Non-aqueous electrolyte secondary battery

By employing insulating protective layers with specific thickness ratios and materials, the battery design mitigates stress concentration at the positive electrode connection parts, enhancing conductivity and mechanical strength while maintaining insulation.

JP7577711B2Active Publication Date: 2024-11-05TOYOTA BATTERY CO LTD +2

Patent Information

Application Number
JP2022129375
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-15
Publication Date
2024-11-05
Estimated Expiration
2042-08-15

AI Technical Summary

Technical Problem

The concentration of stress at the bent portions of the positive electrode connection parts in non-aqueous electrolyte secondary batteries, such as lithium-ion batteries, leads to strain on the metal foil, composite material layers, and separators, which can compromise the integrity and performance of the battery.

Method used

The battery design includes a negative electrode and a positive electrode with insulating protective layers of varying thicknesses to distribute the bending stress, ensuring the positive electrode connection parts are bent inwardly and reducing the burden on the separator and composite layers, using boehmite and PVdF as insulating materials with specific thickness ratios.

Benefits of technology

This design reduces the mechanical stress on the positive electrode components, enhances conductivity, and maintains insulation, thereby improving the mechanical strength and reducing internal resistance in the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577711000001
    Figure 0007577711000001
  • Figure 0007577711000002
    Figure 0007577711000002
  • Figure 0007577711000003
    Figure 0007577711000003
Patent Text Reader

Abstract

To reduce the burden in foil collection of a positive electrode connection part, a positive electrode base material, positive electrode mixture layers, a separator, and the like in performing foil collection of the positive electrode connection part of a nonaqueous electrolyte secondary battery.SOLUTION: In a positive electrode plate having insulation protective layers each provided on a positive electrode base material 111 composed of Al foil, positive electrode mixture layers 112, a positive electrode connection part 113, and a position adjacent to the positive electrode mixture layers 112 on both surfaces of the positive electrode connection part 113 to face a negative electrode mixture layer, a relation between the thickness DOUT [μm] of an outer insulation protective layer 114a and the thickness DIN [μm] of an inner insulation protective layer 114b is a relation of DIN<DOUT. Also, the thickness DIN [μm] of the inner insulation protective layer 114b is, for example, 5.0 to 11.6 [μm]. The thickness DOUT [μm] of the outer insulation protective layer 114a depends on the thickness DC [μm] of the positive electrode base material and the thickness DA [μm] of the positive electrode mixture layers 112, and has a relation of DA-DC≤DOUT≤DA.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nonaqueous electrolyte secondary battery, and more particularly to a nonaqueous electrolyte secondary battery having an insulating protective layer, which reduces the burden on the separator and other components of the nonaqueous electrolyte secondary battery. [Background technology]

[0002] 2. Description of the Related Art Non-aqueous electrolyte secondary batteries, typified by lithium ion secondary batteries, have high energy density and high capacity and are therefore used as power sources for driving electric vehicles (EVs), hybrid vehicles (HVs), and the like.

[0003] In general, a lithium ion secondary battery is constructed by stacking positive and negative electrode plates with a separator between them to form an electrode body, and housing the electrode body in a battery case filled with an electrolyte. In particular, in recent years, wound-type lithium ion secondary batteries, in which strip-shaped positive and negative electrode plates are stacked with a separator between them, and the stack is wound in the longitudinal direction in this state to form an electrode body in a compressed state and housed in a battery case, have been widely adopted because of their efficiency and compactness.

[0004] In the invention described in Patent Document 1, in an electrode body in which such positive and negative plates are stacked with a separator interposed therebetween, the respective tip ends of the negative electrode connection part 103 and the positive electrode connection part 113 are aligned as shown in Fig. 6(a). Then, as shown in Fig. 6(b), the negative electrode connection part 103 at one end of the electrode body 10, which is a current collector, in the width direction W is collected and joined to the negative electrode current collector 13. Similarly, the positive electrode connection part 113 at the other end is collected and joined to the positive electrode current collector 15. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-089857 Summary of the Invention [Problem to be solved by the invention]

[0006] However, even if the tips of the connection parts are aligned, when the connection parts are gathered, the connection parts on the periphery are suddenly bent toward the center. When the connection parts are suddenly bent, stress is concentrated at the bent part, which causes a problem of putting a strain on the base material made of metal foil, the composite layer containing resin, the thin resin separator, etc.

[0007] The problem to be solved by the nonaqueous electrolyte secondary battery of the present invention is to reduce the burden on the positive electrode connection part, the positive electrode substrate, the positive electrode mixture layer, the separator, etc., when the positive electrode connection part is assembled. [Means for solving the problem]

[0008] In order to solve the above problems, the nonaqueous electrolyte secondary battery of the present invention comprises a negative electrode plate having a negative electrode substrate made of a band-shaped metal foil of a constant width, a negative electrode mixture layer formed on each of both sides of the negative electrode substrate, and a negative electrode connection part formed at one end in the width direction of the negative electrode substrate and where the negative electrode mixture layer is not formed; a positive electrode substrate made of a band-shaped metal foil of a constant width, a positive electrode mixture layer formed on each of both sides of the positive electrode substrate, a positive electrode connection part formed at the other end in the width direction of the positive electrode substrate and where the positive electrode mixture layer is not formed, and insulating protection layers provided on both sides of the positive electrode connection part adjacent to the positive electrode mixture layer and facing the negative electrode mixture layer. a negative electrode current collecting part at one end of the electrode body in the width direction and a positive electrode current collecting part at the other end of the electrode body, the positive electrode current collecting part being collected and joined; and a positive electrode current collecting part at the other end of the electrode body, the positive electrode current collecting part being collected and joined. The nonaqueous electrolyte secondary battery is characterized in that, in the insulating protective layers formed on both sides of the positive electrode current collecting part, an outer insulating protective layer formed on a surface farther from the positive electrode current collecting part in the stacking direction of the stacked electrode body is formed to be thicker than an inner insulating protective layer formed on a surface closer to the positive electrode current collecting part in the stacking direction of the electrode body.

[0009] The thickness of the inner insulating protective layer is preferably such that, when the positive electrode connection portion is assembled into a foil, the inner insulating protective layer is folded at the end of the negative electrode plate. In this case, the thickness of the inner insulating protective layer may be 11.6 μm or less.

[0010] The thickness of the inner insulating protective layer is preferably a thickness that ensures insulation of the inner insulating protective layer at the end of the negative electrode plate when the positive electrode connection part is collected into a foil. In this case, when the insulating protective layer is composed of insulating particles made of boehmite and a binder made of PVdF, and the mass ratio of boehmite to PVdF is in the range of 70:30 to 90:10, the thickness of the inner insulating protective layer can be 5.0 μm or more.

