 2.5 to 5.
[0025] 1.1.3 Deodorant nanofillers The sealing layer further comprises a sintered body having a primary particle size in the range of 10 to 29 nm and a specific surface area of 35 to 60 m 2 The deodorant nanofiller contains one or more types of deodorant nanofillers having an oil absorption in the range of 20 to 90 g / 100 g and an oil absorption in the range of 20 to 90 g / 100 g, in an amount of 0.3 to 2 wt %. The deodorant nanofiller may be, for example, an inorganic one. Specific examples include zirconium phosphate; aluminosilicate (zeolite), zinc aluminosilicate; carbonates such as sodium carbonate, sodium hydrogencarbonate, and calcium carbonate; and metal oxides such as calcium oxide, magnesium oxide, aluminum oxide, zinc oxide, copper oxide, iron oxide, titanium oxide, and alum. In addition, compounds of these compounds and compounds carrying metals such as copper, silver, zinc, and titanium may also be used. Among these, zinc oxide nanofiller is preferred.
[0026] The deodorant nanofiller such as zinc oxide has a primary particle diameter in the range of 10 to 29 nm, preferably in the range of 12 to 28 nm, and more preferably in the range of 15 to 26 nm. The primary particle diameter can be derived, for example, by measuring the specific surface area by a gas adsorption method and theoretically calculating from the measured value. The specific surface area of the deodorant nanofiller, such as zinc oxide, is 35 to 60 m 2 / g, but preferably 40 to 55 m 2 / g, and the oil absorption is in the range of 20 to 90 g / 100 g, preferably in the range of 25 to 85 g / 100 g. Each can be determined by a conventional method. The deodorant nanofiller is contained in the sealing layer in the range of 0.3 to 2% by weight, preferably in the range of 0.5 to 1.5% by weight.
[0027] 1.1.4 Other The sealing layer may contain an antiblocking agent or a lubricant within a range that does not impair the effects of the present invention, in order to make the surface of the resin film smooth and prevent the resin films from adhering to each other. Examples of such antiblocking agents include commonly used inorganic silica, kaolin, zeolite, etc., and organic crosslinked acrylic beads, etc. Examples of lubricants include calcium stearate, etc. These may be used alone or in combination of two or more. The amount of the antiblocking agent and lubricant added can be adjusted appropriately depending on the type of resin, etc., but is suitably 0.05 to 30 parts by weight, and preferably 0.5 to 20 parts by weight, per 100 parts by weight of the resin constituting the layer.
[0028] The sealing layer may contain an appropriate amount of an antibacterial agent or other additives within a range that does not impair the effects of the present invention. Examples of such antibacterial agents include inorganic antibacterial agents such as metal oxides containing silver ions, copper ions, or zinc ions, and organic antibacterial substances.
[0029] 1.2 Base material layer The base layer is 13 It is mainly composed of a crystalline polypropylene resin with a mesopentad fraction of 95% or more as determined by C nuclear magnetic resonance spectroscopy. The crystalline polypropylene resin preferably has a melting point of 155° C. to 165° C. Furthermore, among the crystalline polypropylene resins having a melting point of 155° C. to 165° C., those having a mesopentad fraction in the range of 95% to 99% are more preferable.
[0030] The crystalline polypropylene-based resin is a copolymer of propylene and other α-olefins. Examples of the α-olefins other than propylene include α-olefins having 2 to 10 carbon atoms, specifically, ethylene, 1-butene, 1-pentene, 1-hexene, and other α-olefins. Among these, α-olefins having 2 to 4 carbon atoms, such as ethylene and 1-butene, are preferred, and ethylene is more preferred. These α-olefins other than propylene may be used alone or in combination of two or more. The content of the α-olefins other than propylene is suitably 1.3% by weight or less, and preferably 0.8% by weight or less.
[0031] Among these crystalline polypropylene-based resins, the melt flow rate (MFR) value measured in accordance with ISO1133 (1997) at 230°C and a load of 21.18N (2.16kg) is preferably within the range of 0.5 to 20g / 10min, and more preferably within the range of 2 to 4g / 10min. Furthermore, among the crystalline polypropylene resins, the density measured according to ISO1183 (1987) is 850 to 950 kg / m 3 Preferably, the range is 860 to 920 kg / m 3 A crystalline polypropylene-based resin in the range of is more preferable.
