Functionalized Rubber
The catalytic addition of nitrene and/or carbene to rubber polymers using a silver-hydrotris(pyrazolyl)borate catalyst addresses the challenge of side reactions in functionalizing rubber, resulting in improved compatibility and maintaining molecular weight distribution for enhanced applications.
Patent Information
- Application Number
- JP2021538131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-28
- Filing Date
- 2019-12-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-12-26
AI Technical Summary
Existing methods for functionalizing rubber polymers, such as styrene-butadiene rubber (SBR) and styrene-ethylene-butylene-styrene (SEBS), often result in undesirable side reactions like chain crosslinking and chain scission, making it difficult to achieve controlled and selective introduction of functional groups for improved compatibility with other materials.
A method involving the catalytic addition of nitrene and/or carbene to rubber polymers using a silver-hydrotris(pyrazolyl)borate catalyst at room temperature, allowing for controlled introduction of functional groups along the polymer chain without side reactions.
This method enables the production of functionalized rubber polymers with improved compatibility and compatibility properties, maintaining the polymer's molecular weight distribution and avoiding undesirable side reactions, thus enhancing their use in various applications.
Smart Images

Figure 0007577062000008 
Figure 0007577062000009 
Figure 0007577062000010
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of functionalized rubbers and methods of preparation. More specifically, the present invention relates to the field of chemical modification of hydrogenated and non-hydrogenated rubbers by metal catalyzed addition of nitrene and / or carbene groups and their use in particular in adhesives, plastic impact modifiers, plastic blend compatibilization, asphalt modification, nanomaterials, and especially in tire compounds. [Background technology]
[0002] Styrene-butadiene synthetic rubbers include polymeric materials derived from styrene and butadiene. These rubbers may contain polymer chains of randomly distributed styrene and butadiene monomers (SBR), but may also be materials containing homopolymers and block copolymers. SBS triblock copolymers consist of a polymer chain of styrene monomer, followed by a polymer chain of butadiene monomer, followed in turn by another polymer chain of styrene monomer. Hydrogenation of the butadiene monomer, i.e., conversion of the diene double bonds to single bonds, results in what is known as SEBS, a block copolymer of styrene-ethylene-butylene-styrene.
[0003] Polymers such as styrene-butadiene or styrene-isoprene triblock or pentablock copolymers containing conjugated dienes and alkenyl aromatic groups are already commercially available and are used in many applications such as adhesives, shoe soles and polymer modification.
[0004] The mechanical behavior of rubber materials determines their industrial applications. For example, the degree of deformation under stress can be important to determine the possible applications of a particular polymeric material. This behavior depends on the physicochemical properties of the polymer, such as composition, molecular weight, and molecular weight distribution. In this sense, the presence of polar groups in the polymer chain is a feature that also influences other polymer properties, such as adhesion and solvent resistance, and is particularly important in polymer blends, as a strategy to improve material performance through interface and morphology modification.
[0005] SBS and SEBS materials are non-polar materials. Therefore, it is often difficult to obtain compatible compositions containing rubber materials with highly engineering plastics, which are usually more polar. Functionalization of polymer substrates with polar groups is a known method that allows modification of their surface energy, mechanical properties, polarity, hydrophilic or hydrophobic, oleophilic or oleophobic, etc. This method can be exploited in applications such as impact modification of engineering plastics, compatibilization of polymer substrates with non-miscible materials such as industrial plastics or silica, adhesives, coatings, compositions suitable for automobile tires, etc.
[0006] However, functionalization of polymer substrates with polar groups remains a challenging task as the process usually leads to undesirable secondary reactions such as chain cross-linking or chain scission reactions.
[0007] There are several methods to obtain functionalized polymers by anionic polymerization. Among them, the methodology of terminating living polymers, especially alkyllithium-initiated living polymers, with electrophiles is probably the most useful. However, this method often leads to incomplete functionalization reactions and by-products (Anionic Polymerization: Principles and Practical Applications”, Hsieh, HL, Quirk, Roderic P., Marcel Dekker Inc, New York, 1996, page 262). Therefore, it is essential to develop better methods to functionalize polymers.
[0008] The use of functionalized initiators in living anionic polymerization is another method to obtain chain-end functionalized polymers. Lithium-containing initiators such as dimethylaminopropyl lithium or (3-(t-butyldimethylsiloxy)propyl) lithium have been disclosed (US Pat. No. 5,552,753; US Pat. No. 6,197,891). The functional groups provided by these types of initiators are not stable under anionic polymerization conditions; therefore, they are protected by other groups, such as alkyl groups, that are stable during polymerization. A final deprotection step is required to obtain functionalized polymers. The obvious drawback of this method is the need to carry out additional protection and deprotection reactions.
[0009] Both the use of functionalized initiators and the termination of living polymers with functional groups allows the incorporation of a limited number of functional groups into each polymer molecule, ie, at its first and / or last termini.
[0010] In this context, the presence of chain-end functional groups can affect the surface and interfacial properties of polymers (Lo Verso, F., Likos, CN, Polymer, 2008, 49, 1425-1434). However, to modify the bulk physical properties of a polymer or to incorporate a higher density of functional groups, it is necessary to incorporate them into repeat units along the polymer chain (intrachain functionalization).
[0011] Few efficient methods for obtaining intrachain functionalized polymers are known so far. Commercially available intrachain functionalized polymers have usually been produced by reactive melt extrusion in the presence of free radical initiators. This method is inefficient because side reactions of chain crosslinking and chain scission frequently occur during the process. Problems arising from the use of radical initiators in the functionalization of polymers include the difficulty in controlling the amount and position of functional groups in the polymer chain, as well as secondary crosslinking and scission reactions that often adversely modify or degrade the polymer backbone.
[0012] Another method to synthesize intrachain functionalized polymers is the use of functionalized monomers in anionic polymerization. The main problem with this approach is the need to first prepare a new monomer for each new functional group. In addition, many important functional groups are not stable to organolithium compounds. Therefore, it is often necessary to protect the functional groups by suitable protecting groups that are stable during the polymerization reaction. This method has the disadvantage that the protecting groups must be removed by a subsequent deprotection reaction. In addition to the above, even when these monomers are functionalized by protected functional groups, they can only be polymerized in a controlled manner to form well-defined polymers, generally at -78 °C in THF (Nakahama, S.; Hirao, A. Prog. Polym. Sci. 1990, 15, 299). In summary, these techniques involving a new monomer for each functional group have two additional steps compared to the general polymerization process; the need to carry out the introduction of protecting groups into the monomers and the deprotection step, and the obvious disadvantages of the prerequisite of low reaction temperature / polar solvent. These conditions are not economically feasible in a commercial process, since in industrial processes anionic polymerizations are generally carried out in hydrocarbon solvents at room temperature or above, and the introduction of costly, time-consuming and inefficient post-polymerization steps is preferably avoided.
[0013] Gonzalez, L. et al. (Rubber Chem Technol, 1996, 69, 266-272) disclose an alternative method of functionalizing SBR for carbon black compatibilization. This method consists of functionalizing the butadiene chains of SBR via nitrene thermal addition of 4-aminobenzenesulfonyl azide. However, this method requires temperatures above 150°C to generate nitrene groups in situ upon azide decomposition. High temperatures lead to the SBR vulcanization process, which increases the crosslink density of the polymer chains. Thus, such thermal functionalization processes are accompanied by the undesirable concomitant effect of increasing the stiffness of the SBR material due to crosslinking side reactions. Moreover, the functionalization level and selectivity of the SBR polymer chains cannot be controlled.
[0014] WO2016 / 170019 discloses a process for functionalizing SBR and polyolefin polymers with monoazides at temperatures between 80 and 250° C. However, this process does not allow selective functionalization of the rubber polymer and requires reactions at high temperatures, which can lead to crosslinking side reactions.