[0011] The thickness of the outer insulating protective layer is preferably set to a thickness such that when the electrode body is constrained in the thickness direction and the thickness is reduced from the state in which the positive electrode connection portion of the electrode body is collected and joined, the outer insulating protective layer does not bend outward by more than an angle set around the end of the positive electrode mixture layer. In this case, the thickness of the outer insulating protective layer can be set to be equal to or greater than the thickness of the positive electrode mixture layer on the same surface minus the thickness of the positive electrode base material. Also, the thickness of the outer insulating protective layer can be set to be equal to or less than the thickness of the positive electrode mixture layer on the same surface.

[0012] The electrode body can be suitably applied to a wound type electrode body that is wound flat. Effect of the Invention

[0013] According to the nonaqueous electrolyte secondary battery of the present invention, it is possible to reduce the burden on the positive electrode connection part, the positive electrode substrate, the positive electrode mixture layer, the separator, and the like when the positive electrode connection part is assembled. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a perspective view of a cell battery of a lithium ion secondary battery. [Diagram 2] FIG. 2 is a schematic diagram showing the configuration of a wound electrode body. [Diagram 3] FIG. 4 is a perspective view showing an end portion in the width direction of a wound electrode body. [Figure 4] FIG. 2 is a schematic diagram showing the configuration of an electrode body of a lithium ion secondary battery. [Diagram 5] FIG. 2 is a schematic diagram showing the dimensions of a positive electrode substrate, a positive electrode mixture layer, and an insulating protective layer of a positive electrode plate of a laminated electrode assembly. [Figure 6] (a) is a schematic cross-sectional view of an electrode body in which a negative electrode plate, a positive electrode plate, and a separator are laminated in a conventional manufacturing process for an electrode body of a lithium-ion secondary battery, as viewed from the AA direction in Fig. 3. (b) is a schematic cross-sectional view of an electrode body in which a negative electrode connection part and a positive electrode connection part are welded to a negative electrode current collector that is a foil-collected negative electrode current collector, and a positive electrode connection part is welded to a positive electrode current collector that is a foil-collected positive electrode current collector, as viewed from the AA direction in Fig. 3. [Figure 7] FIG. 4 is a schematic diagram showing a foil collection base position of a positive electrode connection part of the present embodiment. [Figure 8] FIG. 13 is a schematic diagram showing the position of a foil collection base point of a positive electrode connection part according to the prior art. [Figure 9] 2 is a schematic diagram of a cross section in the width direction W of a state in which a positive electrode connecting portion is collected and welded to a positive electrode current collecting portion. FIG. [Figure 10] FIG. 1 is a schematic diagram of a widthwise cross section of a lithium-ion secondary battery in a state in which the positive electrode connection portion is collected into a foil and welded to a positive electrode current collector, and then pressure is applied to restrain the lithium-ion secondary battery as a battery stack, compressing the entire electrode body in the thickness direction. [Figure 11] 4 is a schematic diagram showing contact between an outer insulating protective layer and a separator in this embodiment. FIG. [Figure 12] FIG. 2 is a schematic diagram showing contact between an outer insulating protective layer and a separator according to the prior art. [Figure 13] FIG. 2 is a perspective view showing a coating machine for an insulating protective layer. [Figure 14] FIG. 2 is a schematic diagram showing the coating of an outer insulating protective layer. [Figure 15] 1 is a table showing the results of an experimental example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] With reference to FIGS. 1 to 15, the nonaqueous electrolyte secondary battery of the present invention will be described taking an embodiment of a lithium ion secondary battery 1 as an example. (Features of this embodiment) The lithium ion secondary battery 1 of this embodiment aims to reduce the burden on the positive electrode substrate 111, the positive electrode mixture layer 112, the separator 120, and the like when the positive electrode connection portion 113 is assembled.

[0016] <Background Art of the Present Embodiment> Here, a conventional electrode assembly 10 that constitutes the background art will be specifically described. Fig. 2 is a schematic diagram showing the configuration of the wound electrode body 10. The electrode body 10 is formed by stacking a negative electrode plate 100, a positive electrode plate 110, and a separator 120 and winding them. Fig. 3 is a perspective view showing an end of the wound electrode body 10 in the width direction W. The wound electrode body 10 has a flat shape overall, and when viewed from the width direction W, it has a shape like a racing track.

[0017] FIG. 6(a) is a schematic cross-sectional view of the electrode body 10 in which the negative electrode plate 100, the positive electrode plate 110, and the separator 120 are laminated in the manufacturing process of the electrode body 10 of such a conventional wound type lithium ion secondary battery 1, as viewed from the AA direction in FIG. 3. As shown in FIG. 6(a), when the negative electrode plate 100 and the positive electrode plate 110 are laminated, the negative electrode plate 100 and the positive electrode plate 110 are laminated with being shifted in the width direction W. As a result, at one end of the width direction W (left side in the figure), a large number of negative electrode connection parts 103 in which the metal foil on which the negative electrode composite layer 102 is not provided is exposed protrude. At the other end of the width direction W (right side in the figure), a large number of positive electrode connection parts 113 on which the positive electrode composite layer 112 is not provided protrude. Insulating protection layer 114 is formed on positive electrode connecting portion 113 at a position facing negative electrode mixture layer 102 via separator 120 so as to be adjacent to positive electrode mixture layer 112. Conventionally, the tip ends of negative electrode connecting portion 103 and positive electrode connecting portion 113 were aligned so as to be at the same position in width direction W.

[0018] FIG. 6(b) is a schematic diagram of a cross section seen from the AA direction in FIG. 3, showing a state in which the negative electrode connection part 103 is collected and welded to the negative electrode current collector 13, and the positive electrode connection part 113 is collected and welded to the positive electrode current collector 15 in a manufacturing process of the electrode body 10 of the conventional lithium ion secondary battery 1. As shown in FIG. 6(b), the tip 103a of the negative electrode connection part 103 and the tip 113a of the positive electrode connection part 113 are compressed in the thickness direction D and collected. The collected negative electrode connection part 103 is welded while being sandwiched between a pair of negative electrode current collectors 13. The collected positive electrode connection part 113 is welded while being sandwiched between a pair of positive electrode current collectors 15. As shown in FIG. 1, the negative electrode current collector 13 is exposed to the outside of the battery case 11 through the lid 12 and is connected to the negative electrode external terminal 14 outside the lithium ion secondary battery 1. The positive electrode current collecting portion 15 is also exposed to the outside of the battery case 11 via the lid 12 and is connected to a positive electrode external terminal 16 outside the lithium ion secondary battery 1 .