[0032] The content of the crystalline polypropylene resin in the resin of the base layer varies depending on the specific type of resin, but can be, for example, within the range of 90.0 to 99.9% by weight, preferably within the range of 98.0 to 99.6% by weight, and more preferably within the range of 99.0 to 99.5% by weight.
[0033] The base layer may further contain an anti-fogging agent for the purpose of imparting anti-fogging performance to the film. In the present invention, it is preferable to design the base layer so that the anti-fogging agent is blended and migrates (bleeds) to the sealing layer side. Such an anti-fogging agent is not particularly limited as long as it is suitable for the purpose, and anti-fogging agents that have been used in conventional anti-fogging films can be used as they are. Specifically, for example, three types of anti-fogging agents, namely, alkyldiethanolamine, alkyldiethanolamine fatty acid ester, and glycerin fatty acid ester, can be mentioned.
[0034] The alkyl group in the alkyldiethanolamine usually has a carbon number of 8 to 22, and preferably a carbon number of 12 to 18. Specific examples of the alkyldiethanolamine include lauryldiethanolamine, myristyldiethanolamine, palmityldiethanolamine, stearyldiethanolamine, and oleyldiethanolamine.
[0035] The fatty acid ester group in the alkyldiethanolamine fatty acid ester is usually a saturated or unsaturated fatty acid ester having 8 to 22 carbon atoms, preferably 12 to 22 carbon atoms, and preferably the latter unsaturated fatty acid ester. Specific examples of the alkyldiethanolamine fatty acid ester include lauryldiethanolamine monostearate, myristyldiethanolamine monooleate, lauryldiethanolamine monostearate, palmityldiethanolamine monostearate, stearyldiethanolamine monopalmitylate, stearyldiethanolamine monostearate, and oleyldiethanolamine monostearate.
[0036] The fatty acid ester group in the glycerin fatty acid ester can be the same as the fatty acid ester group in the alkyldiethanolamine fatty acid ester. The number of carboxyl groups of the fatty acid that undergoes dehydration condensation with the hydroxyl group of glycerin is preferably 1 or 2, and more preferably 1 fatty acid ester monoglyceride.
[0037] The above anti-fogging agents are used in the form of one kind or a mixture of two or three kinds in the same system, or in the form of a mixture of two or three kinds in a different system. Among them, it is more preferable to use a mixture of three kinds in a different system, that is, a three-component mixture of alkyldiethanolamine, alkyldiethanolamine fatty acid ester, and fatty acid ester monoglyceride, with alkyldiethanolamine fatty acid ester as the main component.
[0038] The amount of the antifogging agent added may be adjusted appropriately depending on the type of the antifogging agent, etc., but is suitably 0.3 to 1.5% by weight, preferably 0.4 to 1.2% by weight, and more preferably 0.5 to 1.0% by weight. If the amount of the antifogging agent added is less than 0.3% by weight, a sufficient antifogging effect may not be obtained, and if it exceeds 1.5% by weight, excessive bleeding out to the surface may occur, resulting in deterioration of transparency.
[0039] 1.3 Other The film of the present invention has at least two layers, the seal layer and the substrate layer, and may have an intermediate layer between the seal layer and the substrate layer.
[0040] The thickness of each layer in the film of the present invention is as follows: The total thickness of the film is within the range of 10 to less than 25 μm, and preferably within the range of 15 to 24 μm. The thickness of the seal layer is, for example, within the range of 1 to 5 μm, and preferably within the range of 1.5 to 4 μm. The thickness of the base layer is, for example, within the range of 7 to 25 μm, and preferably within the range of 15 to 22 μm.
[0041] The film of the present invention may further contain various additives in appropriate amounts, such as nucleating agents, antioxidants, flame retardants, antistatic agents, fillers, pigments, etc., in addition to the additives described above. In addition to the above layers, the film of the present invention may have other layers such as an aperture-imparting layer and a gas barrier layer.
[0042] The film of the present invention preferably has the following physical properties. (1) Loop stiffness <loop crush resistance> The film of the present invention preferably has a strength of 2.0 mN or less in the MD direction (the direction in which the film is formed) and 4.0 mN or less in the TD direction (a direction at an angle of 90 degrees from the direction in which the film is formed). The lower limit values for each direction are, for example, 0.6 mN in the MD direction and 1.4 mN in the TD direction. The loop stiffness can be measured using a commercially available loop stiffness measuring device (for example, LOOP STIFFNESS TESTER (registered trademark) manufactured by Toyo Seiki Seisakusho Co., Ltd.) in accordance with the functions of the measuring device.