[0015] Thus, there is a need for a rubber functionalization process that improves compatibility with other materials without the drawbacks of undesirable concomitant reactions that affect the rubber chains, such as crosslinking.
[0016] In the work of Beltran A. et al. (Macromolecules, 2012, 45 (23), 9267-9274) the functionalization of SBR rubber with carboxylic acid polar groups at room temperature is disclosed. This reaction is carried out using the copper catalyst hydrotris(3,4,5-tribromopyrazolyl)borate (Tp Br3It consists of the in situ catalytic formation of carbene groups from ethyl diazoacetate in the presence of copper (Cu). Ethyl diazoacetate reacts with the catalyst to produce a metal-carbene species that adds the carbene to the double bond of the butadiene monomer. However, the copper catalyst is very difficult to remove and the resulting rubber becomes unstable over time due to oxidation and side reactions on storage.
[0017] Thus, there is a need in the art for an economical and versatile rubber functionalization process that improves compatibility with other materials without the drawbacks of undesirable concomitant reactions affecting the rubber chains, such as crosslinking or chain scission reactions. Improved rubber compatibility paves the way for blends with polar materials and their industrial use in some compositions. Summary of the Invention
[0018] The authors of the present invention have surprisingly found that addition of nitrenes and / or carbenes to rubber polymer chains is possible, resulting in selective rubber functionalization without secondary reactions such as chain scission or crosslinking. The inventors have further found that the process of the present invention produces rubbers with improved compatibilization properties. These and further advantages are described in detail below and defined by the claims.
[0019] Thus, the present invention provides a general method for the controlled introduction of several functional groups along the polymer chain (intrachain functionalization), in the desired amount, at the desired site or position, and of the desired type, into diene homopolymers and copolymers, and alkenyl aromatic diene copolymers, said homopolymers or copolymers being hydrogenated or non-hydrogenated. Furthermore, according to some variants of the present invention, the polymers may be chain end functionalized.
[0020] Thus, in a first aspect, the present invention provides a compound of formula Tp x reacting a rubber polymer with at least one source of nitrene or carbene in the presence of a catalyst of Ag;x represents a hydrotris(pyrazolyl)borate ligand.
[0021] A second aspect of the present invention relates to a compound comprising at least one group -NH n SO2(C6H4)R 1 Functionalized with R 1 are independent of each other, H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, I, Br, Cl, F, NO2, CF3, OR 3 , COOR 3 , O.C.O.R. 3 Selected from R 3 are independent, H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 aryl, and n is 0 or 1.
[0022] A third aspect of the present invention relates to a rubber polymer obtainable by the process of the present invention.
[0023] The fourth aspect of the present invention relates to the functionalization of rubber polymers using the formula Tp x The use of Ag as a catalyst, Tp x represents a hydrotris(pyrazolyl)borate ligand.
[0024] Finally, a fifth aspect of the present invention relates to the use of the functionalized rubbery polymers of the present invention in asphalt compositions, tire compositions, adhesive compositions, tie layer compositions, sealant compositions, coating compositions, reinforcing compositions, overmold compositions, plastic impact modification, engineering plastic blend compatibilization, fiber and nonwoven compositions, nanomaterials, medical devices, cable compositions, and binders for electrodes of lithium ion secondary batteries. [Brief description of the drawings]
[0025] These and other features and advantages of the present invention will be clearly understood from a consideration of the following detailed description of the invention, which is given by way of example only and is not intended to be limiting, and which refers to the drawings in which:
[0026] [Figure 1] Representative reaction scheme for the functionalization of saturated rubbers such as SEBS. [Diagram 2] Representative reaction scheme for the functionalization of unsaturated rubbers such as SBS and SBR. [Diagram 3] 1H NMR spectrum of a functionalized sample of SEBS with NT groups using naphthalene as the internal standard. [Figure 4] Top: GPC of starting SEBS. Bottom: GPC of NT-functionalized SEBS. [Diagram 5] Notched Charpy impact at 25°C (top) and -30°C (bottom) of three comparative samples and a sample of the invention. [Figure 6] SEM image of comparison sample 2. [Figure 7] SEM image of comparative sample 3. [Figure 8] SEM image of Sample 4 of the present invention. Detailed Description of the Invention
[0027] Unless otherwise defined, all technical and scientific terms and expressions used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.
[0028] Methods of the Invention The first aspect of the present invention is a compound of formula Tp x reacting a rubber polymer with at least one source of nitrene or carbene in the presence of a catalyst of Ag; x It relates to a method for functionalizing rubber polymers, wherein Ag represents a hydrotris(pyrazolyl)borate ligand.
[0029] The reaction of the present invention is a catalytic reaction, and the catalyst Tp xAg can be synthesized from nitrene or carbene sources, respectively, to produce the very short-lived intermediate metal-nitrene Tp x Ag = NR species or metal-carbene Tp x Ag=CR 2 Generate seeds.
[0030] Without wishing to be bound by any particular theory, it is believed that in the process of the present invention, the reaction occurs via C-H insertion of the nitrene or carbene, where the nitrene or carbene may insert into a carbon-to-hydrogen covalent bond of the rubber polymer chain, or via addition of the nitrene or carbene across a double bond to form a three-membered ring.
[0031] "Nitrene or carbene source" is understood as a reactant that leads to the formation of a metal-nitrene or metal-carbene species in the presence of a metal catalyst. A non-limiting example of a nitrene source is PhINSO2(C6H4)R 1 , NaClNSO2(C6H4)R 1 and N3SO2(C6H4)R 1 and R 1 are independent of each other, H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, I, Br, Cl, F, NO2, CF3, OR 3 , COOR 3 , O.C.O.R. 3 and N.R. 3 2 is selected, R 3 are independently H, C 1-6 Alkyl, C 3-7 Cycloalkyl and C 6-10 aryl.
[0032] In a preferred embodiment, the nitrene source is an iminophenyliodonane; preferably, the nitrene source is of the formula PhINSO2(C6H4)R defined above. 1 It is a compound of the formula:
[0033] In one embodiment, R in the nitrene source defined above 1is C 1-6 alkyl; preferably C 1-3 More preferably, R 1 is a methyl group.
[0034] In certain cases, the nitrene source is PhINTs, where Ts represents the -SO2-tolyl group, also known as the tosyl group.
[0035] Non-limiting examples of carbene sources are N2CHCO2R and N2C(R')CO2R, where R is C 1-6 Alkyl, C 3-7 Cycloalkyl and C 6-10 aryl groups. Preferably, R is selected from C 1-6 alkyl; more preferably C 1-3 More preferably, R is an alkyl group; even more preferably, R is ethyl. R' is C 1-6 Alkyl or C6-C 12 It is an aryl group.
[0036] In one embodiment, the hydrotris(pyrazolyl)borate ligand Tp x has the formula [ka] [In the formula, Ra, Rb and Rc are independently H, halogen, C 1-6 Alkyl, C 1-6 Haloalkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, halogen substituted C 6-10 Aryl, and C 1-6 Alkyl-substituted C 6-10 aryl.
[0037] In certain embodiments, Ra, Rb and Rc are independently selected from H, Br, Cl, Me, Et, iPr, tBu, CF3, Cy, Ph and p-Cl-C6H4.
[0038] In certain embodiments, the hydrotris(pyrazolyl)borate ligand Tp x Hydrotris(3,4,5-tribromopyrazolyl)borate (Tp Br3 ), hydrotris(3-phenyl-pyrazolyl)borate (Tp Ph ), hydrotris(3,5-dimethyl-4-bromopyrazolyl)borate (Tp *,Br ), hydrotris(3,5-bis(trifluoromethyl)-4-bromopyrazolyl)borate (Tp (CF3)2,Br ) and hydrotris(3,5-dimethyl-pyrazolyl)borate (Tp * ).