[0019] 4 is a schematic diagram showing the configuration of an electrode body 10 of a lithium-ion secondary battery 1. In the negative electrode plate 100, a negative electrode composite layer 102 is formed on both sides of a negative electrode substrate 101 made of Cu foil or the like. One end (left side in the figure) of the negative electrode composite layer 102 is provided with a negative electrode connection part 103 extending in the one end direction, where the negative electrode composite layer 102 is not formed and the negative electrode substrate 101 is exposed.

[0020] A positive electrode plate 110 is disposed on the negative electrode plate 100 via a separator 120. In the positive electrode plate 110, a positive electrode composite layer 112 is formed on both sides of a positive electrode substrate 111 made of Al foil or the like. At the other end (right side in the figure) of the positive electrode composite layer 112, a positive electrode connection portion 113 where the positive electrode composite layer 112 is not formed and the positive electrode substrate 111 is exposed is provided so as to extend in the other end direction. The positive electrode composite layer 112 is shorter than both ends of the negative electrode composite layer 102 in the width direction W and is formed in the inner range. Therefore, a part of the positive electrode connection portion 113 where the Al foil is exposed faces the negative electrode composite layer 102 via the separator 120. Therefore, in the lithium ion secondary battery 1 of this embodiment, an insulating protection layer 114 is provided at a position adjacent to the positive electrode composite layer 112 on both sides of the positive electrode connection portion 113 and facing the negative electrode composite layer 102.

[0021] Here, of the insulating protective layers 114 formed on both sides of the positive electrode connection part 113, the insulating protective layer 114 formed on the surface farther from the positive electrode current collector 15 in the stacking direction of the electrode body 10 is referred to as the "outer insulating protective layer 114a." Additionally, the insulating protective layer 114 formed on the surface closer to the positive electrode current collector 15 in the stacking direction of the electrode body 10 is referred to as the "inner insulating protective layer 114b."

[0022] <Characteristics of the Configuration of the Insulating Protective Layer 114 of the Present Embodiment> 5 is a schematic diagram showing the dimensions of the positive electrode substrate 111, the positive electrode composite layer 112, and the insulating protective layer 114 of the positive electrode plate 110 of the laminated electrode body 10. C [μm] is a thickness of approximately 10 to 20 [μm], and the positive electrode connection portion 113 where the positive electrode substrate 111 is exposed also has the same thickness.

[0023] Thickness D of one side of the positive electrode mixture layer 112 formed on the positive electrode substrate 111 A [μm] is approximately 15 to 30 [μm] on one side. Thickness D of the outer insulating protective layer 114a OUT [μm] and the thickness D of the inner insulating protective layer 114b IN The relationship in [μm] is expressed by the following formula (1).

[0024] D IN <D OUT ...Formula (1) In addition, the thickness D of the inner insulating protective layer 114b IN [μm] is, for example, 5.0 [μm] or more and 11.6 [μm] or less.

[0025] Thickness D of the outer insulating protective layer 114a OUT [μm] is the thickness D of the positive electrode substrate 111 C [μm] and the thickness D of the positive electrode mixture layer 112 A [μm] and is related by the following equation (2).

[0026] D A -D C ≦D OUT ≦D A…Formula (2) (Action of this embodiment) The operation of this embodiment thus configured will now be described.

[0027] <Thickness D of the inner insulating protective layer 114b IN Effects of being thin [μm]> Thickness D of the outer insulating protective layer 114a OUT [μm] Thickness D of the inner insulating protective layer 114b IN Because it is so thin (μm), it has the following effects:

[0028] The positive electrode connection portion 113 sandwiched between the insulating protective layers 114 has a thickness D of the inner insulating protective layer 114b. IN By reducing the thickness D [μm], a bending moment occurs in which the positive electrode connection part 113 bends inward, but it becomes difficult to bend outward. IN By setting [μm] to a predetermined value or less, it becomes easier to bend inward.

[0029] Here, the position where the positive electrode connecting portion 113 is bent toward the positive electrode current collecting portion 15 is referred to as the "foil collecting base position P1". Fig. 8 is a schematic diagram showing the foil collection base position P1 of the positive electrode connecting portion 113 of the prior art. In Fig. 8, the part below and the left side of the center CC shown in Fig. 6(b) are omitted in order to conceptually explain the invention. Also, the number of layers is extremely small. This is common to Figs. 7 to 10.

[0030] As shown in FIG. 8, the insulating protective layer 114 of the prior art has a thickness D of the outer insulating protective layer 114a. OUT [μm] and the thickness D of the inner insulating protective layer 114b IN In order to ensure insulation, the thickness D of the inner insulating protective layer 114b of this embodiment is IN For this reason, the positive electrode connecting portion 113 is less likely to bend inward, and when the foil is collected, the foil collection base position P1 at which the positive electrode connecting portion 113 bends becomes the insulating protective layer end 114e, which is the coated end of the insulating protective layer 114 where the metal foil is exposed.

[0031] 7 is a schematic diagram showing a foil collection base position P1 of the positive electrode connecting portion 113 of this embodiment. As shown in FIG. 7, the positive electrode connecting portion 113 on which the insulating protective layer 114 is formed is collected at the positive electrode current collecting portion 15 of the electrode body 10. In this case, the thickness D IN Specifically, the thickness D of the inner insulating protective layer 114b is IN For example, the thickness (μm) of the positive electrode connection portion 113 is equal to or smaller than 11.6 μm. Therefore, regardless of the insulating protective layer 114, the foil collection base position P1 of the positive electrode connection portion 113 becomes the negative electrode slit end 100e of the negative electrode plate 100.

[0032] Therefore, the length of the positive electrode connection part 113 in the conventional technology is shorter than the length of the positive electrode connection part 113 required for the positive electrode connection part 113 in this embodiment to be collected by the positive electrode current collecting part 15. In other words, the position of the tip 113t of the positive electrode connection part 113 shown in FIG. 7 moves toward the tip (right side in FIG. 7) from the position of the tip 113t of the positive electrode connection part 113 shown in FIG. 8. Then, the length W1 of the positive electrode current collecting part 15 in this embodiment that contacts with the positive electrode connection part 113 can be made longer than the length W2 of the positive electrode current collecting part 15 in the conventional technology that contacts with the positive electrode connection part 113. Therefore, a larger area can be secured in the current collecting joint area of ​​the positive electrode current collecting part 15 at the tip of the positive electrode connection part 113. Therefore, the electrical conductivity is improved, and the internal resistance DC-IR is reduced, and the mechanical strength of the welding can also be increased.

