Method for producing secondary battery materials from black mass
A multi-step process for recovering lithium and secondary battery precursor metals from black mass in secondary battery scraps enhances recovery rates and purity, addressing low efficiency and environmental issues in existing methods.
Patent Information
- Application Number
- JP2023545250
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing methods for recovering lithium and secondary battery precursor metals from black mass in secondary battery scraps suffer from low recovery rates and high impurity levels, with varying auxiliary raw material usage and significant environmental impact.
A multi-step process involving firing, preliminary extraction, evaporation, leaching, liquid purification, and phosphate precipitation to produce high-purity lithium carbonate and nickel, cobalt, and manganese compounds, minimizing auxiliary raw material use and impurities.
Achieves recovery rates of 92% or more lithium and 95% or more nickel, cobalt, and manganese, reducing environmental pollution by recycling battery by-products and lowering processing costs.
Smart Images

Figure 0007577255000001 
Figure 0007577255000002 
Figure 0007577255000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing secondary battery materials such as lithium and precursor raw materials for secondary batteries (nickel (Ni), cobalt (Co), manganese (Mn)) from black mass recovered from secondary battery scrap. [Background technology]
[0002] In recent years, research has been continuously conducted into recovering lithium contained in black mass recovered from secondary battery scraps. A pre-extraction method is used in which black mass is reduced and fired to convert lithium peroxide to lithium carbonate, which is then distributed in a lithium aqueous solution and extracted, or a post-extraction method is used in which black mass is leached in a complex sulfate solution, and lithium is separated and extracted in a later process.
[0003] In the pre-extraction method, black mass is reduced and fired in a nitrogen atmosphere to reduce the lithium contained in the black mass to lithium carbonate, which is then recovered through a water leaching process, allowing high-purity lithium carbonate to be recovered with a very low impurity concentration. However, the lithium reduction rate is limited, so the lithium recovery rate is only about 85%.
[0004] The post-extraction method is a relatively simple process, since lithium is separated after black mass is extracted with a complex sulfate solution. However, the lithium waste rate due to the process by-products generated through various impurity removal processes is high, and the lithium recovery rate is only about 80%.
[0005] In addition, there is a problem that the amount of auxiliary materials such as hydrogen peroxide added when extracting black mass into sulfuric acid solution can differ by more than two times depending on whether the black mass is calcined or not. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to solve the problems associated with the pre-extraction and post-extraction processes of lithium from black mass and to improve the recovery rate of lithium and secondary battery precursor metals. [Means for solving the problem]
[0007] In order to solve the above problems, a method for producing a secondary battery material from black mass according to an embodiment of the present invention includes a calcination process (S10) for calcining black mass, a pre-extraction process (S20) for dissolving the calcined black mass obtained in the calcination process (S10) in water to separate the calcined black mass into a lithium (Li) solution and a cake, a first evaporation and concentration process (S30) for evaporating and concentrating the lithium (Li) solution produced in the pre-extraction process (S20) to produce lithium carbonate (Li2CO3) crystals, and a leaching process for leaching the cake separated in the pre-extraction process (S20). The process includes a first purification step (S40) of removing copper and aluminum from the leaching solution produced by the leaching step (S40), a post-extraction step (S60) of neutralizing the solution from the first purification step (S50) and separating it into a lithium (Li) solution and a cake containing Ni, Co, and Mn (NCM cake), and a transfer step of transferring the lithium carbonate (Li2CO3) crystals produced by the first evaporation and concentration step (S30) and the lithium (Li) solution separated by the post-extraction step (S60) to a lithium hydroxide (LiOH) production step.
