Manufacturing method for flanged paper cup

A laminate structure with a specific density range and low-density biomass polyethylene resin, combined with targeted heating, enhances flange strength in paper cups while minimizing environmental footprint and equipment issues.

JP7577602B2Active Publication Date: 2024-11-05NISSIN FOODS HOLDINGS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021075729
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-28
Publication Date
2024-11-05
Estimated Expiration
2041-04-28

AI Technical Summary

Technical Problem

Existing methods fail to optimize the use of biomass polyethylene resin for enhancing the strength of flanges in paper cups, particularly due to the lack of consideration for flange strength in the transition from fossil fuels to biomass materials.

Method used

A method involving a laminate structure with an outer polyethylene resin layer having a density of 0.91 g/cm³ to 0.93 g/cm³, blended with low-density biomass polyethylene resin, and an inner polyethylene resin layer, combined with specific heating processes to improve flange strength without adhesives.

Benefits of technology

The method results in flanged paper cups with improved flange strength and reduced environmental impact, maintaining high productivity by preventing resin accumulation on manufacturing equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577602000004
    Figure 0007577602000004
  • Figure 0007577602000001
    Figure 0007577602000001
  • Figure 0007577602000002
    Figure 0007577602000002
Patent Text Reader

Abstract

To provide a flanged paper cup capable of achieving small environmental load and high strength of a flange.SOLUTION: Provided is a manufacturing method for a flanged paper cup formed of a flanged trunk part and a bottom part. A trunk part is constituted of a laminate body formed by laminating an outer face polyethylene resin layer, a paper base material and an inner face polyethylene resin layer in this order. The resin density of the outer face polyethylene resin layer is 0.91 g / cm3 or more and less than 0.93 g / cm3. The outer face polyethylene resin layer includes a low density biomass polyethylene resin with density of 0.91 g / cm3 or more and less than 0.93 g / cm3. The manufacturing method for the flanged paper cup includes: a molding process of molding a top edge of the trunk part into a flange shape; and a heating process of applying heat after flange molding, thereby providing a flanged paper cup with excellent flange strength.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a flanged paper cup having excellent strength. [Background technology]

[0002] In order to achieve the Sustainable Development Goals (SDGs), it is desirable to move away from fossil fuels, and the use of biomass materials has been proposed as one way to achieve this. As a representative example of biomass materials, biomass resins are being put to practical use.

[0003] Polylactic acid (PLA) is known as a biomass resin, but it has not yet come into widespread use because its properties are significantly different from general-purpose resins such as polyethylene and PET. For this reason, efforts are being made to produce ethylene from renewable plant raw materials and use it to synthesize biomass-derived polyethylene resin (hereinafter referred to as "biomass polyethylene resin") (Patent Document 1).

[0004] However, because polyethylene resin has a wide range of uses, the optimal use of biomass polyethylene resin for each use has not been clarified. In particular, flange strength, which is an important characteristic for the use of paper cups, which is the subject of the present invention, has not been taken into consideration at all (Patent Documents 2 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2011-506628 [Patent Document 2] JP 2014-133338 A [Patent Document 3] JP 2015-214365 A [Patent Document 4] JP 2017-196777 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a flanged paper cup that has a small environmental impact and has excellent flange strength. [Means for solving the problem]

[0007] The present inventors discovered that the flange strength is significantly improved by blending a low-density biomass polyethylene resin into the outer polyethylene resin layer, and thus completed the present invention.

[0008] That is, one embodiment of the present invention is a method for manufacturing a flanged paper cup comprising a body part having a flange formed therein and a bottom part, the body part being made of a laminated body having an outer polyethylene resin layer, a paper base material, and an inner polyethylene resin layer laminated in this order, and the resin density of the outer polyethylene resin layer is 0.91 g / cm 3 More than 0.93g / cm 3 The outer polyethylene resin layer has a density of 0.91 g / cm 3 More than 0.93g / cm 3 The present invention relates to a method for manufacturing a flanged paper cup, which comprises a molding process for molding the upper end of the body into a flange shape, and a heating process for applying heat after the flange is molded, and the method comprises the steps of:

[0009] One embodiment relates to a method for producing the flanged paper cup described above, characterized in that the heating step is heating by convection and / or thermal radiation.

