Polymer particles, thickeners and compositions
Polymer particles with controlled molecular weight and size distribution address uneven solubility and viscosity issues, ensuring uniform viscosity and stable composition, enhancing coating quality.
Patent Information
- Application Number
- JP2022511502
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing polymer particles with varying particle sizes exhibit non-uniform solubility and viscosity due to differences in molecular weight, leading to uneven composition viscosity and the formation of joint powders, which affect coating properties and appearance.
Polymer particles with a predetermined difference in molecular weight and particle size distribution, characterized by specific formulas, are designed to gradually dissolve in a dissolution medium, preventing sudden viscosity changes and joint powder formation.
The polymer particles achieve uniform viscosity increase and stable maintenance, improving coating properties and reducing appearance defects in compositions.
Smart Images

Figure 0007577733000007 
Figure 0007577733000001 
Figure 0007577733000002
Abstract
Description
[Technical field]
[0001] The present invention relates to polymer particles and a thickener containing the same. [Background technology]
[0002] Compositions containing a dissolving medium (e.g., a solvent) have been used in cosmetics, medicines, adhesives, paints, and the like. In such compositions, a thickener is used to adjust the viscosity according to the application. As the thickener, an organic thickener is preferably used because it has a higher thickening effect than inorganic thickeners such as montmorillonite and silica.
[0003] As the organic thickener, polymer particles made of polymers such as carboxymethyl cellulose, polyvinyl alcohol, acrylic polymer, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl methyl ether, and carboxyvinyl polymer are used. For example, Patent Document 1 discloses that acrylic polymer particles having a particle size of 10 μm to 5 mm are used as the thickener. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-127504 A Summary of the Invention [Problem to be solved by the invention]
[0005] The polymer particles can exert a thickening effect by dissolving them in a dissolving medium. The polymer particles have a particle size distribution and contain a plurality of polymer particles with different particle sizes. Until now, it was thought that the molecular weight of the polymer particles would not change significantly even if the particle size of the polymer particles differed. However, according to the study by the present inventor, it was found that the molecular weight of the polymer particles varies depending on the particle size of the polymer particles, and the difference in the molecular weight of the polymer particles increases as the particle size deviates from the average particle size, and as a result, the solubility and thickening effect of each polymer particle also differ.
[0006] When such polymer particles are dissolved in a dissolution medium, low and high viscosity parts are generated in the composition, and the viscosity of the composition becomes non-uniform. In such a case, it becomes difficult to make the viscosity of the composition uniform even if the composition is stirred for a long time.
[0007] On the other hand, in order to make the solubility and thickening effect of the polymer particles uniform, it is possible to use polymer particles with a narrow particle size distribution. However, in such a case, since the dissolution behavior of each polymer particle is uniform, when the polymer particles are dissolved in the dissolution medium, the polymer particles start to dissolve all at once, which leads to a rapid increase in the viscosity of the composition, and it is easy to generate a gel-like mass called tangled powder before all the polymer particles are dissolved. Tangled powder occurs when the surface of the polymer particles partially dissolves in the dissolution medium and these polymer particles adhere to each other. Since the surface of the tangled powder is covered with a gel-like layer, the contact area between the polymer particles inside the tangled powder and the dissolution medium is extremely reduced. Therefore, even if the composition is stirred for a long time, it becomes difficult to dissolve the polymer particles contained in the tangled powder in the dissolution medium, and the tangled powder remains in the composition.
[0008] As described above, if splices occur in the composition or the viscosity of the composition becomes uneven, problems such as a decrease in the coatability of the composition, difficulty in forming a coating film with a uniform thickness, or the occurrence of whitened areas in the coating film, resulting in a poor appearance, may occur.
[0009] Therefore, the present invention provides polymer particles that can be dissolved in a dissolution medium without producing splices and that can uniformly increase the viscosity of a composition, as well as a thickener and composition that use the polymer particles. [Means for solving the problem]
[0010] [Polymer particles] The present inventors have conducted extensive research to solve the above-mentioned problems, and have found that by providing a predetermined difference in molecular weight in polymer particles having a predetermined particle size distribution, the polymer particles can be gradually dissolved in a dissolution medium at an appropriate speed while suppressing a sudden increase in viscosity of the composition. Such polymer particles can be dissolved uniformly in the dissolution medium without causing splices, and can increase the viscosity of the composition uniformly. Therefore, according to the present invention, it is possible to provide polymer particles that exhibit excellent thickening stability. Furthermore, according to the polymer particles of the present invention, after the viscosity of the composition is increased uniformly, the increased viscosity can be stably maintained in a uniform state.
[0011] That is, the polymer particles of the present invention have a number average particle diameter of 1 to 50 μm and a coefficient of variation in the number-based particle size distribution of 30% or more. The weight average molecular weight of the entire polymer particles is A, The weight average molecular weight of small particles, the cumulative percentage of which from the small diameter side in the number-based particle size distribution of the polymer particles is 5% or less, is defined as B, When the weight average molecular weight of the large particles having a particle diameter 5 times or more the number average particle diameter of the polymer particles is C, It is characterized in that the following formulas (1) and (2) are satisfied. 0.90≦(B / A)<1.0...Equation (1) (C / B)<1.25...Equation (2)
[0012] In the present invention, among the polymer particles, polymer particles having a cumulative percentage of 5% or less from the small diameter side in the particle size distribution based on the number of polymer particles are referred to as "small particles". Such small particles have a particle size of not more than a particle size (D5) at which a cumulative percentage of 5% from the small diameter side in the particle size distribution based on the number of polymer particles is obtained.
[0013] In the present invention, "polymer particles having a cumulative percentage of several hundred particles of X% from the small diameter side in the number-based particle size distribution of polymer particles" refers to polymer particles having a particle diameter at which the cumulative percentage of several hundred particles of X% in the above particle size distribution.
[0014] Furthermore, among the polymer particles, polymer particles having a particle diameter of 5 times or more the number average particle diameter of the polymer particles are referred to as "large particles".
[0015] The number average particle diameter of the polymer particles is 1 to 50 μm, preferably 2 to 30 μm, and more preferably 2 to 20 μm. When the number average particle diameter is 1 μm or more, the thickening effect of the polymer particles is improved. Also, when the number average particle diameter is 50 μm or less, the thickening effect of the polymer particles is improved.
[0016] When the polymer particles are used in a dental composition described later, the number average particle size of the polymer particles is 1 to 50 μm, preferably 10 to 50 μm, more preferably 15 to 48 μm, and more preferably 20 to 48 μm. When the number average particle size is 1 μm or more, the thickening effect of the polymer particles on the dental composition is improved. When the number average particle size is 50 μm or less, the thickening effect of the polymer particles on the dental composition is improved.
[0017] The coefficient of variation in the particle size distribution based on the number of polymer particles is 30% or more, preferably 35% or more, more preferably 40% or more. When the coefficient of variation is 30% or more, the polymer particles contain a wide range of polymer particles having different particle sizes, and it is possible to provide an appropriate difference in solubility for each particle size of the polymer particles. This allows the polymer particles to be gradually dissolved in the dissolution medium starting from the polymer particles with small particle sizes, making it possible to prevent all the polymer particles from dissolving at the same time. Therefore, the polymer particles can be dissolved in the dissolution medium without generating splices, and the polymer particles can uniformly increase the viscosity of the composition.
[0018] On the other hand, the coefficient of variation in the particle size distribution based on the number of polymer particles is preferably 80% or less, more preferably 75% or less. When the coefficient of variation is 80% or less, the difference in solubility between small particles and large particles can be kept within a suitable range. When the difference in solubility between small particles and large particles is too large, the small particles dissolve in the dissolution medium in a short time, while it takes time for the dispersion medium to penetrate into the inside of the large particles, and the large particles may not dissolve sufficiently.
[0019] In the polymer particles, the value (B / A) obtained by dividing the weight average molecular weight (B) of the small particles by the weight average molecular weight (A) of the entire polymer particles is set to satisfy 0.90≦(B / A)<1.0 [Formula (1)]. The value (B / A) preferably satisfies 0.901≦(B / A)≦0.999, and more preferably satisfies 0.93≦(B / A)≦0.99. When the value (B / A) is within the above range, a predetermined difference can be provided in the molecular weight of the polymer particles, and the polymer particles can be gradually dissolved in the dissolution medium starting from the polymer particles with small particle diameters, making it possible to suppress the simultaneous dissolution of all the polymer particles. Therefore, the polymer particles can be dissolved in the dissolution medium without generating splices, and the polymer particles can uniformly increase the viscosity of the composition.
[0020] In the polymer particles, the value (C / B) obtained by dividing the weight average molecular weight (C) of the large particles by the weight average molecular weight (B) of the small particles satisfies (C / B)<1.25 [formula (2)]. The value (C / B) preferably satisfies 1<(C / B)<1.25, more preferably satisfies 1.02≦(C / B)≦1.23, and more preferably satisfies 1.05≦(C / B)≦1.21. When the value (C / B) is within the above range, a predetermined difference can be provided in the molecular weight of the polymer particles, and the polymer particles can be gradually dissolved in the dissolution medium starting from the polymer particles with small particle diameters, making it possible to suppress all the polymer particles from dissolving at once. As a result, in the composition, the thickening by the polymer particles can be stably performed over time while suppressing a sudden thickening, and the viscosity of the composition can be made uniform.
[0021] In the polymer particles, it is preferable that the value (C / A) obtained by dividing the weight average molecular weight (C) of the large particles by the weight average molecular weight (A) of the entire polymer particles satisfies the following formula (3). 1.0<(C / A)≦1.10...Equation (3)
[0022] In this way, in the polymer particles, the above value (C / A) preferably satisfies 1.0<(C / A)≦1.10 [formula (3)], more preferably satisfies 1.01≦(C / A)≦1.10, more preferably satisfies 1.01≦(C / A)≦1.09, and more preferably satisfies 1.02≦(C / A)≦1.09. When the above value (C / A) is within the above range, a predetermined difference can be provided in the molecular weight of the polymer particles, and the dissolution of the large particles in the dissolution medium can be slower than that of polymer particles having a particle diameter smaller than that of the large particles, making it possible to suppress the simultaneous dissolution of all the polymer particles. Therefore, the polymer particles can be dissolved in the dissolution medium without generating splices, and the polymer particles can uniformly increase the viscosity of the composition.
[0023] The weight average molecular weight (A) of the entire polymer particles is 100×10 3 ~2,000×10 3is preferred, 200×10 3 ~1,500×10 3 It is more preferable that the weight average molecular weight (A) of the entire polymer particles is 100×10 3 When the weight average molecular weight (A) of the entire polymer particles is 2,000×10 or more, the thickening effect of the polymer particles can be improved. When the thickening effect of the polymer particles is low, the amount of the polymer particles to be added increases, which may cause splices to be generated when the polymer particles are added to a dissolution medium. 3 When the weight average molecular weight (A) of the entire polymer particles is 2,000×10 or less, the time required for dissolving the polymer particles in the dissolution medium can be appropriately shortened. 3 If the difference in solubility between the small particles and the large particles is too large, the small particles will dissolve in the dissolution medium in a short time, while the dispersion medium will take time to penetrate into the inside of the large particles, which may result in insufficient dissolution of the large particles or adhesion of the large particles to each other to cause splicing.
[0024] The weight average molecular weight (B) of the small particles contained in the polymer particles is 90×10 3 ~1,800×10 3 is preferred, 180×10 3 ~1,500×10 3 is more preferable, 180×10 3 ~1,430×10 3 is more preferable, 180×10 3 ~1,400×10 3 is particularly preferred. The weight average molecular weight (B) of the small particles is 90×10 3If the weight average molecular weight (B) of the small particles is 1,800×10 or more, the dissolution rate of the small particles can be prevented from becoming too high. If the dissolution rate of the small particles is too high, the small particles will dissolve in the dissolution medium faster than they can be uniformly dispersed in the dissolution medium, and high viscosity areas may occur locally in the composition. In such cases, polymer particles having a particle size larger than the small particles may be captured in the locally high viscosity area in the composition before completely dissolving, resulting in splicing. In addition, if the weight average molecular weight (B) of the small particles is 1,800×10 3 If the particle size is equal to or less than this, it becomes possible to dissolve the polymer particles in the dissolution medium gradually, starting from the polymer particles having a smaller particle size.
[0025] The weight average molecular weight (C) of the large particles contained in the polymer particles is 110 × 10 3 ~2,200×10 3 is preferred, 220×10 3 ~1,600×10 3 It is more preferable that the weight average molecular weight (C) of the large particles is 110×10 3 When the weight average molecular weight (C) of the large particles is 2,200×10 or more, the solubility can be differentiated for each particle size of the polymer particles, and this makes it possible to dissolve the polymer particles in the dissolution medium gradually, starting from the polymer particles with smaller particle sizes. 3 Below this, excellent solubility of the large particles in the dissolution medium can be ensured, and the difference in solubility between the small particles and the large particles can be within an appropriate range.