[0008] According to an embodiment of the present invention, a method for producing a secondary battery material from black mass includes a phosphate precipitation step (S70) of producing a lithium phosphate (Li3PO4) cake by adding phosphoric acid (H3PO4) and sodium hydroxide (NaOH) to the lithium (Li) solution separated in the post-extraction step (S60), and a sulfate preparation step (S70) of producing a lithium sulfate (Li2SO4) solution by dissolving the lithium carbonate (Li2CO3) crystals produced in the first evaporation and concentration step (S30) and the lithium phosphate (Li3PO4) cake from the phosphate precipitation step (S70) in sulfuric acid. The method further includes a sulfate preparation step (S80), a carbonate precipitation step (S90) of precipitating lithium carbonate (Li2CO3) by adding sodium carbonate (Na2CO3) to the lithium sulfate (Li2SO4) produced in the sulfate preparation step (S80), a hydroxide preparation step (S100) of preparing a lithium hydroxide (LiOH) solution by adding calcium oxide (CaO) and water to the lithium carbonate (Li2CO3), and a second evaporation and concentration step (S110) of evaporating and concentrating the lithium hydroxide (LiOH) solution produced in the hydroxide preparation step (S100).
[0009] The method for producing a secondary battery material from black mass according to one embodiment of the present invention further includes a weak acid leaching process (S120) in which the NCM cake produced in the post-extraction process (S60) is dissolved with sulfuric acid to produce a solution containing Ni, Co, and Mn (NCM solution), a second purification process (S130) in which impurities are removed from the NCM solution produced in the weak acid leaching process (S120), and a process (S140) of delivering the NCM solution that has undergone the second purification process (S130) to, for example, a factory or facility that produces precursor raw materials.
[0010] The method for producing a secondary battery material from black mass according to an embodiment of the present invention further includes a step of repulping the NCM cake produced in the post-extraction step (S60) two or more times to remove residual sodium salts.
[0011] The first purification step (S50) includes a step of adding sodium hydrogen sulfide (NaHS) to remove copper (Cu) and adding sodium hydroxide (NaOH) to remove aluminum (Al).
[0012] The method for producing a secondary battery material from black mass according to an embodiment of the present invention further includes a step of evaporating and concentrating the lithium sulfate (Li2SO4) solution produced in the sulfate producing step (S80) to separate it into lithium sulfate (Li2SO4) crystals and phosphoric acid (H3PO4) filtrate.
[0013] The method for producing a secondary battery material from black mass according to an embodiment of the present invention further includes a repulping process for removing residual sodium salt from the lithium carbonate (Li2CO3) cake produced in the carbonate precipitation process (S90).
[0014] According to an embodiment of the present invention, the method for producing a secondary battery material from black mass further includes a step of removing impurities by adding aluminum sulfate (Al2(SO4)3) to the solution in the sulfate producing step (S80). Effect of the Invention
[0015] According to the present invention, the recovery rate of lithium (Li) can be achieved at 92% or more through a high-yield process using black mass recovered from secondary batteries, and the recovery rates of nickel (Ni), cobalt (Co) and manganese (Mn), which are the raw materials for secondary batteries, can be achieved at 95% or more. In addition, there is an effect that a large amount of battery by-products can be recycled to reduce environmental pollution problems.
[0016] According to the present invention, the amount of auxiliary materials used during sulfuric acid leaching can be reduced through the process of reduction and calcination for pre-extraction of lithium.
[0017] According to the present invention, impurities can be removed to a concentration sufficient for producing a high-purity NCM complex sulfate solution by adjusting the number of times of the purification step and the pH.
[0018] According to the present invention, by combining a pre-extraction process, which is a dry process, and a post-extraction process, which is a wet process, the recovery rate of valuable metals such as nickel (Ni), cobalt (Co), and manganese (Mn) can be improved, and lithium (Li) can be effectively separated from black mass.