[0043] (2) Heat seal strength of the back panel The film of the present invention preferably has a seal strength in the TD direction of 4.0 N / 15 mm or more at 130° C. The upper limit can be, for example, about 10 N / 15 mm. The seal strength can be measured by the following steps: joining two pieces of film, setting the sealing temperature to 130°C, heat-fusing with an appropriate pressure, cutting a sample so that the fusion width is 10 mm in TD direction × 10 mm in MD direction and the sample width is 50 mm in TD direction × 10 mm in MD direction, and spreading the unfused end of the film 180 degrees and peeling it in the TD direction.
[0044] 2. Manufacturing method of the film of the present invention The film of the present invention can be produced by a known production method. However, taking into consideration the productivity and the physical properties of the finished film, it is preferable to produce the film of the present invention by forming a flat sheet by extrusion molding and then sequentially biaxially stretching it.
[0045] More specifically, the resin and components such as the deodorant nanofiller constituting the sealing layer, and the resin and desired components constituting the base layer are respectively fed into each extruder set at an appropriate temperature, and the resin is melted and kneaded in the extruder, and then extruded into a sheet from a T-die at 210°C to 250°C. In this case, a feed block method or a multi-manifold method may be used to form a multi-layer structure of two or three layers. The extruded sheet is cooled and solidified by a cooling roll at 25°C, and sent to a longitudinal stretching process. The longitudinal stretching is performed by a heating roll set at 120°C to 140°C, and is stretched in the longitudinal direction (hereinafter referred to as MD direction) depending on the speed difference between the rolls. There is no particular limit to the number of these heating rolls, but at least two rolls, one on the low speed side and one on the high speed side, are required. The stretching ratio of the longitudinal stretching is 4 to 6 times, preferably 4.5 to 5.5 times. Next, it is sent to a transverse stretching process using a tenter, and stretched in the transverse direction (hereinafter referred to as TD direction). The tenter is divided into preheating, stretching, and annealing zones, with the preheating zone set at 165°C to 175°C, the stretching zone at 165°C to 170°C, and the annealing zone at 165°C to 170°C. The stretching ratio in the stretching zone is preferably about 6 to 10 times. After stretching, the film is cooled and fixed in the annealing zone, and then wound up by a winder to become a film roll.
[0046] In the production of the film of the present invention, it is preferable to carry out a known surface treatment such as corona discharge treatment, flame treatment, ultraviolet irradiation treatment, etc., after leaving the annealing zone of the tenter and before winding up with a winder, and it is particularly preferable to carry out corona discharge treatment from the viewpoint of simplicity. By carrying out the surface treatment, it is possible to impart wetting tension to the surface of the film and enhance the anti-fogging effect, and also to enhance the adhesion to printing ink when printing is carried out on the film surface. This corona discharge treatment may be carried out on both the sealing layer surface and the base layer surface, or on either the sealing layer surface or the base layer surface. In particular, when the sealing layer surface is subjected to corona discharge treatment, the migration of the anti-fogging agent added to the base layer to the sealing layer surface proceeds smoothly, and the effect of the anti-fogging agent can be fully exerted, so that the addition of a small amount of anti-fogging agent is sufficient. The strength of the corona discharge treatment is 1.8×10 2 ~9.0×10 2 J / m 2 In the case of both-side treatment, both sides may have the same strength or different strengths.
[0047] The surface wet tension of the biaxially oriented polypropylene resin film (film of the present invention) thus obtained is preferably 38 to 44 mN / m. If the wet tension is less than 38 mN / m, the antifogging properties are not sufficiently exhibited, and in the case of printing, the adhesion of the printing ink is poor, which is undesirable. If the wet tension exceeds 44 mN / m, the antifogging agent bleeds out to the surface severely, which causes whitening and blocking, and also causes a decrease in the melt-cutting seal strength, which is undesirable.
[0048] 3. Packaging bag and packaging body according to the present invention Next, a packaging bag formed from the film of the present invention (hereinafter referred to as "the bag of the present invention") and a package in which the contents are deaerated and sealed therein (hereinafter referred to as "the package of the present invention") will be described in detail.