[0039] In certain embodiments, the catalyst in the process of the present invention is a precursor Tp x It is used in the form AgL, where L is a ligand selected from aprotic solvents such as acetonitrile, THF, or acetone. In this case, the L ligand dissociates first, forming the active catalyst Tp x Become Ag.
[0040] The rubber polymer used in the process of the present invention is understood to be either a hydrogenated or non-hydrogenated copolymer comprising a conjugated diene and an alkenyl aromatic monomer, or a diene homopolymer or copolymer comprising a conjugated diene monomer, preferably butadiene. The meaning of non-hydrogenated is well known in the art, but is further clarified herein as a rubber polymer resulting from the copolymerization or homopolymerization of the above monomers and which has not undergone hydrogenation of the diene unsaturation.
[0041] In certain embodiments, the rubber polymer is hydrogenated. In other certain embodiments, the rubber polymer is not hydrogenated.
[0042] According to a particular embodiment, in the case of hydrogenated copolymers, at least 50%, preferably more than 85%, more preferably more than 95% of the original diene unsaturation of the polymer is hydrogenated. According to another particular embodiment, less than 1% of the aromatic units are hydrogenated. The hydrogenation of the rubber polymer can be monitored by various analytical techniques, such as infrared spectroscopy (IR) and nuclear magnetic resonance (NMR).
[0043] Non-limiting examples of alkenyl aromatic monomers that form rubber polymers for use in the process of the present invention include styrene, vinylpyridines (2-vinylpyridine, 4-vinylpyridine, etc.), vinylnaphthalenes (1-vinylnaphthalene, 2-vinylnaphthalene, etc.), 1,2-diphenyl-4-methylhexene, and mixtures thereof. The alkenyl aromatic monomer is preferably C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-15 Aryl and C 1-6 Alkyl(C 6-10 ) aryl.
[0044] Representative examples of substituted alkenyl aromatic monomers include α-methylstyrene, vinyltoluene, 3-methylstyrene, 3,5-diethylstyrene, 2-ethyl-4-benzylstyrene, 4-phenylstyrene, 4-p-tolylstyrene, 4-(tert-butyl)-styrene, 2,4-divinyltoluene, 1-α-methylvinylnaphthalene, 2-α-methylvinylnaphthalene, 4,5-dimethyl-1-vinylnaphthalene, silylated styrenes and mixtures thereof.
[0045] In a preferred embodiment, the alkenyl aromatic monomer is selected from styrene, α-methylstyrene, 3-methylstyrene, 3,5-diethylstyrene, 2-ethyl-4-benzylstyrene, 4-phenylstyrene, 4-p-tolylstyrene, 4-(tert-butyl)-styrene, optionally substituted styrene groups such as silylated styrene, and mixtures thereof. More preferably, the alkenyl aromatic monomer is styrene.
[0046] Non-limiting examples of conjugated diene monomers which form the rubber polymers used in the process of the present invention include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-3-ethyl-1,3-butadiene, 2-methyl-3-ethyl-1,3-pentadiene, 1,3-hexadiene, 2-methyl-1,3-hexadiene, 1,3-heptadiene, 3-methyl-1,3-heptadiene, 4-methyl-1,3-hexadiene, 5-methyl-1,3-hexadiene, 6-methyl-1,3-hexadiene, 7-methyl-1,3-hexadiene, 8-methyl-1,3-hexadiene, 9-methyl-1,3-hexadiene, 10-methyl-1,3-hexadiene, 11-methyl-1,3-hexadiene, 12-methyl-1,3-hexadiene, 13-methyl-1,3-hexadiene, 14-methyl-1,3-hexadiene, 15-methyl-1,3-hexadiene, 16-methyl-1,3-hexadiene, 17-methyl-1,3-hexadiene, 18-methyl-1,3-hexadiene, 19-methyl-1,3-hexadiene, 20-methyl-1,3-hexadiene, 21-methyl-1,3-hexadiene, 22-methyl-1,3-hexadiene, 23-methyl-1,3-hexadiene, 24-methyl-1,3-hexadiene, 25-methyl-1,3-hexadiene, 26-methyl-1,3-hexadiene, 27-methyl-1,3-hexadiene, butadiene, 1,3-octadiene, 3-butyl-1,3-octadiene, 3,4-dimethyl-1,3-hexadiene, 3-n-propyl-1,3-pentadiene, 4,5-diethyl-1,3-octadiene, 2,4-diethyl-1,3-butadiene, 2,3-di-n-propyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, farnesene, myrcene and mixtures thereof.
[0047] In a preferred embodiment, the conjugated diene monomer is selected from 1,3-butadiene or isoprene. More preferably, the conjugated diene monomer is 1,3-butadiene.
[0048] The different monomers forming part of the polymer used in the method of the present invention may be arranged in any monomer sequence (block, tapered or random or a combination thereof).
[0049] The polymers used in the methods of the invention can also be linear or branched. Branched polymers include graft polymers, star polymers, brush copolymers and comb copolymers.
[0050] Preferably, the rubber polymer used in the process of the present invention is a copolymer containing styrene, butadiene or isoprene monomer units, or a diene homopolymer or copolymer containing diene monomer units. More preferably, the rubber polymer used in the process of the present invention is selected from the group consisting of polybutadiene (PBR), polyisoprene, isoprene-butadiene copolymer, styrene-butadiene copolymer (SBR), styrene-isoprene copolymer, styrene-butadiene-styrene triblock copolymer (SBS), styrene-isoprene-butadiene copolymer and styrene-ethylene-butylene-styrene copolymer (SEBS). In a preferred embodiment, the styrene-butadiene copolymer (SBR) is a styrene-butadiene random copolymer or a tapered block copolymer.
[0051] The relative amounts of styrene, butadiene or isoprene monomer units in the rubber polymer can be any suitable amount for purposes of the process of the present invention depending on the particular needs of the final product.
[0052] In certain embodiments, the rubber polymer comprises more than 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10% styrene monomer units based on the total number of monomers in the polymer. In preferred embodiments, the rubber polymer comprises at least 10, 20, 30, 40, 50, 60, 70, 80, 85, or more than 90% styrene monomer units based on the total number of monomers in the polymer.
[0053] In certain embodiments, the rubber polymer comprises more than 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10% butadiene monomer units relative to the total number of monomers in the polymer. In preferred embodiments, the rubber polymer comprises at least 10, 20, 30, 40, 50, 60, 70, 80, 85, or more than 90% butadiene monomer units relative to the total number of monomers in the polymer.
[0054] In certain embodiments, the rubber polymer comprises more than 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10% isoprene monomer units relative to the total number of monomers in the polymer. In preferred embodiments, the rubber polymer comprises at least 10, 20, 30, 40, 50, 60, 70, 80, 85, or more than 90% isoprene monomer units relative to the total number of monomers in the polymer.
[0055] In other specific embodiments, the rubber polymer contains less than 90, 80, 70, 60, 50, 40, 30, 20, or 10% styrene monomer units based on the total number of monomers in the polymer.
[0056] In other specific embodiments, the rubber polymer contains less than 90, 80, 70, 60, 50, 40, 30, 20, or 10% butadiene monomer units based on the total number of monomers in the polymer.
[0057] In other specific embodiments, the rubber polymer contains less than 90, 80, 70, 60, 50, 40, 30, 20, or 10% isoprene monomer units relative to the total number of monomers in the polymer.
[0058] Copolymer rubbers containing a conjugated diene monomer and an alkenyl aromatic monomer typically contain 2% to 50% by weight of an alkenyl aromatic monomer, such as styrene, and 50% to 98% by weight of a conjugated diene monomer, such as 1,3-butadiene.