[0033] In this embodiment, the inner insulating protective layer 114b comes into contact with the negative electrode slit end 100e via the separator 120 when bent. Therefore, it is necessary to ensure insulation with the negative electrode composite material layer 102 in the event that the separator 120 is damaged. For this reason, the thickness D of the inner insulating protective layer 114b is IN However, when the positive electrode connection portion 113 is assembled, the thickness is required to ensure insulation of the inner insulating protective layer 114b at the position of the negative electrode slit end 100e of the negative electrode plate 100.

[0034] In this embodiment, specifically, the insulating protective layer 114 is composed of insulating particles made of boehmite and a binder made of PVdF. The mass ratio of the boehmite to the PVdF is in the range of 70:30 to 90:10. In such a case, the thickness D of the inner insulating protective layer 114b is IN Insulation can be ensured by making the thickness 5.0 μm or more.

[0035] <Thickness D of the outer insulating protective layer 114a IN Effects of being thick [μm] The thickness D of the outer insulating protective layer 114a of the lithium ion secondary battery 1 of this embodiment IN The thick [μm] provides the following effects.

[0036] FIG. 9 is a schematic diagram of a cross section in the width direction W, showing a state in which the positive electrode connecting portion 113 is collected into a foil and welded to the positive electrode current collecting portion 15. 7, in this embodiment, when the positive electrode connecting portion 113 is collected, the positive electrode connecting portion 113 is bent with the negative electrode slit end 100e of the negative electrode plate 100 as the collection base position P1. At this time, the inner insulating protective layer 114b comes into contact with the negative electrode slit end 100e via the separator 120.

[0037] 10 is a schematic diagram of a cross section in the width direction W in a state in which the lithium-ion secondary battery 1 is compressed in the thickness direction D as a whole by applying pressure to the lithium-ion secondary battery 1 as a battery stack and restraining the lithium-ion secondary battery 1 after the positive electrode connection parts 113 are collected and welded to the positive electrode current collector 15. After the positive electrode connection parts 113 are collected and welded to the positive electrode current collector 15 to assemble the lithium-ion secondary battery 1, a plurality of the lithium-ion secondary battery 1 cells are stacked together and restrained by applying pressure in the stacking direction with a restraining tool. The lithium-ion secondary battery 1 is then maintained at a high temperature for an aging process or the like.

[0038] As shown in FIG. 9, the electrode body 10 immediately after the positive electrode connection portion 113 is collected and welded to the positive electrode current collector 15 has a thickness D E1 When the electrode assembly 10 is subsequently restrained at a high temperature in an aging process or the like, it is compressed to a thickness D E2At this time, the thickness D of the electrode body 10 is E1 is compressed to thickness D E2 However, since the length of the positive electrode connecting portion 113 does not change, the outer bending point P2 where the outer insulating protective layer 114a is bent is pushed upward relative to the electrode body 10. For this reason, the outer bending point P2 shown in Fig. 9 comes into contact with the upper (outer) separator 120 as shown in Fig. 10.

[0039] 12 is a schematic diagram showing the contact between the outer insulating protective layer 114a and the separator 120 in the present embodiment of the prior art. IN and the thickness D of the outer insulating protective layer 114a OUT and the thickness D of the outer insulating protective layer 114a is the same. OUT However, the thickness D of this embodiment OUT Therefore, the distance between the outer bending point P2 and the separator 120 before bending becomes large, and therefore, when the outer bending point P2 comes into contact with the separator 120 after bending, the bending angle θ2 centered on the base end 113e of the positive electrode connection portion of the positive electrode substrate 111 becomes relatively large. This places a large burden on the outer insulating protective layer 114a and the positive electrode substrate 111.

[0040] 11 is a schematic diagram showing the contact between the outer insulating protective layer 114a and the separator 120 in this embodiment. IN Thickness D of the outer insulating protective layer 114a OUT The thickness D of the outer insulating protective layer 114a is thicker. OUT However, the thickness of the conventional technology D OUT 1. As a result, the distance between the outer bending point P2 and the separator 120 before bending is reduced. Therefore, even if the outer bending point P2 comes into contact with the separator 120 after bending, the bending angle θ1 centered on the base end 113e of the positive electrode connecting portion of the positive electrode substrate 111 becomes smaller than the bending angle θ2. Therefore, no large burden is placed on the outer insulating protective layer 114a and the positive electrode substrate 111.

[0041] Specifically, the thickness D of the outer insulating protective layer 114a OUT [μm] is the thickness D of the positive electrode substrate 111C [μm] and the thickness D of the positive electrode mixture layer 112 A [μm] and is related by the following equation (2).

[0042] D A -D C ≦D OUT ≦D A …Formula (2) (Configuration of the first embodiment) The configuration of the lithium ion secondary battery 1 according to this embodiment having the above-mentioned characteristics will be described in detail below.

[0043] <Basic structure of lithium-ion secondary battery 1> FIG. 1 is a perspective view of a lithium-ion secondary battery 1. As shown in FIG. 1, the lithium-ion secondary battery 1 is configured as a cell battery. The lithium-ion secondary battery 1 includes a rectangular parallelepiped battery case 11 having an opening on the upper side. The battery case 11 includes a lid 12 that seals the battery case 11. An electrode body 10 is housed inside the battery case 11. A nonaqueous electrolyte 17 is injected into the battery case 11 through an injection hole (not shown). The battery case 11 and the lid 12 are made of a metal such as an aluminum alloy. The lithium-ion secondary battery 1 is configured as a sealed battery container by attaching the lid 12 to the battery case 11. The lithium-ion secondary battery 1 also includes a negative electrode external terminal 14 and a positive electrode external terminal 16 on the lid 12, which are used for charging and discharging power.

[0044] <Electrode body 10> FIG. 2 is a schematic diagram showing the configuration of the wound electrode body 10. The electrode body 10 is formed by winding a negative electrode plate 100, a positive electrode plate 110, and a separator 120 arranged between them flatly. In the negative electrode plate 100, a negative electrode composite layer 102 is formed on a negative electrode substrate 101. On one end side of the width direction W (winding axis direction) perpendicular to the winding direction (winding direction L), a negative electrode connection part 103 is provided where the negative electrode composite layer 102 is not formed and the negative electrode substrate 101 is exposed. In the positive electrode plate 110, a positive electrode composite layer 112 is formed on a positive electrode substrate 111. On the other end side of the width direction W (winding axis direction) perpendicular to the winding direction (winding direction L) of the positive electrode substrate 111, a positive electrode connection part 113 is provided where the positive electrode composite layer 112 is not formed and the positive electrode substrate 111 is exposed.