[0019] According to the present invention, the process of recovering lithium from the lithium (Li) solution in the post-extraction process having a high impurity content and the process of recovering lithium carbonate (Li2CO3) from the lithium (Li) solution in the pre-extraction process having a relatively low impurity content after evaporation and concentration are separated and operated as separate purification processes, thereby reducing lithium loss in the lithium purification process and reducing processing costs. [Brief description of the drawings]
[0020] [Figure 1] This is a process diagram of transferring lithium (Li) produced from black mass through a pre-extraction process and a post-extraction process to a lithium hydroxide (LiOH) production process. [Diagram 2] FIG. 1 is a process diagram for producing high-purity lithium hydroxide (LiOH). [Diagram 3] FIG. 1 is a process diagram for producing a high-purity NCM (Ni, Co, Mn) solution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present invention will now be described with reference to the drawings.
[0022] FIG. 1 is a process diagram of the transfer of lithium (Li) produced from black mass through a pre-extraction process and a post-extraction process to a lithium hydroxide (LiOH) production process.
[0023] [Firing process (S10)] This is a process in which black mass is put into a firing furnace and reduced and fired in a nitrogen (N2) atmosphere at 800-900°C for 1-3 hours. The reaction in the furnace is as shown below (Equation 1).
[0024] 2Li(NCM)O2+2CO→Li2CO3+NCM+(NCM)O+CO2…(Formula 1)
[0025] By calcining black mass in an inert nitrogen atmosphere, lithium (Li) can be converted into a form that dissolves in water. In the process of reducing and calcining black mass for lithium pre-extraction, some high oxides (Me2O3, Me=Ni, Co, Mn) are reduced to low oxides (MeO, Me=Ni, Co, Mn), reducing the amount of auxiliary materials (H2O2, hydrogen peroxide) used during sulfuric acid leaching.
[0026] [Preliminary extraction process (S20)] This is a process in which water is added to the calcined black mass that has been reduced and calcined in the calcination process (S10) and lithium (Li) is leached and separated at 20-30°C for 1-3 hours to produce a lithium carbonate (Li2CO3) solution. More than 65% of the total lithium (Li) can be obtained by separating it from the reduced and calcined black mass using water.
[0027] Through the pre-extraction process (S20), it is possible to reduce the operating costs and auxiliary raw material costs of the subsequent phosphate precipitation process (S70), and it is possible to minimize the inclusion of impurities in the high-purity lithium hydroxide (LiOH) manufacturing process, thereby reducing the processing costs of the lithium hydroxide (LiOH) manufacturing process.
[0028] [First evaporation concentration step (S30)] This is a process for producing lithium carbonate (Li2CO3) crystals by evaporating and concentrating the filtrate from the pre-extraction process (S20).
[0029] [Leaching process (S40)]
[0030] In the pre-extraction step (S20), the cake produced by pre-extracting lithium is reduced and leached with sulfuric acid (H2SO4) and hydrogen peroxide (H2O2) at 80 to 85°C for 8 hours. The reaction formula is as follows:
[0031] MeO+H2SO4→MeSO4+H2O [Me=Ni / Co / Mn]…(Eq. 2)
[0032] Me2O3+2H2SO4+H2O2→2MeSO4+2H2O+O2…(Formula 3)
[0033] Me+H2SO4→MeSO4+H2[Me=Ni / Co / Mn]…(Formula 4)
[0034] When nickel (Ni), cobalt (Co) and manganese (Mn) are leached from the cake from which lithium (Li) has been pre-extracted through the pre-extraction process (S20), the amount of auxiliary materials used can be minimized and stable process management can be achieved in a continuous process.
[0035] [First liquid purification process (S50)] In contrast to solvent extraction, which requires complex equipment configuration, environmental risks, and high processing costs, this is a primary liquid purification process that is designed to remove impurities such as copper (Cu), aluminum (Al), and silicon (Si) from the leaching solution (sulfate solution) produced in the leaching process (S40) using only a simple precipitation reaction, improving the efficiency of impurity removal.
[0036] The copper removal (Cu) process involves adding sodium hydrogen sulfide (NaHS) (1.2eq) and reacting it at 60~80℃ for 4 hours to precipitate and remove Cu in the liquid as CuS, and the reaction formula is as follows (Formula 5). Here, the unit eq means equivalent, which means a fixed amount allocated to each element or compound based on the quantitative relationship of substances in a chemical reaction.
