Atomic Layer Etching and Ion Beam Etching Patterning
The combination of atomic layer etching and ion beam etching addresses the challenges of patterning MRAM by minimizing sidewall redeposition and tapering, enabling efficient etching of high aspect ratio and dense pitch structures in MRAM devices.
Patent Information
- Application Number
- JP2022515725
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-17
- Filing Date
- 2020-09-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-09-09
AI Technical Summary
Current patterning techniques for semiconductor devices, particularly magnetic random access memory (MRAM), face challenges such as tapered geometries, sidewall redeposition, and sidewall corrosion, leading to device failure due to non-volatile compounds and limitations in etching small critical dimension (CD) or densely pitched features.
A method combining atomic layer etching (ALE) and ion beam etching (IBE) is employed, where ALE forms volatile byproducts and IBE removes residue, minimizing sidewall redeposition and tapering, while IBE trims the MRAM sidewalls to a vertical shape.
This integrated approach effectively patterns dense MRAM arrays without redeposition or corrosion, overcoming limitations of IBE by allowing etching of high aspect ratio and dense pitch structures, ensuring vertical sidewalls and reducing device failure risks.
Smart Images

Figure 0007577115000001 
Figure 0007577115000002 
Figure 0007577115000003
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority to U.S. Application No. 62 / 901,702, filed Sep. 17, 2019, which is incorporated by reference herein for all purposes. [Background technology]
[0002] The discussion of the background art provided herein is intended to provide a general overview of the present disclosure. Nothing described in this Background section, and potentially any aspect of this specification, is admitted, expressly or impliedly, as prior art to this application.
[0003] FIELD OF THE DISCLOSURE The present disclosure relates to methods of forming semiconductor devices on a semiconductor wafer, and more particularly, to selective etching of semiconductor devices.
[0004] In the formation of semiconductor devices, magnetic random access memories (MRAMs) may be formed using a pattern transfer process. Such a pattern transfer process employs an etching process. MRAM stacks contain non-volatile ferromagnetic materials (such as cobalt (Co), iron (Fe), manganese (Mn), nickel (Ni), platinum (Pt), palladium (Pd), and ruthenium (Ru)) that are extremely difficult to pattern without the use of complex techniques such as ion beam etching (IBE), reactive ion etching (RIE), and wet chemistry. Despite years of development, current patterning techniques still suffer from many shortcomings, such as tapered features and sidewall redeposition that causes shorting of magnetic tunnel junctions (MTJs) to the pinned layer, as well as corrosion that causes damage to the MTJ layer. In some conventional techniques, chlorine-containing chemistries are used for metal etching, but the post-etch by-products include non-volatile compounds. The non-volatile compounds can then be redeposited on the sidewalls of the features. However, as devices become smaller and the fabrication of various types of structures becomes more complex, some of the etch by-products may redeposit on other exposed areas of the substrate, causing defects and ultimately device failure.
[0005] For large critical dimension (CD) structures with wide pitch, single-step or multi-step IBE recipes may be sufficient. However, for features with small CDs or tight pitches below 100 nm, patterning by IBE is challenging. A particular limitation is the blocking of ion incidence by the mask, which prevents effective etching and trimming of the MRAM stack. Summary of the Invention
[0006] To achieve the foregoing in accordance with the objectives of the present disclosure, a method is provided for selectively etching a stack of layers relative to a mask, an atomic layer etch is provided for at least partially etching the stack of layers to form at least some residue, and an ion beam etch is provided for etching the stack of layers to remove at least some of the residue from the atomic layer etch.
[0007] In another embodiment, an apparatus for selectively etching a layer stack relative to a mask is provided. A vacuum transfer module is provided. An atomic layer etch chamber is connected to the vacuum transfer module. An ion beam etch chamber is connected to the vacuum transfer module. An encapsulation chamber is connected to the vacuum transfer module. A controller is controllably connected to the vacuum transfer module, the atomic layer etch chamber, the ion beam etch chamber, and the encapsulation chamber. The controller is configured to control the vacuum transfer module to transfer the layer stack from the vacuum transfer module to the atomic layer etch chamber, control the atomic layer etch chamber to provide an atomic layer etch of the layer stack, control the vacuum transfer module to transfer the layer stack to the ion beam etch chamber, control the ion beam etch chamber to provide an ion beam etch of the layer stack, control the vacuum transfer module to transfer the layer stack from the ion beam etch chamber to the encapsulation chamber, and control the encapsulation chamber to provide encapsulation of the layer stack.
[0008] These and other features of the present disclosure are described in more detail below in the detailed description of the present disclosure taken in conjunction with the following drawings. [Brief description of the drawings]
[0009] The present disclosure is illustrated by way of example, and not limitation, in the figures of the accompanying drawings, in which like reference numbers refer to similar elements and in which:
[0010] [Figure 1] 1 is a high level flow chart of an embodiment.
[0011] [Figure 2A] 1 is a schematic cross-sectional view of a laminate processed according to an embodiment. [Figure 2B] 1 is a schematic cross-sectional view of a laminate processed according to an embodiment. [Figure 2C] 1 is a schematic cross-sectional view of a laminate processed according to an embodiment.
[0012] [Diagram 3] 1 is a more detailed flow chart of an atomic layer etching process.
[0013] [Figure 4] A more detailed flow chart of the modification steps.
[0014] [Figure 5A] 4A-4C are cross-sectional views of metal layers processed according to embodiments in greater detail; [Figure 5B] 4A-4C are cross-sectional views of metal layers processed according to embodiments in greater detail; [Figure 5C] 4A-4C are cross-sectional views of metal layers processed according to embodiments in greater detail;
[0015] [Figure 6] Schematic diagram of an atomic layer etch chamber system.
[0016] [Figure 7] Schematic diagram of an ion beam etching chamber.
[0017] [Figure 8] 1 is a schematic top view of a processing tool that may be used in embodiments.