[0049] The bag of the present invention or the package of the present invention can be formed by using the film of the present invention with an automatic packaging machine or the like. Examples of the automatic packaging machine include a vertical pillow packaging machine and a horizontal pillow packaging machine, of which the vertical pillow packaging machine or the automatic vertical pillow packaging machine is preferred. Specifically, for example, the film of the present invention is formed into a cylindrical shape with the sealing layer on the inner surface in a former of a vertical pillow packaging machine, the ends of the film are heat-sealed along the machine direction (MD), and then the lower end of the tubular film is heat-sealed in a direction perpendicular to the machine direction (TD), thereby forming the bag of the present invention. Next, a fixed amount of contents is placed into the bag of the present invention, the bag and contents are sandwiched between sponge, the air inside the bag is pushed out to degas it, and then the bag is heat-sealed in a direction (TD) perpendicular to the machine direction (MD) of the film, thereby producing a package of the present invention in which the contents are degassed and sealed inside.
[0050] Contents to be vacuum sealed in the bag of the present invention include, for example, agricultural products such as fruits and vegetables, with fruits and vegetables being preferred. Examples of such fruits and vegetables include vegetables such as green onions, bean sprouts, spinach, broccoli, and green peppers; and cut vegetables such as cabbage, lettuce, and carrots. The bag of the present invention has excellent content conformity, and is therefore preferably used for contents that are prone to breaking or crushing. Contents that are prone to breaking or crushing include some fruits and vegetables, and the bag of the present invention is preferably used for such fruits and vegetables. In particular, the bag of the present invention is preferably used for bean sprouts. EXAMPLES
[0051] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0052] Manufacturing of biaxially oriented polypropylene films The raw materials used are as follows: R-PP: Propylene-ethylene-butene copolymer (MFR: 5.0 g / 10 min, melting point: 125°C, density: 0.9 g / cm 3 ) HPP: Propylene homopolymer (MFR: 2.5g / 10min, melting point: 160℃, density: 0.9g / cm 3 ) PE-1: Ethylene-propylene-1-hexene copolymer (MFR: 3.5 g / 10 min, melting point: 60°C, density: 0.88 g / cm 3 ) PE-2: Ethylene-1-octene copolymer (MFR: 3.0 g / 10 min, melting point: 68°C, density: 0.875 g / cm 3 ) Deodorant 1: Zinc oxide (primary particle size: 20 nm, specific surface area: 50 m 2 / g, oil absorption: 30g / 100g) Deodorant 2: Zinc oxide (primary particle size: 90 nm, specific surface area: 10 m 2 / g, oil absorption: 20g / 100g) Deodorant 3: Zinc oxide (primary particle size: 25 nm, specific surface area: 45 m 2 / g, oil absorption: 84g / 100g)
[0053] A biaxially oriented polypropylene film having a seal layer and a base layer with the composition shown in Table 1 below was produced by the following procedure. The resins and deodorants constituting each layer were fed into the respective extruders, co-extruded from a multi-layer T-die at 230°C, and cooled and solidified with a cooling roll at 25°C to obtain a raw sheet. The sheet was then heated to 130°C and roll-stretched 4.6 times in the MD direction, preheated in a tenter at a set temperature of 165°C, stretched 10 times in the TD direction at a set temperature of 165°C, annealed at a set temperature of 166°C, and after exiting the tenter, the base layer side was stretched to 6.6 x 10 2 J / m 2 The surface layer is 4.8×10 2 J / m 2 After subjecting the film to a corona discharge treatment, the film was wound up on a winding machine to obtain a biaxially oriented polypropylene film (the film of the present invention, etc.).
[0054] The physical properties of the film obtained above were measured as follows.
[0055] <Anti-fog property measurement method> 100mL of 30℃ water was placed in a cup with a diameter of 80mm. A 120mm square sample film was placed over the cup with the measurement surface (seal layer) facing the cup. The film was fixed in place so that there were no gaps between the sample film and the cup. After leaving the film at 5℃ for 30 minutes, the size of the water droplets on the sample film was visually scored, the average score was taken, and any decimal points were rounded off. (N=3) 5 points: The water droplets are large and there is no cloudiness at all. 4 points: The droplets are large, but 20% of the bottom of the glass is not visible. 3 points: 50% of the bottom of the cup is visible, but the other 50% is cloudy and cannot be seen. 2 points: The droplets are small and cloudy, but 20% of the bottom of the glass is visible. Score 1: The droplets are small and cloudy, and the bottom of the glass is completely invisible.