[0037] 2CuSO4+2NaHS→2CuS↓+Na2SO4+H2SO4…(Formula 5)
[0038] The dealumination (Al) process involves adding sodium hydroxide (NaOH) (pH 4.0) and reacting for 8 hours at 70-85°C to precipitate and remove aluminum (Al) as Al(OH). The reaction formula is as follows (Formula 6).
[0039] Al2(SO4)3+6NaOH→2Al(OH)3↓+3Na2SO4…(Formula 6)
[0040] In the process of precipitating aluminum (Al) into Al(OH)3, some of the Fe and Si are co-precipitated and removed.
[0041] [Post-extraction step (S60)] The filtrate from the first purification step (S50) is neutralized (pH 10-12) with sodium hydroxide (NaOH) and reacted at 70-85°C for 4 hours to precipitate and recover nickel (Ni), cobalt (Co), and manganese (Mn), while lithium (Li) is distributed in the filtrate and separated. In the post-extraction step (S60), the precipitation rate of nickel (Ni), cobalt (Co), and manganese (Mn) is 99.9% or more.
[0042] The filtered NCM cake is repulped two or more times to remove residual sodium salts. The sodium content in the cake is reduced from 3.43% to 0.4%.
[0043] FIG. 2 is a process diagram for producing high purity lithium hydroxide (LiOH).
[0044] The high-purity lithium hydroxide (LiOH) manufacturing process is a process in which lithium sulfate (Li2SO4) is manufactured by adding sulfuric acid to lithium carbonate (Li2CO3) recovered through the above-mentioned pre-extraction process (S20) and first evaporation and concentration process (S30) and lithium phosphate (Li3PO4) precipitated from the lithium solution separated and recovered through the post-extraction process (S60), lithium carbonate (Li2CO3) is manufactured by adding sodium carbonate (Na2CO3) to the lithium sulfate, and lithium hydroxide (LiOH) solution is manufactured by adding calcium oxide (CaO) to the lithium carbonate (Li2CO3) and evaporating and concentrating it, thereby manufacturing high-purity lithium carbonate (Li2CO3) and high-purity lithium hydroxide (LiOH·H2O) with excellent lithium recovery rate. The specific high-purity lithium hydroxide (LiOH) manufacturing process is as follows.
[0045] [First evaporation concentration step (S30)] As described above, this is the process of producing lithium carbonate (Li2CO3) crystals by evaporating and concentrating the filtrate from the pre-extraction process (S20).
[0046] [Phosphate precipitation step (S70)] This is a process in which phosphoric acid (H3PO4) (1.2eq) is added to the lithium (Li) solution produced in the post-extraction process (S60) and reacted at 70~85℃ for 2 hours to precipitate and recover lithium (Li) in the form of lithium phosphate (Li3PO4). Sodium hydroxide (NaOH) is added to neutralize the solution to pH 10.0~12.0, and the reaction formula is as follows:
[0047] 3Li2SO4+2H3PO4→2Li3PO4↓+3H2SO4…(Formula 7)
[0048] Li2CO3+H3PO4→Li3PO4↓+H2O+CO2…(Formula 8)
[0049] H2SO4+2NaOH→Na2SO4+2H2O…(Formula 9)
[0050] Lithium phosphate (Li3PO4) has a lower solubility than lithium carbonate (Li2CO3), so the lithium (Li) precipitation recovery rate (94.0%) is high (the solubility of lithium phosphate (Li3PO4) is Li 0.07g / L at 25°C, and the solubility of lithium carbonate (Li2CO3) is Li 2.4g / L at 25°C). The concentration of lithium (Li) in the filtrate from the phosphate precipitation step (S70) is 0.1g / L, and the lithium loss is 6.0%.