[0018] [Figure 9] FIG. 1 is a schematic diagram of a computer system that may be used to implement embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present disclosure will now be described in detail with reference to several preferred embodiments thereof, as illustrated in the accompanying drawings. In the following description, several specific details are set forth in order to provide a thorough understanding of the present disclosure. However, it will be apparent to one skilled in the art that the present disclosure may be practiced without some or all of these specific details. In other instances, well-known process steps and / or structures have not been described in detail in order not to unnecessarily obscure the present disclosure.
[0020] During semiconductor wafer processing, features may be etched through metal-containing layers. In the formation of magnetic random access memories (MRAM), multiple thin metal layers or films may be etched in succession to form stacks of magnetic tunnel junctions.
[0021] A magnetic tunnel junction (MTJ) consists of a thin dielectric barrier layer between two magnetic materials. Electrons pass through the barrier by the process of quantum tunneling. This can serve as the basis for magnetic memories that use spin-transfer torque.
[0022] Spin-transfer torque is an effect whereby the orientation of the magnetic layers in an MTJ can be changed using spin-polarized current. Charge carriers (e.g., electrons) have a property known as spin. Spin is a small amount of angular momentum inherent to the carrier. The current is typically unpolarized (50% spin-up electrons, 50% spin-down electrons). By passing a current through a thick magnetic layer (usually called the "pinned layer"), a spin-polarized current can be created that has more electrons of either spin. If this spin-polarized current is directed to a second, thinner magnetic layer (the "free layer"), angular momentum can be transferred to this layer and change its orientation. This effect can also be used to excite vibrations or to flip the orientation of a magnet.
[0023] Spin-transfer torque can be used to flip active elements in magnetic random access memories. Spin-transfer magnetic random access memories (STT-RAM or STT-MRAM) have the advantages of low power consumption and good scalability over conventional magnetoresistive random access memories (MRAM). MRAM uses magnetic fields to flip active elements.
[0024] Patterning of spin-transfer-transfer-memory (STT-RAM) devices is performed by reactive ion etching followed by ion beam etching (IBE) or full inert gas angle IBE. Reactive ion etching (RIE) processes typically result in tapered shapes and heavy sidewall redeposition of etch by-products. Also, chemical damage to the MgO layer limits RIE to be the only process for MRAM patterning.
[0025] IBE technology has been developed to transfer MRAM patterns while minimizing damage to the MTJ caused by reactive species. A common approach is to first perform IBE at normal incidence to shape the MTJ and minimize footing, and then provide IBE at oblique incidence to provide sidewall cleaning and remove redeposition from the initial step. Sidewall redeposition is present during pattern transfer because IBE relies on sputtering of inert ions. Cycles of IBE and oxidation are typically performed to remove shorting paths and stop at the MgO tunnel barrier, preserving the pristine continuous free layer for spin transport.
[0026] A method for plasma dry etching an MRAM stack is described in U.S. Patent No. 9,806,252, issued Oct. 31, 2017 by Tan et al., entitled "Dry Plasma Etch Method To Pattern MRAM Stack," which is incorporated by reference for all purposes. A method for providing ion beam etching is described in U.S. Patent No. 9,257,295, issued Feb. 9, 2016 by Singh et al., entitled "Ion Beam Etching System," which is incorporated by reference for all purposes.
[0027] For large critical dimension (CD) structures with wide pitch, single-step or multi-step IBE recipes may be sufficient. However, for features with small CDs or tight pitches below 100 nm, patterning by IBE is challenging. A particular limitation is the blocking of the ion incident by the mask. This limitation prevents effective etching and trimming of the MRAM stack.
[0028] In an embodiment, the primary pattern transfer is achieved by atomic layer etching (ALE). The ALE process incorporates Si species to form volatile etch by-products of cobalt (Co) and iron (Fe) containing materials. The chemical etching mechanism allows for minimal sidewall redeposition. ALE can therefore pattern tight pitches without aspect ratio limitations. Although a halogen plasma was included, the ALE process minimizes damage to the MgO compared to RIE because the Ar step of the ALE cycle removes and purges reactive species. The ALE process opens up the MRAM stack and defines the overall shape.
[0029] In this embodiment, a second step of IBE processing is applied to the MRAM pillars defined by the ALE. The IBE step contributes to the removal of sidewall residues minimizing potential damage from surfaces that have absorbed halogen species. IBE further trims the MRAM sidewalls towards a vertical profile. Because the ALE is used to etch the MTJ stack forming volatile by-products, the IBE step is not used in incidence angle mode to pattern the MRAM, but rather for cleaning at a grazing angle to remove stack residues and / or footing.
[0030] The integrated process of ALE and IBE has advantages in two aspects: 1) The IBE step efficiently removes halogen species on the surface and sidewalls of the MRAM stack. For ALE patterning, residual halogen species, such as from the chamber walls, are a concern as they leave a chlorinated surface layer. The sidewall residues can degrade electrical properties, causing device shorts or electrical signal degradation. Inert ions also remove the halogenated surface layer while leaving minimal halogen residues. 2) The integrated flow avoids the limitations of IBE for patterning high aspect ratio or dense pitch structures. Since the chemical etching with ALE mainly defines the MRAM pillars, the patterning limitations are no longer limited by the ion incidence angle with IBE. The integration used in the embodiments provides a solution for patterning high density MRAM arrays without redeposition or erosion across the MTJ sidewalls.
[0031] FIG. 1 is a high level flow chart of an embodiment for ease of understanding. In this embodiment, the stack is subjected to atomic layer etching (step 104). The stack may include multiple layers of different materials. For example, the stack may include one or more layers of magnetic material used in conventional MRAM. FIG. 2A is a schematic cross-sectional view of an exemplary stack 200 that may be processed using the process shown in FIG. 1. The stack 200 may be made of silicon or silicon oxide (Si / SiO 2 The first tantalum (Ta) layer 208 is on a substrate having a Si / SiO 22. A first Ta layer 208 is overlying the first Ta layer 204. A platinum (Pt) layer 212 is overlying the first Ta layer 208. A cobalt platinum alloy (CoPt) layer 216 is overlying the Pt layer 212. A magnesium oxide (MgO) layer 220 is overlying the CoPt layer 216. A cobalt iron boron (CoFeB) layer 224 is overlying the MgO layer 220. A second Ta layer 228 is overlying the CoFeB layer 224. A ruthenium (Ru) layer 232 is overlying the second Ta layer 228. A patterned mask is formed over the stack 200. In this embodiment, the patterned mask is formed over the SiO 2 layer 244 under the Ru layer 244. 2 A titanium nitride layer 236 is provided below layer 240. In this embodiment, an optional Ru layer 244 opening etch is provided prior to the atomic layer etch (step 104). The Ru layer 244 opening etch is provided using an oxygen-containing plasma.
