Low radioactive alumina powder and its manufacturing method
A method for producing low-radioactivity alumina powder by dispersing and drying alumina in acidic solutions with silane coupling agents reduces uranium content to 5 ppb, addressing cost and security issues in existing methods, suitable for high thermal conductivity applications.
Patent Information
- Application Number
- JP2023196007
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-21
- Filing Date
- 2023-11-17
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-11-17
AI Technical Summary
Existing methods for producing low-radioactivity alumina powder are expensive and pose security risks, and they struggle to achieve uranium contents below 8 ppb, which is necessary for high thermal conductivity applications like chip packaging fillers.
A method involving firing aluminum hydroxide with low uranium content, dispersing it in an acidic solution, replacing the solvent with a silane coupling agent, and drying to reduce uranium content to 5 ppb or less, using specific conditions and agents.
The method effectively reduces uranium content to 5 ppb or less, ensuring low radioactivity and suitability for high thermal conductivity applications.
Smart Images

Figure 0007577182000002 
Figure 0007577182000003 
Figure 0007577182000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of alumina, and in particular to low radioactive alumina powder and a method for producing the same. [Background technology]
[0002] With the development of new energy vehicles and 5G communication industries, the amount of heat generated by chips and other devices with signal transmission and memory functions during operation is rapidly increasing. In order to ensure the reliability of the devices during operation, it is necessary to improve the heat dissipation performance of the devices. Therefore, spherical alumina, which has higher thermal conductivity, is usually selected as the packaging filler instead of spherical silicon oxide.
[0003] In order to avoid "soft errors" occurring when the signal of the element is transmitted, it is necessary to strictly manage and control the radioactive elements such as uranium (U) and thorium (Th) in the filler. Since the content of uranium (U) element in ordinary alumina reaches several hundred ppb, it is necessary to obtain a low-radioactive raw material with a low content of uranium (U) element so that a low-radioactive spherical alumina product that meets the requirements can be obtained after spheroidization. Japanese patent JP-A11-92136 uses high-purity aluminum powder (uranium, thorium content < 1 ppb) as the raw material for spheroidization to obtain a low-radioactive spherical alumina product by the deflagration method, but this method is expensive and has certain security risks. Chinese patent CN102249276A discloses a low-radioactive spherical alumina product with a specific surface area SSA of 0.3 to 3 m 2 The aluminum hydroxide having a uranium content of less than 10 ppb, more preferably 8 ppb or less, is used as raw material at a temperature of 1000° C. / g, and then sprayed into a flame, and the powder is collected to obtain a spherical alumina product, but the U content of the obtained spherical alumina can only reach a level of 8 ppb or less. In order to further reduce the uranium (U) content in the product and meet the need for a lower uranium (U) content in the spherical alumina product, the present invention reports a method for producing low radioactive alumina powder. Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention provides a low radioactivity alumina powder having a surface uranium content of 5 ppb or less and a method for producing the same. [Means for solving the problem]
[0005] In order to achieve the above object, the present invention provides the following technical solutions: S1 is a process for obtaining alumina powder by calcining aluminum hydroxide having a surface uranium content of 30 ppb or less in a roasting device; S2: Prepare an acidic solution with pH<4, then soak the alumina powder in the acidic solution and disperse it uniformly for 0.5-2 h; After separating the dispersed powder from the acidic solution, the powder is placed in a solvent containing a silane coupling agent for 0.5 to 6 hours for solvent replacement (S3); and S4, after separating the solvent-substituted powder, drying the powder under conditions of 100 to 120°C for 2 to 6 hours to obtain low-radioactive alumina powder having a surface uranium content of 5 ppb or less.
[0006] Preferably, in the S1, the specific surface area of the aluminum hydroxide is 60 m 2 / g or more, and the average particle size is 2 to 100 μm.
[0007] Preferably, in the above S1, the firing is carried out at 500 to 1200° C. for 0.5 to 4 hours.
[0008] Preferably, in S2, the acidic solution is one or more of hydrochloric acid, nitric acid, boric acid, and citric acid.