[0051] Preferably, a step for removing P (0.5 g / l) (dephosphorization (P) step) may be required to purify the filtrate from the phosphate precipitation step (S70). The dephosphorization step can be carried out at 50 to 70° C. and pH 5.5 to 6.5 for 4 hours. The reaction formula is as follows:
[0052] Al2(SO4)3+2H3PO4→2AlPO4+3H2SO4…(Eq. 10)
[0053] [Sulfate manufacturing process (S80)] This is a process to produce lithium sulfate (Li2SO4) solution (Li 35g / l) by leaching the cake containing lithium phosphate (Li3PO4) produced in the phosphate precipitation process (S70) and the lithium carbonate (Li2CO3) crystals produced in the first evaporation and concentration process (S30) in sulfuric acid. At this time, the temperature is 60-80℃, the reaction time is 2 hours, and the pH is 2.0 or less. The reaction formula is as follows.
[0054] 2Li3PO4+3H2SO4→3Li2SO4+2H3PO4…(Formula 11)
[0055] Li2CO3+H2SO4→Li2SO4+H2O+CO2…(Formula 12)
[0056] The solution (lithium carbonate (Li2CO3) solution) produced in the lithium (Li) pre-extraction process (S20) is evaporated and concentrated to recover lithium carbonate (Li2CO3), which is then fed to the sulfate production process (S80).
[0057] Since the lithium carbonate (Li2CO3) does not go through the phosphate precipitation process (S70), the amount of phosphoric acid (H3PO4) and sodium hydroxide (NaOH) used is reduced by more than 40%, and the loss of lithium (Li) distributed to the filtrate of the phosphate precipitation process (S70) is greatly reduced.
[0058] Preferably, the lithium sulfate (Li2SO4) solution produced in the sulfate production process (S80) can be evaporated and concentrated to separate it into lithium sulfate (Li2SO4) crystals and phosphoric acid (H3PO4) filtrate. The phosphoric acid (H3PO4) filtrate can be recycled to the phosphate precipitation process (S70) and used as a secondary material for lithium precipitation. The evaporated condensed water generated in the evaporation and concentration process can be recycled as a process liquid for the lithium (Li) pre-extraction process. This can reduce the amount of waste liquid generated outside the system and the amount of new water flowing into the system.
[0059] [Carbonate precipitation process (S90)] This is a process in which lithium carbonate (Li2CO3) is precipitated by adding sodium carbonate (Na2CO3) to lithium sulfate (Li2SO4) produced in the sulfate production process (S80) and reacting it at 80~85℃ for 4 hours. The reaction formula is as follows.
[0060] Li2SO4+Na2CO3→Li2CO3↓+Na2SO4…(Formula 13)
[0061] Preferably, a repulping step can be carried out to remove residual sodium (Na) salts from the cake of the carbonate precipitation step (S90). To minimize the loss of lithium (Li), repulping is carried out at 80°C (Li 1.6g / L). The filtrate (Li 1.6g / L) of the carbonate precipitation step (S90) is recycled to the phosphate precipitation step (S70).
[0062] Preferably, impurities (P, Fe, etc.) in the solution of the sulfate salt production process (S80) can be removed through a dephosphorization (P) process before precipitating lithium carbonate (Li2CO3). By adding aluminum sulfate (Al2(SO4)3) to the solution produced in the sulfate salt production process (S80), adjusting the pH to 5.0-6.0, and reacting at 50-70°C for 4 hours, most of the phosphorus (P) can be precipitated and removed, and iron (Fe) and other impurities can also be co-precipitated and removed. The reaction formula is as follows:
[0063] Al2(SO4)3+2H3PO4→2AlPO4+3H2SO4…(Eq. 14)
[0064] [Hydroxide manufacturing process (S100)] This is a process in which calcium oxide (CaO) and water are added to the lithium carbonate (Li2CO3) cake produced in the carbonate precipitation process (S90) and reacted at 70~80℃ for 2 hours to convert it into lithium hydroxide (LiOH) solution. The reaction formula is as follows.