[0010] One embodiment relates to a method for producing the flanged paper cup described above, wherein the polyethylene resin layer contains at least 0.5 mass % or more of low-density biomass polyethylene resin. Effect of the Invention

[0011] With the completion of this invention, it has become possible to manufacture flanged paper cups that have a small environmental impact and excellent flange strength. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an enlarged view of a flange of a paper cup according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention relates to a method for manufacturing a flanged paper cup comprising a body portion having a flange formed thereon and a bottom portion. The details will be described below.

[0014] Flanged Paper Cup Body The body is made of a laminate of an outer polyethylene resin layer, a paper base material, and an inner polyethylene resin layer, in that order. By using a laminate having a polyethylene resin layer, it is possible to join the body to the bottom and form a flange without using adhesives or the like.

[0015] Body: Paper base material There are no particular limitations on the paper base material that constitutes the laminate, but uncoated paper, coated paper, etc. can be used. In addition, in order to achieve strength as a container, the basis weight of the paper base material is 150 to 400 g / m 2 Preferably, more preferably, 250 to 350 g / m 2 It is.

[0016] Uncoated paper can be produced by adding fillers such as clay, talc, titanium dioxide, calcium carbonate, aluminum hydroxide powder, etc. to the raw pulp, and, if necessary, adding sizing agents, paper strength agents, fixing agents, etc. In addition, to improve the paper surface strength, chemicals such as styrene resin, styrene-maleic acid resin, starch, carboxymethyl cellulose, polyvinyl alcohol, polyacrylamide, etc. may be coated on the surface.

[0017] Coated paper can be obtained by preparing a coating liquid containing pigments such as calcium carbonate, titanium dioxide, and aluminum hydroxide, and adhesives such as polyvinyl alcohol, styrene-butadiene latex, and methyl methacrylate-butadiene latex, and applying the liquid to the surface.

[0018] Body: Polyethylene resin layer Polyethylene resin layers are laminated on both sides of the paper base material. As described above, by laminating polyethylene resin layers (an outer polyethylene resin layer and an inner polyethylene resin layer) on both sides of the paper base material, it is possible to join the body and the bottom and form a flange without using adhesives or the like.

[0019] In the present invention, the outer polyethylene resin layer has a resin density of 0.91 g / cm 3 More than 0.93g / cm 3 and density is 0.91 g / cm 3 More than 0.93g / cm 3 It is necessary to contain a low-density biomass polyethylene resin of less than 0.91 g / cm. 3 More than 0.93g / cm 3 and density is less than 0.91 g / cm 3 More than 0.93g / cm 3 By including a low density biomass polyethylene resin of less than 1000 g / m2, the strength of the flange can be improved.

[0020] Here, biomass polyethylene resin refers to polyethylene resin synthesized from plant-derived ethylene. Plant-derived ethylene can be produced by a well-known method using ethanol obtained by fermenting plants (corn, sugarcane, tapioca, etc.) as a raw material. In the present invention, polyethylene resin derived from fossil fuels is referred to as petrochemical polyethylene resin and is distinguished from biomass polyethylene resin.

[0021] In addition, the "biomass ratio" (concentration of biomass-derived carbon in polyethylene resin) is a value measured by measuring the amount of biomass-derived carbon by radioactive carbon (C14) measurement, and more specifically, it refers to the amount of biomass-derived carbon (mass%) in total carbon calculated by measurement according to the biobased concentration test standard "ASTM-D6866-20". Carbon dioxide in the atmosphere contains a certain amount of C14, and the amount of C14 in plants that grow by absorbing carbon dioxide from the atmosphere is also about the same. On the other hand, fossil fuels contain almost no C14. Therefore, by measuring the proportion of C14 contained in polyethylene resin, the biomass-derived carbon concentration in polyethylene resin, the "biomass ratio", can be calculated.

[0022] In addition, even if it is biomass polyethylene resin, it is high density biomass polyethylene resin (density 0.93 cm 3 In the above cases, the adhesiveness of the resin is poor and the strength of the flange cannot be improved.

[0023] The low-density biomass polyethylene resin blended in the inner polyethylene resin layer is preferably 70% by mass or less, and more preferably 50% by mass or less. As shown in Fig. 1, the inner polyethylene resin layer is the exterior of the flange and is the part that comes into direct contact with the flange molding machine. Therefore, if too much low-density biomass polyethylene resin with excellent adhesive properties is blended, fine resin pieces (dust) tend to adhere and accumulate on the flange molding machine in the primary heating step, which can lead to reduced productivity and quality.

