Water- and oil-repellent film-forming liquid composition and method for producing same

By bonding fluorine-based functional groups to metal oxide particles and silica sol-gel in a specific ratio, the composition addresses the limitations of conventional film-forming liquids, achieving enhanced oil repellency, strength, and reduced fingerprint visibility.

JP7577472B2Active Publication Date: 2024-11-05MITSUBISHI MATERIALS ELECTRONICS CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020120307
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-14
Publication Date
2024-11-05
Estimated Expiration
2040-07-14

AI Technical Summary

Technical Problem

Conventional film-forming liquid compositions using fluorine-containing composite particles fail to achieve high oil repellency, film strength, and hardness, and are prone to fingerprint visibility issues.

Method used

A liquid composition is developed by bonding fluorine-based functional groups to metal oxide particles and silica sol-gel, with specific ratios of metal oxide particles, fluorine-containing compounds, and silica sol-gel, to enhance oil repellency, film hardness, and reduce fingerprint visibility.

Benefits of technology

The composition achieves high oil repellency, improved film strength, and reduced fingerprint visibility, with excellent adhesion to substrates and uniform film formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577472000015
    Figure 0007577472000015
  • Figure 0007577472000016
    Figure 0007577472000016
  • Figure 0007577472000001
    Figure 0007577472000001
Patent Text Reader

Abstract

To provide a liquid composition that forms a film which, in comparison with a film formed with a conventional liquid composition, has higher water repellency, oil repellency, film strength, and film hardness and which makes fingerprints on the film surface inconspicuous.SOLUTION: A liquid composition for forming a water- and oil-repellent film comprises: metal oxide particles (B) having an average particle diameter of 2 nm to 90 nm, to which is bonded a first fluorine-based functional group component (A1) containing a perfluoroether structure represented by formula (1); a silica sol gel (C) containing a second fluorine-based functional group component (A2) containing the perfluoroether group structure represented by formula (1); and a solvent (D). When a total amount of components except the solvent (D) is set to 100 mass%, a content ratio of a sum of the first fluorine functional group component (A1) and the second fluorine functional group component (A2) is 1 mass% to 30 mass% and a mass ratio (C:B) is in a range of 10:90 to 90:10.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid composition for forming a water- and oil-repellent film having water and oil repellency, and a method for producing the same, and more particularly to a liquid composition for forming a water- and oil-repellent film containing metal oxide particles, and a method for producing the same. [Background technology]

[0002] So far, there has been disclosed a method for producing fluorine-containing nanocomposite particles, which includes a step (first step) of preparing a dispersion of an inorganic compound by dispersing an inorganic compound such as SiO2, CaCO3, TiO2, etc. in an organic solvent such as an alcohol, and a step (second step) of adding a fluorine compound containing a perfluoroalkyl group and a catalyst to the dispersion of the inorganic compound to synthesize a composite material in which the inorganic compound and the fluorine compound are nanocomposite (for example, see Patent Document 1 (paragraphs

[0047] ,

[0057] , and paragraphs

[0067] to

[0070] ).

[0003] Patent Document 1 describes that in the second step, a silane coupling agent containing silicon alkoxide such as tetramethoxysilane (TMOS) or tetraethoxysilane (TEOS) may be added to the dispersion liquid of the inorganic compound. Patent Document 1 also describes that when fluorine-containing nanocomposite particles are dispersed in water or an organic solvent such as alcohol to prepare a dispersion liquid of fluorine-containing nanocomposite particles, and this dispersion liquid is used as a coating agent, it becomes possible to impart functions such as water- and oil-repellency and hydrophilic and oil-repellency to the surfaces of various materials.

[0004] However, in the dispersion liquid (film-forming liquid composition) of fluorine-containing nanocomposite particles produced by the manufacturing method described in Patent Document 1, the inorganic compound (metal oxide particles) is hydrophilic and oil-repellent, so it was not possible to improve the hardness and strength of the film formed while maintaining the oil-repellent properties of the film.

[0005] For this reason, fluorine-containing composite particles that can exhibit higher water repellency and oil repellency than conventional ones have been proposed (for example, see Patent Document 2 (Claim 1, paragraphs

[0008] ,

[0039] to

[0054] )). The fluorine-containing composite particles are composite particles in which the surfaces of silica-based fine particles are covered with 1) a fluorine-containing compound and 2) at least one type of fluorine-containing group formed by siloxane bonding between the silicon of the silica-based fine particles, the fluorine-containing compound being a compound containing a functional group A represented by [-Si(OR)3] (wherein the three R's are the same or different and represent hydrogen or an alkyl group having 1 to 10 carbon atoms) on at least one end side of a main chain made of perfluoropolyether, and the fluorine content per unit surface area of ​​the silica-based fine particles is 0.8 mg / m 2 ~1.0g / m 2 It is characterized in that:

[0006] The above-mentioned fluorine-containing composite particles are manufactured by mixing silica-based fine particles or their dispersion with a solution of a fluorine-containing compound, and in particular by mixing the two and then stirring the mixture. The dispersion of silica-based fine particles and the solution of the fluorine-containing compound are prepared by dispersing them in water, a water-soluble organic solvent, or a mixture thereof. By mixing the dispersion of silica-based fine particles with the solution of the fluorine-containing compound and then stirring the mixture, a part or all of the functional group A can sufficiently react with the silica on the surface of the silica-based fine particles or the functional group on the silica surface to reliably form a siloxane bond.

[0007] After the stirring is completed, the fluorine-containing composite particles described in Patent Document 2 are obtained in the form of a slurry. Depending on the application, the fluorine-containing composite particles can be used as is in the form of a slurry, or can be used in the form of a substantially dried powder after subjecting the slurry to solid-liquid separation, washing, or other treatments as necessary. The fluorine-containing composite particles can also be used in the form of a dispersion obtained by further dispersing the fluorine-containing composite particles in a solvent. In addition, the slurry can be separated into a solid-liquid separation, and the cake obtained is dispersed in another solvent to obtain a dispersion. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2018-39987 A [Patent Document 2] International Publication No. WO2019 / 026816 Summary of the Invention [Problem to be solved by the invention]

[0009] In the film-forming liquid compositions disclosed in Patent Document 2, such as a slurry of fluorine-containing composite particles and a dispersion obtained by dispersing fluorine-containing composite particles in a solvent, the liquid composition can be applied to various articles to form a coating film on the surface of the article, thereby imparting water repellency and / or oil repellency to the article. However, there are problems in that the oil repellency is still insufficient, and the binding strength between the fluorine-containing composite particles is not sufficiently strong, so that the strength and hardness of the formed film are not high, and further improvement is required.