[0026] As described above, the polymer particles contain a plurality of polymer particles having different particle diameters. The polymer particles satisfy the relationship of the above formula (1) and formula (2) to provide a predetermined difference in the molecular weight of the polymer in the polymer particles, and it is preferable that in such particles, the molecular weight of the polymer contained in the polymer particles increases as the particle diameter of the polymer particles increases while satisfying the relationship of the above formula (1) and (2). In this way, the polymer particles in which the molecular weight of the polymer gradually increases as the particle diameter increases while providing a predetermined difference in the molecular weight of the polymer, when the polymer particles are dissolved in a dissolving medium to thicken the composition, can suppress a sudden increase in the viscosity of the composition obtained, and can increase the viscosity of the composition at an appropriate speed, thereby exhibiting better thickening stability.
[0027] When the weight average molecular weight of the first medium particles, which have a cumulative percentage of more than 20% and not more than 50% from the small diameter side in the number-based particle size distribution of the polymer particles, is D, it is preferable that the value (D / A) obtained by dividing the weight average molecular weight (D) of the first medium particles by the weight average molecular weight (A) of the entire polymer particles satisfies the following formula (4). 0.93<(D / A)<1.00...Equation (4)
[0028] In the polymer particles, the above value (D / A) preferably satisfies 0.93<(D / A)<1.00 [formula (4)], more preferably satisfies 0.96<(D / A)<1.00, more preferably satisfies 0.97≦(D / A)<1.00, and more preferably satisfies 0.97<(D / A)<1.00. When the above value (D / A) is within the above range, a predetermined difference can be provided in the molecular weight of the polymer particles, and the polymer particles can be gradually dissolved in the dissolution medium starting from the polymer particles with small particle diameters, making it possible to suppress the simultaneous dissolution of all the polymer particles. Therefore, the polymer particles can be dissolved in the dissolution medium without generating splices, and the polymer particles can uniformly increase the viscosity of the composition.
[0029] In the polymer particles, the weight average molecular weight (D) of the first medium particle is preferably larger than the weight average molecular weight (B) of the small particle. The value (D / B) obtained by dividing the weight average molecular weight (D) of the first medium particle by the weight average molecular weight (B) of the small particle preferably satisfies the following formula (5). 1.0<(D / B)<1.1...Equation (5)
[0030] In the polymer particles, the above value (D / B) preferably satisfies 1.0<(D / B)<1.1, and more preferably satisfies 1.001<(D / B)<1.081. When the above value (D / B) satisfies the above formula (5), the polymer particles can be dissolved in the dissolution medium gradually from the polymer particles having a small particle size, and it is possible to prevent all the polymer particles from dissolving at once.
[0031] When the weight average molecular weight of the second medium particles, which account for more than 50% and 80% or less of the cumulative number of particles from the small diameter side in the number-based particle size distribution of the polymer particles, is E, it is preferable that the value (E / A) obtained by dividing the weight average molecular weight (E) of the second medium particles by the weight average molecular weight (A) of the entire polymer particles satisfies the following formula (6). 1.00<(E / A)<1.08 Equation (6)
[0032] In the polymer particles, the above value (E / A) preferably satisfies 1.00<(E / A)<1.08 [formula (6)], more preferably satisfies 1.00<(E / A)≦1.07, and more preferably satisfies 1.01≦(E / A)≦1.06. When the above value (E / A) is within the above range, a predetermined difference can be set in the molecular weight of the polymer particles, and the polymer particles can be gradually dissolved in the dissolution medium starting from the polymer particles with small particle diameters, making it possible to prevent all the polymer particles from dissolving at the same time. Therefore, the polymer particles can be dissolved in the dissolution medium without generating splices, and the polymer particles can uniformly increase the viscosity of the composition.
[0033] In the polymer particles, the weight average molecular weight (E) of the second medium particles is preferably larger than the weight average molecular weight (D) of the first medium particles. The value (E / D) obtained by dividing the weight average molecular weight (E) of the second medium particles by the weight average molecular weight (D) of the first medium particles preferably satisfies the following formula (7). 1.0<(E / D)<1.2...Equation (7)
[0034] In the polymer particles, the value (E / D) preferably satisfies 1.0<(E / D)<1.2, more preferably satisfies 1.01≦(E / D)<1.15, and even more preferably satisfies 1.01≦(E / D)<1.10. When the value (E / D) satisfies the formula (7), the polymer particles can be dissolved in the dissolution medium gradually starting from the polymer particles having a small particle size, and it becomes possible to prevent all the polymer particles from dissolving at once.
[0035] In the polymer particles, the weight average molecular weight (C) of the large particles is preferably larger than the weight average molecular weight (E) of the second medium particles. The value (C / E) obtained by dividing the weight average molecular weight (C) of the large particles by the weight average molecular weight (E) of the second medium particles preferably satisfies the following formula (8). 1.0<(C / E)<1.1...Equation (8)
[0036] In the polymer particles, the value (C / E) preferably satisfies 1.0<(C / E)<1.1, and more preferably satisfies 1.00<(C / E)<1.06. When the value (C / E) satisfies the formula (8), the polymer particles can be dissolved in the dissolution medium gradually from the polymer particles having a small particle size, and it is possible to prevent all the polymer particles from dissolving at the same time.
[0037] In the present invention, when calculating the value (B / A) in the above formula (1), the value (C / B) in the above formula (2), the value (C / A) in the above formula (3), the value (D / A) in the above formula (4), the value (D / B) in the above formula (5), the value (E / A) in the above formula (6), the value (E / D) in the above formula (7), and the value (C / E) in the above formula (8), if the calculated value is divisible, the divisible value is used, and if the calculated value is not divisible, the non-divisible value is not rounded off to the nearest whole number, and the actually calculated value is used to determine whether or not each of the above formulas (1) to (8) is satisfied. In addition, in Tables 1 and 2 in the examples described later, for convenience, the values (B / A), (C / B), (C / A), (D / A), (D / B), (E / A), (E / D), and (C / E) are rounded to four decimal places.
[0038] In the present invention, among the polymer particles, those polymer particles whose cumulative percentage of the number of polymer particles from the small diameter side in the number-based particle size distribution is more than 20% and not more than 50% are referred to as "first medium particles." Also, those polymer particles whose cumulative percentage of the number of polymer particles from the small diameter side in the number-based particle size distribution are more than 50% and not more than 80% are referred to as "second medium particles."
[0039] The weight average molecular weight (D) of the first medium particle is 95×10 3 ~1,900×10 3 is preferred, 185×10 3 ~1,450×10 3 When the weight average molecular weight (D) of the first medium particle is within the above range, it is possible to provide a difference in solubility for each particle size of the polymer particles, and this makes it possible to dissolve the polymer particles in the dissolution medium gradually, starting from the polymer particles with the smallest particle size.
[0040] The weight average molecular weight (E) of the second medium particle is 115×10 3 ~2,100×10 3 is preferred, 210×10 3 ~1,550×10 3When the weight average molecular weight (E) of the second medium particles is within the above range, it is possible to provide a difference in solubility for each particle size of the polymer particles, and this makes it possible to dissolve the polymer particles in the dissolution medium gradually, starting from the polymer particles with smaller particle sizes.
[0041] The particle diameter (D5) of the polymer particles is preferably 1 to 10 μm, more preferably 1 to 7 μm, and more preferably 1 to 5 μm. When the particle diameter (D5) is 1 μm or more, the surface area per unit volume of the small particles becomes moderately large, increasing the degree of contact with the dissolution medium, and the polymer particles are easily dissolved in the dissolution medium without splicing. When the particle diameter (D5) is 10 μm or less, the dissolution medium easily penetrates into the inside of the small particles. The particle diameter (D5) of the polymer particles means a particle diameter corresponding to a cumulative percentage of 5% from the small diameter side in the particle size distribution based on the number of polymer particles.
[0042] The content of large particles in the polymer particles is preferably 0.1% or less, more preferably 0.08% or less, and more preferably 0.05% or less, based on the number of particles. By making the content of large particles 0.1% or less, it is possible to reduce the occurrence of high viscosity parts in the composition due to the large particles. This makes it possible to increase the viscosity of the composition more uniformly, and furthermore, to stably maintain the uniform state of the increased viscosity. The content of large particles is a percentage based on the number of particles, that is, a value expressed as a percentage of the number of large particles to the total number of polymer particles (100 x number of large particles / total number of polymer particles).
[0043] The content of large particles in the polymer particles is preferably 0.005% or more, more preferably 0.01% or more, based on the number of particles.By making the content of large particles 0.005% or more, the difference in solubility between small particles and large particles can be made within a suitable range.This allows the polymer particles to be dissolved in the dissolution medium gradually, starting from the polymer particles with small particle diameters, and makes it possible to prevent all polymer particles from dissolving at once.
[0044] The large particles are preferably contained within a range of 95% or more of a cumulative percentage of several hundred particles from the small diameter side in the particle size distribution based on the number of polymer particles.
[0045] The particle size distribution based on the number of polymer particles may be measured using a general-purpose measuring device. The particle size distribution based on the number of polymer particles is measured, for example, using a Coulter Multisizer (registered trademark) 3 (a measuring device manufactured by Beckman Coulter, Inc.). The measurement is performed using an aperture calibrated according to the Multisizer (registered trademark) 3 user's manual published by Beckman Coulter, Inc.
[0046] The aperture used in the measurement is appropriately selected depending on the size of the polymer particles to be measured. Current (aperture current) and Gain are appropriately set depending on the size of the selected aperture. For example, when an aperture having a size of 50 μm is selected, Current (aperture current) is set to −800 and Gain is set to 4.
[0047] The measurement sample is prepared by dispersing 0.1 g of polymer particles in 10 mL of 0.1% by mass aqueous solution of nonionic surfactant using a touch mixer (manufactured by Yamato Scientific Co., Ltd., "TOUCHMIXER MT-31") and an ultrasonic cleaner (manufactured by Vervoclear Co., Ltd., "ULTRASONIC CLEANER VS-150") to prepare a dispersion. During the measurement, the beaker is gently stirred to prevent air bubbles from being introduced, and the measurement is stopped when 100,000 polymer particles are measured, and a particle size distribution based on the number of particles is obtained.
[0048] Then, based on the obtained particle size distribution, the particle diameter (D5) corresponding to 5% of the cumulative number-based percentage of particles from the small diameter side is calculated.
[0049] Based on the obtained particle size distribution, the particle size corresponding to 50% of the cumulative number-based percentage from the small diameter side is calculated as the "number-average particle size of polymer particles." Based on the obtained particle size distribution, the coefficient of variation (CV) in the number-based particle size distribution of polymer particles is calculated according to the following formula. Coefficient of variation (%) = (Standard deviation of particle size distribution based on the number of polymer particles) ÷number average particle size of polymer particles) × 100
[0050] Based on the obtained particle size distribution, the content (%) of large particles having a particle diameter of 5 times or more the number average particle diameter is calculated.
[0051] The weight average molecular weight of the whole polymer particles is the weight average molecular weight of the polymer contained in the whole polymer particles, and can be measured using GPC (gel permeation chromatography). The weight average molecular weight here means the weight average molecular weight converted into polystyrene. Specifically, 0.003 g of polymer particles as a sample is dissolved in 10 mL of tetrahydrofuran (THF) at room temperature for 24 hours or more, and then filtered through a non-aqueous 0.45 μm chromatographic disk to obtain a measurement solution, and the weight average molecular weight of the whole polymer particles is obtained from a calibration curve of a standard polystyrene prepared in advance. Then, five measurement solutions are prepared according to the above procedure, and GPC measurement is performed for each measurement solution to measure the weight average molecular weight of the whole polymer particles contained in each measurement solution. The arithmetic mean value of the five measured values obtained in this way is obtained, and the arithmetic mean value is rounded off to the nearest hundredth to obtain the "weight average molecular weight (A) of the whole polymer particles". The measurement conditions of the chromatography are as follows. ·Equipment: High-speed GPC equipment Product name: Tosoh HLC-8320GPC EcoSEC-WorkStatio n (RI detector built-in) ·Analysis conditions Column: TSKgel SuperHZM-H x 2 (4.6mm I.D. x 15cm L x 2) Guard column: TSKguardcolumn SuperHZ-H x 1 (4.6mm ID x 2cm L) Flow rate: Sample side 0.175mL / min, Reference side 0.175mL / min Detector: Built-in RI detector Concentration: 0.3g / L Injection volume: 50μL Column temperature: 40℃ System temperature: 40℃ Eluent:THF
[0052] (Creating a calibration curve) The standard polystyrene samples used for the calibration curve are "TSK standard POLYSTYRENE" manufactured by Tosoh Corporation, having weight average molecular weights of 500, 2630, 9100, 37900, 102000, 355000, 3840000, and 5480000, and "Shodex STANDARD" manufactured by Showa Denko KK, having a weight average molecular weight of 1030000.