[0059] The method of the present invention has the surprising advantage of making it possible to produce functionalized rubber polymers without undesirable side reactions such as chain scission, chain crosslinking or oxidation. Thus, the method of the present invention does not change the polydispersity index (PDI) of the rubber polymer. In other words, in the method of the present invention, the PDI of the rubber polymer used is at least 90%, preferably at least 95%, of the PDI of the functionalized rubber polymer obtained. In a preferred embodiment, the PDI of the rubber polymer used is equal to or substantially the same as the PDI of the functionalized rubber polymer obtained.
[0060] Those skilled in the art will readily understand the meaning of PDI (polydispersity index), which is w / M n As a result of the above, w is the weight average molar mass of the molecular weight distribution of the polymer, and M n is the number average molar mass of the molecular weight distribution of a polymer. A homogeneous polymer is composed of molecules of equal mass and therefore has a PDI value of 1, whereas a heterogeneous or dispersed polymer is characterized by a PDI value greater than 1. The higher the PDI value of a polymer, the more dispersed said polymer is.
[0061] In the present disclosure, the weight-average molar mass M w is determined by GPC (gel permeation chromatography). In the present disclosure, the number average molar mass M n is determined in a similar manner.
[0062] In certain embodiments, the methods of the present invention do not use copper, which has the added advantage that the resulting functionalized polymer does not undergo oxidation reactions upon storage.
[0063] In certain embodiments, the method of the present invention effects the functionalization reaction without the need for heating, i.e. the reaction is effected at room temperature without heating. In a preferred embodiment, the method of the present invention is carried out at a temperature of 120°C or less, preferably 90°C or less, preferably 80°C or less, preferably 0-50°C, more preferably 10-40°C, even more preferably 15-35°C.
[0064] In a particular embodiment, the method of the present invention is carried out in a solution. In one embodiment, the reaction is carried out in the presence of an organic solvent, such as hydrocarbon solvents and halogenated hydrocarbon solvents, such as cyclohexane, dichloroethane, dichloromethane, n-hexane, pentane, isooctane, methylcyclohexane, isohexane, n-heptane, n-octane, benzene, toluene, xylene, petroleum ether, and mixtures thereof.
[0065] In the process of the present invention, the molar ratio between the catalyst and the nitrene or carbene source molecule is 1:100 to 1:10, preferably 1:75 to 1:20, more preferably 1:75 to 1:30.
[0066] The amount of nitrene or carbene source can vary depending on the desired rate of functionalization. In certain embodiments, the molar ratio between the nitrene / carbene source and the rubber polymer is 1:100 to 1:3, preferably 1:50 to 1:5, and more preferably 1:30 to 1:5.
[0067] One skilled in the art will readily determine the reaction time necessary for functionalization to occur.
[0068] In certain embodiments, the methods of the invention require a minimum of 1, 5, 10, 30, or 60 minutes, hi other specific embodiments, the methods of the invention require a minimum of 2, 4, 6, 8, 10, 12, 14, 18, 24, or 48 hours.
[0069] In another particular embodiment, the method of the present invention requires an inert atmosphere, examples of which are nitrogen and argon atmospheres.
[0070] In one embodiment, after the reaction is complete, the functionalized rubber polymer is recovered from the organic solvent, for example, by decantation, filtration, centrifugation, and other means known to those skilled in the art. In a particular embodiment of the method of the present invention, the crude functionalized polymer is isolated by the addition of a polar solvent to cause its precipitation. Examples of suitable polar solvents are lower alcohols containing 1 to 4 carbon atoms, such as methanol, ethanol, isopropanol, n-propanol, t-butanol, and mixtures thereof.
[0071] In particular, in the method described herein, there is no need to protect the functional groups to avoid interference with the anionic growing chain during the anionic polymerization process, since the functional groups are introduced in a post-polymerization step. Thus, one of the advantages of the present invention over the prior art, e.g., the use of functional monomers, is the elimination of two typical steps in the functionalization process during anionic polymerization: protection of the functional groups before polymerization and their deprotection after polymerization.
[0072] A further advantage of the present invention is that it offers the possibility to introduce several functional groups or functionalities depending on the source of nitrene or carbene used. Moreover, the reaction occurring in the present process is a simple addition without side reactions, so the basic polymer structure (monomer content and distribution, structure and molecular weight distribution) is not changed.
[0073] Without wishing to be bound by any particular theory, it is believed that in saturated rubbers such as SEBS, the main reactive sites are the tertiary CH bonds, which are converted to the corresponding -NHR or -CH2CO2R groups, respectively (see Figure 1). And, when the rubber is an unsaturated rubber such as SBS or SEBR, the main reactive sites are the double C=C bonds, which are converted to the corresponding aziridine or cyclopropane (see Figure 2). As shown in the examples and GPC data, no crosslinking process is observed. This is in contrast to prior art methods where rubber polymers are functionalized under thermally induced radical reaction conditions, which results in crosslinking and chain scission by-products.
[0074] Functionalized Polymers of the Invention A second aspect of the present invention relates to a compound comprising at least one group -NH n SO2(C6H4)R 1 A rubber polymer functionalized with R 1 are independent of each other, H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, I, Br, Cl, F, NO2, CF3, OR 3 , COOR 3 , O.C.O.R.3 and N.R. 3 2 is selected, R 3 are independent of each other, H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 aryl; and n is 0 or 1. A value of 0 corresponds to the formation of an aziridine functionality.
[0075] In a preferred embodiment, R 1 is C 1-6 Alkyl, I, Br, Cl, F, COOH, COO-C 1-6 Preferably, the phenyl aromatic ring is selected from the group consisting of C alkyl, C aryl, C aryls ... 1-6 Alkyl, I, Br, Cl, F, COOH, COO-C 1-6 R selected from the group consisting of alkyl 1 It is substituted with a substituent.
[0076] In certain embodiments, n is 1.
[0077] In yet another specific embodiment, n is 0.
[0078] In certain embodiments, the functionalized rubbery polymer comprises from 0.01 to 20 wt. % of —NH based on the total weight of the functionalized rubbery polymer. n SO2(C6H4)R 1 part, R 1 is as defined above. In this context, the term moiety is to be construed as equivalent to functional group and is used to identify those groups resulting from reaction with a nitrene source. Preferably, the functionalized rubber polymer comprises 0.01 to 5 weight percent of -NH based on the total weight of the functionalized rubber polymer. n SO2(C6H4)R 1 part, more preferably 0.01 to 2% by weight of -NH n SO2(C6H4)R 1 Includes parts.
[0079] In preferred embodiments, the functionalized rubbery polymer is characterized by a polydispersity index (PDI) of less than 3, less than 2, preferably less than 1.5, more preferably less than 1.3, and even more preferably less than 1.2.
[0080] A functionalized rubber polymer, like the rubber polymer used in the process of the present invention, is understood to be either a hydrogenated or non-hydrogenated copolymer comprising a conjugated diene and an alkenyl aromatic monomer, or a diene homopolymer or copolymer comprising a conjugated diene monomer.
[0081] In certain embodiments, the functionalized rubber polymer is hydrogenated. In other certain embodiments, the functionalized rubber polymer is not hydrogenated.
[0082] According to a particular embodiment, at least 50%, preferably more than 85%, more preferably more than 95% of the original diene unsaturation of the functionalized polymer is hydrogenated. According to another particular embodiment, less than 1% of the aromatic units are hydrogenated.
[0083] Suitable and preferred embodiments of the alkenyl aromatic monomer, the conjugated diene monomer and the rubber polymer are as defined above with respect to the method of the present invention. In the present invention, the molecular weight of the disclosed polymer is determined by the molecular weight M at the distribution peak. p The molecular weight of the polymer of the present invention can be adjusted according to the requirements and can be adjusted by changing the amount of polymerized monomer, but usually it is related to the molecular weight M p is about 1,000 g / mol to about 10,000,000 g / mol. Preferably, the M p is in the range of about 5,000 g / mol to about 500,000 g / mol, more preferably 20,000 to 400,000 g / mol. The molecular weight of the polymer synthesized by the method of the present invention can be conveniently measured by the GPC method.