[0010] An object of the present invention is to provide a liquid composition for forming a water- and oil-repellent film, which forms a film having higher water repellency, oil repellency, film strength and film hardness and on whose surface fingerprints are less noticeable, as compared with films formed from conventional liquid compositions, and a method for producing the same. [Means for solving the problem]

[0011] The present inventors have focused on the fact that by bonding fluorine-based functional group components to metal oxide particles and by incorporating fluorine-based functional group components into silica sol-gel, the formed film has higher oil repellency, and that by forming a film by binding metal oxide particles together with fluorine-containing silica sol-gel, the hardness and abrasion resistance of the film are improved, and unevenness is formed on the film surface, improving fingerprint resistance, and have arrived at the present invention.

[0012] The first aspect of the present invention is the following: Any one of the formulas (19) to (27) Shown in 、 First fluorine-based compound containing perfluoroether structure compound(A1)-bound average particle size of 2 nm to 90 nm Fluorine-containing Metal oxide particles (B) and the following Any one of the formulas (19) to (27) Shown in 、 Secondary fluorine-containing perfluoroether structure compound Contains (A2) Fluorine-containing The silica sol-gel (C) and the solvent (D) are included, and when the amount of all components excluding the solvent (D) is taken as 100 mass %, the first fluorine compound (A1) and the second fluorine compound The total content of (A1) and (A2) is 1% by mass to 30% by mass, Fluorine-containing Silica sol-gel (C) and the above Fluorine-containing The water- and oil-repellent film-forming liquid composition is characterized in that the mass ratio (C:B) of the metal oxide particles (B) is in the range of 10:90 to 90:10.

[0013] [ka] [ka]

[0014] In the above formulas (19) to (27), R is a methyl group or an ethyl group.

[0016] A second aspect of the present invention is the invention based on the first aspect, wherein the first fluorine compound The content of (A1) is, in terms of mass ratio, compound The water- and oil-repellent film-forming liquid composition has a content ratio of (A2) or more.

[0017] A third aspect of the present invention is an invention based on the first aspect, Fluorine-containing Metal oxide particles (B) Metal oxide particles for use in are oxide particles of one or more metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.

[0018] A fourth aspect of the present invention is an invention based on the first aspect, Fluorine-containing The silica sol-gel (C) is Fluorine-containingThe water / oil repellent film-forming liquid composition contains 0.5 to 20% by mass of an alkylene group component having 2 to 7 carbon atoms, when the silica sol-gel (C) is taken as 100% by mass.

[0019] A fifth aspect of the present invention is the invention based on the first aspect, wherein the solvent (D) is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms, and an organic solvent other than the alcohol.

[0020] A sixth aspect of the present invention is a method for manufacturing a semiconductor device, as shown in FIG. A method for producing a water- and oil-repellent film-forming liquid composition according to a first aspect, comprising: Fluorine-containing metal oxide particles (B) Dispersion and fluorine-containing silica sol-gel solution (C) and mixing the above to produce a water- and oil-repellent film-forming liquid composition. Production of water- and oil-repellent film-forming liquid composition This is the method.

[0021] A seventh aspect of the present invention is an invention based on the fifth aspect, and as shown in FIG. 1, the fluorine-containing metal oxide particles (B) The dispersion liquid of the metal oxide particles is mixed with a fluorine-based compound. (A1) and then adding and mixing water and a catalyst to the mixture to prepare a water- and oil-repellent film-forming liquid composition.

[0022] An eighth aspect of the present invention is an invention based on the sixth aspect, Fluorine-containing metal oxide particles Metal oxide particles used in (B) wherein the oxide particles are one or more metal oxide particles selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.

[0023] A ninth aspect of the present invention is an invention based on the fifth aspect, comprising the steps of: (C) However, silicon alkoxide, alcohol and fluorine-based compound (A2) The method for producing a water- and oil-repellent film-forming liquid composition is a method for producing a water- and oil-repellent film-forming liquid composition by adding a catalyst to a mixed liquid obtained by mixing the above and water. Effect of the Invention

[0024] In the water- and oil-repellent film-forming liquid composition according to the first aspect of the present invention, when a film is formed, the first fluorine compound (A1) is bonded Fluorine-containing The second fluorine-containing compound (A2) Fluorine-containing Silica Sol Gel (C) Since the metal oxide particles are bonded to each other by the solvent, the formed film has very high oil repellency. ,film The hardness and abrasion resistance of the film can be improved. Since the surface of the film formed is not smooth, fingerprints left on the film surface are less noticeable.

[0025] In the water- and oil-repellent film-forming liquid composition according to the second aspect of the present invention, compound (A1) is the second fluorine compound (A2) or the second fluorine compound Since it contains more silica sol-gel (C ) Since it contains very little fluorine, it provides excellent coating appearance and adhesion.

[0026] In the liquid composition according to the third aspect of the present invention, Fluorine-containing Metal oxide particles (B) Use for Since the metal oxide particles are one or more types of metal oxide particles selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr, it is possible to select metal oxide particles suitable for the application or usage environment of the film to be formed from among the many types of metal oxide particles.

[0027] In the liquid composition according to the fourth aspect of the present invention, Fluorine-containing Since the silica sol gel contains 0.5% by mass to 20% by mass of an alkylene group component having 2 to 7 carbon atoms, the water- and oil-repellent film adheres well to the substrate on which it is formed, and the thickness of the water- and oil-repellent film becomes uniform, thereby imparting even more excellent oil-repellent performance to the water- and oil-repellent film.

[0028] In the liquid composition according to the fifth aspect of the present invention, the solvent (D) is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms, and an organic solvent other than this alcohol, so that the drying speed of the liquid composition is improved and the viscosity of the liquid composition is reduced. Therefore, this liquid composition is easy to handle and has excellent film-forming properties on a substrate.

[0029] In the method for producing a liquid composition according to the sixth aspect of the present invention, as shown in FIG. (B) Dispersion and fluorine-containing silica sol-gel solution (C) and a liquid composition for forming a water- and oil-repellent film are produced by mixing the above. As a result, metal oxide particles having water- and oil-repellent particle surfaces are present in the silica sol gel containing a fluorine-based compound, and when the liquid composition is formed into a film, an even greater layer of water- and oil-repellency is imparted to the film.