[0032] FIG. 3 is a more detailed flow chart of the atomic layer etch (step 104). The atomic layer etch includes multiple cycles, each cycle including a modification step (step 304) and an activation step (step 308). FIG. 4 is a more detailed flow chart of the modification step. A modification gas is provided (step 404). The modification gas may be any suitable gas capable of modifying a surface to facilitate the activation step. For example, the modification gas may be a halogen-containing gas. In one embodiment, the modification gas is 5-200 sccm of silicon tetrachloride (SiCl 4 The modified gas is turned into a plasma (step 408). In some exemplary conditions, the plasma may be generated using a plasma power of about 100 to about 900 W (Watts). The temperature during this operation may be about 60 to about 200° C. The chamber pressure during this operation may be about 1 to about 500 mTorr. Without being bound to any particular theory, the plasma may be generated using a SiCl 4 The molecules are said to dissociate to produce chlorine and Si-Cl species. In some examples, a pulsed bias may be applied. The Si-Cl species form a modified layer of Si-Cl moieties that are adsorbed on the metal layer. For different metals M in different layers, the chlorine and Si-Cl moieties are adsorbed on the different metals M to produce MSiCl. xwhere x is an integer from 1 to 3 inclusive. This atomic layer may be a monolayer, may be thicker than a monolayer, or may be an incomplete monolayer.
[0033] 5A-5C illustrate the molecular interactions while the stack is being processed. In particular, FIG. 5A-5C show the stack of FIG. 2A being processed. FIG. 5A is an enlarged schematic view of a portion of the CoFeB layer 224. SiCl 4 The modified gas is converted into a plasma of species including Si508 and Cl512. The species in the plasma are SiCl x (x is an integer from 1 to 3 inclusive). In addition, there may be individual chloride ions. The bias is SiCl x The species are accelerated into the CoFeB layer 224. x The bonded layer 224 bonds to the exposed top surface of CoFeB layer 224 and forms a monolayer.
[0034] In this embodiment, the modification step (step 304) stops after the monolayer is formed. x 1 is an enlarged schematic diagram of a portion of the CoFeB layer 224 after a monolayer of has been formed to form a modified surface of the portion of the CoFeB layer 224. The bias, and / or the modification gas flow, and / or the plasma power may be stopped.
[0035] After the atomic layers are formed and the modification step (step 304) is completed, the stack 200 is subjected to an activation step (step 308). The activation step may include providing a gas capable of being activated, such as a gas capable of generating a plasma. For example, the activation gas may be a noble gas. In this embodiment, the stack 200 is exposed to an argon (Ar) plasma to provide the activation step (step 308). In this embodiment, an activation gas comprising Ar is provided. The activation gas is activated. The activation gas may be activated by forming the activation gas into a plasma. The plasma may be generated using a plasma power of about 100 to 900 W. The temperature during this operation may be about 60 to about 300° C. The chamber pressure during this operation may be about 1 to about 500 mTorr. The Ar plasma is provided with MSiClx The molecules are volatilized and MSiCl x The molecules can be removed. As a result, the modified surface of the metal layer can be selectively etched with respect to the mask. The surface modification can then be used to etch the stack 200. In other embodiments, thermal activation can be used to activate the activation gas.
[0036] 5C is an enlarged schematic view of a portion of the CoFeB layer 224 during the activation stage. Argon ions 516 are accelerated by a bias towards the CoFeB layer 224. The Ar ions 516 react with MSiCl x The complex is activated (M represents the metal, in this case CoFeB) and reacted with volatile MSiCl x Complex 520 is formed. The bias is MSiCl x The Ar ions 516 are provided with enough energy to volatilize the complexes 520, but not enough energy to etch the redeposited residues. The steps of providing a modification step (step 304) and an activation step (step 308) are repeated cyclically multiple times to provide an atomic layer etch (step 104) of the layer stack 200.
[0037] 2B is a schematic cross-sectional view of stack 200 after ALE (step 104) is applied. A residue layer 248 of redeposited residual material is formed on the sidewalls of stack 200. Residue layer 248 includes residues of metal materials, silicon, and chlorine. Some of the chlorine may migrate to certain layers, such as MgO layer 220, and erode the layers to form MgO regions impregnated with chlorine 252. The deposition of residue layer 248 on the sidewalls of stack 200 causes the etch of stack 200 to taper as shown with a non-vertical surface.
[0038] After ALE (step 104) of the stack 200 is completed, the stack 200 is subjected to IBE (step 108). Ion beam etching refers to the removal of atoms by physical sputtering using an inert gas. The physical sputtering is provided by momentum exchange between ions of the inert gas and the material to be etched by collisions between the ions. In an embodiment, the chamber pressure is kept below 20 mTorr. The low pressure reduces ion collisions with the gas and reduces the possibility of plasma formation. In this embodiment, the ions are argon ions. In other embodiments, other ions different from those provided by the activated gas may be used. The ions are accelerated to have an energy in the range of 50 to 1800 volts (V). The ions have sufficient energy to sputter the residue layer 248 and the M atoms or molecules.
[0039] 2C is a schematic cross-sectional view of stack 200 after IBE (step 108) is applied. IBE (step 108) removes residue layer 248 and chlorine 252 that has impregnated MgO layer 220. IBE (step 108) also removes or reduces taper. In this example, the sidewalls of stack 200 are vertical due to taper removal by IBE (step 108).
