Barrier layers for cellulosic substrates
A second coating of animal and vegetable waxes enhances the gas-tightness and water-tightness of cellulose packaging, addressing the impermeability issues of existing cellulose-based materials and enabling long-term food storage with biodegradability.
Patent Information
- Application Number
- JP2021562156
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-19
- Filing Date
- 2020-04-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-04-20
AI Technical Summary
Existing cellulose-based packaging materials lack sufficient gas-tightness and water-tightness, especially for food packaging applications, and current coatings often rely on non-biodegradable polymers.
A second coating composed primarily of animal and/or vegetable waxes and/or lipids is applied over a first coating, which may include flaxseed oil, carnauba wax, and beeswax, to enhance the gas-tightness and water-tightness of cellulose substrates.
The coating provides high impermeability, abrasion resistance, and flexibility, making the packaging environmentally friendly and suitable for long-term storage of food products while being fully biodegradable.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for applying a flowable, biodegradable first coating that increases gas-tightness to a cellulose-containing substrate to produce a coated substrate. [Background technology]
[0002] Packaging made of cellulose, especially molded pulp, cardboard, and paper, is increasingly in demand. Cellulose fibers are a highly used material that is very easy to recycle. Recycled raw materials (wood, paper, etc.) are also ideal for the production of cellulose packaging. Cellulose is processed, for example, in a pulp molding process. An aqueous pulp with cellulose fibers is produced, from which fibers are molded. Using a simple scooping process, water is sucked through a suction mold and the cellulose fibers are deposited on the porous surface of the suction mold. In a transfer process, the molded body formed by the suction mold is conveyed to a transfer mold and molded from both sides. Additional heat processing and pressing methods may be used, which improve the surface quality of the molded body. Alternatively, cellulose can be processed into paper or cardboard and used as packaging material.
[0003] It is known from the prior art to render cellulose-containing substrates substantially gas-tight by means of coatings. For this purpose, the substrates can be coated with cellulose fibers, in particular with microfibrils and / or nanofibrils made of, for example, cellulose.
[0004] Such coating methods are known from publications such as EP 3444399, JP 2015-227517, JP 2012-011651, WO 2017 / 144009, EP 2529942 and WO 2017 / 072124. The substrate coated with cellulose fibrils is further coated with a polymer such as polyethylene or polypropylene, but also with a biodegradable polymer such as polylactic acid or polyvinyl alcohol. Summary of the Invention
[0005] The object of the present invention is to produce a nearly gas-tight and water-tight package for food packaging made primarily from natural raw materials.
[0006] According to the invention, this object is achieved in that a second waterproof coating, composed mainly of animal and / or vegetable waxes and / or lipids, is applied to the first coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The second coating may, for example, contain at least 90% by weight of animal and / or vegetable waxes and / or lipids. The second coating may contain at least 70% by weight of animal and / or vegetable waxes.
[0008] The first coating and / or the second coating may be applied by a spraying method.
[0009] In other words, the sealing layer applied to the cellulose substrate can be made water- and moisture-resistant by applying a layer of natural waxes and / or fats. The natural waxes and / or fats consist mainly of esters of fatty acids and, as oil-soluble products, are readily biodegradable according to test method CEC-L-33-A-93. Thus, the entire coated packaging can be disposed of and recycled in an environmentally friendly manner, since it is mainly composed of cellulose fibers, possibly other natural ingredients, and natural fats or waxes.
[0010] Specifically, the second coating is Linseed oil, Carnauba wax, and / or ·Beeswax The composition may contain at least one of the following components:
[0011] Linseed oil is used to improve the malleability of the oil-wax mixture that forms the second coating and to minimize brittleness after drying. Pure linseed oil, i.e., medicinal grade, fully purified, should be used. Linseed oil is one of the oils that does not harden easily and has been used for centuries to impregnate wood. A layer of linseed oil alone has open pores, i.e., water and air can pass through to a small extent, and is not suitable for permanently sealed food packaging.
[0012] Carnauba wax is a very hard wax of tropical origin with a high melting point (approximately 85-89°C). It has little odor or taste and is waterproof. When dry it is very brittle and hardens within a few seconds. Its hardness also makes it very abrasion resistant. The wax is approved for packaging food products and has long been used as a coating to extend the shelf life of e.g. mangoes, confectionery, etc.
[0013] Beeswax is a wax produced in Europe and elsewhere that is less hard than carnauba wax. By mixing it with carnauba wax, beeswax helps to reduce its brittleness. It has little inherent odor or taste and is approved for food-related uses. Its melting point is about 65°C.
[0014] In particular, the second coating 20-30% by weight of linseed oil, 40-60% by weight of carnauba wax, and 30-40% beeswax by weight It may contain the component.
[0015] This mixture has the positive properties of the three components: high impermeability and abrasion resistance, odorless or tasteless, and high flexibility at ambient temperature. The coating properties of this mixture combined with the underlayer of cellulose microfibrils or cellulose nanofibrils are highly suitable to meet the requirements of water resistance and gas tightness necessary for food packaging.