[0053] The method for creating the calibration curve is as follows. First, the standard polystyrene samples for the calibration curve are grouped into group A (those with a weight-average molecular weight of 1,030,000), group B (those with weight-average molecular weights of 500, 9,100, 102,000, and 3,480,000), and group C (those with weight-average molecular weights of 2,630, 37,900, 355,000, and 5,480,000). 5 mg of the standard polystyrene sample with a weight-average molecular weight of 1,030,000 belonging to group A is weighed out and then dissolved in 20 mL of THF, and 50 μL of the resulting solution is injected into the sample-side column. 10 mg, 5 mg, 5 mg, and 5 mg of the standard polystyrene samples with weight-average molecular weights of 500, 9,100, 102,000, and 3,480,000 belonging to group B are weighed out, respectively, and then dissolved in 50 mL of THF, and 50 μL of the resulting solution is injected into the sample-side column. Standard polystyrene samples belonging to group C with weight average molecular weights of 2630, 37900, 355000, and 5480000 were weighed out at 5 mg, 5 mg, 5 mg, and 1 mg, respectively, and dissolved in 40 mL of THF, and 50 μL of the resulting solution was injected into the sample column. A calibration curve (cubic equation) was created from the retention times of these standard polystyrene samples using the HLC-8320GPC dedicated data analysis program GPC Workstation (EcoSEC-WS), and this was used as the calibration curve for polystyrene-equivalent weight average molecular weight measurement.
[0054] The weight average molecular weight of the small particles is the weight average molecular weight of the polymer contained in the small particles. The weight average molecular weight of the large particles is the weight average molecular weight of the polymer contained in the large particles. The weight average molecular weights of the small particles and the large particles are values measured using GPC. After classifying the polymer particles in a general manner and collecting the small particles or the large particles contained in the polymer particles, the weight average molecular weight of the small particles or the weight average molecular weight of the large particles can be measured in the same manner as the above-mentioned method for measuring the weight average molecular weight of the entire polymer particles.
[0055] The weight average molecular weight of the first medium particle is the weight average molecular weight of the polymer contained in the first medium particle. The weight average molecular weight of the second medium particle is the weight average molecular weight of the polymer contained in the second medium particle. The weight average molecular weights of the first medium particle and the second medium particle are each a value measured using GPC. After classifying the polymer particles in a general manner and collecting the first medium particle or the second medium particle contained in the polymer particle, the weight average molecular weight of the first medium particle or the weight average molecular weight of the second medium particle can be measured in the same manner as the above-mentioned method for measuring the weight average molecular weight of the entire polymer particle.
[0056] The polymer particles of the present invention contain a polymer. Examples of the polymer include cellulose-based polymers such as carboxymethyl cellulose, methyl cellulose, and hydroxyethyl cellulose, polyvinyl-based polymers such as polyvinyl alcohol, polyvinyl pyrrolidone, and polyvinyl benzyl ether copolymers, acrylic polymers, and styrene-based polymers. Among them, acrylic polymers and styrene-based polymers are preferred, and acrylic polymers are more preferred, since polymer particles excellent in thickening effect, solvent resistance, water resistance, and / or chemical resistance can be obtained. The polymers may be used alone or in combination of two or more kinds.
[0057] The acrylic polymer is a polymer of raw material monomers containing preferably 50% by mass or more of an acrylic monomer. The acrylic monomer is not particularly limited, and examples thereof include acrylate, acrylic acid, methacrylate, and methacrylic acid. The acrylic monomer may be used alone or in combination of two or more kinds.
[0058] Examples of the acrylate include alkyl acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, and isobutyl acrylate. Examples of the methacrylate include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, and isobutyl methacrylate. Among these, methacrylates are preferred, alkyl methacrylates are more preferred, and methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, and isobutyl methacrylate are more preferred.
[0059] The content of the acrylic monomer component in the acrylic polymer is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more.
[0060] The acrylic polymer may also be a copolymer of the acrylic monomer and a vinyl monomer copolymerizable with the acrylic monomer. That is, the acrylic polymer may be a copolymer of raw material monomers including the acrylic monomer and a vinyl monomer copolymerizable with the acrylic monomer. Examples of such vinyl monomers include styrene monomers such as styrene, α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene, and monomers having a vinyl group such as vinyl acetate and acrylonitrile.
[0061] As the acrylic polymer, a polymer of an acrylic monomer and a copolymer of an acrylic monomer and a styrene monomer are preferred, and a polymer of an acrylic monomer is more preferred.
[0062] As the acrylic polymer, a polymer of alkyl methacrylate is preferable, and a polymer of methyl methacrylate, a polymer of ethyl methacrylate, and a copolymer of methyl methacrylate and ethyl methacrylate are preferable. By using polymer particles containing these acrylic polymers in a dental composition described later, the mechanical strength of the hardened product of the dental composition can be improved.
[0063] When the polymer particles contain an acrylic polymer, the content of the acrylic polymer in the polymer particles is preferably 70% by mass or more, more preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. By making the content of the acrylic polymer 70% by mass or more, polymer particles having excellent thickening effect, solvent resistance, water resistance, and / or chemical resistance can be obtained.
[0064] The styrene polymer is a polymer of raw material monomers containing preferably more than 50% by mass of a styrene monomer. The styrene monomer is not particularly limited, and examples thereof include styrene, α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene. Among them, styrene is preferable. The styrene monomer may be used alone or in combination of two or more kinds.
[0065] The styrene polymer may be a copolymer of the styrene monomer and a vinyl monomer copolymerizable with the styrene monomer. That is, the styrene polymer may be a copolymer of raw material monomers including the styrene monomer and a vinyl monomer copolymerizable with the styrene monomer. Examples of such vinyl monomers include bifunctional monomers such as acrylic monomers, (meth)acrylonitrile, dimethyl maleate, dimethyl fumarate, diethyl fumarate, ethyl fumarate, divinylbenzene, alkylene glycol dimethacrylate, and polyethylene glycol di(meth)acrylate. Note that (meth)acrylonitrile means acrylonitrile or methacrylonitrile.
[0066] The content of the styrene-based monomer component in the styrene-based polymer preferably exceeds 50% by mass, more preferably 80% by mass or more, and even more preferably 95% by mass or more.
[0067] When the polymer particles contain a styrene-based polymer, the content of the styrene-based polymer in the polymer particles is preferably 70% by mass or more, more preferably 85% by mass or more, more preferably 90% by mass or more, and more preferably 95% by mass or more. By making the content of the styrene-based polymer 70% by mass or more, polymer particles excellent in thickening effect, solvent resistance, water resistance, and / or chemical resistance can be obtained.
[0068] The polymer contained in the polymer particles may be crosslinked by a polyfunctional monomer. Therefore, raw material monomer may contain a polyfunctional monomer. However, since the solubility of the polymer particles in the dissolving medium is improved, it is preferable that the polymer contained in the polymer particles is slightly crosslinked by a polyfunctional monomer, and more preferable that the polymer is not crosslinked by a polyfunctional monomer.
[0069] The polyfunctional monomer is a monomer having a plurality of polymerizable functional groups (e.g., vinyl groups, epoxy groups, isocyanate groups, etc.). The polyfunctional monomer preferably has a plurality of vinyl groups as the functional group. Examples of the polyfunctional monomer include acrylic polyfunctional monomers such as 1,10-decanediol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, decaethylene glycol di(meth)acrylate, pentadecaethylene glycol di(meth)acrylate, pentacontahexaethylene glycol di(meth)acrylate, pentaerythritol tetra(meth)acrylate, 1,3-butylene di(meth)acrylate, and allyl(meth)acrylate, and aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, or derivatives thereof. In the present invention, the (meth)acrylate means an acrylate or a methacrylate. The polyfunctional monomers may be used alone or in combination of two or more kinds.
[0070] The content of the polyfunctional monomer in the raw material monomer is preferably 1.0 mass% or less, more preferably 0.6 mass% or less, and particularly preferably 0 mass% based on the total amount of the raw material monomer. When the content of the polyfunctional monomer is 1.0 mass% or less, the solubility of the polymer particles in the dissolution medium can be improved, and thus the polymer particles can be uniformly dissolved in the dissolution medium without generating splices.
[0071] [Method of producing polymer particles] The method for producing polymer particles of the present invention is not particularly limited as long as it can produce polymer particles that satisfy the number average particle size, the coefficient of variation in the particle size distribution based on the number, and the formulas (1) and (2), and can be produced by polymerizing raw material monomers in a general manner in the presence of a polymerization initiator as necessary. The polymerization method is not particularly limited, and general polymerization methods such as suspension polymerization, seed polymerization, bulk polymerization, and solution polymerization can be used. Among them, suspension polymerization is preferred because it is easy to set a predetermined difference in the molecular weight of the obtained polymer particles. Emulsion polymerization is a polymerization method in which raw material monomers are dispersed in an aqueous medium described later and polymerized in the presence of a polymerization initiator and an emulsifier, and is included in suspension polymerization.
[0072] The polymerization initiator is not particularly limited as long as it can initiate the polymerization of the raw material monomer. Examples of the polymerization initiator include organic peroxides such as benzoyl peroxide, lauroyl peroxide, and t-butylperoxy 2-ethylhexanoate, and azo-nitrile compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), and 2,2'-azobis(2,4-dimethylvaleronitrile). The 10-hour half-life temperature of the polymerization initiator is preferably 40 to 80°C. The polymerization initiator may be used alone or in combination of two or more kinds.
[0073] The amount of the polymerization initiator used is preferably 0.01 to 10 parts by mass, more preferably 0.01 to 7 parts by mass, and particularly preferably 0.01 to 5 parts by mass, per 100 parts by mass of the raw material monomer, since this allows the polymerization of the raw material monomer to be smoothly initiated.
[0074] The method for producing polymer particles of the present invention preferably includes a polymerization step of producing polymer particles by suspension polymerizing raw material monomers in an aqueous medium in the presence of a polymerization initiator. The suspension polymerization is preferably carried out by dispersing droplets of a raw material mixture (oil phase) containing raw material monomers and a polymerization initiator in an aqueous medium (aqueous phase) to obtain a dispersion, and polymerizing the raw material monomers in this dispersion. The raw material monomers preferably contain a monomer containing a vinyl group, more preferably contain an acrylic monomer and / or a styrene monomer, and more preferably contain an acrylic monomer. The raw material monomers may be used alone or in combination of two or more.
[0075] In order to adjust the weight-average molecular weight of the resulting polymer particles, the raw material mixture may contain a molecular weight regulator. Examples of the molecular weight regulator include mercaptans such as n-octyl mercaptan and tert-dodecyl mercaptan; α-methylstyrene and α-methylstyrene dimer; terpenes such as γ-terpinene and dipentene; and halogenated hydrocarbons such as chloroform and carbon tetrachloride. The weight-average molecular weight of the polymer particles can be adjusted by adjusting the content of the molecular weight regulator. The molecular weight regulator may be used alone or in combination of two or more kinds. The amount of the molecular weight regulator used is preferably 0.01 to 1 part by mass, more preferably 0.05 to 1 part by mass, based on 100 parts by mass of the raw material monomer.
[0076] The aqueous medium is not particularly limited, and examples thereof include water, a water-soluble organic medium (a lower alcohol (alcohol having 5 or less carbon atoms) such as methanol or ethanol), and a mixed medium of water and a water-soluble organic medium, and preferably contains water. The amount of the aqueous medium used is preferably 100 to 1000 parts by mass relative to 100 parts by mass of the raw material monomer in order to stabilize the polymerization.
[0077] A dispersion stabilizer may be contained in the aqueous medium. Examples of the dispersion stabilizer include phosphates such as calcium phosphate, magnesium phosphate, aluminum phosphate, and zinc phosphate; pyrophosphates such as calcium pyrophosphate, magnesium pyrophosphate, aluminum pyrophosphate, and zinc pyrophosphate; poorly water-soluble inorganic compounds such as calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, and colloidal silica; and water-soluble polymers such as polyvinylpyrrolidone and polyvinyl alcohol. Among these, it is preferable to use those that are decomposed by acid and dissolved in water (for example, calcium carbonate, tricalcium phosphate, magnesium hydroxide, magnesium pyrophosphate, and calcium pyrophosphate), since the dispersion stabilizer can be easily removed after the polymerization step. The dispersion stabilizers may be used alone or in combination of two or more.
[0078] The amount of the dispersion stabilizer used is preferably 0.1 to 20 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the raw material monomer, in order to ensure the fluidity of the suspension containing the polymer particles while providing excellent dispersibility of the polymer particles in the suspension.
[0079] Since the polymer particles obtained by suspension polymerization of droplets of a raw material mixture (oil phase) containing raw material monomers and a polymerization initiator are agglomerated, it is preferable to contain a water-soluble polymerization stabilizer in the aqueous medium. The polymerization stabilizer is not particularly limited, and examples thereof include nitrites such as sodium nitrite, sulfites, hydroquinones, ascorbic acids, water-soluble vitamin B, citric acid, polyphenols, etc., and nitrites are preferred, and sodium nitrite is more preferred. The polymerization stabilizer may be used alone or in combination of two or more kinds.
[0080] The amount of the polymerization stabilizer used is preferably 0.005 to 0.1 part by mass, and more preferably 0.005 to 0.05 part by mass, per 100 parts by mass of the aqueous medium, since the polymerization stabilizer can more effectively suppress the aggregation of the polymer particles.
[0081] In order to further stabilize the suspension (reaction liquid) during suspension polymerization, a surfactant may be contained in the aqueous medium. As the surfactant, any of anionic surfactants, cationic surfactants, nonionic surfactants and zwitterionic surfactants may be used. The surfactants may be used alone or in combination of two or more.