[0030] In the method for producing a liquid composition according to the seventh aspect of the present invention, a fluorine-based compound is added and mixed into a dispersion liquid of metal oxide particles, and water and a catalyst are added and mixed into this mixture, so that the fluorine-containing metal oxide particles (B) A uniformly dispersed dispersion is obtained.

[0031] In a method for producing a liquid composition according to an eighth aspect of the present invention, Used for fluorine-containing metal oxide particles (B) Since the metal oxide particles are one or more types of metal oxide particles selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn, and Zr, it is possible to produce a liquid composition containing metal oxide particles that are suitable for the application or usage environment of the film to be formed from among many types of metal oxide particles.

[0032] In a ninth aspect of the present invention, there is provided a method for producing a liquid composition, comprising the steps of: preparing a fluorine-containing silica sol-gel liquid by adding and mixing a catalyst to a mixture of a silicon alkoxide, an alcohol, a fluorine-based compound and water; (C) acts as a binder for the fluorine-containing metal oxide particles, and when the liquid composition is formed into a film on the surface of a substrate, firmly binds the film to the surface of the substrate and imparts further improved water and oil repellency to the film. [Brief description of the drawings]

[0033] [Figure 1] FIG. 2 is a flow diagram for producing the water- and oil-repellent film-forming liquid composition of the present embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a water- and oil-repellent film formed on a substrate according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] Next, an embodiment of the present invention will be described with reference to the drawings.

[0035] [Method for producing water- and oil-repellent film-forming liquid composition] The water- and oil-repellent film-forming liquid composition is generally produced by the following method. As shown in Fig. 1, metal oxide particles 11 and an organic solvent 12 are mixed to prepare a metal oxide particle dispersion 13. A fluorine-based compound 14 containing a first fluorine-based functional group component (A1) is mixed with this dispersion 13, and water 15 and a catalyst 16 are further mixed to prepare a fluorine-containing metal oxide particle dispersion 17. Meanwhile, a silicon alkoxide 21, an alcohol 22, a fluorine-based compound 23 containing a second fluorine-based functional group component (A2), water 25, and optionally an alkylene group component 24 are mixed, and a catalyst 26 is added to this mixture to prepare a fluorine-containing silica sol-gel liquid 27. A solvent 28 is mixed with this fluorine-containing silica sol-gel liquid 27, and this mixture is mixed with the above-mentioned dispersion liquid 17 of fluorine-containing metal oxide particles to produce a water- and oil-repellent film-forming liquid composition 30. Each step will be described in detail below.

[0036] [Preparation of Metal Oxide Particle Dispersion] First, a dispersion liquid of metal oxide particles is prepared by dispersing metal oxide particles in an organic solvent. The metal oxide particles have an average particle size of 2 nm to 90 nm, preferably 2 nm to 85 nm. If the average particle size is less than 2 nm, the metal oxide particles are likely to aggregate and are difficult to disperse in the medium. If the average particle size exceeds 90 nm, the metal oxide particles will fall off from the water-repellent and oil-repellent film when the liquid composition is formed into a film. Examples of metal oxide particles include particles of SiO2, Al2O3, MgO, CaO, TiO2, ZnO, and ZrO2, mixed particles of these, and composite oxide particles such as MgAl2O4. Examples of organic solvents include methanol, ethanol, isopropanol (hereinafter sometimes referred to as IPA), tetrahydrofuran, hexane, chloroform, toluene, ethyl acetate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), acetone, and fluorine-based solvents. Among these, alcohols such as methanol, ethanol, and isopropanol, which have a boiling point of less than 120° C. and a carbon number of 1 to 4, are preferred. In this specification, the average particle size of metal oxide particles refers to the average value of particle sizes measured by image analysis at 200 points among particle shapes observed with a transmission electron microscope (TEM).

[0037] [Preparation of Fluorine-Containing Metal Oxide Particle Dispersion] Next, a fluorine-based compound containing the first fluorine-based functional group component (A1) represented by the above formula (1) or formula (2) is added to the prepared dispersion of metal oxide particles to synthesize a nanocomposite material of the metal oxide particles and the first fluorine-based functional group component (A1). To further promote the reaction, water and a catalyst are added. This prepares a dispersion of fluorine-containing metal oxide particles.

[0038] The catalyst may be an organic acid, an inorganic acid, or a titanium compound, and examples of the organic acid include formic acid and oxalic acid, examples of the inorganic acid include hydrochloric acid, nitric acid, and phosphoric acid, and examples of the titanium compound include tetrapropoxytitanium, tetrabutoxytitanium, tetraisopropoxytitanium, and titanium lactate. The catalyst is not limited to the above. As the water, it is preferable to use ion-exchanged water or pure water to prevent the inclusion of impurities.

[0039] The fluorine-based compound containing the first fluorine-based functional group component (A1) is represented by the following general formula (3) or formula (4). More specifically, the perfluoroether group in the formula (3) or formula (4) may include the perfluoroether structures represented by the following formulae (5) to (13).

[0040] [ka]

[0041] [ka]

[0042] [ka]

[0043] Examples of X in the above formulae (3) and (4) include structures represented by the following formulae (14) to (18). Note that the following formula (14) shows an example containing an ether bond, the following formula (15) an ester bond, the following formula (16) an amide bond, the following formula (17) a urethane bond, and the following formula (18) a sulfonamide bond.

[0044] [ka]

[0045] In the above formulas (14) to (18), R 2 and R 3is a hydrocarbon group with 0 to 10 carbon atoms, R 4 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 3 Examples of the hydrocarbon group include alkylene groups such as methylene and ethylene groups. 4 Examples of the hydrocarbon group include alkyl groups such as methyl and ethyl groups, as well as phenyl groups.

[0046] In addition, in the above formula (3) and formula (4), R 1 Examples of the alkyl group include a methyl group and an ethyl group.

[0047] In addition, in the above formula (3) and formula (4), Z is not particularly limited as long as it is a hydrolyzable group that can be hydrolyzed to form a Si-O-Si bond. Specific examples of such hydrolyzable groups include alkoxy groups such as methoxy, ethoxy, propoxy, and butoxy groups, aryloxy groups such as phenoxy and naphthoxy groups, aralkyloxy groups such as benzyloxy and phenethyloxy groups, and acyloxy groups such as acetoxy, propionyloxy, butyryloxy, valeryloxy, pivaloyloxy, and benzoyloxy groups. Among these, it is preferable to apply a methoxy group or an ethoxy group.