[0016] In practice, the fluid first coating solution for producing the first coat may have cellulose nanofibrils or microfibrils dissolved in water. Nanocellulose has cellulose microfibrils with a median diameter in the range of 30-100 nm, and / or cellulose nanofibrils with a median diameter in the range of 5-20 nm. Industrially distributed cellulose fibrils are often a mixture of microfibrils and nanofibrils. Experiments have demonstrated that a mixture of 2 wt.% nanocellulose and 98 wt.% water is useful as a first coating. If a higher cellulose content is selected, the deformation of the fiber-containing substrate due to moisture can be reduced or avoided, and the drying time can be shortened. In practice, a cellulose content of 2-10 wt.% of the first coating solution was suitable.
[0017] However, there are other organic materials in the coating that increase the impermeability of the cellulose substrate to the penetration of gases. For example, casein powder may be mixed with water and modified with calcium hydroxide. Casein increases the impermeability and mechanical strength of the substrate. Casein modified with calcium hydroxide also becomes water repellent to some extent. It is also possible to modify casein with baking soda, but this does not make it water repellent. Coating with casein is particularly suitable for dairy products and manufactures that may produce casein. Due to the strength-increasing effect of the casein coating, the substrate can be used as a substitute for plastics, for example, in the manufacture of disposable cutlery. Disposable cutlery can also be made from a cellulose-coated substrate with a waterproof second layer. On the other hand, casein coating can significantly increase the strength, so the substrate can be used to form, for example, knives, where strength is important.
[0018] In practice, 30 g of casein powder was soaked in 100 ml of water for about 8-10 hours, 30 g of calcium hydroxide was added and stirred. After adding another 50 ml of water, the solution was strained and used for coating. This coating may be applied after the coating with cellulose fibers or instead of the coating with cellulose fibers. The first coating may also contain both cellulose fibers and casein.
[0019] Whey is also suitable as a component of the first coating. Whey can be denatured by heat (90-100°C). Whey as part of the first coating also increases the strength of the coated substrate. The whey coating itself is not water repellent and therefore must be made waterproof with a second coating.
[0020] Finally, gel-forming ingredients such as agar (gelatin from algae) or psyllium husk (seed husk of the psyllium species Plantago indica and Plantago afra) are suitable for addition to the first coating. For this purpose, agar powder is mixed with water and denatured at 100°C for 1 minute. It hardens and gels upon cooling. The gel may be applied to the substrate, forming a thin layer that fills the substrate's pores, increases its strength and repels water.
[0021] A similar effect is achieved when crushed psyllium husk is soaked in water and allowed to swell for about 20 minutes before being applied to a substrate.
[0022] As mentioned above, the components of the first coating can be dissolved in water and applied simultaneously. However, it is also possible to apply the various components of the first non-waterproof coating to the substrate in several application processes.
[0023] The first coating may be first dried before the second coating of natural waxes and lipids is applied. The first coating containing water will not mix with the second coating of oils and waxes, and therefore it is desirable to dry thoroughly before the second coating is applied.
[0024] As mentioned earlier, the substrate itself is formed from cellulosic fibers. In particular, the substrate can be manufactured as a thin-walled product using a pulp molding process, with or without subsequent pressing or thermoforming.
[0025] The substrate may be in many different forms, e.g. ·cup, ·pot, ·container, ·knife, ·fork, ·spoon, ·dish The shape may be:
[0026] The substrate may function as food packaging or disposable tableware or cutlery. Particularly when used as disposable cutlery, the increased strength that can be achieved by the various components of the first coating is extremely important.
[0027] Furthermore, the production of capsules can be envisaged, which are filled with powders for preparing drinks, in particular ground coffee beans. There is an increasing demand for individually wrapped, single-serving containers of coffee. For this purpose, various packaging techniques are used. Pure aluminium packaging provides a high level of tightness, and the coffee packaged in it can be stored for long periods. However, this also requires a lot of energy and high material costs in the production of the packaging, and results in a large amount of waste. So-called coffee pods are portions of coffee wrapped in a cellulose fleece. This packaging weighs less than aluminium packaging and can also be biodegraded more easily. However, the pad lacks tightness, and therefore the coffee packaged in it cannot be stored for very long or loses its aroma.
[0028] The single-use coffee container made of the capsule made of the substrate described herein has a high degree of sealing, which is much higher than that of the pad made of uncoated cellulose fibers. As a result, coffee can be stored for a much longer period of time. The capsule may be sealed with a cover layer, for example a paper layer having the above-mentioned coating. The capsule is made of only natural raw materials, i.e. cellulose and natural waxes and lipids, and can be easily disposed of or recycled.
[0029] To produce capsules, a tray, i.e. a monolayer with several recesses, can be first produced using a pulp molding process. This tray and the recesses are first sprayed with a suspension containing nanocellulose. After this first coating has dried, a mixture of wax and oil, in particular 25% by weight linseed oil, 50% by weight carnauba wax and 25% by weight beeswax, is applied as a second coating. This second coating can be sprayed or the substrate with the first coating can be immersed in this mixture, and then the wax / oil mixture penetrates deep into the pores of the cellulose substrate with the first coating by heating and is distributed evenly. In this way, the tightness of the final product is increased.