[0082] Examples of anionic surfactants include sodium oleate; fatty acid oils such as castor oil potassium; alkyl sulfate ester salts such as sodium lauryl sulfate and ammonium lauryl sulfate; alkyl benzene sulfonates such as sodium dodecyl benzene sulfonate; alkyl naphthalene sulfonates; alkanesulfonates; dialkyl sulfosuccinates such as sodium dioctyl sulfosuccinate; alkenyl succinates (dipotassium salts); alkyl phosphate ester salts; naphthalene sulfonate-formaldehyde condensates; polyoxyethylene alkyl ether sulfates such as polyoxyethylene alkyl phenyl ether sulfate salts and sodium polyoxyethylene lauryl ether sulfate; polyoxyethylene alkyl sulfate ester salts.
[0083] Examples of the cationic surfactant include alkylamine salts such as laurylamine acetate and stearylamine acetate; and quaternary ammonium salts such as lauryltrimethylammonium chloride.
[0084] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxysorbitan fatty acid esters, polyoxyethylene alkylamines, glycerin fatty acid esters, and oxyethylene-oxypropylene block polymers.
[0085] Examples of the zwitterionic surfactant include lauryl dimethylamine oxide, phosphate surfactants, and phosphite surfactants.
[0086] In the polymerization step, it is preferable to polymerize the raw material monomer in a dispersion in which droplets of a raw material mixture (oil phase) containing raw material monomers and a polymerization initiator are dispersed. In the polymerization step, the dispersion is heated using a general-purpose heating device, and the raw material monomer is polymerized while maintaining the dispersion at a preset polymerization reference temperature as much as possible. In the polymerization step, the temperature of the dispersion may have a temperature range, but it is preferable to keep it at a substantially constant temperature as much as possible.
[0087] In the polymerization step, the polymerization standard temperature of the dispersion is not particularly limited, but is preferably 50 to 110°C, more preferably 60 to 100°C. When the polymerization standard temperature of the dispersion is 50°C or higher, polymerization proceeds at a moderate speed, and polymer particles having a predetermined molecular weight can be obtained. When such polymer particles are dispersed in a dissolution medium to prepare a composition, the viscosity of the composition can be suppressed from increasing rapidly, and the viscosity of the composition can be prevented from becoming uneven, and the viscosity of the composition can be stably increased. When the polymerization standard temperature of the dispersion is 110°C or lower, the polymer of the raw material monomer can be suppressed from being decomposed by depolymerization, and polymer particles having a predetermined difference in molecular weight can be obtained. As a result, when the polymer particles are put into the dissolution medium, they can be dissolved without causing splices in the dissolution medium, and the viscosity of the composition can be increased uniformly.
[0088] In the polymerization process, in order to maintain the temperature of the dispersion at the polymerization reference temperature as much as possible, the heating of the dispersion by a heating device is repeatedly started and stopped. However, it is difficult to maintain the temperature of the dispersion at the polymerization reference temperature throughout the entire polymerization process, and the temperature of the dispersion repeatedly fluctuates above and below the polymerization reference temperature while tracing a waveform, for example, like a sine curve.
[0089] As described above, the temperature of the dispersion in the polymerization process (polymerization temperature) fluctuates above and below the polymerization reference temperature. The polymerization temperature is preferably controlled to (polymerization reference temperature-0.5°C) ≦ polymerization temperature < (polymerization reference temperature +0.5°C), and more preferably to (polymerization reference temperature-0.3°C) ≦ polymerization temperature ≦ (polymerization reference temperature +0.3°C), except for the heat generation process described below. In this way, by controlling the polymerization temperature, it is possible to stably proceed with the polymerization of the raw material monomers while preventing the difference in molecular weight of each polymer particle from becoming too large.
[0090] The reference polymerization temperature is a temperature at which the raw material monomer in the dispersion is polymerized, and is set in advance. However, as described above, the polymerization temperature usually fluctuates up and down with a similar fluctuation range, so that in a stable polymerization state where the polymerization conversion rate of the raw material monomer is 10% or more and less than 50%, the arithmetic mean value of the minimum and maximum temperatures of the dispersion can be regarded as the reference polymerization temperature.
[0091] On the other hand, in the latter half of the polymerization of the raw material monomer, i.e., when the polymerization conversion rate is 50% or more, internal heat generation occurs suddenly due to an increase in the polymerization rate of the raw material monomer and an increase in the viscosity of the dispersion (heat generation process). Note that, in the present invention, the polymerization conversion rate refers to a value calculated based on the following formula. Polymerization conversion rate (%) = 100 x amount of raw monomer consumed by polymerization / total amount of raw monomer
[0092] In the conventional temperature control, the same temperature control was performed in the heat generation step and before the heat generation step in the polymerization step, so that the heat generation in the heat generation step could not be sufficiently controlled, leading to a rapid temperature rise in the dispersion, and the unreacted raw material monomer reacts rapidly in a short time, causing a rapid increase in the viscosity of the dispersion. As a result, the heating of the dispersion by the heating device becomes uneven due to the increase in the viscosity of the dispersion, and the difference in molecular weight of each polymer particle becomes too large. As a result, there is a large difference in the solubility and thickening effect of each polymer particle, which results in problems such as splicing when the polymer particles are introduced into the dissolving medium and the viscosity of the composition thickened by the polymer particles becoming uneven overall.
[0093] Therefore, in the present invention, in the heat generation process occurring near the end point of polymerization of the raw material monomer, the polymerization temperature is controlled by cooling the dispersion so that it is preferably (polymerization reference temperature + 2.0 ° C) or less, more preferably (polymerization reference temperature + 1.5 ° C) or less, and more preferably (polymerization reference temperature + 1.0 ° C) or less. This cooling effect is greater for small particles than for large particles because the total surface area is greater. Therefore, the suppression effect of the polymerization reaction by the cooling is greater for small particles than for large particles, and the molecular weight of the polymer contained in the small particles is made smaller than the molecular weight of the polymer contained in the large particles, so that an appropriate difference in the molecular weight of the polymer can be formed. That is, by controlling the polymerization temperature to (polymerization reference temperature + 2.0 ° C) or less, it is possible to suppress the excessive difference in the cooling effect due to the difference in particle size, and to provide an appropriate difference in the molecular weight of each polymer particle.
[0094] In the heat generation step, it is preferable to control the cooling of the dispersion so that the polymerization temperature is equal to or higher than (reference polymerization temperature + 0.5° C.). By setting the polymerization temperature to equal to or higher than (reference polymerization temperature + 0.5° C.), it is possible to create an appropriate difference in the polymerization rate within the particles due to the difference in particle size, and to create an appropriate difference in the molecular weight of each polymer particle.
[0095] Since the heat generation process occurs in the latter half of the polymerization, it can be determined that the heat generation process has occurred when the temperature of the dispersion exceeds the maximum temperature within the range of the polymerization conversion rate in which the polymerization reaction is stably proceeding and is not less than 10% and less than 50%, and temperature control in the heat generation process can be started.
[0096] After the heat generation in the heat generation step has ended, it is preferable to carry out temperature control similar to that before the heat generation step and to carry out the polymerization reaction of the raw material monomers sufficiently, thereby obtaining polymer particles having a predetermined difference in molecular weight.
[0097] The end of the heat generation in the heat generation step can be determined in the same manner as the start of the heat generation step, as described above. Specifically, the end of the heat generation step can be determined when the temperature of the dispersion falls below the maximum temperature in the range of the polymerization conversion rate at which the polymerization reaction is stably performed, which is 10% or more and less than 50%.
[0098] The duration of the polymerization step after the start of the heat generation step is preferably 60 minutes or more, more preferably 120 minutes or more, and more preferably 180 minutes or more. The duration of the polymerization step after the heat generation step is preferably 360 minutes or less, more preferably 300 minutes or less, and more preferably 240 minutes or less. When the duration of the polymerization step after the heat generation step is 60 minutes or more, the polymerization reaction of the raw material monomers is almost completed, thereby removing the heat of polymerization, and polymer particles having a predetermined difference in molecular weight can be obtained.
[0099] The method for producing polymer particles of the present invention preferably includes a step of classifying the polymer particles obtained after the polymerization step. In this classification step, fine particles having a small particle size and coarse particles having a large particle size are removed from the polymer particles after the polymerization step, and the number average particle size and coefficient of variation of the polymer particles can be adjusted to be within a predetermined range.
[0100] The extent to which coarse particles are removed by classification is not particularly limited, but it is preferable to remove at least a portion of the coarse particles from the polymer particles before classification by classification until the content of large particles having a particle diameter 5 times or more the number average particle diameter in the polymer particles after classification becomes 0.1% or less, preferably 0.08% or less, and more preferably 0.05% or less, on a number basis.
[0101] The extent to which fine particles are removed by classification is not particularly limited, but it is preferable to remove at least a portion of the fine particles from the polymer particles before classification by classification until the particle diameter (D5) at which the cumulative percentage of the fine particles from the small diameter side in the number-based particle size distribution of the polymer particles after classification corresponds to 5% becomes 1.03 times or more, preferably 1.03 to 1.5 times, and more preferably 1.05 to 1.5 times the particle diameter (D5') at which the cumulative percentage of the fine particles from the small diameter side in the number-based particle size distribution of the polymer particles before classification corresponds to 5%.
[0102] The method of classifying polymer particles is not particularly limited as long as fine particles and coarse particles can be removed by classification, and examples thereof include air classification (wind classification) and screen classification (sieve classification). Among them, air classification is preferred because it can perform classification with high accuracy without causing clogging due to fine particles and coarse particles. Air classification refers to a method of classifying particles by utilizing air flow. Screen classification refers to a method of supplying particles onto a screen and vibrating the screen to classify the particles on the screen into particles that pass through the meshes of the screen and particles that do not pass through.
[0103] Examples of the air flow classification include: (1) a method in which polymer particles are placed in an air flow, the polymer particles are collided with a screen, and the polymer particles are classified into those that pass through the meshes of the screen and those that do not; (2) a method in which polymer particles are placed in a swirling air flow, and the polymer particles are classified into two particle size groups, large and small, by the interaction between the centrifugal force imparted to the polymer particles by the swirling air flow and the air flow toward the center of the swirling air flow; and (3) a classification method utilizing the Coanda effect.
[0104] Examples of the air classifier that performs the above-mentioned (1) air classifier include those commercially available under the trade name "Blower Sifter" from Euglop Co., Ltd., the trade name "Hibolter" from Toyo Hightec Co., Ltd., and the trade name "Microsifter" from Makino Sangyo Co., Ltd. Examples of the air classifier that performs the above-mentioned (2) air classifier include those commercially available under the trade name "Turbo Classifier (registered trademark)" from Nisshin Engineering Co., Ltd. and the trade name "Spedic Classifier" from Seishin Enterprise Co., Ltd. Examples of the air classifier that performs the above-mentioned (3) air classifier include a Coanda type air classifier (elbow jet classifier) commercially available from Matsubo Co., Ltd. The above-mentioned three classification methods can be used depending on the properties of the polymer particles to be classified and the degree to which coarse particles and fine particles are to be removed. In order to accurately remove coarse particles, it is preferable to use the air classifier of (1). In addition, in order to accurately remove fine particles, it is preferable to use the air classifier of (2).
[0105] The polymer particles of the present invention not only have an excellent thickening effect, but also can be dissolved uniformly in a dissolution medium without forming splices, and can increase the viscosity of a composition uniformly. Furthermore, the polymer particles of the present invention can stably maintain the uniform state of the increased viscosity after the viscosity of the composition is increased uniformly. Therefore, since the polymer particles of the present invention have an excellent thickening effect, they are suitable for use as a thickener for cosmetics, pharmaceuticals, adhesives, paints, etc.
[0106] [Composition] The composition of the present invention is obtained by dissolving the above-mentioned polymer particles in a dissolution medium. By dissolving the polymer particles in a dissolution medium, the viscosity of the obtained composition can be increased. The composition contains a polymer in which the polymer particles are dissolved in a dissolution medium. That is, the composition contains a dissolution medium and a solution of the polymer particles.
[0107] The dissolution medium is not particularly limited as long as it can dissolve at least the polymer particles among the components contained in the composition. Examples of the dissolution medium include a solvent and a monomer that is polymerized by irradiation with ionizing radiation. The dissolution medium may be used alone or in combination of two or more kinds.
[0108] The solvent is not particularly limited, and examples thereof include water and organic solvents. The organic solvent is not particularly limited, and examples thereof include monohydric alcohols such as methanol, ethanol, propanol, isopropanol, n-butanol, tert-butanol, and 2-ethylhexyl alcohol, polyhydric alcohols such as ethylene glycol, propylene glycol, and butylene glycol, monoethers of polyhydric alcohols such as ethylene glycol monoethyl ether and ethylene glycol monobutyl ether, cyclic ethers such as tetrahydrofuran, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone, benzene, toluene, xylene, ethyl ether ... Examples of the solvent include aliphatic or aromatic hydrocarbons such as dibenzene, hexane, heptane, octane, isododecane, cyclopentane, cyclohexane, and liquid paraffin, halogenated hydrocarbons such as carbon tetrachloride and chlorobenzene, animal and vegetable oils such as sunflower oil, olive oil, soybean oil, corn oil, castor oil, beef tallow, jojoba oil, and squalane, silicones such as dimethylpolysiloxane and methylphenylpolysiloxane, esters such as butyl acetate, octyldodecyl oleate, cetyl octanoate, cetyl ethylhexanoate, glyceryl triisooctanate, neopentyl glycol diisooctanate, and tricaprylin. The solvents may be used alone or in combination of two or more.