[0024] It is also preferable to make the resin density of the inner polyethylene resin layer higher than that of the outer polyethylene resin layer. As shown in Fig. 1, the inner polyethylene resin layer is the exterior of the flange and is the part that comes into direct contact with the flange molding machine during the molding process. Therefore, by making the density of the inner polyethylene resin layer higher than that of the outer polyethylene resin layer and making it less likely to soften or melt, it is possible to prevent resin pieces from adhering to and accumulating on the flange molding machine.

[0025] Body: Flange There is no particular limitation on the shape of the flange, and it is possible to employ a round flange or a bent flange as shown in Figure 1. The method of forming the flange will be described later.

[0026] bottom The bottom part is made of at least a paper base material. In the present invention, since a polyethylene resin layer is formed on the inner surface of the body part, the body part and the bottom part can be joined even if a polyethylene resin layer is not formed on the bottom part. However, from the viewpoint of waterproofing, it is preferable to laminate a polyethylene resin layer on the inner surface of the bottom part. In the present invention, the inner polyethylene resin layer of the body part is referred to as the "inner polyethylene resin layer", and the polyethylene resin layer formed on the inner surface of the bottom part is referred to as the "bottom-inner polyethylene resin layer".

[0027] Manufacturing method of flanged paper cup Next, a method for manufacturing a flanged paper cup will be described.

[0028] How to make the torso First, an example of a method for producing the body will be described. First, a laminate having an inner polyethylene resin layer, a paper base material, and an outer polyethylene resin layer in this order is punched out into a fan shape. Next, the laminate is rolled up so that the inner polyethylene resin layer is on the inside, and the ends are heat-sealed to produce a cylindrical body.

[0029] Body manufacturing method: Lamination conditions Here, an example of a method for laminating a polyethylene resin layer onto a paper substrate is extrusion lamination. The extrusion lamination method can be appropriately selected from the single lamination method, the tandem lamination method, the sandwich lamination method, the coextrusion lamination method, and the like.

[0030] The temperature of the polyethylene resin (directly below the T-die) during lamination is preferably 260 to 350° C., more preferably 280 to 330° C. Within this range, the laminate strength between the polyethylene resin layer and the paper substrate can be made suitable. In addition, the surface temperature of the cooling roll is preferably controlled within the range of 10 to 50° C.

[0031] The thickness of the polyethylene resin layer after lamination is not particularly limited, but is preferably 30 to 150 μm, more preferably 40 to 100 μm, in which case sufficient cup strength can be achieved after the cup is molded.

[0032] Moreover, if the take-up speed is too slow, the productivity is poor, so the take-up speed is preferably 40 m / min or more, more preferably 60 m / min. On the other hand, if the take-up speed is too fast, the polyethylene resin is likely to neck in, and the productivity is likely to decrease. Therefore, the pulling speed is preferably 130 m / min or less, more preferably 110 m / min or less.

[0033] Next, the air gap will be described. Here, the air gap refers to the distance from the extrusion opening of the T-die to the nip roll.

[0034] If the air gap during lamination is too wide, the polyethylene resin will neck in and productivity will decrease, so the air gap is preferably 250 mm or less, and more preferably 200 mm or less.

[0035] In the present invention, it is preferable to perform a surface treatment with ozone gas and / or oxygen gas while the polyethylene resin is passing through the air gap. By performing a surface treatment with ozone gas and / or oxygen gas, it is possible to promote the formation of an oxide film and improve the adhesive strength with the substrate layer. There is no particular restriction on the amount of ozone gas and / or oxygen gas to be treated, but from the viewpoint of promoting the oxidation of the polyethylene resin, a treatment amount of 0.5 mg / m 2 The above is preferred.

[0036] How to make the bottom An example of a method for producing the bottom will be described. First, a laminate consisting of a bottom / inner polyethylene resin layer and a paper base material (not necessarily including a bottom / inner polyethylene resin layer) is punched into a circle. Next, the peripheral edge of the punched laminate is folded by a press to produce the bottom.

[0037] Joining the body and bottom The bottom part with the folded periphery is fitted into the body part. At this time, the lower end of the body part is folded so that the periphery of the bottom part is sandwiched in the gap. Next, the body member and the bottom plate member are joined by heat welding or the like.