[0048] Specific examples of the fluorine-based compound containing the first fluorine-based functional group component (A1) having the perfluoroether structure represented by the above formula (3) or (4) include structures represented by the following formulas (19) to (27), in which R is a methyl group or an ethyl group.

[0049] [ka]

[0050] [ka]

[0051] [Preparation of fluorine-containing silica sol-gel liquid] First, a mixed solution is prepared by mixing tetramethoxysilane or tetraethoxysilane as silicon alkoxide, an alcohol having a boiling point of less than 120° C. and a carbon number of 1 to 4, a fluorine-based compound containing the second fluorine-based functional group component (A2) represented by the above formula (1) or formula (2), and water. At this time, an epoxy group-containing silane as an alkylene group component may be mixed together. Specific examples of this silicon alkoxide include tetramethoxysilane (TMOS) and its oligomers, or tetraethoxysilane (TEOS) and its oligomers. For example, in order to obtain a highly durable water-repellent and oil-repellent film, it is preferable to use tetramethoxysilane, while in order to avoid methanol generated during hydrolysis, it is preferable to use tetraethoxysilane.

[0052] The second fluorine-based functional group component (A2) contained in the fluorine-based compound is represented by the above-mentioned formula (1) or formula (2), and the specific fluorine-based compound containing the first fluorine-based functional group component (A1) and the specific fluorine-based compound containing the second fluorine-based functional group component (A2) may be the same or different.

[0053] Specific examples of the epoxy group-containing silane that is the alkylene group component include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and polyfunctional epoxysilane. The alkylene group component is contained in an amount of 1% by mass to 40% by mass, preferably 2.5% by mass to 20% by mass, based on the total mass of the silicon alkoxide and the alkylene group component. If the alkylene group component is less than the lower limit of 1% by mass, when a film is formed on a substrate that does not contain a hydroxyl group, the adhesion to the substrate becomes insufficient. If the alkylene group component exceeds the upper limit of 40% by mass, the durability of the formed film decreases. If the epoxy group-containing silane is contained so that the alkylene group component is in the above range of 1% by mass to 40% by mass, the epoxy group also opens in the hydrolysis polymerization process and contributes to polymerization, which improves leveling during the drying process and makes the film thickness uniform. When the substrate contains a hydrophilic group such as glass, the content of the alkylene group component may be very small or may be zero.On the other hand, when the substrate does not contain a hydrophilic group, the content of the alkylene group component in the silica sol-gel (C) is preferably 0.5% by mass to 20% by mass.

[0054] Examples of the alcohol having 1 to 4 carbon atoms and a boiling point of less than 120°C include the above-mentioned alcohols. In particular, methanol or ethanol are preferred. This is because these alcohols are easily mixed with silicon alkoxide. As the water, it is preferable to use ion-exchanged water or pure water to prevent the inclusion of impurities. A mixed solution is prepared by adding an alcohol having 1 to 4 carbon atoms and water to silicon alkoxide, or to silicon alkoxide and epoxy group-containing silane, and stirring the mixture at a temperature of 10°C to 30°C for 5 to 20 minutes.

[0055] A catalyst is added to the mixed liquid prepared above. Examples of the catalyst include organic acids, inorganic acids, and titanium compounds. At this time, the liquid temperature is preferably kept at 30°C to 80°C, and the mixture is stirred for preferably 1 hour to 24 hours. This prepares a fluorine-containing silica sol-gel liquid. Note that alcohol may be added to the fluorine-containing silica sol-gel liquid for the next step.

[0056] When the alcohol is added and mixed, the fluorine-containing silica sol-gel liquid contains 2% by mass to 50% by mass of silicon alkoxide, 20% by mass to 98% by mass of alcohol having 1 to 4 carbon atoms, 0.1% by mass to 40% by mass of water, and 0.01% by mass to 5% by mass of catalyst. When an epoxy group-containing silane, which is an alkylene group component, is mixed, the epoxy group-containing silane is contained up to a maximum of 30% by mass.

[0057] The reason why the proportion of the alcohol having 1 to 4 carbon atoms is limited to the above range is that if the proportion of alcohol is less than the lower limit, silicon alkoxide does not dissolve in the solution and separates, and the reaction solution is easily gelled during the hydrolysis reaction of silicon alkoxide; on the other hand, if it exceeds the upper limit, the amount of water and catalyst required for hydrolysis is relatively small, so the reactivity of hydrolysis decreases, polymerization does not proceed, and the adhesion of the film decreases.The reason why the proportion of water is limited to the above range is that if it is less than the lower limit, the hydrolysis rate slows down, polymerization does not proceed, and the adhesion of the water-repellent and oil-repellent film becomes insufficient; on the other hand, if it exceeds the upper limit, the reaction solution gels during the hydrolysis reaction, and the silicon alkoxide compound does not dissolve in the alcohol aqueous solution due to the excessive water, causing the problem of separation.

[0058] The SiO2 concentration (SiO2 content) in the silica sol-gel is preferably 1% by mass to 40% by mass. If the SiO2 concentration is less than the lower limit, polymerization is insufficient, and the adhesion of the film is reduced and cracks are likely to occur, while if the SiO2 concentration exceeds the upper limit, the proportion of water becomes relatively high, silicon alkoxide does not dissolve, and the reaction solution gels.

[0059] The organic acid, inorganic acid or titanium compound functions as a catalyst for promoting the hydrolysis reaction. Examples of organic acids include formic acid and oxalic acid, examples of inorganic acids include hydrochloric acid, nitric acid and phosphoric acid, and examples of titanium compounds include tetrapropoxytitanium, tetrabutoxytitanium, tetraisopropoxytitanium, and titanium lactate. The catalyst is not limited to the above. The reason why the proportion of the catalyst is limited to the above range is that if it is less than the lower limit, the reactivity is poor and polymerization is insufficient, so that a film is not formed, while if it exceeds the upper limit, there is no effect on reactivity, but the substrate on which the film is formed is easily corroded by the remaining acid.