[0045] <End Configuration of Electrode Body 10> 3 is a perspective view showing the end of the wound electrode body 10 in the width direction. The negative electrode plate 100, the positive electrode plate 110, and the separator 120 are wound to form a flat electrode body 10 shaped like a racing track when viewed from the width direction W. The upper and lower ends are semicircular, and the negative electrode plate 100 and the positive electrode plate 110 form a "curved surface portion R." The center portion is linear, and the negative electrode plate 100 and the positive electrode plate 110 form a "flat surface portion F." In this embodiment, the straight line of the portion corresponding to the winding axis is called the "center C."

[0046] 3 (the right end in the drawing), the positive electrode connection part 113 is collected and is electrically and mechanically fixed by welding to the positive electrode current collecting part 15. Note that FIG. 3 is just an example, and the shape is not limited thereto.

[0047] <Laminate of electrode body 10> Fig. 4 is a schematic diagram showing the configuration of the laminate of the electrode body 10 of the lithium ion secondary battery 1. As shown in Fig. 4, the electrode body 10 of the lithium ion secondary battery 1 includes a negative electrode plate 100, a positive electrode plate 110, and a separator 120. The negative electrode plate 100 includes a negative electrode composite layer 102 on both sides of a negative electrode substrate 101. The positive electrode plate 110 includes a positive electrode composite layer 112 on both sides of a positive electrode substrate 111. The negative electrode plate 100 and the positive electrode plate 110 are stacked with the separator 120 interposed therebetween to form a laminate. This laminate is wound in the longitudinal direction around the winding axis and shaped into a flat electrode body 10.

[0048] <Negative electrode plate 100> As shown in FIG. 4, a negative electrode plate 100 is formed by forming a negative electrode composite layer 102 on both sides of a negative electrode substrate 101. In this embodiment, the negative electrode substrate 101 is made of Cu foil. The negative electrode substrate 101 serves as a base for the aggregate of the negative electrode composite layer 102, and also functions as a current collecting member that collects electricity from the negative electrode composite layer 102. In the negative electrode plate 100, the negative electrode composite layer 102 is formed on the metallic negative electrode substrate 101. In the first embodiment, the negative electrode active material is a material capable of absorbing and releasing lithium ions, and a powdered carbon material made of graphite or the like is used.

[0049] The negative electrode plate 100 is produced, for example, by kneading a negative electrode active material, a solvent, and a binding material (binder), applying the kneaded negative electrode mixture to the negative electrode substrate 101, and drying it. <Positive electrode plate 110> 4, positive electrode plate 110 is formed by forming positive electrode composite layer 112 on both sides of positive electrode substrate 111. In this embodiment, positive electrode substrate 111 is made of Al foil or Al alloy foil. Positive electrode substrate 111 serves as a base as an aggregate for positive electrode composite layer 112, and also functions as a current collecting member that collects electricity from positive electrode composite layer 112.

[0050] The positive electrode plate 110 has a positive electrode composite layer 112 formed on the surface of a positive electrode substrate 111. The positive electrode composite layer 112 has a positive electrode active material. The positive electrode active material is a material capable of absorbing and releasing lithium, and for example, lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), etc. may be used. Alternatively, a material in which LiCoO2, LiMn2O4, and LiNiO2 are mixed in any ratio may be used.

[0051] Positive electrode mixture layer 112 also contains a conductive material. As the conductive material, for example, carbon black such as acetylene black (AB) or ketjen black, or graphite can be used.

[0052] The positive electrode plate 110 is produced, for example, by kneading a positive electrode active material, a conductive material, a solvent, and a binding material (binder), applying the kneaded positive electrode mixture to the positive electrode substrate 111, and drying it. <Separator 120> The separator 120 is a nonwoven fabric made of polypropylene or the like for holding the nonaqueous electrolyte 17 between the negative electrode plate 100 and the positive electrode plate 110. As the separator 120, a porous polymer membrane such as a porous polyethylene membrane, a porous polyolefin membrane, and a porous polyvinyl chloride membrane, or a lithium ion or ion conductive polymer electrolyte membrane can be used alone or in combination. When the electrode body 10 is immersed in the nonaqueous electrolyte 17, the nonaqueous electrolyte 17 permeates the separator 120 from the end toward the center.

[0053] <Insulating protective layer 114> In the positive electrode plate 110 of this embodiment, the insulating protective layer 114 is formed as described above. Insulating particles are dispersed and fixed by a binder in the insulating protective layer 114. The insulating protective layer 114 is formed by applying an insulating protective paste to the surface of the positive electrode substrate 111 along the edge of the positive electrode composite layer 112 and drying the paste.

[0054] The insulating protection paste is a paste in which a solvent is added to a binder to make it liquid, and insulating particles are dispersed in the paste. A dispersant is also added to disperse the insulating particles evenly within the paste.

[0055] The insulating particles are disposed between the negative electrode composite layer 102 and the positive electrode substrate 111 (positive electrode connection portion 113) to provide electrical insulation. Examples of insulating particles include ceramics obtained by sintering metal oxides, which have high insulating properties and hardness sufficient to prevent the intrusion of foreign matter. Specifically, particles of boehmite, alumina, or the like are used. In this embodiment, boehmite is used.

[0056] <Boehmite> Boehmite is an aluminum hydroxide (γ-AlO(OH)) mineral and a component of the aluminum ore bauxite. It exhibits a vitreous to pearlescent luster, a Mohs hardness of 3-3.5, and a specific gravity of 3.00-3.07. It has high insulating, heat-resistant, and hardness properties, and industrially it can be used as an inexpensive flame-retardant additive for fire-resistant polymers.

[0057] Boehmite has the chemical composition AlO(OH) or Al2O3·H2O, and is generally a chemically stable alumina monohydrate produced by heating or hydrothermally treating alumina trihydrate in air. Boehmite has a high dehydration temperature of 450-530°C, and by adjusting the production conditions, it can be controlled into various shapes such as plate-like boehmite, needle-like boehmite, and hexagonal plate-like boehmite. In addition, the aspect ratio and particle size can be controlled by adjusting the production conditions.

[0058] The binder may be, for example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid, polyacrylate, etc. In this embodiment, polyvinylidene fluoride (PVdF) is used.