[0065] Li2CO3(s)+CaO(s)+H2O→2LiOH(aq)+CaCO3(s)…(Equation 15)
[0066] When the concentration of lithium (Li) in the solution is up to 10 g / L, the conversion rate to lithium hydroxide (LiOH) is over 95%.
[0067] Preferably, the hydroxide salt production step (S100) can be carried out twice.
[0068] Preferably, a repulping step can be carried out to recover lithium (Li) contained in the calcium carbonate (CaCO3) residue produced in the hydroxide salt production step (S100).
[0069] [Second evaporation concentration step (S110)] This process produces LiOH·H2O product by evaporating and concentrating the lithium hydroxide (LiOH) solution produced in the hydroxide salt production process (S100) in a nitrogen (N2) atmosphere. The total recovery rate of lithium (Li) up to the LiOH·H2O production process is over 92%. FIG. 3 is a process diagram for producing a high-purity NCM (Ni, Co, Mn) solution, and relates to a process for producing an NCM solution by leaching and purifying the cake produced in the post-extraction step (S60) with sulfuric acid.
[0070] In the first purification step (S50), the pH is stepwise increased to pH 4 to primarily remove impurities, and then in the second purification step (S130), the pH is adjusted to pH 5 to remove impurities to a concentration sufficient for producing a high-purity NCM complex sulfate solution. The residue from the second purification step (S130) is reused in the leaching step (S40), minimizing valuable metals (Ni, Co, Mn, and Li) distributed as process by-products and increasing the recovery rate. The specific steps are as follows:
[0071] [Weak acid leaching process (S120)] The NCM cake from which lithium (Li) has been separated in the post-extraction process (S60) is leached in sulfuric acid (H2SO4) (pH 1.5-2.5) at 60-80°C for 4 hours. A small amount of reducing agent can be added to improve the dissolution rate of the NCM cake. In this case, the reducing agent is hydrogen peroxide (H2O2).
[0072] [Second liquid purification process (S130)] This is a secondary purification process that removes copper (Cu) and aluminum (Al) contained in the NCM solution produced by the weak acid leaching process (S120) to 5 mg / L or less. The copper removal process involves adding 1.2 eq of sodium hydrogen sulfide (NaHS) and reacting at 60-80°C for 4 hours. The aluminum removal process involves reacting at pH 4.0-5.5 and at a temperature of 70-85°C for 8 hours.
[0073] [NCM solution delivery step (S140)] The NCM solution from which copper and aluminum have been removed through the second purification step (S130) is sent to, for example, a factory or facility that produces precursor materials, and is manufactured according to the composition.
[0074] [Example] In this example, LiOH·H2O product and NCM solution were prepared through the above-mentioned process. The detailed conditions for each process are as follows.
[0075] Firing step (S10) - Firing was carried out in a furnace at 900°C in a nitrogen (N2) atmosphere for 2 hours.
[0076] Pre-extraction step (S20) - Water at 25°C was added to the calcined black mass that had been reduced and calcined in the calcination step (S10), and leaching was carried out for 2 hours.
[0077] The filtrate from the first evaporation concentration step (S30)-pre-extraction step (S20) was evaporated and concentrated.
[0078] The cake produced by pre-extracting lithium in the leaching process (S40)-pre-extraction process (S20) was charged with sulfuric acid and 60% hydrogen peroxide (H2O2) to perform leaching for 8 hours at a temperature of 80°C with a nickel (Ni) concentration of 100g / L in the filtrate and a final pH of 3.0. The amount of hydrogen peroxide (H2O2) charged was 5wt% of the cake raw material.
[0079] 1.2 eq of 30% sodium hydrogen sulfide (NaHS) was added to the leaching solution produced in the first purification step (S50)-leaching step (S40), and a copper removal (Cu) step was carried out at a temperature of 70°C for 4 hours. Sodium hydroxide (NaOH) was then added (pH 4.0), and a dealumination (Al) step was carried out at a temperature of 85°C for 8 hours.