[0084] A third aspect of the present invention relates to the functionalized rubbery polymers obtainable by the process of the present invention.
[0085] In certain embodiments, the functionalized rubber polymer obtained by the method of the present invention is a -NH n SO2(C6H4)R 1 and -CH n+1 R 2 and R 1 are independently H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, I, Br, Cl, F, NO2, CF3, OR 3 , COOR 3 , O.C.O.R. 3 and N.R. 3 2 is selected, R 3 are independently H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 aryl; R 2 are each independently selected from -COR, and R is C 1-6 Alkyl, C 3-7 Cycloalkyl and C 6-10 is an aryl group, and n is 0 or 1. A value of 0 corresponds to the formation of an aziridine or cyclopropane functionality.
[0086] In a preferred embodiment, the functionalized rubber polymer obtained by the process of the present invention is a -NH n SO2(C6H4)R 1 and R 1 and n is as defined above.
[0087] In a preferred embodiment, R 1 is C 1-6 Alkyl, I, Br, Cl, F, COOH, COO-C 1-6 Preferably, the phenyl aromatic ring is selected from the group consisting of C alkyl, C aryl, C aryls ... 1-6 Alkyl, I, Br, Cl, F, COOH, COO-C 1-6 R selected from the group consisting of alkyl 1 It is substituted with a substituent.
[0088] In another preferred embodiment, the functionalized rubber polymer obtained by the process of the present invention is -CH n+1 R 2 and R 2 and n is as defined above.
[0089] In another preferred embodiment, R is C 1-3 It is an alkyl group.
[0090] In another preferred embodiment, R 2 is -CO2Et.
[0091] In certain embodiments, n is 1.
[0092] In yet another specific embodiment, n is 0.
[0093] In certain embodiments, the functionalized rubbery polymer obtained by the method of the present invention has from 0.01 to 20 wt. % of -NH based on the total weight of the functionalized rubbery polymer. n SO2(C6H4)R 1 part, R 1 is as defined above. In this context, the term moiety is to be construed as equivalent to functional group and is used to identify those groups resulting from reaction with a nitrene source. Preferably, the functionalized rubber polymer comprises 0.01 to 5 weight percent of -NH based on the total weight of the functionalized rubber polymer. n SO2(C6H4)R 1 part, more preferably 0.01 to 2% by weight of -NH n SO2(C6H4)R 1 Includes parts.
[0094] In another preferred embodiment, the functionalized rubber polymer obtained by the process of the present invention has 0.01 to 20 wt. % of -CH based on the total weight of the functionalized rubber polymer. n+1 R 2 Including R 2is as defined above. In this context, the term moiety is to be construed as equivalent to functional group and is used to identify those groups resulting from reaction with a carbene source. Preferably, the functionalized rubber polymer contains 0.01 to 5 weight percent of -CH based on the total weight of the functionalized rubber polymer. n+1 R 2 part, more preferably 0.01 to 2% by weight of -CH n+1 R 2 Includes parts.
[0095] In a preferred embodiment, the functionalized rubbery polymer obtained by the process of the present invention is characterized by a polydispersity index (PDI) of less than 3, less than 2, preferably less than 1.5, more preferably less than 1.3, and even more preferably less than 1.2.
[0096] In one embodiment, the functionalized rubber polymer obtained by the process of the present invention is particularly characterized by the presence of the above-mentioned catalyst Tp, which is embedded or occluded in the structure of the polymer. x In one embodiment, the functionalized rubber polymer obtained by the process of the present invention contains silver ions, in particular Ag(I), Ag(II) or Ag(III) ions, particularly embedded or occluded in the structure of the polymer. The amount of catalyst or silver ions may range from 0.1 to 5% by weight based on the total weight of the functionalized rubber polymer containing the embedded or occluded catalyst or silver ions. In another embodiment, the functionalized rubber polymer obtained by the process of the present invention does not contain copper ions, particularly embedded or occluded in the structure of the polymer.
[0097] All disclosed embodiments and claims relating to the rubbery polymers of the present invention are construed as being applicable to the rubbery polymers obtained by the processes of the present invention.
[0098] Uses and applications The present inventors have surprisingly found that Tp x Formula Tp represents a hydrotris(pyrazolyl)borate ligand xIt has been found that Ag catalysts have several advantages in the functionalization of rubber polymers. Therefore, the present invention is not limited to the novel polymers and their synthesis methods, but also includes their uses and applications.
[0099] Thus, the fourth aspect of the present invention relates to the use of a compound of the formula Tp in the functionalization of a rubber polymer. x It concerns the use of Ag as a catalyst, and Tp x represents a hydrotris(pyrazolyl)borate ligand.
[0100] In one embodiment, the hydrotris(pyrazolyl)borate ligand Tp x has the formula [ka] [In the formula, Ra, Rb and Rc are independently H, halogen, C 1-6 Alkyl, C 1-6 Haloalkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, halogen substituted C 6-10 Aryl, and C 1-6 Alkyl-substituted C 6-10 aryl.
[0101] In certain embodiments, Ra, Rb and Rc are independently selected from H, Br, Cl, Me, Et, iPr, tBu, CF3, Cy, Ph and p-Cl-C6H4.
[0102] In certain embodiments of the fourth aspect of the present invention, the hydrotris(pyrazolyl)borate ligand Tp x Hydrotris(3,4,5-tribromopyrazolyl)borate (Tp Br3 ), hydrotris(3-phenyl-pyrazolyl)borate (Tp Ph ), hydrotris(3,5-dimethyl-4-bromopyrazolyl)borate (Tp *,Br ), hydrotris(3,5-bis(trifluoromethyl)-4-bromopyrazolyl)borate (Tp(CF3)2,Br ) and hydrotris(3,5-dimethyl-pyrazolyl)borate (Tp * ).
[0103] In certain embodiments, the catalyst is a precursor Tp x It is used in the form AgL, where L is a ligand selected from aprotic solvents such as acetonitrile, THF, or acetone. In this case, the L ligand dissociates first, forming the active catalyst Tp x Become Ag.
[0104] The rubber polymer functionalized according to the fourth aspect of the invention is as described above. In certain embodiments, the polymer is selected from the group consisting of polybutadiene, polyisoprene, isoprene-butadiene copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-butadiene-styrene copolymer, styrene-isoprene-butadiene copolymer and styrene-ethylene-butylene-styrene copolymer.
[0105] As shown in the following examples, the method of the present invention makes it possible to obtain functionalized rubbery polymers with improved properties. Thus, the inventors have surprisingly found a method for producing rubbery polymers with improved compatibility properties. Enhanced physical properties, as well as polymer compatibility and polarity, are important properties of the resulting in-chain functionalized polymers, which give them advantages over non-functionalized or end-of-chain functionalized rubbery polymers. In addition, the surface activity can be modified (high or low surface energy), which is useful in applications where improved adhesion, miscibility, dispersibility, or wettability control is desired. When the in-chain functionalized rubbery polymers of the present invention are mixed with non-functionalized polymers, the functional groups of different nature from those of the non-functionalized polymers cause them to be selectively located at the surface of the mixture, thereby modifying the surface properties even with small amounts of in-chain functionalized polymer.
[0106] In view of the above, a fifth aspect of the present invention relates to the use of the functionalized rubbery polymer of the present invention, or obtainable by the process of the present invention, in asphalt compositions, tire compositions, adhesive compositions, tie layer compositions, sealant compositions, coating compositions, reinforcing compositions, overmold compositions, plastic impact modification, engineering plastic blend compatibilization, fiber and nonwoven compositions, nanomaterials, medical devices, cable compositions, and binders for electrodes of lithium ion secondary batteries.
[0107] The functionalized rubbery polymers of the present invention or obtained by the method of the present invention can be used in adhesive compositions, which can be hot melt adhesives, solvent-based adhesives or reactive adhesives (wherein components capable of reacting with the in-chain functional groups of the polymer are purposefully added), including light, UV and radiation cured compositions.