[0059] <Combination of insulating particles and binder> In this embodiment, the insulating protective layer 114 is composed of insulating particles made of boehmite and a binder made of PVdF. The mass ratio of boehmite to PVdF is in the range of 70:30 to 90:10. In addition, in this embodiment, the thickness D of the inner insulating protective layer 114b is IN In this range, when separator 120 is broken, even if inner insulating protective layer 114b comes into direct contact with negative electrode composite layer 102 at negative electrode slit end 100e, insulation can be ensured and a short circuit can be avoided.

[0060] <Nonaqueous electrolyte 17> The nonaqueous electrolyte 17 shown in FIG. 13 is a composition in which a supporting salt is contained in a nonaqueous solvent. Here, ethylene carbonate (EC) can be used as the nonaqueous solvent. Alternatively, one or more materials selected from the group consisting of propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), etc. can be used. Also, one or more lithium compounds (lithium salts) selected from LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, etc. can be used as the supporting salt.

[0061] (Method of Coating Insulating Protective Layer 114) An example of a method for coating the insulating protective layer 114 of this embodiment will be described below. In the insulating protective layer 114 of this embodiment, the thickness D of the outer insulating protective layer 114a is OUT and the thickness D of the inner insulating protective layer 114b IN The thicknesses are different. The thickness difference can be achieved by adjusting the viscosity of the paste, the solid content NV, the discharge amount and discharge speed of the coater 5, the conveying speed of the positive electrode substrate 111, and the like. In addition, as described below, the difference in the gap of the die nozzle 51 can also be used. Of course, it goes without saying that these methods can be appropriately combined to achieve an appropriate thickness.

[0062] <Configuration of Coating Machine 5> FIG. 13 is a perspective view showing a coater 5 in the coating step of this embodiment. As shown in FIG. 13, the coater 5 is provided with a stage 57 serving as a base. The stage 57 is provided with a positioning guide 58 for transporting the pre-cut positive electrode substrate 111 made of Al foil formed in a long strip shape. The positive electrode substrate 111 is drawn out from a supply reel (not shown) and transported on the stage 57 by a transport means. A gate-shaped die nozzle 51 is provided at the end of the stage 57 on the upstream side in the transport direction of the positive electrode substrate 111, in a direction perpendicular to the transport direction, so as to straddle the positive electrode substrate 111. The die nozzle 51 is provided with a first die 52 for storing the positive electrode composite paste. The first die 52 is a space provided at a position corresponding to the position where the positive electrode composite layer 112 is formed. The positive electrode composite paste is supplied from a supply means (not shown) and stored in the first die 52. The second die 54 is a space provided at a position corresponding to the position where the insulating protective layer 114 is to be formed. An insulating protective paste is supplied from a supplying means (not shown) and stored in the second die 54. The first die 52 and the second die 54 are adjacent to each other and aligned in the same straight line.

[0063] First nozzle 53 is a nozzle that communicates from the lower part of first die 52 to a position where positive electrode mixture layer 112 of positive electrode substrate 111 on stage 57 is to be formed. When the internal pressure of first die 52 is increased by a pressurizing means (not shown), a predetermined amount of positive electrode mixture paste is discharged from first nozzle 53 to the position where positive electrode mixture layer 112 of positive electrode substrate 111 is to be formed.

[0064] The second nozzle 55 is a nozzle that communicates from the bottom of the second die 54 to a position on the stage 57 where the insulating protective layer 114 of the positive electrode substrate 111 is to be formed. When the internal pressure of the second die 54 is increased by a pressurizing means (not shown), a predetermined amount of insulating protective paste is discharged from the second nozzle 55 to the position where the insulating protective layer 114 of the positive electrode substrate 111 is to be formed. In this manner, the positive electrode composite layer 112 and the inner insulating protective layer 114b are formed on the surface that will become the inner side of the positive electrode substrate 111.

[0065] Next, on the portion that will become the outer side of positive electrode substrate 111, positive electrode composite layer 112 and outer insulating protective layer 114a are formed. FIG. 14 is a schematic diagram showing an example of coating of the outer insulating protective layer 114a. The coating of the outer insulating protective layer 114a is basically the same as the coating of the inner insulating protective layer 114b. However, the back surface is supported by a backup roll 59 instead of the stage 57. When coating the outer insulating protective layer 114a on the outer surface, as shown in FIG. 14, the positive electrode composite layer 112 and the inner insulating protective layer 114b are already formed on the inner surface of the positive electrode substrate 111. At this time, the inner surface of the positive electrode substrate 111 is brought into contact with a backup roll 59 instead of the stage 57, and the die nozzle 51 is set with a predetermined gap G1 between them. At this time, the thickness D of the inner insulating protective layer 114b is 100 mm. IN is the thickness D of the positive electrode mixture layer 112 A Therefore, when gap G1 is set at the portion of positive electrode composite layer 112, inner insulating protective layer 114b sticks to backup roll 59, and gap G2 at the portion of inner insulating protective layer 114b becomes larger than gap G1. By utilizing this gap G2, thickness D OUT The thickness D of the inner insulating protective layer 114b IN The coating step is not limited to this simultaneous coating method, and positive electrode mixture layer 112 and insulating protection layer 114 may be formed separately.

[0066] (Experimental Example of the Present Embodiment) FIG. 15 is a table showing the results of the experimental examples. In this experiment, the positive electrode substrate 111 has a thickness D C The thickness of the positive electrode mixture layer 112 on one side is 12 μm. A For this reason, the thickness D A of the positive electrode composite layer 112 on one side minus the thickness D A of the positive electrode substrate 111 was C The value of [ is commonly 12.8 [μm].

[0067] The experiment was evaluated based on the following four criteria: Criterion 1: In the lithium ion secondary battery 1 of this embodiment, the thickness D of the outer insulating protective layer 114a OUT [μm] and the thickness D of the inner insulating protective layer 114b IN The relationship between [μm] and D IN <D OUT The standard is that

[0068] Criterion 2: Thickness D of the inner insulating protective layer 114b IN The standard value for [μm] is 11.6 [μm] or less. Criterion 3: Thickness D of the inner insulating protective layer 114b IN The standard value for [μm] is 5.0 [μm] or more.

[0069] Criterion 4: Thickness D of the outer insulating protective layer 114a OUT [μm] is D A -D C ≦D OUT ≦D A The relationship is the basis. It should be noted that these criteria 1 to 4 indicate the preferred ranges of the present invention and are not intended to limit the invention.

[0070] <Experimental Example 1> The total thickness of the insulating protective layer is 22.4 [μm], and the thickness D of the inner insulating protective layer 114b IN 9.9 [μm], and the thickness D of the outer insulating protective layer 114a OUT is 12.5 [μm].