[0040] The ALE (step 104) can etch higher aspect ratio features than the IBE process alone. Also, features provided by the above embodiments can have higher pitch than features formed by the IBE process alone. The ALE process alone can result in more tapered stacking with sidewall deposition. If the IBE process (step 108) is not provided, the chlorine 252 that permeates and attacks the MgO layer 220 would etch a portion of the MgO layer 220. The IBE process (step 108) can reduce or eliminate the taper and the residue layer 248. The IBE process (step 108) can remove the chlorine 252 that permeates the MgO layer 220 without etching a portion of the MgO layer 220.
[0041] In this embodiment, ALE (step 104) can etch all layers of stack 200 in one recipe. Because stack 200 is relatively thin (e.g., less than 30 nm thick), ALE (step 104) can be performed in less than 15 minutes. The IBE process (step 108) can also remove or reduce a footer on the bottom surface of stack 200. In other embodiments, ALE (step 104) at least partially etches stack 200.
[0042] In various embodiments, stack 200 may be a stack of MRAM. In various embodiments, stack 200 may be a magnetic tunnel junction (MTJ) consisting of a thin dielectric barrier layer between two magnetic materials. In various embodiments, stack 200 includes at least one metal-containing layer. The metal-containing layer may include at least one of Cr, Mo, Ir, Ti, Ru, Mn, Ni, Pd, Ta, Co, Fe, Mg, and Pt. In an example, stack 200 includes at least one MgO layer. Other stacks may have other transition metals (e.g., group IV transition metals, group V transition metals, and group VI transition metals) including metals such as Cu in the first, second, and third columns.
[0043] In the above embodiment, the modifying gas is SiCl 4 In another embodiment, the modifying gas comprises a halosilane. Examples of halosilanes are iodosilanes, bromosilanes, chlorosilanes, hydrochlorosilanes, and fluorosilanes. Specific chlorosilanes include tetrachlorosilane, trichlorosilane, dichlorosilane, monochlorosilane, chloroallylsilane, chloromethylsilane, dichloromethylsilane, chlorodimethylsilane, chloroethylsilane, t-butylchlorosilane, di-t-butylchlorosilane, chloroisopropylsilane, chloro-sec-butylsilane, t-butyldimethylchlorosilane, thexyldimethylchlorosilane, SiHCl-(N(CH 3 ) 2 ) 2In some embodiments, silicon in the modified gas may be replaced with germanium, carbon, titanium, or tin. In various embodiments, the modified gas includes a halogen-containing gas that includes an element selected from the group consisting of silicon, germanium, carbon, titanium, and tin. In other embodiments, metallic silicon and molecular chlorine (MSiCl x ) may be more generally described as a metal tetrel halogen molecule. In this specification and claims, a metal tetrel halogen molecule is defined as a molecule having at least one metal atom, at least one halogen atom, and at least one of the following Group 14 elements: silicon, germanium, silicon, titanium, and tin. When the metal tetrel halogen molecule includes silicon, the metal tetrel halogen molecule is a volatile metal-silo complex. In another embodiment, M(SiCl 3 )(CO) to produce SiCl 4 and CO precursors may be used. In another embodiment, MCl x (H 2 O) y To form Cl 2 and H 2 A precursor of O may be used. In another embodiment, methanol (CH 3 OH) precursors may be used.
[0044] In other embodiments, the reactive gas may be another noble gas other than Ar. In other embodiments, the reactive gas may be carbon monoxide (CO), water (H 2 O), CH 3 OH, or ammonia (NH 3 ) The reactant gas is converted into reactant gas ions.
[0045] In some embodiments, ALE (step 104) may be used to provide an overetch. The overetch may be performed using silicon or silicon oxide (Si / SiO 2) layer 204. The overetch reduces the taper of the stack 200 etched by ALE (step 104). The overetch silicon or silicon oxide (Si / SiO 2 During the etch of the .sup.2+.sup.3) layer 204, less material is redeposited and the residual layer 248 may be etched away and the taper may be reduced. An overetch may be used to reduce or eliminate the stack footer.
[0046] One or more additional processes may be performed on the stack before, during, or after the above steps in the above embodiments. For example, an additional IBE opening step may be used to partially open stack 200 before ALE (step 104). Such a step may open the CoFeB layer and allow opening of the CoFeB layer without exposing the CoFeB to halogen. In another embodiment, ALE (step 104) and IBE (step 108) may be provided cyclically for at least two cycles. Such a process may have a slow throughput.
[0047] Additionally, the sequence of the exemplary processes described above may be modified in any beneficial manner. For example, other embodiments may provide an IBE before an ALE to etch a layer, and then use an IBE after the ALE to remove residue. Still other embodiments may etch one or more layers using an IBE, then etch one or more layers using an ALE, then etch one or more layers using an IBE, and then etch one or more layers using an ALE.
[0048] 6 shows a schematic of an example of an ALE chamber system 600 that may be used in the ALE process to provide an embodiment of a process chamber that may be used in the ALE process (step 104). The ALE chamber system 600 includes a plasma reactor 602 having a plasma processing confinement chamber 604 therein. A plasma power supply 606 regulated by a plasma matching network 608 supplies power to a transformer coupled plasma (TCP) coil 610 located near a dielectric inductive power window 612 to generate a plasma 614 in the plasma processing confinement chamber 604 by providing inductively coupled power. A pinnacle 672 (PINNACLE is a registered trademark) extends from a chamber wall 676 of the plasma processing confinement chamber 604 to the dielectric inductive power window 612 to form a pinnacle ring. The pinnacle 672 is angled relative to the chamber wall 676 and the dielectric induced power window 612 such that the interior angles of the pinnacle 672 and the chamber wall 676 and the pinnacle 672 and the dielectric induced power window 612 are each greater than 90° and less than 180°. The pinnacle 672 provides an angled ring near the top of the plasma processing confinement chamber 604 as shown. The TCP coil (top power) 610 may be configured to generate a uniform diffusion profile within the plasma processing confinement chamber 604. For example, the TCP coil 610 may be configured to generate a toroidal power distribution in the plasma 614. The dielectric induced power window 612 is provided to space the TCP coil 610 from the plasma processing confinement chamber 604 while allowing energy to pass from the TCP coil 610 to the plasma processing confinement chamber 604. The TCP coil 610 functions as an electrode to provide radio frequency (RF) power to the plasma processing confinement chamber 604. A wafer bias voltage power supply 616, regulated by a bias matching network 618, provides power to an electrode 620 to set a bias voltage for a substrate 666. The substrate 666 is supported by the electrode 620, so that the electrode functions as a substrate support. A controller 624 controls the plasma power supply 606 and the wafer bias voltage power supply 616.