[0060] [Water- and oil-repellent film-forming liquid composition] The water- and oil-repellent film-forming liquid composition of the present embodiment is produced by the above-mentioned production method, and contains metal oxide particles (B) to which the first fluorine-based functional group component (A1) is bonded, silica sol-gel (C) containing the second fluorine-based functional group component (A2), and a solvent (D) (indicated by reference numeral 28 in FIG. 1). Examples of the solvent (D) include water, methanol, ethanol, isopropanol (hereinafter sometimes referred to as IPA), tetrahydrofuran, hexane, chloroform, toluene, ethyl acetate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), acetone, and fluorine-based solvents. These fluorine-based functional group components (A1) and (A2) have a perfluoroether structure represented by the above general formula (1) or formula (2), and are contained in the liquid composition in a total amount of 1% by mass to 30% by mass when the amount of all components other than the solvent (D) is taken as 100% by mass. If the total content ratio of the fluorine-based functional group components (A1+A2) is less than 1 mass%, the formed film cannot be imparted with oil repellency, and if it exceeds 30 mass%, the film repels water, etc., resulting in poor film-forming properties. The total content ratio of the fluorine-based functional group components (A1+A2) is preferably 2 mass% to 28 mass%.

[0061] In addition, it is preferable that the first fluorine functional group component (A1) is contained in the same mass proportion as the second fluorine functional group component (A2) or in a larger amount than the second fluorine functional group component (A2), since this results in excellent appearance and adhesion of the coating film.

[0062] As described above, the fluorine-based compound contained in the water- and oil-repellent film-forming liquid composition of the present embodiment has a perfluoroether group in which a plurality of short-chain perfluoroalkyl groups and perfluoroalkylene groups having a carbon number of 6 or less are bonded to an oxygen atom in the molecule, and the fluorine content in the molecule is high, so that the formed film can be imparted with excellent water- and oil-repellency. Specific examples of the perfluoroether structure include the structures represented by the above formulas (19) to (27).

[0063] Furthermore, the liquid composition for forming the water- and oil-repellent film of this embodiment needs to have a mass ratio (C:B) of the silica sol-gel (C) and the metal oxide particles (B) in the range of 10:90 to 90:10. That is, when the total amount of the silica sol-gel (C) and the metal oxide particles (B) is taken as 100 mass%, if the silica sol-gel (C) is less than 10 mass% and the metal oxide particles (B) is more than 90 mass%, the binder component in the liquid composition becomes too small, and the formed film is easily peeled off from the substrate in the Cellophane Tape (registered trademark) test of the film described later. On the other hand, if the metal oxide particles (B) are less than 10 mass% and the silica sol-gel (C) is more than 90 mass%, the metal oxide particles are too small, and the film is easily peeled off from the substrate in the film strength test described later. The preferred mass ratio (C:B) is 20:80 to 80:20.

[0064] Since the water- and oil-repellent film-forming liquid composition of the present embodiment contains a dispersion liquid of fluorine-containing metal oxide particles and a fluorine-containing silica sol-gel liquid, when a film is formed on a substrate surface, it imparts even more excellent oil repellency compared to conventional liquid compositions, and provides a water- and oil-repellent film with excellent adhesion to the substrate surface and high strength that is difficult to peel off.

[0065] [Method of forming a water-repellent and oil-repellent film on a substrate surface] To form the water-repellent and oil-repellent film on the surface of a substrate, the water-repellent and oil-repellent film-forming liquid composition is applied to the substrate, and then dried at room temperature in the air to harden the liquid composition. The substrate is not particularly limited, but may be metal plates such as stainless steel (SUS), aluminum, and iron, glass such as window glass and mirrors, tiles, plastics such as polyvinyl chloride (PVC), or polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. The coating method of the liquid composition may be screen printing, bar coating, die coating, doctor blade, spin coating, brush coating, etc.

[0066] As shown in FIG. 2, the water- and oil-repellent film 2 formed on the surface of the substrate 1 is composed of a large number of metal oxide particles 3 whose particle surfaces are covered with fluorine-based functional group components and bound together by fluorine-containing silica sol-gel 4 as a binder. The water- and oil-repellent film 2 contains metal oxide particles 3 bound with fluorine-based functional group components and fluorine-containing silica sol-gel 4, so that the oil-repellent performance of the film is maintained. In addition, the metal oxide particles 3 having an average particle size of 2 nm to 90 nm are bound together in the film 2 by the silica sol-gel 4, so that the hardness and abrasion resistance of the film 2 can be improved. In addition, the presence of the metal oxide particles 3 makes the film surface uneven, and there is an advantage that after a fingerprint is attached to the surface of the film 2, the fingerprint is less noticeable on the film surface. The film thickness can be controlled by changing the particle size of the metal oxide particles and the content ratio of the metal oxide particles in the film components. EXAMPLES

[0067] Next, examples of the present invention will be described in detail together with comparative examples. First, Synthesis Examples 1-9 and Comparative Synthesis Examples 1-2 for preparing a dispersion liquid of metal oxide particles will be described, followed by Synthesis Examples 10-13 and Comparative Synthesis Example 3 for preparing a fluorine-containing silica sol-gel liquid, and then Examples 1-9 and Comparative Examples 1-7 for producing a water- and oil-repellent film-forming liquid composition using these Synthesis Examples and Comparative Synthesis Examples will be described.

[0068] [Synthesis Examples 1 to 9 for preparing metal oxide particle dispersion liquid, and Comparative Synthesis Examples 1 to 2] <Synthesis Example 1> 1.50 g of the fluorine-based compound represented by the above formula (19) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of silicon dioxide with an average particle size of 12 nm (IPA-ST, manufactured by Nissan Chemical Industries, Ltd., SiO2 concentration 30%). Next, 0.10 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added and mixed at 40°C for 2 hours to obtain a dispersion of silicon dioxide (silica) particles in which the fluorine-based compound is bonded to the silicon dioxide particles.

[0069] <Synthesis Example 2> In a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 45 nm (IPA-ST-L, manufactured by Nissan Chemical Industries, Ltd., SiO2 concentration 30%), 1.50 g of the fluorine-based compound represented by the above formula (20) was added and mixed. Next, 0.10 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles.

[0070] <Synthesis Example 3> In a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 80 nm (IPA-ST-ZL, manufactured by Nissan Chemical Industries, Ltd., SiO2 concentration 30%), 1.50 g of the fluorine-based compound represented by the above formula (21) was added and mixed. Next, 0.10 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles.

[0071] <Synthesis Example 4> 0.75 g of the fluorine-based compound represented by the above formula (22) was added and mixed into a beaker containing 50.0 g of the same silicon dioxide IPA dispersion as in Synthesis Example 3. Next, 0.05 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles.

[0072] <Synthesis Example 5> 2.25 g of the fluorine-based compound represented by the above formula (23) was added and mixed into a beaker containing 50.0 g of the same silicon dioxide IPA dispersion as in Synthesis Example 3. Next, 0.15 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles.