[0109] In the monomer that is polymerized by irradiation with ionizing radiation, examples of the ionizing radiation include X-rays, gamma rays, ultraviolet rays, visible light, and electron beams. Examples of the monomer that is polymerized by irradiation with ionizing radiation include acrylic monofunctional monomers, acrylic polyfunctional monomers, and styrene monofunctional monomers. Among them, acrylic monofunctional monomers and acrylic polyfunctional monomers are preferred, and acrylic monofunctional monomers are more preferred. Examples of the acrylic monofunctional monomers are not particularly limited, and examples include acrylic acid, methacrylic acid, and (meth)acrylate. The monomer that is polymerized by irradiation with ionizing radiation may be used alone or in combination of two or more.
[0110] Examples of the (meth)acrylate in the monomer that polymerizes upon irradiation with ionizing radiation include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and lauryl (meth)acrylate, benzyl (meth)acrylate, 2-(N,N-dimethylamino)ethyl (meth)acrylate, 2,3-dibromopropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 10-hydroxypropyl (meth)acrylate. Decyl (meth)acrylate, propylene glycol mono(meth)acrylate, glycerin mono(meth)acrylate, erythritol mono(meth)acrylate, N-methylol (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, N-(dihydroxyethyl) (meth)acrylamide, (meth)acryloyloxydodecylpyridinium bromide, (meth)acryloyloxydodecylpyridinium chloride, (meth)acryloyloxyhexadecylpyridinium chloride, and (meth)acryloyloxydecylammonium chloride. Among them, alkyl (meth)acrylate is preferred, alkyl methacrylate is more preferred, and methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, and isobutyl methacrylate are more preferred. Note that (meth)acrylamide means acrylamide or methacrylamide.
[0111] Examples of the acrylic polyfunctional monomer that can be polymerized by irradiation with ionizing radiation include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, nonaethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1 aliphatic acrylic polyfunctional compounds such as 3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolmethane tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; Monomers; aromatic acrylic polyfunctional monomers such as 2,2-bis((meth)acryloyloxyphenyl)propane, 2,2-bis[4-(2-hydroxy-3-(meth)acryloyloxyphenyl)]propane, 2,2-bis(4-(meth)acryloyloxyethoxyphenyl)propane, 2,2-bis(4-(meth)acryloyloxydiethoxyphenyl)propane, and 2,2-bis(4-(meth)acryloyloxypropoxyphenyl)propane; 11-(meth)acryloyloxyphenyl Examples of the acrylic polyfunctional monomers include acrylic polyfunctional monomers containing an acidic group such as 1,1-undecanedicarboxylic acid, 4-(meth)acryloyloxyethyl trimellitic acid and its anhydride, 2-methacryloyloxyethyl dihydrogen phosphate, bis(2-methacryloyloxyethyl)hydrogen phosphate, and 10-methacryloyloxydecyl dihydrogen phosphate; and acrylic polyfunctional monomers containing a basic group such as N,N-dimethylaminoethyl methacrylate. Note that (meth)acryloyloxy means acryloyloxy or methacryloyloxy.
[0112] The composition of the present invention is obtained by dissolving polymer particles in a dissolution medium. It is preferable that the difference between the solubility parameter of the dissolution medium and the solubility parameter of the polymer contained in the polymer particles is small. This makes it easier for the polymer particles to become compatible with the dissolution medium, and makes it easier to dissolve the polymer particles uniformly in the dissolution medium without generating splices. Furthermore, after the viscosity of the composition is uniformly increased by the polymer particles, it is also possible to more stably maintain the uniform state of this increased viscosity.
[0113] When the polymer particles contain an acrylic polymer and / or a styrene polymer, the dissolution medium contained in the composition is preferably toluene, n-heptane, methyl methacrylate, butyl acetate, ethyl acetate, methyl ethyl ketone, acetone, or cyclohexane, and more preferably toluene, cyclohexane, or methyl methacrylate. The difference between the solubility parameters of these dissolution media and the solubility parameters of the acrylic polymer and / or the styrene polymer is small.
[0114] The blending amount of the polymer particles in the composition is preferably 0.1 to 100 parts by mass, more preferably 1 to 50 parts by mass, relative to 100 parts by mass of the dissolution medium. The content of the dissolved polymer particles in the composition is preferably 0.1 to 100 parts by mass, more preferably 1 to 50 parts by mass, relative to 100 parts by mass of the dissolution medium.
[0115] The composition preferably contains a synthetic resin or an oligomer that polymerizes by irradiation with ionizing radiation. By containing a synthetic resin in the composition, the composition can be formed into a desired shape such as a coating film. The synthetic resin may be any of an ionizing radiation curable resin, a thermoplastic resin, or a thermosetting resin. The synthetic resin may be used alone or in combination of two or more kinds. Examples of the thermoplastic resin include polyolefin resins such as acrylic resins, polycarbonates, polyester resins, polyethylene resins, and polypropylene resins, and polystyrene resins. Among them, acrylic resins, polycarbonates, polyester resins, and polystyrene resins are preferred because of their excellent transparency. The thermoplastic resins may be used alone or in combination of two or more kinds.
[0116] Examples of the thermosetting resin include a thermosetting urethane resin made of an acrylic polyol and an isocyanate prepolymer, a phenol resin, a urea melamine resin, an epoxy resin, an unsaturated polyester resin, and a silicone resin.
[0117] The ionizing radiation curable resin means a resin that is cured by irradiation with ionizing radiation. Examples of ionizing radiation include X-rays, γ-rays, ultraviolet rays, visible light, and electron beams. Examples of the ionizing radiation curable resin include polyfunctional (meth)acrylate resins; polyfunctional urethane acrylate resins synthesized from diisocyanates, polyhydric alcohols, and (meth)acrylic acid esters having hydroxyl groups, and the like. The ionizing radiation curable resin is preferably a polyfunctional (meth)acrylate resin, and more preferably a polyfunctional (meth)acrylate resin synthesized from a polyhydric alcohol polyfunctional (meth)acrylate having three or more (meth)acryloyl groups in one molecule. Specific examples of polyhydric alcohol polyfunctional (meth)acrylates having three or more (meth)acryloyl groups in one molecule include trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, 1,2,4-cyclohexane tetra(meth)acrylate, pentaglycerol triacrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol triacrylate, and tripentaerythritol hexaacrylate. The ionizing radiation curable resins may be used alone or in combination of two or more. (Meth)acrylic acid means acrylic acid or methacrylic acid. (Meth)acryloyl means acryloyl or methacryloyl.
[0118] In addition to the above, examples of the ionizing radiation curable resin include polyether resins having an acrylate functional group, polyester resins having an acrylate functional group, epoxy resins having an acrylate functional group, alkyd resins having an acrylate functional group, spiroacetal resins having an acrylate functional group, polybutadiene resins having an acrylate functional group, and polythiolpolyene resins having an acrylate functional group.
[0119] When the ionizing radiation curable resin is cured by irradiation with ultraviolet light, the composition preferably contains a photopolymerization initiator. By using the photopolymerization initiator, the ionizing radiation curable resin can be cured by ultraviolet light irradiation. Furthermore, when the composition contains a monomer that polymerizes by irradiation with ionizing radiation or an oligomer that polymerizes by irradiation with ionizing radiation, the composition preferably contains a photopolymerization initiator. By using the photopolymerization initiator, the monomer that polymerizes by irradiation with ionizing radiation or the oligomer that polymerizes by irradiation with ionizing radiation can be polymerized by ultraviolet light irradiation to cure the composition.
[0120] The photopolymerization initiator is not particularly limited. Examples of the photopolymerization initiator include acetophenones, benzoins, benzophenones, phosphine oxides, ketals, α-hydroxyalkylphenones, α-aminoalkylphenones, anthraquinones, thioxanthones, azo compounds, peroxides (described in JP-A No. 2001-139663, etc.), 2,3-dialkyldione compounds, disulfide compounds, fluoroamine compounds, aromatic sulfonium compounds, onium salts, borate salts, active halogen compounds, and α-acyloxime esters.
[0121] Examples of the acetophenones include acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, 1-hydroxydimethylphenyl ketone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-4-methylthio-2-morpholinopropiophenone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone. Examples of the benzoins include benzoin, benzoin benzoate, benzoin benzenesulfonic acid ester, benzoin toluenesulfonic acid ester, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether. Examples of the benzophenones include benzophenone, 2,4-dichlorobenzophenone, 4,4-dichlorobenzophenone, and p-chlorobenzophenone. Examples of the phosphine oxides include 2,4,6-trimethylbenzoyldiphenylphosphine oxide. Examples of ketals include benzyl methyl ketals such as 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of α-hydroxyalkylphenones include 1-hydroxycyclohexyl phenyl ketone. Examples of α-aminoalkylphenones include 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone.
[0122] Preferred examples of commercially available photopolymerization initiators include those available from BASF Japan Ltd. under the trade name "Irgacure (registered trademark) 651" (2,2-dimethoxy-1,2-diphenylethan-1-one), BASF Japan Ltd. under the trade name "Irgacure (registered trademark) 184", and BASF Japan Ltd. under the trade name "Irgacure (registered trademark) 907" (2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one).
[0123] The amount of the photopolymerization initiator used is preferably 0.5 to 20 parts by mass, more preferably 1 to 10 parts by mass, and particularly preferably 1 to 8 parts by mass, per 100 parts by mass of the total amount of the monomer and oligomer of the ionizing radiation curable resin.
[0124] The composition of the present invention may contain a pigment. Examples of the pigment include inorganic pigments such as titanium oxide, calcium carbonate, aluminum, copper, mica, iron oxide, and carbon black, and organic pigments such as phthalocyanine blue, phthalocyanine green, dioxazine violet, toluidine red, perylene, quinacridone, and benzidine yellow. The pigment may be used alone or in combination of two or more kinds.
[0125] The composition of the present invention may contain a filler. Examples of the filler include inorganic fillers. Examples of the inorganic fillers include metal oxides such as amorphous silica, quartz, alumina, titania, zirconia, barium oxide, yttrium oxide, lanthanum oxide, and ytterbium oxide; silica-based composite oxides such as silica-zirconia, silica-titania, silica-titania-barium oxide, and silica-titania-zirconia; glasses such as borosilicate glass, aluminosilicate glass, and fluoroaluminosilicate glass; metal fluorides such as barium fluoride, strontium fluoride, yttrium fluoride, lanthanum fluoride, and ytterbium fluoride; inorganic carbonates such as calcium carbonate, magnesium carbonate, strontium carbonate, and barium carbonate; and metal sulfates such as magnesium sulfate and barium sulfate. The fillers may be used alone or in combination of two or more.
[0126] The inorganic filler may be surface-treated with a silane coupling agent, such as γ-methacryloxypropyltrimethoxysilane or vinyltrimethoxysilane.
[0127] The composition of the present invention may contain other additives such as a viscosity modifier, an antifoaming agent, a light stabilizer, a weathering stabilizer, a heat stabilizer, an ultraviolet absorber, an antioxidant, a leveling agent, a pigment dispersant, a pH adjuster, a polymerization inhibitor, an antibacterial agent, an X-ray contrast agent, a fluorescent agent, etc. These other additives may be used alone or in combination of two or more.
[0128] The composition of the present invention is preferably used as a coating composition. In the present invention, the viscosity of the composition can be easily adjusted to a desired range by using the above-mentioned polymer particles as a thickener, and a composition with uniform composition and viscosity can be obtained. Therefore, the composition of the present invention has excellent coatability and can form a coating film with a uniform thickness.
[0129] Furthermore, the polymer particles of the present invention can be dissolved uniformly in a dissolution medium without forming splinters, and can increase the viscosity of the composition uniformly. If the viscosity of the composition is not uniform, when the composition is applied, whitened areas are formed in the resulting coating film, which leads to poor appearance. However, the polymer particles of the present invention can reduce the occurrence of such poor appearance.
[0130] Therefore, the composition of the present invention can form a coating film that is uniform in thickness and composition and reduces the occurrence of defective appearance.
[0131] The coated body of the present invention has a substrate and a coating film laminated and integrated on one surface of the substrate. The coating film can be made of the above-mentioned composition. Examples of the substrate material include cement, tile, metal, synthetic resin, and glass. Examples of the synthetic resin used for the substrate include, but are not limited to, polyester resins such as polyethylene terephthalate, triacetyl cellulose resins, polystyrene resins, acrylic resins, polycarbonate resins, and cycloolefin resins.
[0132] The coating film can be formed by applying the composition to any coating surface such as a substrate to prepare a coating film, drying the coating film, and then curing the coating film as necessary. As a method for applying the composition to the coating surface, known methods such as reverse roll coating, gravure coating, die coating, comma coating, and spray coating can be used.