[0056] <Loop stiffness measurement method> A sample (200 mm x 25 mm) was prepared long in the measurement direction, and the compressive strength was measured using a LOOP STIFFNESS TESTER (registered trademark) made by Toyo Seiki Seisakusho Co., Ltd., with an indenter pressing speed of 3.3 mm / sec and an indenter pressing width of 10 mm. The average value was taken as the loop stiffness value (N=3).
[0057] <Heat seal strength measurement method> Two sample films are put together, set to a sealing temperature of 130°C, and heated at a pressure of 0.26 MPa for 0.5 seconds to fuse. A heat sealer HG-100-2 made by Toyo Seiki Seisakusho Co., Ltd. is used for the sealing and fusing. The sample is cut so that the fusion width is 10 mm in the TD direction × 10 mm in the MD direction, and the sample width is 50 mm in the TD direction × 10 mm in the MD direction. The film at one end that is not fused is then spread out 180 degrees, and the heat seal strength is measured by peeling it off at a pulling speed of 200 mm / min in the TD direction at room temperature using a HEIDON (registered trademark) TYPE:17 peel strength tester made by Shinto Scientific Co., Ltd. The results thus obtained are multiplied by 1.5, and the average value is taken as the heat seal strength. (N=5)
[0058] [Table 1]
[0059] As is clear from Table 1, the film of the present invention (Example) had excellent anti-fogging and deodorizing properties on the sealing surface and excellent sealing strength compared to the comparative film (Comparative Example), despite having a smaller total layer thickness. When the raw material of the sealing layer was changed from propylene random copolymer resin and polyethylene resin (Example 1 and Example 5) to propylene homopolymer (Comparative Example 3), the antifogging property and sealing strength of the sealing surface were significantly decreased. Also, as can be seen from the comparison between Example 3 and Comparative Example 2, when the mesopentad fraction was low, the antifogging property and sealing strength of the sealing surface were significantly decreased. Similarly, when the deodorant particles were changed (Example 7 and Comparative Example 1), the sealing strength was significantly decreased.
[0060] [Examples 8 to 14 and Comparative Examples 6 to 10] Production of Packages
[0061] Using the films of the present invention obtained above, packages of the present invention (Examples 8 to 14) corresponding to Examples 1 to 7, respectively, and comparative packages (Comparative Examples 6 to 10) corresponding to Comparative Examples 1 to 5, respectively, were manufactured by the following procedure.
[0062] The film was set in an automatic weighing and packaging machine DT-1080 (manufactured by Taisei Machinery Co., Ltd.) and bags were made. First, a former was used to make a cylindrical (200 mm wide) film with a seal layer on the inside, and the ends of the film were heat-sealed at 130°C along the flow direction (MD), and then the lower end of the heat-sealed cylindrical film was heat-sealed at 140°C in the direction perpendicular to the flow direction (TD), forming a cylindrical film (bag) with the bottom and back heat-sealed and the top open.
[0063] Next, a fixed amount of the contents (bean sprouts, 200 g) was placed into each of the cylindrical films (bags) obtained above. After that, the films were heat-sealed at a temperature of 140°C at intervals of 210 mm in the direction (TD) perpendicular to the machine direction (MD) of the film, and the center of the heat-sealed portion was cut horizontally.
[0064] By the above process, the present invention package and the comparative package (the present invention package, etc.) were formed, which were filled with the contents and had the top and bottom sealed. The heat seal width in this production was 10 mm. The bag size of the produced package was 210 mm in the machine direction (MD) x 195 mm in the width direction (TD).
[0065] The packages of the present invention containing bean sprouts as the contents were stored in a refrigerator set at 10° C. for 4 days, and then the samples were used for the actual package evaluation as follows. The results are shown in Table 2.