[0073] <Synthesis Example 6> In a beaker containing 50.0 g of a methanol dispersion of zirconium dioxide having an average particle size of 3 nm (SZR-M, manufactured by Sakai Chemical Industry Co., Ltd., ZrO2 concentration 30%), 8.00 g of the fluorine-based compound represented by the above formula (27) was added and mixed. Next, 4.05 g of water was added and mixed. Furthermore, 0.035 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of zirconium dioxide particles.

[0074] <Synthesis Example 7> 2.70 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 6 nm (TKD-701, manufactured by Teika Co., Ltd., TiO2 concentration 18%). Next, 0.97 g of water was added and mixed. Furthermore, 0.010 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of titanium dioxide particles.

[0075] <Synthesis Example 8> 0.03 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of alumina and silicon dioxide with an average particle size of 60 nm (Baylal AS-L10, manufactured by Taki Chemical Industry Co., Ltd., 3Al2O3·2SiO2 concentration 10%). Next, 0.02 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of alumina and silicon dioxide particles.

[0076] <Synthesis Example 9> 0.30 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of zinc oxide having an average particle size of 25 nm (MZ-500, manufactured by Teika Co., Ltd., ZnO concentration 30%). Next, 0.11 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same procedure as in Synthesis Example 1 was repeated to obtain a dispersion of zinc oxide particles.

[0077] <Comparative Synthesis Example 1> 0.75 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 230 nm (R32, Sakai Chemical Industry Co., Ltd., TiO2 concentration 30%). Next, 0.27 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of titanium dioxide particles.

[0078] <Comparative Synthesis Example 2> To a beaker containing 50.0 g of the same IPA dispersion as in Synthesis Example 1, 0.10 g of water was added and mixed without adding any fluorine-based compound. Furthermore, 0.005 g of nitric acid was added, and the rest of the procedure was the same as in Synthesis Example 1 to obtain a dispersion of silicon dioxide particles.

[0079] Table 1 below shows the details of the dispersions of fluorine-containing metal oxide particles of Synthesis Examples 1 to 9 and Comparative Synthesis Example 1, and the dispersion of fluorine-free metal oxide particles of Comparative Synthesis Example 2. In Table 1, all of the Rs in the formulas of fluorine-containing silanes represented by formulas (19) to (22) and (27) as fluorine-based compounds are ethyl groups.

[0080] [Table 1]

[0081] [Synthesis Examples 10 to 13 for preparing fluorine-containing silica sol-gel liquid, Comparative Synthesis Example 3] <Synthesis Example 10> 0.24 g (0.8 mass%) of the fluorine-based compound represented by the above formula (27) was added to a beaker containing 28.5 g of trimers to pentamers of tetramethoxysilane (TMOS) (manufactured by Mitsubishi Chemical Corporation, product name: MKC Silicate MS51) and 59.7 g of ethanol, and mixed. Next, 1.5 g of 3-glycidoxypropyltrimethoxysilane (GPTMS: manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403), which is an epoxy group-containing silane as an alkylene group component, and 10 g of water were added and mixed. Furthermore, 0.1 g of nitric acid was added and mixed at 30°C for 3 hours to obtain a fluorine-containing silica sol-gel liquid.

[0082] <Synthesis Example 11> To a beaker containing 24.0 g of the same TMOS trimer to pentamer as in Synthesis Example 10 and 59.7 g of ethanol, 0.06 g (0.2 mass%) of the fluorine-based compound represented by the above formula (27) was added and mixed. Next, 6.0 g of the same GPTMS as in Synthesis Example 10 as an alkylene group component and 10 g of water were added and mixed. Furthermore, 0.1 g of nitric acid was added and mixed at 30° C. for 3 hours to obtain a fluorine-containing silica sol-gel liquid.

[0083] <Synthesis Example 12> To a beaker containing 29.8 g of the same TMOS trimer to pentamer as in Synthesis Example 10 and 59.8 g of ethanol, 3.00 g (10.0 mass%) of the fluorine-based compound represented by the above formula (27) was added and mixed. Next, 0.2 g of the same GPTMS as in Synthesis Example 10 as an alkylene group component and 10 g of water were added and mixed. Furthermore, 0.1 g of nitric acid was added and mixed at 30° C. for 3 hours to obtain a fluorine-containing silica sol-gel liquid.

[0084] <Synthesis Example 13> 0.30 g (1.0 mass%) of the fluorine-based compound represented by the above formula (27) was added to a beaker containing 30.0 g of tetraethoxysilane (TEOS) and 56.9 g of ethanol, and mixed. Next, 10 g of water was added without adding any alkylene group component, and mixed. Furthermore, 0.1 g of nitric acid was added, and mixed at 30°C for 3 hours to obtain a fluorine-containing silica sol-gel liquid.

[0085] <Comparative Synthesis Example 3> To a beaker containing 28.5 g of the same TMOS trimer to pentamer as in Synthesis Example 11 and 59.6 g of ethanol, 1.5 g of the same GPTMS as in Synthesis Example 10 as an alkylene group component and 10 g of water were added and mixed without adding any fluorine-based compound. Furthermore, 0.1 g of nitric acid was added and mixed at 30°C for 3 hours to obtain a fluorine-free silica sol-gel liquid.

[0086] Table 2 below shows the details of the fluorine-containing silica sol-gel solutions of Synthesis Examples 10 to 13 and the fluorine-free silica sol-gel solution of Comparative Synthesis Example 3.

[0087] [Table 2]

[0088] [Examples 1 to 9 and Comparative Examples 1 to 7 for the production of water- and oil-repellent film-forming liquid compositions] <Example 1> 26.0 g of solvent was added to 1.9 g of the fluorine-containing silica sol-gel liquid obtained in Synthesis Example 10 and mixed. The solvent was prepared by mixing 1.0 g of diacetone alcohol and 3.0 g of isopropyl glycol with 22.0 g of industrial alcohol (AP-7, manufactured by Nippon Alcohol Industry Co., Ltd.). Then, 1.5 g of the dispersion liquid of the metal oxide particles of Synthesis Example 1 was added and mixed to prepare a water- and oil-repellent film-forming liquid composition. The contents are shown in Table 3 below.