[0009] Preferably, in the step S2, the dispersion method is one of dispersion by stirring, dispersion by ultrasonic wave, and dispersion by a rocking reactor.
[0010] Preferably, in S3, the silane coupling agent includes one of hexamethyldisilazane, hexamethyldisiloxane, methyltrimethoxysilane, and methyltriethoxysilane.
[0011] Preferably, in S3, the solvent includes one of ethanol and n-hexane. Effect of the Invention
[0012] The present invention aims to design a low-radioactivity alumina powder and a manufacturing method thereof, by reducing the surface uranium content in the alumina material to a level of 5 ppb or less, and dispersing the alumina in an acidic solution, and dispersing the uranium adsorbed on the surface of the alumina single crystal under acidic conditions into the solution to produce uranyl ions (UO2 2+ ) and then displace it with the solvent of the silane coupling agent, and the acidic solution remaining in the alumina gap under the action of surface tension and the uranyl ions (UO2 2+ ) is replaced outside the alumina powder, and finally, high-temperature drying treatment is performed to reduce the uranium content, reducing the uranium content of the raw material from approximately 30 ppb to less than 5 ppb, thereby meeting the needs of producing low-radioactivity spherical alumina. [Brief description of the drawings]
[0013] [Figure 1] 1 is a scanning electron micrograph of the surface topography of low-radioactivity alumina powder. [Diagram 2] 1 is a scanning electron micrograph of the surface topography of low-emissivity spherical alumina powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Example 1 (1) Surface uranium content is 30 ppb or less, and the specific surface area is 60 m 2 Aluminum hydroxide powder with a molecular weight of 40 μm or more and an average particle size of 40 μm was calcined at 1000°C for 4 hours to obtain alumina powder.
[0015] (2) The calcined alumina powder was immersed in a hydrochloric acid solution of pH 3.5, and stirred and ultrasonically dispersed for 1 hour.
[0016] (3) The alumina powder was separated from the solution and immersed in a n-hexane solution containing hexamethyldisiloxane for 3 hours to exchange the solvent.
[0017] (4) The alumina powder in the solution was separated and dried at 120℃ for 4h to obtain low radioactive alumina powder.
[0018] Example 2 (1) Surface uranium content is 30 ppb or less, and the specific surface area is 60 m 2 Aluminum hydroxide powder with a molecular weight of 1000g or more and an average particle size of 10 μm was calcined at 1000°C for 4 hours to obtain alumina powder.
[0019] (2) The calcined alumina powder was immersed in a hydrochloric acid solution of pH 3.5, and stirred and ultrasonically dispersed for 1 hour.
[0020] (3) The alumina powder was separated from the solution and soaked in a solution of hexamethyldisiloxane in n-hexane for 3 hours to exchange the solvent.
[0021] (4) The alumina powder in the solution was separated and dried at 120℃ for 4h to obtain low radioactive alumina powder.
[0022] Example 3 (1) Surface uranium content is 30 ppb or less, and the specific surface area is 60 m 2 Aluminum hydroxide powder with a molecular weight of 5 μm or more and an average particle size of 5 μm was calcined at 1000°C for 4 hours to obtain alumina powder.
[0023] (2) The calcined alumina powder was immersed in a hydrochloric acid solution of pH 3.5, and stirred and ultrasonically dispersed for 1 hour.
[0024] (3) After separating the alumina powder from the solution, it was immersed in a solution of hexamethyldisiloxane in n-hexane and subjected to solvent exchange for 3 hours.
[0025] (4) The alumina powder in the solution was separated and dried at 120℃ for 4h to obtain low radioactive alumina powder.
[0026] Example 4 The low radioactive alumina powder obtained in Example 3 was spheroidized using a spheroidization technique in which the flame region formed by the combustion of natural gas and oxygen gas was used as the spheroidization region. The average particle size of the spheroidized sample was 4.5 μm.