[0108] In the case of hot melt adhesives, the functional groups present in the in-chain functionalized polymers interact with the resin and the substrate, improving compatibility with the resin and interaction with the substrate, resulting in an adhesive with improved tack, peel and shear properties. Interaction with the substrate is improved by the formation of hydrogen bonds or by specific interactions of the functional groups in the polymer with the substrate. Similar behavior is expected when in-chain functionalized polymers are added to solvent-based adhesives.
[0109] The hot melt adhesive composition may include at least one additive selected from the group consisting of tackifying resins, stabilizers, plasticizers and antioxidants. In some of these applications, about 15-30 parts by weight, more preferably about 18-25 parts by weight, of the in-chain functionalized polymers of the present invention are mixed with other components of conventional adhesive formulations such as tackifiers, stabilizers, plasticizers and antioxidants to impart improved properties to these adhesive compositions compared to adhesives prepared in the same composition using the same type of polymer without the introduction of functional groups. Examples of suitable tackifiers include resins that are compatible with the polymer and have high and low softening points. These include hydrogenated resins, colophony esters, polyterpene resins, terpene phenolic resins and coumarone-indene resins. In some exemplary modes, the amount of fixing resin in the composition ranges from about 45 to 65% by weight. Plasticizers commonly known as extender oils include mineral oils, paraffin oils and naphthenic oils. In some exemplary embodiments, the amount of plasticizer in the composition ranges from about 15 to 30% by weight. The antioxidant is usually added to the adhesive composition in an amount of about 0.05 to 3% by weight. Examples of antioxidants include phenolic compounds and thio compounds. In a preferred embodiment, the composition comprises about 15 to 30% by weight of tackifier resin, about 15 to 30% by weight of plasticizer, and about 0.05 to 2% by weight of antioxidant. In a preferred embodiment, the adhesive composition can be used in multiple applications, such as packaging adhesives, labels and adhesive tapes, constructions, and as pressure-sensitive adhesives used in the manufacture of disposable elastic articles.
[0110] For reactive adhesives, the in-chain functionalized polymer is required to have a functional group that can be reacted or activated by light, radiation or UV light. The functional group of the polymer of the present invention placed in the adhesive formulation can thus react with the substrate or with another chemical present in the adhesive formulation, such as a two pot adhesive.
[0111] Another use of the functionalized polymers of the present invention is in sealant compositions comprising the polymers of the present invention.
[0112] Another application of the functionalized polymers of the present invention are in coating compositions, where the polymers of the present invention aid in adhering to the substrate and / or aid in making the surface being coated more hydrophobic or hydrophilic, depending on the functional groups attached to the polymer.
[0113] Furthermore, the polymers of the present invention are useful for reinforcing materials or for making composite materials, which means that they can be mixed with reinforcing or reinforced materials. The reinforced materials can be preferably selected from the group consisting of asphalt, adhesives, plastics, tires and nanomaterials. Good results are obtained when plastics selected from polyamides, polyurethanes, polyethers, polysulfones, polyetherketones, polyetheretherketones, polyetherimides, polycarbonates, polyesters, polystyrenes and their copolymers are reinforced. The reinforced materials or compounds are useful for making articles, which can be, for example, extrusions, injection moldings, compression moldings or tires.
[0114] Another application of the functionalized polymer is modified asphalt, which includes asphalt mixed with the polymer of the present invention. The asphalt may include about 1-25% by weight of the polymer based on the total weight of the asphalt and the polymer. Preferably, the modified asphalt includes about 5-20% by weight of the polymer. These asphalt mixtures modified with the polymer of the present invention can be used in applications such as roads, asphalt membranes, etc.
[0115] Another application of the functionalized polymers of the present invention relates to modified materials comprising a mixture of the polymer of the present invention with a plastic of any nature, more preferably an engineering plastic. The polymer of the present invention may be added to virgin plastics to improve their physical properties, especially their impact resistance. The mixture typically comprises about 0.01-90% by weight, preferably about 1-40% by weight, of the polymer, based on the total weight of the mixture. According to one embodiment, the plastic comprises at least one polymer selected from polystyrene, polybutadiene, polyisoprene, and block or progressive random copolymers, preferably prepared from monomers selected from the group consisting of styrene, butadiene and isoprene, and preferably having an average molecular weight of the distribution peak of about 3,000-300,000 g / mol. Although a wide variety of engineering plastics can be mixed, the engineering plastics are preferably selected from the group consisting of polyamides, polyurethanes, polyethers, polysulfones, polyetherketones, polyetheretherketones, polyimides, polyetherimides, polycarbonates, polyesters, polystyrenes and copolymers thereof. The polymer of the present invention preferably comprises polystyrene as its mixture in the plastic.
[0116] The polymers of the invention are useful for obtaining fibers and nonwovens, preferably prepared by electrospinning, spunbonding, meltblowing or any other known method. Depending on the functionality possessed by the in-chain functionalized polymer, it is possible to obtain fibers of the polymer with a hydrophilic or hydrophobic surface. Of particular interest are hydrophobic surfaces that are water repellent and self-cleaning. In general, fluorine groups are known to confer hydrophobicity due to their low surface energy. These polymer fibers can be advantageously used in applications for obtaining special clothing, surgical threads, etc.
[0117] The polymers of the present invention are also useful for producing organic or inorganic nanomaterials with improved properties, given the high probability of interactions, both physical or chemical, between the functional groups present in the polymers of the present invention and complementary functional groups present on the nanoparticles.
[0118] The polymers of the present invention are also useful in medical applications such as the manufacture of medical tubing, especially by incorporating biocompatible functional groups into the polymer chain.
[0119] The polymers of the present invention are also useful for preparing compositions for cable applications, where thermoplastic elastomers (TPEs) derived from the functionalized polymers of the present invention are added to the formulations and then crosslinked to obtain fire-resistant halogen-free cables useful as insulation in the electrical or automotive field.
[0120] In further preferred embodiments of the present invention, the above preferred specific embodiments are combined. The present invention also relates to such combinations of preferred specific embodiments.
[0121] Throughout the specification and claims, the word "comprises" and variations thereof are not intended to exclude other technical features, additives, components or steps. For those skilled in the art, other objects, advantages and features of the invention must be gathered partly from the specification and partly from the practice of the invention. EXAMPLES
[0122] The present invention will now be described by way of examples to illustrate the construction and testing of exemplary embodiments, although it will be understood that the invention is in no way limited to the following examples.
[0123] All polymerizations and hydrogenations in the following examples were carried out in an autoclave reactor of 2 L internal volume equipped with control systems for temperature, agitation, and flow meters, as well as nitrogen inlet, outlet and sampling lines.
[0124] The resulting polymer was analyzed by gel permeation chromatography (GPC) and by elution with CDCl3 at 500 MHz. 1 It was characterized by HNMR technique.
[0125] The isolated polymer samples were analyzed by GPC and M w , M n and PDI were shown to be similar to those of the corresponding starting materials, confirming the absence of chain scission or chain cross-linking processes.
[0126] The identity of the groups incorporated into the polymer chain is 1 HNMR spectroscopy confirmed the presence of typical resonances for, for example, CH2CO2Et, CHCO2Et (cyclopropane), NHT and NT (aziridine). 1 The H NMR spectra were identified by several characteristic resonances of the polymer and by integration of such resonances with respect to the resonances of added external standards, the relative amount of the functional group incorporated in each case was determined. In this way, the percentage of incorporation was calculated 1 Determined by HNMR.
[0127] Example 1. Functionalization of SEBS with [N-(p-toluenesulfonyl)imino]phenyliodinane This functionalization reaction was repeated three times with different amounts of reactants, see table below for details.