[0133] The composition of the present invention is preferably used as a dental composition. When the composition of the present invention is used as a dental composition, the dental composition preferably contains a dissolution medium containing a monomer that is polymerized by irradiation with ionizing radiation, and a solution of polymer particles. The dental composition preferably further contains a photopolymerization initiator.
[0134] In addition, the dental composition is a preferred embodiment of the composition of the present invention limited to dental use. Therefore, the components (dissolving medium, dissolved polymer particles, photopolymerization initiator, etc.) contained in the dental composition are the same as those described above in the composition of the present invention, so detailed description is omitted.
[0135] The dental composition is suitably used as a composite resin for treating a missing tooth or a cavity. When treating a missing tooth or a cavity in dental treatment, a cavity is formed in the tooth by grinding a part of the tooth. By filling the cavity with the dental composition and then hardening it, the tooth can be restored to its original shape before the dental treatment.
[0136] In the present invention, the viscosity of the dental composition can be adjusted to a desired range by using the above-mentioned polymer particles as a thickener, and thus a dental composition in a paste form can be preferably obtained. As described above, the polymer particles can be dissolved uniformly in the dissolution medium without causing splices, and can increase the viscosity of the dental composition uniformly. Furthermore, the polymer particles can stably maintain the uniform state of the increased viscosity after the viscosity of the dental composition is increased uniformly. Such a dental composition has excellent filling properties and elongation fluidity, and also has reduced stickiness and stringiness.
[0137] The dental composition of the present invention has excellent filling properties, which allows the dental composition to be filled into the cavity formed in the tooth while reducing the formation of bubbles. The inner surface of the cavity generally has fine irregularities, and when filling the dental composition into the cavity of the tooth, the dental composition must flow sufficiently into the concaves of the fine irregularities of the inner surface of the cavity. However, if the dental composition contains splinters or has an uneven viscosity, the dental composition cannot flow sufficiently into the concaves of the fine irregularities of the inner surface of the cavity, and bubbles may form between the inner surface of the tooth cavity and the filled dental composition. Such bubbles may reduce the adhesive strength between the inner surface of the tooth cavity and the filled dental composition, which may cause the dental composition to fall off from the tooth after hardening. However, the dental composition of the present invention has excellent filling properties, and when filling the cavity of the tooth, the dental composition can flow sufficiently into the concaves of the inner surface of the tooth cavity to reduce the formation of bubbles.
[0138] In addition, the dental composition has excellent extension fluidity and can be uniformly extended and flowed. When the dental composition contains splints, the splints partially inhibit the flow of the dental composition, so that the extension fluidity of the dental composition becomes non-uniform, and it may be difficult to uniformly fill the dental composition in the tooth cavity with the dental composition. In addition, when the viscosity of the dental composition is non-uniform, the extension fluidity of the dental composition also becomes non-uniform, and it may be difficult to uniformly fill the dental composition in the tooth cavity with the dental composition. However, the dental composition of the present invention has excellent extension fluidity and can be uniformly extended and flowed, so that such a dental composition can be easily and uniformly filled in the tooth cavity.
[0139] Furthermore, the dental composition is excellent in operability because the occurrence of stickiness and stringiness is reduced. When the dental composition contains splints, the dental composition may become sticky. Furthermore, when the viscosity of the dental composition is not uniform, the dental composition may cause a phenomenon called stringiness. In dental treatment, operations such as scooping the dental composition with a dental tool such as a spatula or probe before filling the dental composition, or removing the dental composition filled in excess with a dental tool after filling the dental composition are performed. When the dental composition becomes sticky or stringy, it becomes difficult to perform the above operations in dental treatment. However, the dental composition of the present invention is also reduced in the occurrence of stickiness and stringiness, and the above operations in dental treatment can be easily performed.
[0140] Furthermore, the dental composition of the present invention has reduced splice formation and a uniformly increased viscosity. Therefore, such a dental composition can form a hardened product that is uniform and has high mechanical strength after hardening. This reduces the occurrence of damage such as chipping and cracking in the hardened product even when stress is applied to the hardened product of the dental composition.
[0141] The dental composition contains a dissolution medium. The dissolution medium preferably contains a monomer that polymerizes when irradiated with ionizing radiation. Since the dissolution medium contains a monomer that polymerizes when irradiated with ionizing radiation, the dental composition can be hardened by irradiating the dental composition with ionizing radiation to polymerize the monomer that polymerizes when irradiated with ionizing radiation. The dissolution medium may also contain a solvent. The monomer that polymerizes when irradiated with ionizing radiation and the solvent contained in the dental composition are as described above in the composition of the present invention, and therefore detailed description thereof will be omitted.
[0142] The content of the dissolved polymer particles in the dental composition is preferably 10 to 100 parts by mass, more preferably 30 to 100 parts by mass, relative to 100 parts by mass of the dissolution medium. That is, the dental composition preferably contains a dissolved polymer particle in 100 parts by mass of the dissolution medium, preferably 10 to 100 parts by mass, more preferably 30 to 100 parts by mass. By setting the content of the dissolved polymer particles within the above range, a dental composition in a preferably paste form is obtained. This allows the dental composition to have excellent filling properties, spreadability, and operability.
[0143] The dental composition preferably contains a photopolymerization initiator. The content of the photopolymerization initiator in the dental composition is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and particularly preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the monomer that is polymerized by irradiation with ionizing radiation. The photopolymerization initiator contained in the dental composition is as described above in the composition of the present invention, and therefore a detailed description thereof will be omitted.
[0144] The dental composition may further contain a synthetic resin, an oligomer that polymerizes upon irradiation with ionizing radiation, a pigment, a filler, a viscosity modifier, an antifoaming agent, a light stabilizer, a weathering stabilizer, a heat stabilizer, an ultraviolet absorber, an antioxidant, a leveling agent, a pigment dispersant, a pH adjuster, a polymerization inhibitor, an antibacterial agent, an X-ray contrast agent, or a fluorescent agent, etc. These are as described above in relation to the composition of the present invention, and therefore detailed description thereof will be omitted.
[0145] The method for producing the dental composition is not particularly limited, but examples thereof include a method in which a dissolution medium containing a monomer that polymerizes when irradiated with ionizing radiation, polymer particles, and, if necessary, a photopolymerization initiator are mixed, and the polymer particles are dissolved in the dissolution medium to obtain the dental composition.
[0146] As described above, the dental composition can form a cured product that is uniform and has high mechanical strength. The method for forming the cured product of the dental composition is not particularly limited, but may be, for example, a method in which the dental composition is irradiated with ionizing radiation to obtain the cured product of the dental composition.
[0147] Furthermore, when the dental composition is used as a composite resin, the method for forming a hardened product of the dental composition is not particularly limited, but examples thereof include a method in which the dental composition is filled into a tooth cavity and then the dental composition is irradiated with ionizing radiation to obtain a hardened product of the dental composition.
[0148] Examples of the ionizing radiation to be irradiated to the dental composition include X-rays, γ-rays, ultraviolet rays, visible light, and electron beams, with ultraviolet rays and visible light being preferred, and ultraviolet rays being more preferred. The ionizing radiation may be used alone or in combination of two or more kinds.
[0149] The dental composition of the present invention is preferably used for the composite resin described above. However, the dental composition of the present invention can also be used for other purposes. Other uses include dental adhesives such as orthodontic adhesives, cavity application adhesives and fissure sealants, denture base materials, denture base mucosa conditioners, fissure sealants, coating materials for tooth surfaces and dental prostheses, dental materials such as dental nail polish, etc. In addition, the hardened product of the dental composition of the present invention can be molded and used as artificial teeth, dentures, CAD / CAM resin blocks, etc. Effect of the Invention
[0150] The polymer particles of the present invention can be dissolved in a dissolution medium without forming splices, and can uniformly increase the viscosity of the composition. [Brief description of the drawings]
[0151] [Figure 1] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0152] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples. EXAMPLES
[0153] Example 1 A raw material mixture containing 100 parts by mass of methyl methacrylate (MMA) as a raw material monomer and 0.4 parts by mass of benzoyl peroxide as a polymerization initiator was prepared. Meanwhile, an aqueous medium mixture was prepared by adding and mixing 5 parts by mass of metathetic magnesium pyrophosphate (magnesium pyrophosphate obtained by metathetic generation method) as a dispersion stabilizer consisting of an acid-soluble poorly water-soluble inorganic compound to 200 parts by mass of deionized water as an aqueous medium, 0.02 parts by mass of sodium nitrite as an aqueous polymerization stabilizer, and 0.10 parts by mass of sodium lauryl sulfate as a surfactant.
[0154] The raw material mixture and the aqueous medium mixture were supplied to a high-speed emulsifying and dispersing homomixer (manufactured by Primix Corporation, product name "MARKII2.5 type"), and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to 3 to 5 μm, to obtain a dispersion in which the raw material mixture was dispersed in the form of droplets in the aqueous medium.
[0155] The dispersion was supplied to a polymerization reactor (autoclave) equipped with a stirrer and a temperature control device including a heating device, and the dispersion was heated to the polymerization reference temperature of 70°C using the heating device while being stirred with the stirrer, to suspension polymerize the raw material monomers (polymerization process). In the polymerization process, the temperature of the dispersion periodically fluctuated up and down around 70°C by temperature control using the temperature control device. In the polymerization process, the minimum temperature of the dispersion when the polymerization conversion rate of the raw material monomer was 10% or more and less than 50% was 69.7°C and the maximum temperature was 70.3°C.
[0156] Near the end of polymerization when the polymerization conversion rate of the raw material monomer reached 98% or more, the temperature of the dispersion exceeded 70.3°C, causing an exothermic process, so the temperature of the dispersion was controlled to 71°C or less by the temperature control device. The exothermic process was determined to have ended when the temperature of the dispersion fell below 70.3°C. Suspension polymerization was continued even after the exothermic process ended. In the polymerization process after the exothermic process ended, the minimum temperature of the dispersion was 69.7°C and the maximum temperature was 70.3°C. Suspension polymerization was carried out for 3 hours after the exothermic process began, to obtain a suspension in which polymethyl methacrylate particles were dispersed in water as polymer particles.
[0157] After the obtained suspension was cooled to room temperature, hydrochloric acid was added to the suspension to decompose the dispersion stabilizer (double decomposition magnesium pyrophosphate). Then, the polymer particles were separated from the aqueous medium by a pressure separator, and the obtained polymer particles were washed with ion-exchanged water. The washed polymer particles were placed in a vacuum dryer and dried by heating.
[0158] Next, the dried polymer particles were air-classified. Specifically, the polymer particles were fed to a classifying rotor type air classifier (trade name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Co., Ltd.), and classified using a fine powder rotor as the classifying rotor, to remove fine particles having a small particle size so that the coefficient of variation in the particle size distribution based on the number was not less than 30% (fine particle removal step). Next, the polymer particles were fed to a blow-through type high-performance sieve machine (manufactured by Toyo Hightec Co., Ltd., trade name "Hibolter") to perform classification, and remove coarse particles having a large particle size so that the coefficient of variation in the particle size distribution based on the number was not less than 30% (coarse particle removal step). This resulted in the polymer particles after classification.
[0159] Example 2 The polymer particles after classification were obtained in the same manner as in Example 1, except that the amount of sodium lauryl sulfate used as a surfactant was set to 0.05 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to be more than 3 μm and not more than 5 μm.
[0160] Example 3 The polymer particles after classification were obtained in the same manner as in Example 1, except that the amount of sodium lauryl sulfate used as a surfactant was set to 0.05 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to be more than 7 μm and not more than 9 μm.
[0161] Example 4 The polymer particles after classification were obtained in the same manner as in Example 1, except that ethyl methacrylate (EMA) was used as the raw material monomer instead of methyl methacrylate, the amount of sodium lauryl sulfate used as the surfactant was 0.05 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to be more than 3 μm and not more than 5 μm.
[0162] Example 5 The polymer particles after classification were obtained in the same manner as in Example 1, except that ethyl methacrylate was used instead of methyl methacrylate as the raw material monomer, the amount of sodium lauryl sulfate used as the surfactant was 0.05 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to 17 to 20 μm.
[0163] Example 6 The polymer particles after classification were obtained in the same manner as in Example 1, except that a raw material mixture containing 100 parts by mass of isobutyl methacrylate (IBMA) as a raw material monomer, 0.05 parts by mass of α-methylstyrene dimer as a molecular weight regulator, and 0.4 parts by mass of benzoyl peroxide as a polymerization initiator was prepared, the amount of sodium lauryl sulfate used as a surfactant was 0.02 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to 45 to 50 μm.
[0164] Example 7 The polymer particles after classification were obtained in the same manner as in Example 1, except that a raw material mixture containing 50 parts by mass of methyl methacrylate and 50 parts by mass of ethyl methacrylate as raw material monomers, 0.6 parts by mass of α-methylstyrene as a molecular weight regulator, and 0.4 parts by mass of benzoyl peroxide as a polymerization initiator was prepared, the amount of sodium lauryl sulfate used as a surfactant was 0.02 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to 30 to 35 μm.