[0071] Therefore, the criteria 1, 2, and 3 are satisfied, and the foil collection base position P1 is also located at the negative electrode slit end 100e. However, the thickness D OUT Since the thickness is less than 12.8 μm, it does not satisfy criterion 4. As a result, bending cannot be sufficiently suppressed, and a load is applied to positive electrode substrate 111 and separator 120.

[0072] <Experimental Example 2> The total thickness of the insulating protective layer is 24.1 [μm], and the thickness D of the inner insulating protective layer 114b IN10.9 [μm], and the thickness D of the outer insulating protective layer 114a OUT is 13.2 [μm].

[0073] Therefore, all of criteria 1, 2, 3, and 4 are satisfied. As a result, the foil collection starting point position P1 is also located at the negative electrode slit end 100e, so the foil collection path can be shortened. In addition, bending is sufficiently suppressed, and no load is applied to the positive electrode substrate 111 and the separator 120.

[0074] <Experimental Example 3> The total thickness of the insulating protective layer is 26.8 [μm], and the thickness D of the inner insulating protective layer 114b IN 11.6 [μm], and the thickness D of the outer insulating protective layer 114a OUT is 15.2 [μm].

[0075] Therefore, all of criteria 1, 2, 3, and 4 are satisfied. As a result, the foil collection starting point position P1 is also located at the negative electrode slit end 100e, so the foil collection path can be shortened. In addition, bending is sufficiently suppressed, and no load is applied to the positive electrode substrate 111 and the separator 120.

[0076] <Experimental Example 4> The total thickness of the insulating protective layer is 25.2 [μm], and the thickness D of the inner insulating protective layer 114b IN 12.0 [μm], and the thickness D of the outer insulating protective layer 114a OUT is 13.2 [μm].

[0077] Therefore, the criteria 1, 3, and 4 are satisfied. As a result, bending is sufficiently suppressed, and no load is applied to the positive electrode substrate 111 and the separator 120. On the other hand, the thickness D IN exceeds the reference value of 11.6 μm, the foil collection base position P1 is located at the insulating protective layer end 114e, the foil collection path cannot be shortened, and the contact area at the positive electrode current collecting portion 15 is reduced.

[0078] <Experimental Example 5> The total thickness of the insulating protective layer is 24.7 [μm], and the thickness D of the inner insulating protective layer 114b IN 13.5 [μm], and the thickness D of the outer insulating protective layer 114a OUT is 11.2 [μm].

[0079] In addition, the thickness D of the inner insulating protective layer 114b IN is the thickness D of the outer insulating protective layer 114a OUT It's thicker. Therefore, criterion 3 is met, but criteria 1, 2, and 4 are not met.

[0080] As a result, since the foil collection base position P1 is located at the insulating protective layer end 114e, the foil collection path cannot be shortened, and the contact area is reduced in the positive electrode current collector 15. In addition, bending cannot be sufficiently suppressed, and a load is applied to the positive electrode substrate 111 and the separator 120.

[0081] <Summary of the experiment> What can be derived from the above experiments is that when criteria 1 to 4 are satisfied, the foil collection path can be shortened because the foil collection base position P1 is located at the negative electrode slit end 100e. In addition, bending is sufficiently suppressed, and no load is applied to the positive electrode substrate 111 and the separator 120.

[0082] If criterion 1 is not satisfied, the bending moment is assumed to be on the outside, and it is physically evident that the insulating protective layer 114 will have difficulty bending inward. Furthermore, if criterion 2 is not satisfied, the inner insulating protective layer 114b is difficult to bend. Therefore, the foil collection base position P1 is located at the insulating protective layer end 114e, and the foil collection path cannot be shortened. As a result, it was found that the contact area in the positive electrode current collector 15 is reduced.

[0083] If criterion 3 is not met, it is known that a problem occurs in the strength of the inner insulating protective layer 114b, although this was not confirmed in this experiment. Moreover, it was found that when criterion 4 is not satisfied, bending cannot be sufficiently suppressed, and a load is applied to the positive electrode substrate 111 and the separator 120.

[0084] The total thickness of the insulating protective layer D IN +D OUT The size of [μm] itself does not directly relate to the quality of the result, but the quality of the result depends on the thickness D IN and the thickness D of the outer insulating protective layer 114a OUT It is clear that it is based on.

[0085] As described above, through this experiment, Experimental Examples 2 and 3 which satisfy the criteria 1 to 4 are preferred examples of this embodiment, and Experimental Examples 1, 4, and 5 are comparative examples of this embodiment, but the present invention is not limited thereto.

[0086] (Effects of this embodiment) (1) According to the lithium ion secondary battery 1 of the present embodiment, there is an advantage that the burden on the positive electrode substrate 111, the positive electrode composite layer 112, the separator 120, and the like when the positive electrode connection portion 113 is assembled can be reduced.

[0087] (2) Thickness D of the outer insulating protective layer 114a formed on the surface farther from the positive electrode current collecting portion 15 in the stacking direction of the electrode body 10 OUT However, the thickness D of the inner insulating protective layer 114b formed on the surface close to the positive electrode current collecting portion 15 is IN This has the effect of making the positive electrode plate 110 easier to bend so as to approach the positive electrode current collecting portion 15.

[0088] (3) In particular, the thickness D of the inner insulating protective layer 114b IN However, when the positive electrode connection portion 113 is folded, the inner insulating protective layer 114b is made to have a thickness such that it bends at the end of the negative electrode plate 100. Specifically, the thickness D IN is 11.6 [μm] or less. Therefore, there is an effect that the path to the positive electrode current collecting portion 15 can be shortened. As a result, there is an effect that the contact area at the positive electrode current collecting portion 15 can be enlarged.

[0089] (4) Thickness D of the inner insulating protective layer 114b IN is a thickness that ensures insulation of the inner insulating protective layer 114b at the end position of the negative electrode plate 100 when the positive electrode connection portion 113 is collected. Specifically, the insulating protective layer 114 is composed of insulating particles made of boehmite and a binder made of PVdF, and the ratio of the mass of boehmite to the mass of PVdF is in the range of 70:30 to 90:10. In this case, the thickness D of the inner insulating protective layer 114b is IN Therefore, even if the insulation of the separator 120 is lost, the insulation of the inner insulating protective layer 114b at the end of the negative electrode plate 100 is guaranteed.

[0090] (5) Thickness D of the outer insulating protective layer 114a OUT However, after the positive electrode connection portion 113 of the electrode body 10 is collected and joined, the electrode body 10 is constrained in the thickness direction D and the thickness is reduced. In this case, the thickness is set so that the outer insulating protective layer 114a does not bend outward by more than the angle θ1 set around the end of the positive electrode mixture layer 112. Therefore, bending is sufficiently suppressed, and there is an effect that no load is applied to the positive electrode substrate 111 and the separator 120.