[0030] The trays may also be re-pressed after the first coating has been sprayed, especially with a heated mold, which will speed up the drying process.
[0031] The wax and lipid of the second coating are heated to a temperature of, for example, 90° C. so as to maintain a liquid state for application. A heated reservoir for the material of the second coating may be placed in close proximity to the drying channel for the first coating. The nozzle for applying the second coating may also be heated. The second coating cools and hardens in the process in a short time (a few seconds). It can then be used as a food packaging.
[0032] The capsules formed by the recesses in the tray are then filled with the intended amount of coffee and sealed with a seal, which may consist of a paper layer also with a first coating of nanocellulose and a second coating of animal and / or vegetable waxes and / or lipids to make it gas-tight and water-resistant.
[0033] The sealing operation is performed using a tool precisely designed to the shape of the tray, which seals between the coffee-filled troughs on the molded pulp web of the tray. The tool has a metal web about 5 mm wide that can be placed on the web between the recesses of the tray. The tool may be heated and pressed onto the tray with pressure, which may be in a counter-mold if necessary. The counter-mold allows the necessary pressure to be applied to the web of the tray and holds the tray exactly in place so that the sealing operation can be performed.
[0034] After the sealing operation, the tray may be cut into individual capsules, but it is also possible to cut into larger sections containing several capsules, which may then be separated by means of scissors or by separation along a perforation made in the sealed web between the two hollow parts of the tray.
[0035] The substrates coated in this way are also found to be suitable for packaging other articles, in particular foodstuffs, which need to be packaged in a substantially gas-tight manner to preserve freshness. In particular, dry foods, such as seasoning mixes or powders for mixing soups, may be packaged in beakers having such a coating. The substrates coated in this way can also be used as plates for meals or cups for drinks, which come into contact with water for short periods of time.
Claims
1. 1. A method for producing a coated substrate, comprising applying a flowable and biodegradable first coating to the substrate, the first coating increasing gas tightness, and solidifying the first coating, the first coating containing cellulose fibers and casein, the cellulose fibers and casein being dissolved in water, the casein being modified with calcium hydroxide, and applying a second waterproof coating, mainly composed of animal and / or vegetable waxes and / or lipids, to the first coating after drying.
2. The second waterproof coating comprises: ・Linseed oil, Carnauba wax, and / or ・Beeswax 2. The method of claim 1, further comprising at least one of the following components:
3. The second waterproof coating comprises: 20 to 30% by weight of linseed oil, 40 to 50% by weight of carnauba wax, and 25-40% by weight beeswax The method according to claim 2, comprising:
4. The flowable first coating comprises water and ·whey, Agar, ・Psyllium husk 4. The method according to claim 1, further comprising at least one of the following components:
5. 5. The method of claim 4, wherein the first coating comprises cellulose fibrils having a median diameter in the range of 30-100 nm and / or nanocellulose having cellulose fibrils having a median diameter in the range of 5-20 nm dissolved in water.
6. 6. The method according to any one of claims 1 to 5, characterized in that the cellulose content of the first coating is 2-10% by weight or more.
7. 10. The method of claim 1 , wherein the first coating is applied in two or more separate application processes.
8. 8. The method of claim 7, wherein different compositions are applied during the application process.
9. 1. A coated substrate formed from cellulose, the substrate having a biodegradable first coating that increases the gas tightness of the substrate, the first coating comprising cellulose fibers and casein, the casein being modified with calcium hydroxide, and a second waterproof coating of primarily animal and / or vegetable waxes and / or lipids disposed on the dried first coating.
10. The second waterproof coating comprises: ・Linseed oil, ・Carnauba wax, ・Beeswax 10. The substrate according to claim 9, comprising at least one of the components:
11. The second waterproof coating comprises: 20 to 30% by weight of linseed oil, 40 to 50% by weight of carnauba wax, and 25-40% by weight beeswax The substrate according to claim 10, characterized in that it contains
12. The first coating comprises: ·whey, Agar, ・Psyllium husk and further comprising at least one of the components The substrate according to any one of claims 9 to 11, characterized in that the first coating comprises, as the cellulose fibers, cellulose fibrils having a median diameter in the range of 30 to 100 nm and / or cellulose fibrils having a median diameter in the range of 5 to 20 nm.
13. 13. The substrate according to any one of claims 9 to 12, characterized in that the substrate mainly contains cellulose fibers.
14. ·container, ·knife, ·fork, ·spoon, 14. The substrate according to claim 9, wherein the substrate has the shape of at least one of the following articles:
15. ·cup, ·pot, ·dish, ・Coffee pods 14. The substrate according to claim 9, wherein the substrate has the shape of at least one of the following articles:
Citation Information
Patent Citations
Coating solution for coating a packaging material to produce a barrier layer, a method for its production and its use
DE102017202887A1
Support coated with a chitosan base layer and method for producing the same
JP2005527710A
Cellulosic materials and methods of making and using same - Patent Application 20070122997
JP2019509403A
Paper manufacture
US1957369A
Coated paper and paper products
US2290633A