[0089] [Table 3]

[0090] <Examples 2 to 9 and Comparative Examples 1 to 7> For Examples 2 to 9 and Comparative Examples 1 to 7, the type and amount of the dispersion liquid of the fluorine-containing metal oxide particles, the type and amount of the fluorine-containing silica sol-gel liquid, and the amount of the same solvent as in Example 1 were determined as shown in Table 3, and the water- and oil-repellent film-forming liquid compositions of Examples 2 to 9 and Comparative Examples 1 to 7 were prepared.

[0091] <Comparative testing and evaluation> The 16 types of liquid compositions obtained in Examples 1 to 9 and Comparative Examples 1 to 7 were applied to a SUS304 substrate having a thickness of 2 mm, a length of 150 mm, and a width of 75 mm using a brush (Nylon Brush Meister manufactured by Suematsu Brush Co., Ltd.) so that the thickness after drying would be 1 to 3 μm, respectively, to form 16 types of coating films. All coating films were left to stand in an air atmosphere at room temperature for 3 hours, and the coating films were dried to obtain 16 types of films on the SUS304 substrate. For these films, the water wettability (water repellency), oil repellency, n-hexadecane sliding property, and appearance of the film were evaluated, and a film strength test, a cellophane tape peeling test, and a fingerprint resistance test were performed. The results are shown in Table 4. The fingerprint resistance of the film is a property in which fingerprints are not easily noticeable on the film surface after they are attached to the film, and fingerprints are easily wiped off when they are attached, as well as fingerprints are not easily attached to the film.

[0092] (1) Water repellency of the film surface (contact angle) Using a Dropmaster DM-700 manufactured by Kyowa Interface Science, ion-exchanged water at 22°C ± 1°C was prepared in a syringe, and a 2μL droplet was ejected from the tip of the needle of the syringe. The film on the SUS304 substrate to be evaluated was then brought close to the droplet, causing the droplet to adhere to the film. The contact angle of the adhered water was measured. The contact angle measured 1 second after the water touched the film surface in a stationary state was analyzed using the θ / 2 method, and this value was used to evaluate the water wettability (water repellency) of the film surface. A value of 84 degrees or more was rated as "good."

[0093] (2) Oil repellency of the film surface (contact angle) Using a Dropmaster DM-700 manufactured by Kyowa Interface Science, n-hexadecane at 22°C ± 1°C was prepared in a syringe, and a 2μL droplet was ejected from the tip of the needle of the syringe. The film on the SUS304 substrate to be evaluated was then brought close to the droplet, allowing the droplet to adhere to the film. The contact angle of the adhered n-hexadecane was measured. The contact angle 1 second after n-hexadecane touched the film surface in a stationary state was analyzed using the θ / 2 method, and this value was used to evaluate the oil repellency of the film surface. A value of 42 degrees or more was rated as "good."

[0094] (3) n-Hexadecane sliding test Using a Dropmaster DM-700 manufactured by Kyowa Interface Science, n-hexadecane at 25±1°C was prepared in a syringe, and 9μL of n-hexadecane was dropped from the syringe onto a horizontally placed polypropylene substrate. The substrate was tilted at a rate of 2° / min, and the tilt angle of the substrate was measured when the n-hexadecane droplet began to move. Even if the contact angle (2) is low, a smaller falling angle means that the substrate has excellent antifouling properties. If it was 50° or less, it was rated as "good". In addition, if there was a trace of the droplet on the substrate surface after the n-hexadecane droplet moved and fell off the substrate, it was rated as "oil stains".

[0095] (4) Appearance of the membrane The film on the SUS304 substrate to be evaluated was visually observed to check whether the film was transparent or not, and whether the film was cloudy or not. A transparent film was rated as "good", and a cloudy film was rated as "bad cloudiness".

[0096] (5) Membrane strength test The contactor described below was applied with a specified load to the film on the SUS304 substrate to be evaluated, and after 10 reciprocating movements under the following conditions, the film on the substrate was visually inspected to see if it peeled off from the substrate. If the film did not peel off, it was judged as "passed", and if it peeled off, it was judged as "failed". (a) Measuring instrument: Static and dynamic friction measuring instrument TL201Tt (Trinity Lab Co., Ltd.) (b) Measurement conditions: ·Traveling distance: 30mm ·Vertical load: 500g weight ·Moving speed: 50mm / sec Contact: 5mm x 15mm neoprene rubber

[0097] (6) Cellophane tape peeling test of film A 1 mm wide cross-cut was made in a grid pattern on the film on the SUS304 substrate to be evaluated, and an adhesive tape (manufactured by Nichiban Co., Ltd., product name "Cellotape (registered trademark)") was applied to the grid-cut film, and a Cellotape (registered trademark) peeling test (hereinafter simply referred to as peeling test) was performed in accordance with the grid tape method of JIS K5600-5-6 (cross-cut method). The denominator was the number of 100 cross-cut squares, and the numerator was the number of squares remaining on the substrate after the peeling test.

[0098] (6) Fingerprint resistance test of film A continuous cellulose fiber nonwoven fabric (manufactured by Asahi Kasei Corporation, product name: BEMCOT M-3II) was placed on the film on the SUS304 substrate to be evaluated, and 100 microliters of artificial fingerprint liquid (based on JIS K 2246) was dropped onto the nonwoven fabric. Black rubber No. 24 (mass 300 g) was placed on the nonwoven fabric, and a weight of 1 kg was placed on top and left to stand for 30 seconds to allow the fingerprint liquid to adhere to the film. The nonwoven fabric was then peeled off, and the fingerprint resistance of the film was visually observed. Films that did not have fingerprint liquid on the surface were rated as "good," and films that had fingerprint liquid on the surface were rated as "poor."

[0099] [Table 4]

[0100] As is clear from Table 4, in Comparative Example 1, a water- and oil-repellent film-forming liquid composition was prepared from the dispersion of titanium dioxide particles of Comparative Synthesis Example 1, which contains metal oxide (titanium dioxide) particles with an average particle diameter of 230 nm, and a film was formed using this liquid composition. Therefore, the average particle diameter of the metal oxide particles in the film was too large, and the metal oxide particles were difficult to bind to the substrate surface with the silica sol-gel, which is the binder component. As a result, the contact angles of water and n-hexadecane were poor, the film was cloudy, and the appearance of the film was poor. In addition, in the strength test of the film, the film peeled off from the substrate, and in the peel test, only 20 squares remained on the substrate, and most of them peeled off. Furthermore, the fingerprint resistance of the film was poor.

[0101] In Comparative Example 2, a liquid composition for forming a water- and oil-repellent film was prepared from the silica sol-gel liquid of Comparative Synthesis Example 3, which did not contain a fluorine-based compound, and a film was formed using this liquid composition, so the sliding angle of n-hexadecane was poor.