[0027] Comparative Example 1 (1) Surface uranium content is 30 ppb or less, and the specific surface area is 60 m 2 Aluminum hydroxide powder with a molecular weight of 40 μm or more and an average particle size of 40 μm was calcined at 1000°C for 4 hours to obtain alumina powder.
[0028] Comparative Example 2 (1) Surface uranium content is 30 ppb or less, and the specific surface area is 60 m 2 Aluminum hydroxide powder with a molecular weight of 5 μm or more and an average particle size of 5 μm was calcined at 1000°C for 4 hours to obtain alumina powder.
[0029] (2) The calcined oxide powder was immersed in a hydrochloric acid solution of pH 3.5, and stirred and ultrasonically dispersed for 1 h.
[0030] (3) The alumina powder was separated from the solution and calcined at 1000℃ for 4h to obtain low radioactive alumina powder.
[0031] Comparative Example 3 The low radioactive alumina powder obtained in Comparative Example 2 was spheroidized using a spheroidization technique, with the flame region formed by the combustion of natural gas and oxygen gas as the spheroidization region. The average particle size of the spheroidized sample was 4.5 μm.
[0032] The surface uranium content of the samples was measured by ICP-MS inductively coupled plasma mass spectrometry. 0.1g of alumina sample was digested in a digestion tank with sulfuric acid, nitric acid, and phosphoric acid for 30 min, then dried and acid-removed at 180°C. After acid removal, the sample was diluted to 100 ml with 1% nitric acid, and the diluted sample was detected by ICP-MS.
[0033] [Table 1]
[0034] As can be seen from the detection results, the manufacturing method described in the present invention can obtain low radioactive alumina powder with a uranium (U) content of less than 5 ppb, and the finer the particle size of the raw material, the better the purification effect. As can be seen from the test results of the comparative example, by dispersing the powder in an acidic solution and using solvent replacement, the uranium (U) content in the alumina powder can be significantly reduced to meet the needs for raw materials for low radioactive spherical alumina.
Claims
1. S1, which obtains alumina powder by calcining aluminum hydroxide having a surface uranium content of 30 ppb or less in a roasting device; S2: preparing an acidic solution with a pH of <4, and then soaking the alumina powder in the acidic solution and dispersing it uniformly for 0.5 to 2 h; After separating the dispersed powder from the acidic solution, the powder is placed in a solvent containing a silane coupling agent for 0.5 to 6 hours for solvent replacement (S3); and S4 of separating the solvent-substituted powder and then drying the powder under conditions of 100 to 120° C. for 2 to 6 hours to obtain a low-radioactive alumina powder having a surface uranium content of 5 ppb or less. A method for producing low radioactive alumina powder.
2. In the above S1, the specific surface area of aluminum hydroxide is 60 m 2 / g or more, and the average particle size is 2 to 100 μm.
2. The method for producing low radioactive alumina powder according to claim 1 .
3. In the above S1, the firing is performed at 500 to 1200 ° C. for 0.5 to 4 h.
2. The method for producing low radioactive alumina powder according to claim 1 .
4. In the step S2, the acid solution is one or more of hydrochloric acid, nitric acid, boric acid, and citric acid; 2. The method for producing low radioactive alumina powder according to claim 1 .
5. In the step S2, the dispersion method is one of dispersion by stirring, dispersion by ultrasonic wave, and dispersion by a rocking reactor; 2. The method for producing low radioactive alumina powder according to claim 1 .
6. In the above S3, the silane coupling agent includes one of hexamethyldisilazane, hexamethyldisiloxane, methyltrimethoxysilane, and methyltriethoxysilane; 2. The method for producing low radioactive alumina powder according to claim 1 .
7. In the above S3, the solvent includes one of ethanol and n-hexane; 2. The method for producing low radioactive alumina powder according to claim 1 .
Citation Information
Patent Citations
Preparation of alumina having extremely low content of radioactive element
JP1981155017A
Anisotropic alumina particle composite, its manufacturing method, resin composition and its manufacturing method
JP2006219356A
Silica particle and its production method
JP2007119331A
Method for producing spherical alumina powder
JP2011236118A