[0049] The plasma power source 606 and the wafer bias voltage power source 616 may be configured to operate at a particular radio frequency (e.g., 13.56 megahertz (MHz), 27 MHz, 2 MHz, 60 MHz, 400 kilohertz (kHz), 2.54 gigahertz (GHz), or a combination thereof). The plasma power source 606 and the wafer bias voltage power source 616 may be appropriately sized to provide a range of power to achieve a desired process performance. For example, in one embodiment, the plasma power source 606 may provide a power in the range of 50-5000 watts, and the wafer bias voltage power source 616 may provide a bias voltage in the range of 20-2000 V. Additionally, the TCP coil 610 and / or the electrode 620 may include two or more auxiliary coils or electrodes. The auxiliary coils or electrodes may be powered by a single power source or multiple power sources.
[0050] As shown in FIG. 6, the ALE chamber system 600 further comprises a gas source / gas supply mechanism 630. The gas source 630 is in fluid communication with the plasma processing confinement chamber 604 through a gas inlet (e.g., gas injector 640). The gas injector 640 may be located at any advantageous location in the plasma processing confinement chamber 604 and may take any form to inject gas. However, the gas inlet may be preferably configured to generate an “adjustable” gas injection profile. The adjustable gas injection profile may independently adjust the respective gas flows to multiple zones of the plasma processing confinement chamber 604. More preferably, the gas injector is mounted in the dielectric induction power window 612. The gas injector may be mounted in, within, or form part of the power window. Process gases and by-products are removed from the plasma processing confinement chamber 604 through a pressure control valve 642 and a pump 644. A pressure control valve 642 and pump 644 also function to maintain a particular pressure inside the plasma processing confinement chamber 604. The pressure control valve 642 can maintain a pressure of less than 1 Torr during processing. An edge ring 660 is disposed around the periphery of the substrate 666. The gas source / gas delivery mechanism 630 is controlled by a controller 624. A Kiyo by Lam Research Corporation of Fremont, Calif. may be used to implement the embodiment.
[0051] FIG. 7 depicts a simplified cross-sectional view of an ion beam etching chamber 700 for performing ion beam etching according to a particular method to illustrate an embodiment of the ion beam etching chamber. In this example, a substrate 701 rests on a substrate support 703. The ion beam etching chamber 700 may include hardware (not shown) for providing electrical and fluidic connections. The electrical connections may be used to provide electricity to the substrate support 703 or, in some cases, an electrostatic chuck located on or within the substrate support 703, and the fluidic connections may be used to provide fluids used to control the temperature of the substrate 701 and the substrate support 703. The substrate support 703 may be heated by a heater (not shown) and / or cooled by a cooling mechanism (not shown). Any suitable cooling mechanism may be used. In one example, the cooling mechanism may involve flowing a cooling fluid through piping in or adjacent to the substrate support 703. The substrate support 703 may be able to rotate and tilt at various speeds and angles, as indicated by the double arrow in FIG. 7. The rotation and tilt cause the ion beam to be incident at successively different angles. The IBE at various angles exposes more of the residue layer 248 to the IBE and removes the residue layer 248 faster.
[0052] A plasma generating gas is supplied to the primary plasma generating region 705. The plasma generating gas is excited by a plasma source 707. In the situation of Figure 7, the plasma source 707 is a coil acting as an inductively coupled plasma source. Other sources such as capacitively coupled sources, microwave sources, or discharge sources may be used in appropriately designed reactors. A plasma is formed in the primary plasma generating region 705. An extraction electrode 709 includes a series of openings 710 through which ions are extracted.
[0053] The apertures 710 may have a diameter of about 0.5-1 cm and a height defined by the thickness of the electrode. The apertures 710 may have a height-to-width aspect ratio (AR) of about 0.01-100.0. In some cases, the apertures 710 are arranged in a hexagon, a square grid, or a spiral, although other patterns may be used. The center-to-center distance between adjacent apertures may be about 1 mm-10 cm. The apertures may be configured to obtain a total open area (i.e., the sum of the areas of each aperture) that is about 0.1-95% of the surface area of the electrode when considering only one side of the electrode (top or bottom). For example, an electrode with a diameter of 40 cm and 500 holes, each with a diameter of 1 cm, would have an open area of about 31% (393 cm 2 Opening area ÷ 1257cm 2 (total area of the aperture 710). The aperture 710 may have different diameters in different electrodes. In some cases, the diameter of the aperture is smaller in the top electrode and larger in the bottom electrode. In one embodiment, the aperture in the bottom electrode 713 is larger (e.g., about 0-30% larger) than the aperture in the focusing electrode 711. In these or other cases, the aperture in the focusing electrode 711 is larger (e.g., about 0-30% larger) than the aperture in the extraction electrode 709.