[0102] In Comparative Example 3, when the total amount of the silica sol-gel (C) and the metal oxide particles (B) is taken as 100% by mass, the amount of the silica sol-gel (C) was 5% by mass, so the binder component in the liquid composition was too small, and in the film peeling test, only 10 squares remained on the substrate, and most of the film peeled off. In addition, the sliding angle of n-hexadecane was poor, and there was an "oil stain". In addition, the film was cloudy and had a poor appearance. Furthermore, the fingerprint resistance of the film was poor.

[0103] In Comparative Example 4, when the total amount of the silica sol-gel (C) and the metal oxide particles (B) is taken as 100 mass%, the metal oxide particles (B) were 5 mass%, so that the amount of the metal oxide particles in the liquid composition was too small, and the film peeled off from the substrate in the film strength test. Furthermore, the fingerprint resistance of the film was poor.

[0104] In Comparative Example 5, the total content (A1+A2) of the fluorine-based functional group component (A1) and the fluorine-based functional group component (A2) was 0.8% by mass, so the formed film could not be imparted with oil repellency, the contact angles of water and n-hexadecane were poor, and the n-hexadecane sliding angle test showed "oil stains". Furthermore, the fingerprint resistance of the film was poor.

[0105] In Comparative Example 6, the total content (A1+A2) of the fluorine-based functional group component (A1) and the fluorine-based functional group component (A2) was 33.4 mass%, so the formed film could not be imparted with oil repellency, and the n-hexadecane fall angle test was 70 degrees. In addition, the film was cloudy and the appearance of the film was poor. Furthermore, the fingerprint resistance of the film was poor.

[0106] In Comparative Example 7, a water- and oil-repellent film-forming liquid composition was prepared from the dispersion of metal oxide particles of Comparative Synthesis Example 2, which does not contain a fluorine-based compound, and a film was formed using this liquid composition, so the contact angles of water and n-hexadecane were poor, and the n-hexadecane sliding angle test showed "oil stains". Furthermore, the fingerprint resistance of the film was poor.

[0107] In contrast, in Examples 1 to 9, the first and second fluorine-based functional group components (A1, A2) were represented by the above-mentioned formulas (19) to (23) and formula (27), the average particle size of the metal oxide particles was in the range of 2 nm to 90 nm, the total content (A1+A2) of the first and second fluorine-based functional group components (A1, A2) in the liquid composition excluding the solvent (D) was 1 mass% to 30 mass%, and the mass ratio (C:B) of the silica sol-gel (C) to the metal oxide particles (B) was in the range of 10:90 to 90:10, which satisfies the scope of the invention of the first aspect. Therefore, the contact angles of water and n-hexadecane, the sliding properties of n-hexadecane, and the appearance of the film were all good, and the film strength test, peel test, and fingerprint resistance test were all passed. [Industrial Applicability]

[0108] The water- and oil-repellent film-forming liquid composition of the present invention is used in fields where oil stains need to be prevented in factories where machine oil is used, in kitchens where oil is scattered, and in range hoods, ventilation fans, refrigerator doors, and the like where oil vapor is present. [Explanation of symbols]

[0109] 1 Base material 2. Water- and oil-repellent film 3 Metal oxide particles 4. Silica sol-gel

Claims

1. Fluorine-containing metal oxide particles (B) having an average particle size of 2 nm to 90 nm and to which a first fluorine-based compound (A1) containing a perfluoroether structure is bonded, the first fluorine-based compound (A1) being represented by any one of the following formulas (19) to (27): A fluorine-containing silica sol-gel (C) containing a second fluorine-based compound (A2) having a perfluoroether structure represented by any one of the following formulas (19) to (27): A solvent (D), the total content of the first fluorine compound (A1) and the second fluorine compound (A2) is 1% by mass to 30% by mass when the total amount of all components excluding the solvent (D) is 100% by mass, A water- and oil-repellent film-forming liquid composition, characterized in that a mass ratio (C:B) of the fluorine-containing silica sol-gel (C) to the fluorine-containing metal oxide particles (B) is in the range of 10:90 to 90:

10. 【Chemistry 6】 【Chemistry 7】 In the above formulas (19) to (27), R is a methyl group or an ethyl group.

2. 2. The water / oil repellent film forming liquid composition according to claim 1, wherein the content ratio of the first fluorine compound (A1) is equal to or greater than the content ratio of the second fluorine compound (A2) in terms of mass ratio.

3. 2. The water- and oil-repellent film-forming liquid composition according to claim 1, wherein the metal oxide particles used for the fluorine-containing metal oxide particles (B) are oxide particles of one or more metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.

4. 2. The water- and oil-repellent film-forming liquid composition according to claim 1, wherein the fluorine-containing silica sol-gel (C) contains an alkylene group component having 2 to 7 carbon atoms in an amount of 0.5% by mass to 20% by mass when the fluorine-containing silica sol-gel (C) is taken as 100% by mass.

5. 2. The water- and oil-repellent film-forming liquid composition according to claim 1, wherein the solvent (D) is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms, and an organic solvent other than the alcohol.

6. A method for producing the water- and oil-repellent film-forming liquid composition according to claim 1, comprising: A method for producing a water- and oil-repellent film-forming liquid composition, which is prepared by mixing a dispersion of fluorine-containing metal oxide particles (B) and a fluorine-containing silica sol-gel liquid (C).

7. 7. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 6, wherein the dispersion of the fluorine-containing metal oxide particles (B) is prepared by adding and mixing the fluorine-based compound (A1) to a dispersion of the metal oxide particles, and then adding and mixing water and a catalyst to the mixture.

8. 8. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 7, wherein the metal oxide particles used for the fluorine-containing metal oxide particles (B) are oxide particles of one or more metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.

9. 7. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 6, wherein the fluorine-containing silica sol-gel liquid (C) is prepared by adding a catalyst to a mixed liquid of a silicon alkoxide, an alcohol, a fluorine-based compound (A2) and water.

Citation Information

Patent Citations

  • Glass subjected to water-repellent treatment and its production

    JP1999092177A

  • Water-repellent film

    JP2009154480A

  • Composition for film formation and method for producing the same, and film

    JP2017171701A

  • Fluorine-containing nanocomposite particle and method for producing the same, and coating agent, oil water separation film and resin composition containing the same

    JP2018039987A

  • Silane compound containing perfluoroether

    JP2020083836A