[0080] Post-extraction step (S60) - Sodium hydroxide (NaOH) was added to the filtrate from the first purification step (S50) to adjust the pH to 11.0, and a separation step was carried out at a temperature of 85°C for 4 hours.
[0081] 1.2 eq of 85% phosphoric acid (H3PO4) was added to the lithium (Li) solution produced in the phosphate precipitation process (S70)-post-extraction process (S60), and sodium hydroxide (NaOH) was added to adjust the pH to 11.0. The precipitation process was carried out for 2 hours at a temperature of 70°C. In addition, 1.5 eq of aluminum sulfate (Al2(SO4)3) was added to purify the filtrate produced in the precipitation process, and the dephosphorization (P) process was carried out for 4 hours at a pH of 6.0 and a temperature of 60°C.
[0082] Sulfate production process (S80) - 1.1 eq of sulfuric acid was added to the cake containing lithium phosphate (Li3PO4) produced in the phosphate precipitation process (S70) and lithium carbonate (Li2CO3) crystals produced in the first evaporation and concentration process (S30) based on a lithium (Li) concentration of 35g / L, and the process was carried out for 2 hours under conditions of pH<2.0. In addition, the lithium sulfate (Li2SO4) solution produced in the sulfate production process (S80) was evaporated and concentrated to separate it into lithium sulfate (Li2SO4) crystals and phosphoric acid (H3PO4) filtrate.
[0083] Carbonate Precipitation Step (S90) - 1.2 eq of sodium carbonate (Na2CO3) was added to the lithium sulfate (Li2SO4) produced in the sulfate production step (S80), and the precipitation step was carried out at a temperature of 85°C for 4 hours.
[0084] 1.05 eq of calcium oxide (CaO) and water were added to the lithium carbonate (Li2CO3) cake produced in the hydroxide production process (S100)-carbonate precipitation process (S90), and the mixture was stirred at 70°C for 2 hours.
[0085] Second Evaporation and Concentration Step (S110)--The lithium hydroxide (LiOH) solution produced in the hydroxide salt production step (S100) was evaporated and concentrated in a nitrogen (N2) atmosphere.
[0086] The leaching process was carried out by adding 1.0 eq of sulfuric acid (H2SO4) and 60% hydrogen peroxide (H2O2) to the NCM cake from which lithium (Li) was separated in the weak acid leaching process (S120) and post-extraction process (S60) in an amount of about 5 wt% of the NCM cake.
[0087] Second purification process (S130) - 1.2 eq of 30% sodium hydrogen sulfide (NaHS) was added to the NCM solution produced by the weak acid leaching process (S120) and a copper removal (Cu) process was carried out at a temperature of 60°C for 4 hours. Sodium hydroxide (NaOH) was then added to adjust the pH to 5.0, and a dealumination (Al) process was carried out at a temperature of 85°C for 8 hours.
[0088] As a result of carrying out the process according to this embodiment, lithium hydroxide (LiOH) corresponding to 92% of the amount of lithium (Li) contained in the black mass can be recovered, which is a higher lithium recovery rate than the conventional pre-extraction method (85%) and the post-extraction method (80%).
[0089] In addition, as a result of carrying out the process according to this embodiment, 95% of nickel (Ni), cobalt (Co) and manganese (Mn) contained in the black mass could be recovered.
[0090] Although the present invention has been described in connection with certain embodiments herein, it should be understood that various modifications and changes may be made without departing from the spirit and scope of the present invention as would be understood by one of ordinary skill in the art to which the present invention pertains, and such modifications and changes are to be considered as falling within the scope of the claims appended hereto.