[0165] Example 8 The polymer particles after classification were obtained in the same manner as in Example 1, except that a raw material mixture containing 50 parts by mass of methyl methacrylate and 50 parts by mass of ethyl methacrylate as raw material monomers, 0.6 parts by mass of α-methylstyrene as a molecular weight regulator, and 0.4 parts by mass of benzoyl peroxide as a polymerization initiator was prepared, the amount of sodium lauryl sulfate used as a surfactant was 0.02 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to 45 to 50 μm.
[0166] Example 9 The polymer particles after classification were obtained in the same manner as in Example 1, except that styrene (St) was used instead of methyl methacrylate as the raw material monomer, the amount of sodium lauryl sulfate used as the surfactant was 0.05 parts by mass, and the aqueous medium was stirred and mixed while adjusting the droplet diameter of the raw material mixture (oil phase) in the aqueous medium (aqueous phase) to 17 to 20 μm.
[0167] Comparative Example 1 Polymer particles were obtained in the same manner as in Example 1, except that the coarse particle removal step and the fine particle removal step were not carried out.
[0168] Comparative Example 2 Classified polymer particles were obtained in the same manner as in Example 1, except that the fine particle removal step was not carried out.
[0169] Comparative Example 3 Classified polymer particles were obtained in the same manner as in Example 1, except that the coarse particle removal step was not carried out.
[0170] Comparative Example 4 The polymer particles after classification were obtained in the same manner as in Example 2, except that in the coarse particle removal step and the fine particle removal step, the coarse particles and the fine particles were removed so that the coefficient of variation in the number-based particle size distribution was 30% or less.
[0171] Comparative Example 5 [Production of seed particles] A separable flask equipped with a stirrer, a thermometer, and a reflux condenser was supplied with 900 parts by mass of deionized water as an aqueous medium, 160 parts by mass of ethyl methacrylate, and 3.2 parts by mass of n-octyl mercaptan as a molecular weight regulator, and the inside of the separable flask was replaced with nitrogen while stirring the contents of the separable flask, and the internal temperature of the separable flask was raised to 65°C. Furthermore, while maintaining the internal temperature of the separable flask at 65°C, an aqueous solution in which 1.0 part by mass of potassium persulfate as a polymerization initiator was dissolved in 100 parts by mass of water was added to the contents in the separable flask, and then polymerization reaction was carried out for 12 hours. The reaction liquid after polymerization was filtered through a wire mesh with a 400 mesh (opening 32 μm) to prepare a raw material slurry containing 14% by mass of seed particles made of polyethyl methacrylate as a solid content. The seed particles contained in this raw material slurry were spherical particles with a volume average particle diameter of 0.76 μm.
[0172] [Production of polymer particles] A raw material mixture was prepared by dissolving 4 parts by mass of 2,2'-azoisobutyronitrile as a polymerization initiator and 4 parts by mass of benzoyl peroxide in 1000 parts by mass of methyl methacrylate (MMA).
[0173] An aqueous medium mixture was prepared by dissolving 8 g of sodium di(2-ethylhexyl)sulfosuccinate as an anionic surfactant in 800 g of deionized water as an aqueous medium.
[0174] The aqueous medium mixture and the raw material mixture were mixed and the resulting mixture was fed to a homogenizer and stirred at a rotation speed of 10,000 rpm for 10 minutes to produce an emulsion. The raw material slurry was added to the emulsion so that the solid content (seed particles) was 4.2 g, and the mixture was stirred at 30° C. for 5 hours to obtain a dispersion.
[0175] To this dispersion, 2,400 parts by mass of an aqueous solution containing 4 mass% polyvinyl alcohol ("GOHSENOL (registered trademark) GM-14L" manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) as a polymer dispersion stabilizer and 0.64 parts by mass of sodium nitrite as a polymerization inhibitor were added, and the mixture was then stirred at 60°C for 5 hours and then at 105°C for 3 hours to carry out a polymerization reaction, thereby obtaining a slurry containing polymer particles (hereinafter referred to as slurry (1)).
[0176] Thereafter, the polymer particles were separated from the slurry (1) using a pressure separator, and the obtained polymer particles were washed with ion-exchanged water. The washed polymer particles were placed in a vacuum dryer and dried by heating.
[0177] Next, the dried polymer particles were subjected to air flow classification in the same manner as in Example 1, except that in the coarse particle removal step and the fine particle removal step, the coarse particles and the fine particles were removed so that the coefficient of variation in the particle size distribution based on the number was 30% or less. Thus, classified polymer particles were obtained.
[0178] Comparative Example 6 In the heat generation step, the temperature of the dispersion was controlled to be 72.7°C or less using a temperature control device, and the maximum temperature of the dispersion in the heat generation step was set to 72.7°C. Except for this, the same procedure as in Example 1 was followed to obtain polymer particles after classification.
[0179] For the polymer particles before classification obtained in Examples 1 to 9 and Comparative Examples 2 to 6, the number average particle size, the coefficient of variation (CV) in the number-based particle size distribution, and the particle size (D5') corresponding to a cumulative percentage of 5% from the small diameter side in the number-based particle size distribution are shown in the "Before classification" column in Table 1.
[0180] For the polymer particles after classification obtained in Examples 1 to 9 and Comparative Examples 2 to 6, and the polymer particles before classification obtained in Comparative Example 1, the number average particle diameter, the coefficient of variation (CV) in the number-based particle size distribution, the particle diameter (D5) corresponding to a cumulative percentage of 5% from the small diameter side in the number-based particle size distribution, the particle diameter 5 times the number average particle diameter (also simply referred to as "5 times particle diameter"), and the content of large particles in the polymer particles are shown in the "After classification" column in Table 1.
[0181] In addition, for each of the polymer particles after classification obtained in Examples 1 to 9 and Comparative Examples 2 to 6, and the polymer particles before classification obtained in Comparative Example 1, the large particles contained in the polymer particles were contained in a range in which the cumulative percentage of the large particles from the small diameter side was 95% or more in the particle size distribution based on the number of polymer particles.
[0182] In addition, for the polymer particles after classification obtained in Examples 1 to 9 and Comparative Examples 2 to 6, and the polymer particles before classification obtained in Comparative Example 1, the weight average molecular weight (A) of the entire polymer particles, the weight average molecular weight (B) of the small particles, and the weight average molecular weight (C) of the large particles are each shown in Table 1.
[0183] [Measurement of weight average molecular weight and number average particle size of each particle contained in polymer particles] Either the polymer particles after classification obtained in the examples or the polymer particles before classification obtained in Comparative Example 1 was selected as the polymer particles to be measured. The selected polymer particles were classified by being supplied to a rotor-type air classifier (product name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Inc.), and classified into polymer particles having the particle size ranges shown below [particles (1), first medium particles, second medium particles, particles (4)]. Particle (1): Polymer particles in which the cumulative percentage of small diameter particles is 20% or less in the number-based particle size distribution of polymer particles First medium particles: Polymer particles having a cumulative percentage of more than 20% and not more than 50% from the small diameter side in the number-based particle size distribution of polymer particles Second medium particles: Polymer particles whose cumulative percentage of the small diameter particles is more than 50% and not more than 80% in terms of the particle size distribution based on the number of polymer particles. Particle (4): Polymer particles in which the cumulative percentage of the smallest diameter particles in the number-based particle size distribution of the polymer particles is more than 80% and less than 100%.
[0184] The number average particle diameters of the particles (1), the first medium particles, the second medium particles, and the particles (4) were measured in the same manner as the method for measuring the number average particle diameter of the polymer particles described above. The results obtained are shown in the column for the number average particle diameter of each polymer particle in Table 2. Furthermore, the weight average molecular weight of the particles (1), the weight average molecular weight (D) of the first medium particles, the weight average molecular weight (E) of the second medium particles, and the weight average molecular weight of the particles (4) were measured in the same manner as the method for measuring the weight average molecular weight of the entire polymer particles described above. The results obtained are shown in the column for the weight average molecular weight of each polymer particle in Table 2.
[0185] Table 2 shows the value (D / A) obtained by dividing the weight average molecular weight (D) of the first medium particle by the weight average molecular weight (A) of the entire polymer particle, the value (E / A) obtained by dividing the weight average molecular weight (E) of the second medium particle by the weight average molecular weight (A) of the entire polymer particle, the value (D / B) obtained by dividing the weight average molecular weight (D) of the first medium particle by the weight average molecular weight (B) of the small particle, the value (E / D) obtained by dividing the weight average molecular weight (E) of the second medium particle by the weight average molecular weight (D) of the first medium particle, and the value (C / E) obtained by dividing the weight average molecular weight (C) of the large particle by the weight average molecular weight (E) of the second medium particle.
[0186] [Evaluation of thickening effect] The thickening effect of the polymer particles after classification obtained in the Examples and Comparative Examples, and the polymer particles before classification obtained in Comparative Example 1 was evaluated according to the following procedure when toluene, methyl methacrylate, or cyclohexane was used as the dissolution medium.
[0187] (Viscosity measurement of composition (1) containing polymer particles: toluene) A composition (1) containing 20 g of polymer particles and 100 g of toluene and a rotor (manufactured by AS ONE, product name "High-speed compatible cross rotor 58947-828") were placed in a 200 mL beaker. The beaker was then placed on a magnetic stirrer (manufactured by AS ONE, product name "REXIM analog type 4-unit RS-4AN"), and the composition (1) was stirred by the rotor in an atmosphere of 25°C. After the start of stirring, the viscosity V1 of the composition (1) after 0.5 hours, the viscosity V2 of the composition (1) after 1 hour, the viscosity V3 of the composition (1) after 1.5 hours, and the viscosity V4 of the composition (1) after 2 hours were measured at 25°C using a B-type viscometer (manufactured by Brookfield AMETEK, product name "LVDV-II") and rotor No. LV-2 as the rotor, with a rotation speed of 60 rpm. The results obtained are shown in Table 3.
[0188] The composition (1) was visually observed 1.5 hours after the start of stirring and 2 hours after the start of stirring to confirm the presence or absence of gel-like undissolved matter (powder). The results are shown in Table 3.
[0189] (Viscosity measurement of composition (2) containing small particles: toluene) The polymer particles were fed to a rotor-type airflow classifier (product name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Co., Ltd.) and classified to obtain small particles having a cumulative percentage of 5% or less from the small diameter side in the particle size distribution based on the number of particles. Next, composition (2) containing 20 g of small particles and 100 g of toluene was stirred in the same manner as in the viscosity measurement of composition (1) described above, and the viscosity V5 of composition (2) after 1.5 hours from the start of stirring and the viscosity V6 of composition (2) after 2 hours were measured. The results are shown in Table 3.
[0190] (Viscosity measurement of composition (3) containing large particles: toluene) The polymer particles were fed to a rotor-type air classifier (product name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Co., Ltd.) and classified to obtain polymer particles (I) having a cumulative percentage of 95% or more from the small diameter side in the particle size distribution based on the number of particles. Next, a composition (3) containing 20 g of polymer particles (I) and 100 g of toluene was stirred in the same manner as in the viscosity measurement of the composition (1) described above, and the viscosity V7 of the composition (3) after 1.5 hours from the start of stirring and the viscosity V8 of the composition (3) after 2 hours were measured. The results obtained are shown in Table 3.
[0191] If the ratio [V7 / V5] of the viscosity V7 of composition (3) to the viscosity V5 of composition (2) is within the range of 0.9 to 1.1 1.5 hours after the start of stirring, the polymer particles can be evaluated as having excellent thickening stability. If the ratio [V7 / V5] is outside the above range, when such polymer particles are dissolved in a dissolution medium, low and high viscosity parts are generated in the composition, resulting in uneven viscosity in the composition.
[0192] (Viscosity measurement of composition (4) containing polymer particles: methyl methacrylate) Composition (4) containing 20 g of polymer particles and 100 g of methyl methacrylate and a rotor (manufactured by AS ONE, product name "High-speed compatible cross rotor 58947-828") were placed in a 200 mL beaker. The beaker was then placed on a magnetic stirrer (manufactured by AS ONE, product name "REXIM analog type 4-row RS-4AN"), and composition (4) was stirred by the rotor in an atmosphere of 25°C. After the start of stirring, the viscosity V9 of composition (4) after 0.5 hours, the viscosity V10 of composition (4) after 1 hour, the viscosity V11 of composition (4) after 1.5 hours, and the viscosity V12 of composition (4) after 2 hours were measured at 25°C using a B-type viscometer (manufactured by Brookfield AMETEK, product name "LVDV-II") and rotor No. LV-2 as the rotor, with a rotation speed of 60 rpm. The results obtained are shown in Table 4.
[0193] The composition (4) was visually observed 1.5 hours after the start of stirring and 2 hours after the start of stirring to confirm the presence or absence of gel-like undissolved matter (powder). The results are shown in Table 4.
[0194] (Viscosity measurement of composition (5) containing small particles: methyl methacrylate) The polymer particles were fed to a rotor-type air classifier (product name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Co., Ltd.) and classified to obtain small particles having a cumulative percentage of 5% or less from the small diameter side in the particle size distribution based on the number of particles. Next, composition (5) containing 20 g of small particles and 100 g of methyl methacrylate was stirred in the same manner as in the viscosity measurement of composition (4) described above, and the viscosity V13 of composition (5) after 1.5 hours from the start of stirring and the viscosity V14 of composition (5) after 2 hours were measured. The results obtained are shown in Table 4.