[0054] A bias V applied to the extraction electrode 709 with respect to the substrate 701 1 The bias V functions to provide kinetic energy to the ions relative to the substrate. This bias is generally positive and may be about 20 to 10,000 volts or more. In certain cases, the bias of the extraction electrode is about 20 to 2,000 volts. Positive ions in the plasma above the extraction electrode 709 are attracted to the lower electrode 713 by the potential difference between electrodes 709 and 713. A focusing electrode 711 is added to focus the ions and repel electrons as needed. The bias V of this electrode is 2 can be positive or negative with respect to the extraction electrode 709, but is generally negatively biased. The bias potential of the focusing electrode 711 is determined by the lens characteristics of the focusing electrode 711. The bias voltage of the focusing electrode 711 is about 1.1 to 20 times the potential V of the extraction electrode. 1 Including the positive voltage, approximately 0.001 to 0.95 × V 1The potential gradient may be on the order of about 1000 V / cm. An exemplary separation distance between adjacent electrodes is within about 0.1-10 cm (e.g., about 1 cm).
[0055] After the ions leave the bottom of the grounded lower electrode 713, they travel in a parallel focused beam if the voltage of the focusing electrode 711 is set to produce a parallel beam. Alternatively, the beam can diverge if the focusing electrode voltage is adjusted to make the ion beam under-focused or over-focused. In many (but not all) cases, the lower electrode 713 is grounded. Using a grounded lower electrode 713 in conjunction with a grounded substrate 701 results in a substantially field-free substrate processing region 715. Having the substrate located in a field-free region prevents electrons or secondary ions resulting from collisions between the ion beam and residual gases or surfaces in the reaction chamber from being accelerated towards the substrate, thereby minimizing the risk of undesired damage or secondary reactions occurring.
[0056] It is also important to prevent the substrate 701 from becoming charged, either from the ion beam itself or from emitted secondary electrons produced during ion beam collisions with the substrate. Neutralization is typically accomplished by adding a low energy electron source (not shown) near the substrate 701. The positive charge of both the ions and the emitted secondary electrons causes the substrate to become positively charged, so low energy electrons near the substrate can be attracted to the positively charged surface and neutralize this charge. This neutralization is much easier to achieve in a field free area.
[0057] In some applications it may be desirable to have a potential difference between the bottom electrode 713 and the substrate 701. For example, if very low energy ions are required, it is difficult to maintain a highly parallel beam over long distances at low energy due to the mutual repulsion of positively charged ions (space charge effect). One solution to this is to apply a negative bias to the bottom electrode 713 with respect to the substrate 701 (or conversely, to positively bias the substrate 701 with respect to the bottom electrode 713). This allows the ions to be extracted with high energy and to decelerate the ions as they approach the substrate.
[0058] Electrode 709, electrode 711, and electrode 713 each have a constant thickness. This thickness may be about 0.5 mm to 10 cm, or about 1 mm to 3 cm (e.g., about 5 mm). Electrode 709, electrode 711, and electrode 713 may each have the same thickness, or may have different thicknesses. Furthermore, the separation distance between extraction electrode 709 and focusing electrode 711 may be the same as, longer than, or shorter than the separation distance between focusing electrode 711 and lower electrode 713.
[0059] The apertures 710 in the extraction electrode 709, focusing electrode 711, and bottom electrode 713 may be precisely aligned with each other. Otherwise, ions will be misdirected and on-wafer etching results will be poor. For example, if one aperture in the focusing electrode 711 is misaligned, one portion of the substrate 701 will be over-etched (excess ions will be directed) and another portion of the substrate 701 will be under-etched (no or few ions will be directed). Therefore, the apertures should be aligned as closely as possible to each other. In various cases, the misalignment between vertically adjacent electrodes is limited to about 1% of the aperture diameter or less (measured by the distance of the linear shift in the aperture position relative to the adjacent aperture).
[0060] Ion beam etching processes are typically performed at low pressure. In some embodiments, the pressure may be about 100 mTorr or less (e.g., about 1 mTorr or less), and in many cases about 0.1 mTorr or less. The low pressure helps to minimize undesirable collisions between the ions and any gas species present in the substrate processing region. In certain cases, reactants at relatively high pressures are provided to an otherwise low pressure ion processing environment.
[0061] In an embodiment, the processing tool may provide a platform that provides a chamber for the ALE process, a chamber for the IBE process, and a chamber for encapsulating the resulting device. FIG. 8 is a top schematic view of a processing tool 800 used in an embodiment. A cassette 802 contains unprocessed wafers before they are processed and holds processed wafers once all processing is completed in the processing tool 800. The cassette 802 can hold many wafers, often as many as 25 wafers. An atmospheric transfer module (ATM) 814 is used to transfer wafers to and from the cassette 802. A load lock station 805 represents at least one device that operates to transfer wafers back and forth between the atmosphere of the ATM 814 and the vacuum of the vacuum transfer module (VTM) 812. The VTM 812 is part of the processing tool and is connected to multiple chambers. There may be different types of chambers. In this embodiment, there are two ALE chambers 600, two ion beam etching chambers 700, and one encapsulation chamber 828. In this embodiment, the ALE chamber 600 is a Kiyo® manufactured by Lam Research, Fremont, California. The ion beam etch chamber 700 is a Kyber® manufactured by Lam Research, Fremont, California. The containment chamber 828 may be a plasma enhanced chemical vapor deposition (PECVD) chamber or another dielectric deposition chamber (such as a VECTOR® PECVD chamber manufactured by Lam Research, Fremont, California). A robotic system within the vacuum transfer module 812 uses a robotic arm to move stacked wafers between the load lock station 805 and the different chambers 600, 700, and chamber 828. The ATM 814 uses a robotic system to transfer wafers between the cassette 802 and the load lock station 805 in a vacuum environment. A controller 835 may be used to control the processing tool 800. The controller 835 may include one or more sub-controllers.A controller 835 , which may comprise one or more sub-controllers, is controllably connected to the vacuum transfer module 812 , the atomic layer etch chamber 600 , the ion beam etch chamber 700 , and the containment chamber 828 .