[0066] <Evaluation of bean sprouts for breakage and crushing> The percentage of broken or crushed sprouts was visually scored, the average score was taken, and any decimal places were rounded off. 5 points: No bent or crushed bean sprouts in the bag. 4 points: Approximately 20% of the bean sprouts in the bag are broken or crushed. 3 points: Approximately 40% of the sprouts in the bag are broken or crushed. 2 points: Approximately 60% of the bean sprouts in the bag are broken or crushed. 1 point: Approximately 80% of the bean sprouts in the bag are broken or crushed.
[0067] <Degassing return evaluation> The number of bags containing the contents that had experienced air infiltration was investigated. The investigation into deaeration reversion was carried out by visually checking whether air had entered the bag and by touching whether the bean sprouts inside the bag had shifted. It was determined that deaeration reversion had occurred when the bag was inflated or the bean sprouts moved. 〇: Less than 3 bags have swelling or bean sprout movement. (No air return) ×: 3 or more bags have swelling or bean sprout movement. (There is air return due to degassing)
[0068] <Deodorization evaluation> To judge the deodorizing effect, five people each smelled one bag, gave it a score, and then took the average score, rounding off any decimal places. 5 points: No smell of decay at all. 4 points: Upon opening the bag, there is a faint smell of decay. 3 points: There is a smell of decay, but if you leave the bag open for 30 minutes the smell goes away. 2 points: There is a strong smell of decay. If you leave the bag open for an hour, the smell will fade. 1 point: The strong, pungent smell of decay persists even after an hour of opening the bag.
[0069] <Color evaluation> For color evaluation, five people visually evaluated one bag each, scoring the color, then took the average score and rounded off to the nearest whole number. 5 points: Bright green with no brown or black areas. 4 points: The green is slightly dull, and brown or black areas account for about 10% of the total. 3 points: The green is dull and the brown / black parts account for about 30% of the total. 2 points: The green is very dull, and brown or black areas account for about 60% of the total. 1 point: There is almost no green, and brown or black parts account for about 80% of the total.
[0070] [Table 2]
[0071] As shown in the above results (Table 2), the packaging of the present invention was equal to or better than the comparative packaging in all of the live cartridge evaluations. Therefore, it is clear that the film or bag of the present invention is excellent in conformity to the contents, deaeration suitability, and freshness preservation of the contents. [Industrial Applicability]
[0072] The film or bag of the present invention is thin and has excellent conformity to the contents, while having sufficient deodorizing properties and sealing strength. Therefore, the film or bag of the present invention, or the package of the present invention in which the contents such as fruits or vegetables (e.g., bean sprouts) are enclosed, is useful for distribution and sales in the fruit and vegetable market, for example.
Claims
1. A biaxially oriented polypropylene-based resin film including at least a seal layer and a base layer, the seal layer containing 50% by weight or more of a propylene-based random copolymer and a polyethylene-based resin, the base layer containing 50% by weight or more of a crystalline polypropylene-based resin having a mesopentad fraction of 95% or more, the total thickness being less than 25 μm, and the seal layer containing a primary particle diameter in the range of 10 to 29 nm and a specific surface area of 35 to 60 m. 2 A freshness-preserving film comprising a deodorant nanofiller having a molecular weight of 0.3 to 2% by weight and an oil absorption of 20 to 90 g / 100 g.
2. 2. The freshness-keeping film of claim 1, wherein the deodorant nanofiller is a zinc oxide nanofiller.
3. The freshness-preserving film according to claim 1 or 2, wherein the loop stiffness of the film is 2.0 mN or less in the MD direction and 4.0 mN or less in the TD direction.
4. The freshness-preserving film according to any one of claims 1 to 3, which forms a sealable packaging bag, seals the contents, and when the air inside is removed, the film comes into close contact with the contents.
5. A freshness-preserving film described in any one of claims 1 to 4, wherein the base layer contains 0.3 to 1.0 weight % of an anti-fogging agent.
6. A packaging bag formed from the freshness-preserving film according to any one of claims 1 to 5.
7. The packaging bag according to claim 6, which is for fruits and vegetables or for bean sprouts.
8. A package comprising fruit or vegetables or bean sprouts vacuum-sealed in the packaging bag according to claim 6 or 7.
Citation Information
Patent Citations
JP1973054881A
Laminated stretched film
JP2003025524A
Packaging material for preserving freshness of greengrocery
JP2003268242A
Polypropylene stretched film and packaging bag
JP2016215439A
Packaging film for food and package for food
JP2018167487A