[0038] Flange forming process In the present invention, the flange forming step includes a molding step of molding at least the upper end of the body into a flange while heating it, and a heating step of applying heat after the flange is molded. This will be described in detail below.

[0039] Molding process The molding process is a process in which the upper end of the body is curled outward little by little to obtain a flange. In order to obtain a square-folded flange (square-folded flange) as shown in Figure 1, the flange formed by curling (round flange) can be fitted into a mold and pressed from above to form a square-folded shape.

[0040] In addition, it is preferable to heat the upper end of the body during molding. By heating, the paper base material softens and becomes easier to mold, improving productivity and yield. It is not necessary to heat it all the time during molding, and the timing and interval of heating can be appropriately changed depending on the thickness and hardness of the paper base material, molding speed, etc. For example, when the paper base material is soft and the molding speed is fast, heating can be performed at the first stage of the molding process or during molding. On the other hand, when the paper base material is thick and the molding speed is slow, it is preferable to heat it while heating it all the time.

[0041] heating process The heating step is a step of applying heat to the flange after the flange is molded. Here, the heating step in the present invention is distinguished from the heating during the molding step because the purpose of the step is different. Specifically, the heating during molding is mainly intended to soften the paper base material, whereas the heating in the heating step is intended to soften and melt the polyethylene resin layer to increase the adhesive strength and fix the flange more firmly.

[0042] In addition, in the heating process, it is necessary to heat the polyethylene resin layer to a degree that softens or melts, and if heating is performed by heat transfer, resin pieces will adhere to and accumulate on the substrate, which is likely to reduce productivity and quality. Therefore, heating by convection and / or thermal radiation, which can reduce contact with the substrate, is preferred. An example of a heating device that uses convection is an oven. An example of a heating device that uses thermal radiation is an infrared heater.

[0043] In addition, the area to be heated can be changed as appropriate depending on the application of the paper cup. Specifically, when the outer polyethylene resin layer is foamed to be used as a foamed paper cup, not only the flange but the entire paper cup can be heated. On the other hand, when the paper cup is used as a non-foamed paper cup, it is necessary to heat only a part of the flange so that the outer polyethylene resin layer does not foam.

[0044] Even if the outer polyethylene resin layer does not contain low-density biomass polyethylene resin and is made only of low-density polyethylene resin derived from fossil fuels, the flange strength is improved by undergoing a heating process. However, low-density polyethylene resin derived from fossil fuels has lower adhesiveness than low-density biomass polyethylene resin, making it difficult to improve the flange strength. EXAMPLES

[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" represent "parts by mass" and "% by mass" unless otherwise noted.

[0046] Polyethylene Resin In this example, biomass-derived low-density biomass polyethylene resin (B-LPDE), high-density biomass polyethylene resin (B-HDPE), and fossil fuel-derived low-density polyethylene resin (F-LDPE) were used. The product names, manufacturers, and resin densities are as shown in Table 1.

[0047] [Table 1]

[0048] Laminate 1 (Step 1) A mixed resin of B-LDPE and B-HDPE (B-LDPE:B-HDPE = 40:60, density 0.943 g / cm) is applied to one side of the paper base material. 3 ) was extrusion laminated to form a 40 μm thick inner polyethylene resin layer. (Step 2) Next, a paper substrate was sandwiched between the two and F-LDPE was extrusion laminated to the side opposite the inner polyethylene resin layer to form a 70 μm thick outer polyethylene resin layer (Laminate 1).

[0049] The paper substrate and lamination conditions are as follows. (Process 1) Paper base material: moisture content 23g / m 2 , basis weight 320g / m 2 Extrusion temperature (T die exit temperature): 320℃ Take-off speed (lamination speed): 60m / min Air gap: 80mm

[0050] (Process 2) Extrusion temperature (T die exit temperature): 310℃ Take-off speed (lamination speed): 60m / min Air gap: 80mm

[0051] Laminates 2 to 10 Laminates 2 to 10 were produced by changing the resin raw material used for the outer polyethylene resin layer as shown in Table 2. The conditions other than the resin raw material (extrusion temperature, take-up speed, etc.) were the same as those for Laminate 1.