[0062] 9 is a high-level block diagram illustrating a computer system 900. The computer system 900 is suitable for implementing the controller 835 used in the embodiments. The computer system 900 may have many physical forms, ranging from integrated circuits, printed circuit boards, and small handheld devices to large supercomputers. The computer system 900 includes one or more processors 902 and may further include an electronic display device 904 (for displaying images, text, and other data), a main memory 906 (e.g., random access memory (RAM)), a storage device 908 (e.g., a hard disk drive), a removable storage device 910 (e.g., an optical disk drive), a user interface device 912 (e.g., a keyboard, touch screen, keypad, mouse, or other pointing device, etc.), and a communication interface 914 (e.g., a wireless network interface). The communication interface 914 allows software and data to be transferred between the computer system 900 and external devices over a link. The system may include a communications infrastructure 916 (eg, a communications bus, crossover bar, or network) to which the devices / modules are connected.
[0063] Information transferred through communications interface 914 may be in the form of signals, which may be electronic, electromagnetic, optical, or other signals that carry signals and may be received by communications interface 914 over a communications link, which may be provided using wire or cable, optical fiber, telephone line, cellular phone link, radio frequency link, and / or other communications line. Using such communications interface 914, one or more processors 902 may receive information from a network or output information to a network in the course of performing the method steps described above. Additionally, method embodiments may be performed on a processor alone or may be performed over a network, such as the Internet, in cooperation with a remote processor that shares some of the processing.
[0064] The term "non-transitory computer-readable medium" is generally used to refer to media such as main memory, secondary memory, removable storage, and storage devices (e.g., hard disks, flash memory, disk drive memory, CD-ROMs, and other forms of persistent memory), and should not be construed to include transitory objects such as carrier waves or carrier signals. Examples of computer-readable code include machine code (e.g., produced by a compiler) and files containing higher level code that are executed by a computer using an interpreter. The computer-readable medium may also be computer code transmitted to a processor by a computer data signal.
[0065] In some embodiments, the computer readable medium may include computer readable code for transferring the stack to the ALE chamber 600, computer readable code for performing the ALE process (step 104), computer readable code for transferring the stack to the ion beam etching chamber 700, computer readable code for performing the ion beam etching (step 108), computer readable code for transferring the stack 200 to the containment chamber 828, computer readable code for encapsulating the stack 200, and computer readable code for removing the stack 200 from the processing tool 800 to an atmosphere. Encapsulating the stack after the stack 200 is etched and before the stack 200 is exposed to the atmosphere prevents the various layers of the stack from oxidizing. Oxidation of the various layers of the stack 200 can cause device failure. The processing tool 800 integrated with the ALE chamber 600, the ion beam etching chamber 700, and the containment chamber 828 provides a faster throughput of etched MRAM.
[0066] While the present disclosure has been described in terms of several preferred embodiments, there are changes, modifications, permutations, and various substitute equivalents that fall within the scope of the present disclosure. It should also be noted that there are many alternative ways of implementing the methods and apparatuses of the present disclosure. It is therefore intended that the following appended claims be interpreted to include all such changes, modifications, permutations, and various substitute equivalents that fall within the true spirit and scope of the present disclosure. The present disclosure may be realized in the following forms. [Form 1] 1. A method for selectively etching a stack relative to a mask, comprising: providing an atomic layer etch to at least partially etch the stack, the atomic layer etch forming at least some residue; providing an ion beam etch of the stack, the ion beam etch removing at least some of the residues from the atomic layer etch; A method comprising: [Form 2] 2. The method of claim 1, further comprising: The step of providing the atomic layer etch includes a plurality of cycles, each cycle comprising: A modification step, providing a modification gas comprising a halogen-containing gas containing an element selected from the group consisting of silicon, germanium, carbon, titanium, and tin; a modification stage including a step of forming a modified surface by converting the modified gas into a plasma, the components of the plasma modifying a portion of the surface of the stack; an activation step, the activation step etching the modified surface of the stack; A method comprising: [Form 3] 3. The method of claim 2, further comprising: The method of claim 1, wherein the halogen-containing gas is selected from the group consisting of iodosilanes, bromosilanes, chlorosilanes, hydrochlorosilanes, and fluorosilanes. [Form 4] 3. The method of claim 2, further comprising: The activation step comprises: providing an activation gas; activating the activation gas; A method comprising: [Form 5] 5. The method of claim 4, further comprising: The method, wherein the activating step further comprises applying a bias. [Form 6] 3. The method of claim 2, further comprising: The method of claim 1, wherein the activation step produces a metal tetrel halogen molecule. [Form 7] 7. The method of claim 6, further comprising: The method of claim 1, wherein the metal tetrel halogen molecule comprises a metal, silicon, and a halogen. [Form 8] 2. The method of claim 1, further comprising: The method, wherein the stack comprises at least one metal-containing layer. [Form 9] 2. The method of claim 1, further comprising: The stack comprises at least one transition metal-containing layer. [Form 10] 2. The method of claim 1, further comprising: The method, wherein the step of providing ion beam etching comprises directing gas ions at successively different angles to the layer stack. [Form 11] 11. The method of claim 10, further comprising: The method, wherein the ion beam etching removes a tapered portion of the stack. [Form 12] 11. The method of claim 10, further comprising: The method, wherein the ion beam etching removes halogens impregnated in metal-containing layers of the stack. [Form 13] 11. The method of claim 10, further comprising: The method of claim 1, wherein the ion beam etching removes chlorine impregnated in the metal-containing layer of the stack without etching the metal-containing layer of the stack. [Form 14] 2. The method of claim 1, further comprising: The step of providing the atomic layer etch includes a plurality of cycles, each cycle comprising: A modification step, providing a modified gas comprising a halogen-containing gas; a modification stage including a step of forming a modified surface by converting the modified gas into a plasma, the components of the plasma modifying a portion of the surface of the stack; an activation step, the activation step etching the modified surface of the stack; A method comprising: [Form 15] 2. The method of claim 1, further comprising: The method comprising providing an ion beam aperture etch prior to providing said atomic layer etch. [Form 16] 1. An apparatus for selectively etching a layered film relative to a mask, comprising: A vacuum transfer module; an atomic layer etching chamber connected to the vacuum transfer module; an ion beam etching chamber connected to the vacuum transfer module; an enclosure chamber connected to the vacuum transfer module; a controller controllably connected to the vacuum transfer module, the atomic layer etch chamber, the ion beam etch chamber, and the containment chamber, controlling the vacuum transfer module to transfer the stack to the atomic layer etching chamber; controlling the atomic layer etch chamber to provide an atomic layer etch of the layer stack; controlling the vacuum transfer module to transfer the stack from the atomic layer etch chamber to the ion beam etch chamber; controlling the ion beam etching chamber to provide ion beam etching of the stack; controlling the vacuum transfer module to transfer the stack from the ion beam etching chamber to the containment chamber; a controller configured to control the encapsulation chamber to provide encapsulation of the stack; and An apparatus comprising: [Form 17] 17. The apparatus according to claim 16, The controller further comprises: controlling the atomic layer etch chamber to provide a modifying gas; An apparatus configured to control the atomic layer etch chamber to form a plasma of the modifying gas, wherein components of the plasma are configured to modify a portion of a surface of the deposition to form a modified surface. [Form 18] 18. The apparatus of claim 17, The controller further comprises: controlling the atomic layer etch chamber to provide an activation gas; An apparatus configured to control the atomic layer etch chamber to activate the activation gas. [Form 19] 19. The apparatus of claim 18, The apparatus, wherein the controller is further configured to control the atomic layer etch chamber to apply a bias.