[0128] The SEBS rubber polymer was dissolved in 1,2-dichloroethane and added with N-(p-toluenesulfonyl)imino]phenyliodinane (PhINTs) and silver hydrotris(3,5-dimethyl-4-bromopyrazolyl)borate catalyst (Tp *,Br Ag) was added.
[0129] The mixture was heated at 80°C under nitrogen for 12 hours. After cooling, methanol (100-200mL) was added and the precipitated functionalized rubber was isolated by filtration and dried under vacuum. The isolated yield of polymer was greater than 95% and the incorporation of NHT units ranged from 1-5% w / w (see table below), corresponding mainly to pendant -NHT groups resulting from insertion of NHT units into the tertiary sites of the rubber chain.
[0130] [Table 1]
[0131] Example 2. Functionalization of Unsaturated Rubber with [N-(p-Toluenesulfonyl)imino]phenyliodinane In a variant of Example 1, working at room temperature in cyclohexane as solvent, modified rubbers with a degree of incorporation of NHT units within the interval of 1-5% were obtained in yields of more than 95%. In this case, the unsaturated rubber was modified upon the formation of an aziridine ring resulting from the addition of an NHT unit to the double bond of the unsaturated rubber.
[0132] Example 3. Functionalization of SEBS with ethyl diazoacetate A cyclohexane solution of rubber and catalyst was prepared with similar concentrations as described in Example 1. Ethyl diazoacetate (EDA) was dissolved in cyclohexane and the solution was added slowly to the above mixture at room temperature for 12 hours using an automated addition system. The mixture was then stirred for an additional hour before removing the solvent under reduced pressure, redissolving in a minimum amount of tetrahydrofuran, and precipitating with methanol. After filtration and drying under vacuum, more than 95% of the mass was recovered. 1 HNMR studies revealed that CHCO2Et groups were incorporated into the polymer chains at 1–5% w / w, leading to the attachment of pendant -CH2CO2Et units.
[0133] Example 4. Functionalization of unsaturated rubber with ethyl diazoacetate In a variation of Example 3, using unsaturated rubber, modified materials were isolated with high mass recovery (>95%). The incorporation of CHCO2Et units occurred on the C=C bonds of the unsaturated rubber, leading to the formation of cyclopropane units. Percentage of incorporation: 1-5% w / w.
[0134] Example 5. Functionalization of saturated rubber with ethyl diazoacetate followed by PhINT The polymer rubber material is Tp in cyclohexane. *,Br When Ag catalyst was used as the reaction medium, sequential functionalization was possible using the same catalyst in a one-pot method.
[0135] Thus, a solution of EDA was first slowly added to a stirred solution of catalyst and rubber at room temperature. After complete addition (12 h), PhINT was added and further stirred at 80 °C for 12 h to yield a rubber with carboxylate and amine functionalities. The isolated material is consistent with the presence of pendant -CH2CO2Et and -NHT groups resulting from metal-catalyzed insertion of carbene-CHCO2Et and nitrene-NT groups, respectively. 1 HNMR spectra were shown. Percentage of incorporation: 1-5% w / w per functional group.
[0136] Example 6. Functionalization of unsaturated rubber with ethyl diazoacetate followed by PhINT In a variation of Example 5, the same protocol was applied to unsaturated rubber to obtain modified materials with cyclopropane and aziridine rings within the rubber structure. Incorporation of both carbene and nitrene was carried out at room temperature, with incorporation occurring within 1-5% w / w of each unit.
[0137] Example 7. Functionalization with various catalysts Tp used in Examples 1 to 6 *,Br Instead of the Ag catalyst, in this example the experiment is repeated but with a composition Tp x Using AgL as a catalyst, Tp x represents the ligand shown in the table below, where L is either acetonitrile or tetrahydrofuran.
[0138] [Table 2]
[0139] Comparative Example 1. Copper-Catalyzed Functionalization Copper Analog Tpx Rubber functionalization also occurred using CuL as a catalyst. However, the presence of some remaining occluded copper ions in the isolated material induced the development of a greenish color and loss of solubility in tetrahydrofuran, proving the presence of a radical-mediated crosslinking process. These impurities followed the appearance of the color of the rubber when exposed to air.
[0140] Comparative Example 1.1. Functionalization of Carbenes with Copper Catalysts and with Catalysts of the Present Invention Tp used for EDA functionalization of unsaturated rubber polymers (SB tapered diblock copolymer (1.0) or SBS triblock copolymer (6.0)) Br3 Cu(NCMe) or Tp *,Br Experiments were carried out to compare the effect of Ag catalysts on the stability of unsaturated rubber. Rubbers were functionalized as follows:
[0141] After dissolving the catalyst and polymer in cyclohexane, a solution of the diazo compound EDA in cyclohexane was added via slow-addition syringe (programmable addition time) under an inert atmosphere. After 12 hours of addition, the volume of the solvent was reduced under reduced pressure and methanol was added to precipitate the rubber. 1 HNMR analysis confirmed the incorporation of the CHCO2Et functional group.
[0142] The resulting functionalized polymers were stored at room temperature for 2 months and their growth was monitored. Interestingly, after 2 months of storage at room temperature, in contrast to the sample functionalized with the silver catalyst, the sample functionalized with the copper catalyst was not completely soluble in THF and a broadening of the molecular weight distribution was observed, proving that there were solubility issues and that undesired crosslinking reactions had occurred in this polymer.
[0143] Comparative Example 1.2. Nitrene Functionalization with Copper Catalyst and Nitrene Functionalization with the Catalyst of the Present Invention Tp used for PhINT functionalization of unsaturated rubber polymers (SBS triblock copolymers) Br3 Cu(NCMe) or Tp *,BrExperiments were carried out to compare the effect of Ag catalysts on the degree of functionalization and molecular weight distribution. Rubber was functionalized as follows:
[0144] Solutions of catalyst and rubber were prepared in cyclohexane under an inert atmosphere in the ratios shown in the table below. Once the rubber was dissolved, the nitrene source was added and the mixture was stirred overnight. Experiments with silver catalyst were carried out at room temperature and those with copper catalyst were carried out at 60°C. The following day, the rubber was precipitated by adding a reduced amount of solvent and methanol under reduced pressure. The rubber was filtered and dried under vacuum and the percentage of "NT" incorporated in the rubber was determined by integration with trimethoxybenzene (TMB) as an internal standard. 1 This was determined by HNMR analysis.
[0145] The table below shows a comparison of both silver and copper catalysts. *,Br Polymers functionalized with Ag catalysts exhibited excellent Tp despite the use of relatively low amounts of catalyst and functionalizing agent and mild reaction conditions. Br3 It was observed to result in a higher level of functionalization compared to that used in the Cu(NCMe) experiments.
[0146] [Table 3]
[0147] Furthermore, it was observed that the functionalized rubber obtained using silver catalyst has a molecular weight distribution similar to that of virgin rubber, while the functionalized rubber using copper catalyst shows a broadening of the molecular weight distribution, indicating the occurrence of undesired crosslinking reactions.
[0148] Example 8. Functionalization with various precursors Instead of the nitrene precursor of PhINT used in Examples 1, 2, 5 and 6, this example consists of repeating the same experiment but using a different nitrene precursor. The nitrene precursor used was PhI=N-SO2(C6H4)R 1 (C6H4)R 1 is C1-6 Alkyl, I, Br, Cl, F, COOH or COO-C 1-6 phenyl para-substituted with alkyl.
[0149] Example 9. Characterization of Functionalized Rubber An isolated, accurately weighed sample of functionalized SEBS, prepared as described in Example 1, was dissolved in CDCl3 and naphthalene was added as an internal standard. 1 The HNMR (400 MHz) spectrum showed a resonance signal centered at 2.48 ppm assigned to the Me group of the tosyl portion of the functionalized rubber, which, when integrated with the naphthalene signal, gave the degree of functionalization shown in the table included in Example 1.