[0052] [Table 2]

[0053] Prototype example 1 The laminate 1 was punched out into a fan shape, rolled up so that the inner polyethylene resin layer was on the inside, and the end was heat sealed to produce a cylindrical body. Separately from the body, the laminate 1 was punched out into a circle, and the peripheral part of the punched out laminate was folded by a press to produce a bottom. Next, the bottom part with the folded peripheral part was fitted into the body, and heat-sealed at 400°C (0.5 seconds x 2 times) to produce a paper cup (without flange).

[0054] Next, the flange was heated at 420°C for 0.3 seconds, and immediately after that, the top end of the body was curled outward to create a flange (round shape). It was then fitted into a mold and pressed from above to form the flange into a square-folded shape, yielding a flanged paper cup (before the heating process). Finally, the flanged paper cup was heated in an oven at 120°C for 360 seconds to obtain a flanged paper cup (Prototype 1). The paper cup had a mouth diameter of 96φ and a height of 107mm.

[0055] Prototype examples 2-10 As shown in Table 3, Prototype Examples 2 to 10 were produced by changing the laminate 1 to laminates 2 to 10. The conditions other than the laminate (molding conditions, heating conditions, aperture, etc.) were the same as those of Prototype Example 1.

[0056] (evaluation) The flange strength and productivity before and after the heating step were evaluated according to the following criteria.

[0057] Flange Strength The compression strength of the flange (hereinafter referred to as "flange strength") was measured using a compression tester under the following measurement conditions: Compression tester: Tensilon RTC-131OA (A&D), 100N load cell Measurement method: The flange was fixed at a position 90 degrees clockwise from the body and heat seal part (when viewed from above the paper cup), and pressure was applied from a position 90 degrees counterclockwise from the body and heat seal part (180 degrees from the fixed position). The strength (N) at which the flange broke was taken as the flange strength.

[0058] Productivity For each prototype, 40,000 paper cups were flanged and evaluated based on the amount and shape of resin pieces adhering to the flange molding machine after molding. ○: No resin pieces attached △: Resin pieces are attached to the parts that are likely to come into contact with the flange (heater, mold) ×: Resin pieces are attached to various parts inside the flange molding machine.

[0059] [Table 3]

[0060] From Table 3, it can be seen that the flange strength is improved by going through the heating process. This is thought to be due to the fact that the low-density polyethylene resin melts during the heating process, resulting in strong adhesion. Furthermore, a comparison of prototype 1 with prototypes 2 to 10 shows that the flange strength after the heating process is further improved by blending low-density biomass polyethylene resin. Furthermore, since there is no difference in the flange strength before the heating process, the effectiveness of low-density biomass polyethylene resin in the heating process is clear. [Explanation of symbols]

[0061] 1. Outer polyethylene resin layer 2. Inner polyethylene resin layer 3...Paper base material

Claims

1. A method for manufacturing a flanged paper cup having a body portion with a flange and a bottom portion, comprising the steps of: The body portion is made of a laminate having an outer polyethylene resin layer, a paper base material, and an inner polyethylene resin layer laminated in this order, The resin density of the outer polyethylene resin layer is 0.91g / cm 3 More than 0.93g / cm 3 is less than The outer polyethylene resin layer has a density of 0.91g / cm 3 More than 0.93g / cm 3 Contains 0.5% by mass or more and 30% by mass or less of low-density biomass polyethylene resin, The resin density of the inner polyethylene resin layer is higher than the resin density of the outer polyethylene resin layer, and A molding process is provided for molding the upper end of the body into a flange shape, and a heating process is provided for applying heat after the flange is molded. A method for manufacturing a flanged paper cup, comprising the steps of:

2. The method for producing a flanged paper cup according to claim 1, characterized in that the heating step is heating by convection and / or thermal radiation.

3. A method for manufacturing a flanged paper cup as described in claim 1 or 2, characterized in that the inner polyethylene resin layer contains 70% or less low-density biomass polyethylene resin.

Citation Information

Patent Citations

  • Heat treatment method for flange part, its heat treatment device and manufacturing method for resin container with flange

    JP2006062353A

  • Paper cup and its manufacturing method

    JP2008189342A

  • Integrated method for the production of ethylene-butylene copolymer, ethylene-butylene copolymer and use of ethylene and 1-butylene as comonomers supplied from renewable natural raw materials.

    JP2011506628A

  • Laminated body provided with resin layer derived from biomass

    JP2014133338A

  • Paper cup

    JP2015214365A