Claims
1. 1. A method for selectively etching a stack relative to a mask, comprising: providing an atomic layer etch to at least partially etch the stack, the atomic layer etch forming at least some residue; providing an ion beam etch of the stack, the ion beam etch removing at least some of the residues from the atomic layer etch; A method comprising:
2. 2. The method of claim 1 , The step of providing the atomic layer etch includes a plurality of cycles, each cycle comprising: A modification step, providing a modification gas comprising a halogen-containing gas containing an element selected from the group consisting of silicon, germanium, carbon, titanium, and tin; a modification stage including a step of forming a modified surface by converting the modified gas into a plasma, the components of the plasma modifying a portion of the surface of the stack; an activation step, the activation step etching the modified surface of the stack; A method comprising:
3. 3. The method of claim 2, The method of claim 1, wherein the halogen-containing gas is selected from the group consisting of iodosilanes, bromosilanes, chlorosilanes, hydrochlorosilanes, and fluorosilanes.
4. 3. The method of claim 2, The activation step comprises: providing an activation gas; activating the activation gas; A method comprising:
5. 5. The method of claim 4, The method, wherein the activating step further comprises applying a bias.
6. 3. The method of claim 2, The method of claim 1, wherein the activation step produces a metal tetrel halogen molecule.
7. 7. The method of claim 6, The method of claim 1, wherein the metal tetrel halogen molecule comprises a metal, silicon, and a halogen.
8. 2. The method of claim 1 , The method, wherein the stack comprises at least one metal-containing layer.
9. 2. The method of claim 1 , The method, wherein the stack comprises at least one transition metal-containing layer.
10. 2. The method of claim 1 , The method, wherein the step of providing ion beam etching comprises directing gas ions at successively different angles to the layer stack.
11. 11. The method of claim 10, The method, wherein the ion beam etching removes a tapered portion of the stack.
12. 11. The method of claim 10, The method, wherein the ion beam etching removes halogens impregnated in metal-containing layers of the stack.
13. 11. The method of claim 10, The method of claim 1, wherein the ion beam etching removes chlorine impregnated into the metal-containing layer of the stack without etching any portion of the metal-containing layer of the stack.
14. 2. The method of claim 1 , The step of providing the atomic layer etch includes a plurality of cycles, each cycle comprising: A modification step, providing a modified gas comprising a halogen-containing gas; a modification stage including a step of forming a modified surface by converting the modified gas into a plasma, the components of the plasma modifying a portion of the surface of the stack; an activation step, the activation step etching the modified surface of the stack; A method comprising:
15. 10. The method of claim 1 further comprising: The method comprising providing an ion beam aperture etch prior to providing said atomic layer etch.
16. 1. An apparatus for selectively etching a layered film relative to a mask, comprising: A vacuum transfer module; an atomic layer etching chamber connected to the vacuum transfer module; an ion beam etching chamber connected to the vacuum transfer module; an enclosure chamber connected to the vacuum transfer module; a controller controllably connected to the vacuum transfer module, the atomic layer etch chamber, the ion beam etch chamber, and the containment chamber, controlling the vacuum transfer module to transfer the stack to the atomic layer etching chamber; controlling the atomic layer etch chamber to provide an atomic layer etch of the layer stack; controlling the vacuum transfer module to transfer the stack from the atomic layer etch chamber to the ion beam etch chamber; controlling the ion beam etching chamber to provide an ion beam etch of the stack to remove at least a portion of the residue formed by the atomic layer etch; controlling the vacuum transfer module to transfer the stack from the ion beam etching chamber to the containment chamber; a controller configured to control the encapsulation chamber to provide encapsulation of the stack; and An apparatus comprising:
17. 17. The apparatus of claim 16, The controller further comprises: controlling the atomic layer etch chamber to provide a modifying gas; An apparatus configured to control the atomic layer etch chamber to form a plasma of the modifying gas, wherein components of the plasma are configured to modify a portion of a surface of the deposition to form a modified surface.
18. 18. The apparatus of claim 17, The controller further comprises: controlling the atomic layer etch chamber to provide an activation gas; An apparatus configured to control the atomic layer etch chamber to activate the activation gas.
19. 20. The apparatus of claim 18, The apparatus, wherein the controller is further configured to control the atomic layer etch chamber to apply a bias.
Citation Information
Patent Citations
Surface treatment apparatus
JP1990116126A
Semiconductor manufacturing apparatus and semiconductor device manufacturing method
JP2013243307A
Buffer station for thermal control of semiconductor substrates transferred therethrough, and method of transferring semiconductor substrates
JP2016105462A
Dry plasma etching method for patterning MRAM stack
JP2016208031A
Atomic layer etching of al203 using combination of plasma and vapor treatments
JP2017157836A