Claims
1. A firing step (S10) of firing black mass in a nitrogen atmosphere; A pre-extraction step (S20) of leaching the calcined black mass from the calcination step (S10) with water to separate it into a lithium (Li) solution and a cake; A first evaporation and concentration step (S30) of evaporating and concentrating the lithium (Li) solution produced in the pre-extraction step (S20) to produce lithium carbonate (Li2CO3) crystals; A leaching step (S40) of leaching the cake separated in the pre-extraction step (S20) with sulfuric acid and hydrogen peroxide; A first purification step (S50) for removing copper and aluminum from the leaching solution produced by the leaching step (S40); A post-extraction step (S60) of neutralizing the solution from the first purification step (S50) and separating it into a lithium (Li) solution and a cake containing Ni, Co, and Mn (NCM cake); The lithium carbonate (Li 2 CO 3 and a transport step of transporting the lithium (Li) solution produced by the post-extraction step (S60) and the lithium carbonate (Li 2 CO 3 ) crystals to a lithium hydroxide (LiOH) production step of producing lithium hydroxide (LiOH) using the lithium carbonate (Li 2 CO 3 ) crystals and the lithium (Li) solution. The lithium hydroxide (LiOH) production process includes: a phosphate precipitation step (S70) of adding phosphoric acid (H3PO4) and sodium hydroxide (NaOH) to the lithium (Li) solution produced by the post-extraction step (S60) to produce a lithium phosphate (Li3PO4) cake; a sulfate preparation step (S80) of preparing a lithium sulfate (Li2SO4) solution by leaching the lithium carbonate (Li2CO3) crystals produced in the first evaporation and concentration step (S30) and the lithium phosphate (Li3PO4) cake produced in the phosphate precipitation step (S70) with sulfuric acid; A carbonate precipitation step (S90) of precipitating lithium carbonate (Li2CO3) by adding sodium carbonate (Na2CO3) to the lithium sulfate (Li2SO4) produced in the sulfate production step (S80); A hydroxide salt producing step (S100) of producing a lithium hydroxide (LiOH) solution by adding calcium oxide (CaO) and water to the lithium carbonate (Li2CO3); and a second evaporation and concentration step (S110) of evaporating and concentrating the lithium hydroxide (LiOH) solution produced in the hydroxide salt production step (S100).
2. a weak acid leaching step (S120) in which the NCM cake produced in the post-extraction step (S60) is leached with sulfuric acid to produce a solution (NCM solution) having a pH of 1.5 to 2.5 and containing Ni, Co, and Mn; A second purification step (S130) for removing impurities from the NCM solution produced in the weak acid leaching step (S120); 2. The method for producing a secondary battery material from black mass according to claim 1, further comprising a step (S140) of transporting the NCM solution that has been subjected to the second purification step (S130) to a factory that produces precursor raw materials for secondary batteries.
3. 3. The method for producing a secondary battery material from black mass according to claim 2, further comprising the step of repulping the NCM cake produced in the post-extraction step (S60) two or more times to remove residual sodium salts.
4. 2. The method for producing a secondary battery material from black mass according to claim 1, wherein the first purification step (S50) includes the steps of adding sodium hydrogen sulfide (NaHS) to remove copper (Cu) and adding sodium hydroxide (NaOH) to remove aluminum (Al).
5. The lithium sulfate (Li 2 SO 4 ) solution was evaporated to obtain lithium sulfate (Li 2 SO 4 ) crystals and phosphoric acid (H 3 P.O. 4 2. The method for producing a secondary battery material from black mass according to claim 1, further comprising the step of separating the black mass into a filtrate.
6. The lithium carbonate (Li 2 CO 3 2. The method for producing a secondary battery material from black mass according to claim 1, further comprising a repulping step for removing residual sodium salts from the cake.
7. In the sulfate production step (S80), aluminum sulfate (Al 2 (SO 4 ) 3 2. The method for producing a secondary battery material from black mass according to claim 1, further comprising the step of removing impurities by introducing a sintered material such as ethyl alcohol.
Citation Information
Patent Citations
Method for purifying lithium hydroxide
JP2012106874A
Coated nickel hydroxide powder for alkaline secondary battery positive electrode active material and method for producing the same
JP2014103004A
Processing method of positive electrode active material waste of lithium ion secondary battery
JP2020072032A
Method for producing lithium hydroxide