[0091] (6) Thickness D of the outer insulating protective layer 114a OUT is the thickness D of the positive electrode mixture layer 112 on the same surface. A from the thickness D of the positive electrode substrate 111 C Therefore, it is possible to effectively suppress bending.

[0092] (7) Thickness D of the outer insulating protective layer 114a OUT However, the thickness D of the positive electrode mixture layer 112 on the same surface A This has the effect of preventing outer insulating protective layer 114a from becoming thicker than positive electrode mixture layer 112.

[0093] (8) The insulating protective layer 114 of this embodiment has the effect of being suitably implemented when the electrode body 10 is a wound-type electrode body that is wound flat. (Other examples) The coating method for the insulating protective layer 114 in this embodiment is merely an example, and the present invention is not limited to this method.

[0094] The drawings illustrated in Figures 1 to 14 have been simplified or deformed for illustrative purposes, and the omission of the number of windings and the number of layers of the electrode body 10, the balance of thickness, width, and length, the amount of deviation, angles, etc. are merely examples and do not limit the present invention.

[0095] In addition, the numerical ranges given as preferred ranges in the embodiments are merely examples, and a person skilled in the art can appropriately optimize the ranges depending on the configuration, materials, etc. of the battery. In the embodiment, the laminate is wound and then shaped into a flat shape, but the wound type lithium ion secondary battery 1 is not necessarily limited to a flat shape. For example, the present invention can be implemented in an electrode body 10 wound into a cylindrical shape. Furthermore, the present invention can be preferably implemented in a so-called stacked type electrode body 10 in which a large number of rectangular positive electrode plates, negative electrode plates, and separators of approximately the same shape are stacked.

[0096] The lithium ion secondary battery 1 of the present embodiment is one embodiment of the present invention, and it goes without saying that the present invention is not limited to the embodiment and can be implemented by a person skilled in the art by adding, deleting, or modifying the configuration thereof, as long as it does not deviate from the scope of the claims. [Explanation of symbols]

[0097] 1...Lithium-ion secondary battery 10...Electrode body 11…Battery case 12…Lid body 13...Negative electrode current collector 14...Negative external terminal 15…Positive electrode current collector 16…Positive external terminal 17...Nonaqueous electrolyte 100: Negative plate 100e: Negative electrode slit end 101...Negative electrode substrate 102...Negative electrode composite layer 103...Negative electrode connection part 110…Positive electrode plate 111...Positive electrode substrate 112: Positive electrode mixture layer 113…Positive electrode connection part 113e…Positive electrode connection base end 114...Insulating protective layer 114a…Outer insulation protective layer 114b…Inner insulating protective layer 114e…Insulating protection layer end 120…Separator C…center R…Curved surface part F...Plane part L…Rolling direction (longitudinal direction) W…Width direction D: Thickness direction D E1 , D E2 [mm]…Electrode thickness D C [μm]…Thickness of the positive electrode substrate 111 D A [μm]…Thickness of one side of the positive electrode mixture layer 112 D OUT [μm]…Thickness of outer insulating protective layer 114a D IN [μm]…Thickness of the inner insulating protective layer 114b P1…Foil collection base point position P2…Outside bending point

Claims

1. a negative electrode plate including a negative electrode substrate made of a band-shaped metal foil having a constant width, a negative electrode composite layer formed on each of both sides of the negative electrode substrate, and a negative electrode connection portion formed at one end in a width direction of the negative electrode substrate and on which the negative electrode composite layer is not formed; a positive electrode plate including a positive electrode substrate made of a band-shaped metal foil having a constant width, a positive electrode mixture layer formed on each of both sides of the positive electrode substrate, a positive electrode connection part formed at the other end in the width direction of the positive electrode substrate and on which the positive electrode mixture layer is not formed, and insulating protection layers provided on both sides of the positive electrode connection part adjacent to the positive electrode mixture layer and facing the negative electrode mixture layer, a separator disposed between the positive electrode plate and the negative electrode plate; An electrode assembly comprising a laminate comprising: a negative electrode current collector to which a negative electrode connection portion at one end in a width direction of the electrode body is collected and joined, and a positive electrode current collector to which a positive electrode connection portion at the other end is collected and joined, In the insulating protective layers formed on both sides of the positive electrode connection part, when a bending moment occurs such that the positive electrode connection part is bent inwardly, an outer insulating protective layer, which is the insulating protective layer formed on the surface opposite to the inner insulating protective layer across the positive electrode connection part, is thicker than an inner insulating protective layer, which is the insulating protective layer formed on the inner surface; The thickness of the outer insulating protective layer is set so that when the electrode body is constrained in the thickness direction and the thickness is reduced from the state in which the positive electrode connection portion of the electrode body is collected and joined, the outer insulating protective layer does not bend outward by more than a set angle centered on the end of the positive electrode mixture layer. a thickness of the outer insulating protective layer being equal to or greater than the thickness of the positive electrode mixture layer on the same surface minus the thickness of the positive electrode substrate;

2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the thickness of the outer insulating protective layer is equal to or less than the thickness of the positive electrode mixture layer on the same surface.

3. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the thickness of the inner insulating protective layer is such that, when the positive electrode connection portion is folded, the inner insulating protective layer is folded at the end of the negative electrode plate.

4. 4. The nonaqueous electrolyte secondary battery according to claim 3, wherein the inner insulating protective layer has a thickness of 11.6 [mu]m or less.

5. 4. The nonaqueous electrolyte secondary battery according to claim 3, wherein the thickness of the inner insulating protective layer is such that, when the positive electrode connection portion is assembled, insulation of the inner insulating protective layer is ensured at the end position of the negative electrode plate.

6. 6. The nonaqueous electrolyte secondary battery according to claim 5, wherein the insulating protective layer is composed of insulating particles made of boehmite and a binder made of PVdF, and when the mass ratio of boehmite to PVdF is in the range of 70:30 to 90:10, the thickness of the inner insulating protective layer is 5.0 μm or more.

7. 7. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrode body is a wound-type electrode body that is wound flat.

Citation Information

Patent Citations

  • Power storage device

    JP2017143003A

  • Positive electrode

    JP2020113486A

  • Power storage device

    JP2020123549A

  • Lithium ion battery

    JP2020173942A

  • Power storage element

    JP2021002422A

Cited By

  • Nonaqueous electrolyte secondary battery

    JP2024077298A