[0150] Furthermore, GPC studies performed on the above samples dissolved in THF revealed that M n = 77517 and PDI = 1.10 were obtained, and the first SEBS (M n = 73964, PDI = 1.11) compared satisfactorily.
[0151] Figures 3 and 4 show the NMR and GPC data.
[0152] Example 10. Charpy impact test and SEM analysis Tests of Charpy impact resistance were carried out at 23° C. and −30° C. on four different samples of polyamide-6 (Comparative Sample 1) and its blends with 20% by weight of SEBS (Comparative Sample 2), with 20% by weight of SEBS-g-MA (1.4% functionalized, Comparative Sample 3; SEBS-g-MA = SEBS functionalized with maleic anhydride by reactive extrusion) and with 10% by weight of SEBS functionalized with NT (4.2% functionalized, Sample 4). The tests were carried out according to standard ISO 179-1.
[0153] Prior to extrusion, the preblend was doped with antioxidant Irganox-1330™ and dried overnight under inert atmosphere at 80° C. The preblend was extruded in a Eurolab™ extruder equipped with six heating zones (210° C., 215° C., 220° C., 225° C., 230° C., 240° C.) and injected into a Sandretto™ 6GV-50 injection molding machine to obtain specimens for impact testing.
[0154] [Table 4]
[0155] Figure 5 is a graphical representation of the data in the table above.
[0156] The impact resistance values measured under different conditions for blends containing only non-functionalized SEBS as the elastomeric component were comparable to those found for pure polyamide-6. The impact resistance was significantly improved for the functionalized SEBS materials, especially the p-toluenesulfonylamine-functionalized SEBS, which provided better values at half the loading of SEBS-g-MA.
[0157] SEM imaging (Phillips XL30 ESEM 20KV microscope) of samples treated with xylene for 96 h at room temperature is shown in Figures 6, 7, and 8. After drying under vacuum overnight, the samples were fractured in liquid nitrogen and a 3-4 nm thick Au / Pd layer was deposited.
[0158] As shown in FIG. 6, the non-functionalized SEBS (Comparative Sample 2) is poorly compatible with polyamide due to the large heterogeneity in shape and size relative to the niche depth, indicating that the morphology of the dispersed phase corresponds to a vein or reef structure with very low levels of polyamide dispersion.
[0159] Figure 7 shows the morphology of Comparative Sample 3. A dispersed morphology of droplets with a relatively uniform size distribution is observed. The shape range was 50-100 nm.
[0160] Figure 8 shows the morphology of Sample 4 of the present invention. SEBS-N(H)Ts produced homogeneous blends with polyamide-6, as confirmed by well-distributed homogeneous morphology with spherical domains ranging from 50-100 nm to 1-2 microns in diameter and with an average size of around 300-400 nm. Thus, p-toluenesulfonylamine functionalized SEBS was highly compatible with polyamide-6.
Claims
1. A method for functionalizing a rubber polymer comprising the steps of: x reacting a rubber polymer with at least one source of nitrene or carbene in the presence of a catalyst of Ag; x represents a tris(pyrazolyl)borate ligand.
2. Hydrotris(pyrazolyl)borate ligand Tp x The method of claim 1 , wherein [Case 1] [In the formula, Ra, Rb and Rc are independently H, halogen, C 1-6 Alkyl, C 1-6 Haloalkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, halogen-substituted C 6-10 Aryl, and C 1-6 Alkyl-substituted C 6-10 aryl.
3. The hydrotris(pyrazolyl)borate ligand Tp x is selected from the group consisting of hydrotris(3,4,5-tribromopyrazolyl)borate, hydrotris(3-phenyl-pyrazolyl)borate, hydrotris(3,5-dimethyl-4-bromopyrazolyl)borate, hydrotris(3,5-bis(trifluoromethyl)-4-bromopyrazolyl)borate and hydrotris(3,5-dimethyl-pyrazolyl)borate.
4. 4. The method of claim 1, wherein the rubber polymer is an optionally hydrogenated copolymer comprising a conjugated diene and an alkenyl aromatic monomer, or an optionally hydrogenated diene homopolymer, or a copolymer comprising a conjugated diene monomer.
5. 5. The method of any one of claims 1 to 4, wherein the rubber polymer is selected from the group consisting of polybutadiene, polyisoprene, isoprene-butadiene copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-butadiene-styrene triblock copolymer, styrene-isoprene-butadiene triblock copolymer, styrene-isoprene-butadiene-styrene block copolymer, styrene-ethylene-propylene-styrene copolymer and styrene-ethylene-butylene-styrene copolymer.
6. At least one source of nitrene is 2 (C 6 H 4 ) R 1 , NaClNSO 2 (C 6 H 4 ) R 1 and N 3 SO 2 (C 6 H 4 ) R 1 wherein R 1 are independent, H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, I, Br, Cl, F, NO 2 , C.F. 3 , OR 3 , COOR 3 , O.C.O.R. 3 and N.R. 3 2 wherein R 3 are each independently H, C 1-6 Alkyl, C 3-7 Cycloalkyl and C 6-10 aryl and / or at least one source of said carbene is selected from N 2 CHCO 2 R and N 2 C(R')CO 2 R, wherein R is C 1-6 Alkyl, C 3-7 Cycloalkyl and C 6-10aryl group, and R′ is C 1-6 Alkyl or C 6 -C 12 The method according to any one of claims 1 to 5, wherein the group is an aryl group.
7. The process according to any one of claims 1 to 6, wherein the reaction is carried out at a temperature below 120°C.
8. At least one group -NH n SO 2 (C 6 H 4 ) R 1 A rubber polymer functionalized with R 1 are each independently H, C 1-6 Alkyl, C 3-7 Cycloalkyl, C 6-10 Aryl, I, Br, Cl, F, NO 2 , C.F. 3 , OR 3 , COOR 3 and O.C.O.R. 3 wherein R 3 are independently H, C 1-6 Alkyl, C 3-7 Cycloalkyl and C 6-10 aryl, said n being 0 or 1, said rubbery polymer being an optionally hydrogenated copolymer comprising a conjugated diene and an alkenyl aromatic monomer.
9. 9. The functionalized rubbery polymer of claim 8, having a polydispersity index of less than 3, said polydispersity index being M w / M n The result is that M w is the weight average molar mass, and M n is the number average molar mass, and M w and M. n as determined by gel permeation chromatography.
10. The functionalized rubbery polymer of claim 8 or 9, selected from the group consisting of styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-butadiene-styrene copolymer, styrene-butadiene-isoprene copolymer and styrene-ethylene-butylene-styrene copolymer.
11. A functionalized rubbery polymer according to any one of claims 8 to 10 comprising from 0.1 to 5 weight percent of -NHnSO2(C6H4)R1 moieties, based on the total weight of said functionalized rubbery polymer.
12. Formula Tp in the functionalization of rubber polymer x The use of a catalyst of Ag, x represents a hydrotris(pyrazolyl)borate ligand.
13. Use of the functionalized rubber polymer according to any one of claims 8 to 11 in asphalt compositions, tire compositions, adhesive compositions, tie layer compositions, sealant compositions, coating compositions, reinforcing compositions, overmold compositions, plastic impact modification, engineering plastic blend compatibilization, fiber and nonwoven compositions, nanomaterials, medical devices, cable compositions, and binders for electrodes of lithium ion secondary batteries.
Citation Information
Patent Citations
Chemicals capable of forming a covalent three-dimensional network
JP2012519206A
Functionalized elastomers, methods of making and uses thereof
JP2018508618A
Method for functionalizing a polymer
JP2018513257A
Process for functionalising polymers
US20180118857A1
Synthesis of copper (i) and silver (i) complexes with a fluorinated trispyrazolylborate ligand and the use thereof in the functionalisation of alkanes
WO2015181415A1