[0195] (Viscosity measurement of composition (6) containing large particles: methyl methacrylate) The polymer particles were fed to a rotor-type air classifier (product name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Co., Ltd.) and classified to obtain polymer particles (I) having a cumulative percentage of 95% or more from the small diameter side in the particle size distribution based on the number of particles. Next, a composition (6) containing 20 g of the polymer particles (I) and 100 g of methyl methacrylate was stirred in the same manner as in the viscosity measurement of the composition (4) described above, and the viscosity V15 of the composition (6) after 1.5 hours from the start of stirring and the viscosity V16 of the composition (6) after 2 hours were measured. The results obtained are shown in Table 4.
[0196] If the ratio [V15 / V13] of the viscosity V15 of composition (6) to the viscosity V13 of composition (5) is within the range of 0.9 to 1.1 1.5 hours after the start of stirring, the polymer particles can be evaluated as having excellent thickening stability. If the ratio [V15 / V13] is outside the above range, when such polymer particles are dissolved in a dissolution medium, low and high viscosity parts are generated in the composition, resulting in uneven viscosity in the composition.
[0197] (Viscosity measurement of composition (7) containing polymer particles: cyclohexane) A composition (7) containing 20 g of polymer particles and 100 g of cyclohexane and a rotor (manufactured by AS ONE, product name "High-speed compatible cross rotor 58947-828") were placed in a 200 mL beaker. The beaker was then placed on a magnetic stirrer (manufactured by AS ONE, product name "REXIM analog type 4-row RS-4AN"), and the composition (7) was stirred by the rotor in an atmosphere of 25°C. After the start of stirring, the viscosity V17 of the composition (7) after 0.5 hours, the viscosity V18 of the composition (7) after 1 hour, the viscosity V19 of the composition (7) after 1.5 hours, and the viscosity V20 of the composition (7) after 2 hours were measured at 25°C using a B-type viscometer (manufactured by Brookfield AMETEK, product name "LVDV-II") and rotor No. LV-2 as the rotor, with a rotation speed of 60 rpm. The results obtained are shown in Table 5.
[0198] The composition (7) was visually observed 1.5 hours after the start of stirring and 2 hours after the start of stirring to confirm the presence or absence of gel-like undissolved matter (powder). The results are shown in Table 5.
[0199] (Viscosity measurement of composition (8) containing small particles: cyclohexane) The polymer particles were fed to a rotor-type air classifier (product name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Co., Ltd.) and classified to obtain small particles having a cumulative percentage of 5% or less from the small diameter side in the particle size distribution based on the number of particles. Next, composition (8) containing 20 g of small particles and 100 g of cyclohexane was stirred in the same manner as in the viscosity measurement of composition (7) described above, and the viscosity V21 of composition (8) after 1.5 hours from the start of stirring and the viscosity V22 of composition (8) after 2 hours were measured. The results obtained are shown in Table 5.
[0200] (Viscosity measurement of composition (9) containing large particles: cyclohexane) The polymer particles were fed to a rotor-type air classifier (product name "Turbo Classifier (registered trademark) TC-25", manufactured by Nisshin Engineering Co., Ltd.) and classified to obtain polymer particles (I) having a cumulative percentage of 95% or more from the small diameter side in the particle size distribution based on the number of particles. Next, a composition (9) containing 20 g of polymer particles (I) and 100 g of cyclohexane was stirred in the same manner as in the viscosity measurement of the above-mentioned composition (7), and the viscosity V23 of the composition (9) after 1.5 hours from the start of stirring and the viscosity V24 of the composition (9) after 2 hours were measured, respectively. The results obtained are shown in Table 5.
[0201] If the ratio [V23 / V21] of the viscosity V23 of composition (9) to the viscosity V21 of composition (8) is within the range of 0.9 to 1.1 1.5 hours after the start of stirring, the polymer particles can be evaluated as having excellent thickening stability. If the ratio [V23 / V21] is outside the above range, when such polymer particles are dissolved in a dissolution medium, low and high viscosity parts are generated in the composition, resulting in uneven viscosity in the composition.
[0202] [Evaluation of coating composition] Furthermore, for the polymer particles after classification obtained in the Examples and Comparative Examples, and the polymer particles before classification obtained in Comparative Example 1, coating compositions and coating films were prepared and evaluated according to the following procedures.
[0203] 20 parts by mass of polymer particles, 100 parts by mass of toluene, and a rotor (manufactured by AS ONE Corporation, product name "High-speed compatible cross rotor 58947-828") were placed in a 200 mL beaker. Then, the beaker was placed in a magnetic stirrer (manufactured by AS ONE Corporation, product name "REXIM analog type 4-unit RS-4AN"), and the rotor was rotated for 2 hours under a 25°C atmosphere, thereby dissolving the polymer particles in toluene, and then the rotor was removed to obtain a coating composition. The obtained coating composition was applied to a polyethylene terephthalate (PET) film (thickness 100 μm, manufactured by FUJIFILM Corporation, product name "FUJIX (registered trademark) OHP film for copiers") using a slit coater so that the film thickness after coating was 75 μm, thereby obtaining a coating film. The coating film was placed in a dryer kept at a temperature of 70°C and dried for 10 minutes to obtain a coating film. As a result, a coated body having a PET film and a coating film laminated and integrated on the surface of the PET film was obtained. The coated body was then cut to obtain a flat square specimen with each side measuring 10 cm. The back side of the PET film in the specimen was irradiated with light from a fluorescent lamp, and the surface of the coating was visually observed and evaluated according to the following criteria. The results are shown in the "Coating Film Evaluation" column in Table 3. A: No white spots or paint spots. B: White spots and paint spots occurred in 1 to 5 places in total. C: There are a total of 6 or more white spots and paint spots.
[0204] If the paint composition contains splints, the splints will cause white spots in the coating film, resulting in poor appearance. Also, if the viscosity of the paint composition is not uniform, the coating film will have uneven thickness (paint spots), which will cause the light passing through the coating film to be non-uniform, resulting in poor appearance.
[0205] [Evaluation of dental compositions] Furthermore, dental compositions were prepared from the classified polymer particles obtained in the Examples and Comparative Examples, or the unclassified polymer particles obtained in Comparative Example 1 according to the following procedures, and the operability of the dental compositions and the 1% compressive strength variation and bending strength of the cured products of the dental compositions were evaluated.
[0206] (Preparation of dental composition) 30 parts by weight of the polymer particles, 70 parts by weight of methyl methacrylate as a monomer that polymerizes when exposed to ionizing radiation, and 0.5 parts by weight of 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (manufactured by BASF Japan, product name "Irgacure (registered trademark) 907") as a photopolymerization initiator were mixed for 5 minutes to dissolve the polymer particles in the methyl methacrylate, thereby obtaining a paste-like dental composition.
[0207] (Evaluation of operability) An aluminum container (manufactured by Toyo Aluminum Echo Products Co., Ltd., product name "A1070-D") was prepared. The aluminum container was composed of a bottom part having a circular planar shape, and a peripheral wall part integrally formed around the entire periphery of the bottom part, upward and diagonally outward. The peripheral wall part was formed in a sawtooth cross section in which a plurality of Λ-shaped mountain folds and V-shaped valley folds were alternately repeated in the circumferential direction. The dental composition prepared above was then filled into the aluminum container using a medicine spoon so that the thickness of the dental composition after filling was 5 mm. The operability of the dental composition when filled was evaluated according to the following criteria. The results are shown in the "operability evaluation" column of Table 6. 5: The dental composition had particularly excellent filling properties, good spreading fluidity, and was easy to handle without becoming sticky or stringy. 4: The dental composition had excellent filling properties, good spreading fluidity, and was easy to handle without becoming sticky or stringy. 3: The dental composition had sufficient filling properties, sufficient spreadability and fluidity, and was able to be handled without becoming sticky or stringy. 2: The filling property and spreading fluidity of the dental composition were insufficient, and the dental composition was sticky and stringy, making it difficult to handle. 1: The filling property and spreading fluidity of the dental composition were particularly insufficient, and the dental composition was very sticky and stringy, making the handling of the dental composition particularly insufficient.
[0208] The filling property of the dental composition was evaluated by visually observing whether the dental composition flows without forming bubbles in the multiple V-shaped cross-sectional recesses formed on the inner surface of the peripheral wall of the aluminum container when the dental composition is filled in the aluminum container, and whether the dental composition is filled uniformly in the aluminum container as a whole. The extension flow property of the dental composition was evaluated by evaluating whether the dental composition can be uniformly extended and flowed when the dental composition is filled in the aluminum container.
[0209] (Evaluation of variation in 1% compressive strength) The dental composition prepared above was irradiated with ultraviolet light at an irradiation intensity of 0.1 W / cm 2 , Accumulated light intensity 0.1J / cm 2 The dental composition was cured by irradiation at 400 nm for 1 hour to obtain a test piece made of the cured dental composition. The test piece had a flat circular shape with a diameter of 40 mm and a thickness of 5 mm.
[0210] The 1% compressive strength of the test specimen was measured under the following measurement conditions using a micro-compression testing machine "MCTM-200" manufactured by Shimadzu Corporation. The test specimen was placed on the lower pressure plate, and the upper pressure indenter arranged on the test specimen was lowered at the following loading speed to gradually compress the test specimen until the maximum load reached 50 gf. The load P (kgf) was then measured at the point where the test specimen was compressed by 1% relative to the thickness of the test specimen before compression, and the 1% compressive strength (kgf / mm2) was calculated based on the following formula (I): 2 When measuring the 1% compressive strength, the loading speed of the upper pressure indenter and the maximum load applied to the test piece can be adjusted appropriately depending on the hardness of the test piece.
[0211] (1% compressive strength measurement conditions) Measuring instrument: Shimadzu Corporation's micro-compression testing instrument "MCTM-200" Measurement environment: 20 to 25°C, relative humidity 65% Upper pressure indenter: 0.5 mm diameter flat indenter (material: diamond) Lower pressure plate: SKS flat plate Test type: Compression test (MODE1) Load speed: 0.0746gf / sec (1% compressive strength calculation formula) 1% Compressive Strength (kgf / mm 2 ) =Load P(kgf) / (0.5mm×0.5mm) Formula (I)
[0212] Using the same procedure as above, the 1% compressive strength was measured at 20 random locations on the test piece. The highest, second highest, lowest, and second lowest 1% compressive strength values were excluded from the 20 measured values, and the arithmetic mean value S of 14 measured values was calculated.
[0213] The absolute value T1 of the difference between the highest 1% compressive strength (maximum value) and the above arithmetic mean value S was calculated. The absolute value T2 of the difference between the lowest 1% compressive strength (minimum value) and the above arithmetic mean value S was calculated. Of the absolute values T1 and T2, the larger one was selected. Using the selected absolute value and the above arithmetic mean value S, the "deviation" was calculated based on the following formula. The deviation was evaluated according to the following evaluation criteria. The results are shown in Table 6. Deviation = Selected absolute value / arithmetic mean value S
[0214] (Evaluation criteria for 1% compressive strength deviation) A: The deviation was less than 0.10. B: The deviation was 0.10 or more and 0.20 or less. C: The deviation was greater than 0.20.
[0215] (Bending strength evaluation) The dental composition prepared above was irradiated with ultraviolet light at an irradiation intensity of 0.1 W / cm 2 , cumulative light intensity 0.1J / cm 2The dental composition was cured by irradiation at 400 nm for 1 hour to obtain a test piece made of the cured dental composition. The test piece had a flat rectangular shape with a length of 40 mm, a width of 10 mm, and a thickness of 5 mm.
[0216] The test piece 10 was placed on a horizontal stand J. As shown in Fig. 1, the test piece 10 on the horizontal stand J was fixed with a support (not shown) in a portion extending from one edge X to 30 mm in the long side direction to form a fixed portion, while the remaining portion was made into a free piece portion that could be bent in the vertical direction.
[0217] The free piece portion of the test piece 10 was bent downward until the angle θ between the tangent (L1) of the fixed portion surface of the test piece 10 and the tangent (L2) of the free piece surface of the test piece 10 became 60°, and was held for 2 seconds, after which the free piece portion was returned to its original state so that it was horizontal. This operation constituted one cycle, and 5 cycles were performed. The free piece portion of the test piece 10 was visually observed and evaluated according to the following criteria. The results are shown in the "Bending strength evaluation" column of Table 6. A: Neither cracks nor whitened areas were generated in the free portion of the test piece. B: Cracks or whitened areas were observed in the free portion of the test piece. C: Both cracks and whitened areas were observed in the free portion of the test piece.
[0218] In the case where a dental composition contains a stepping member, when bending stress is applied to a cured product of the dental composition, cracks may occur from the stepping member. If the viscosity of the dental composition is non-uniform, when bending stress is applied to a cured product of the dental composition, the cured product will not be able to follow the bending stress, resulting in whitened areas.
[0219] [Table 1] TIFF0007577733000001.tif246153
[0220] [Table 2] TIFF0007577733000002.tif189153
[0221] [Table 3] TIFF0007577733000003.tif246153
[0222] [Table 4] TIFF0007577733000004.tif235153
[0223] [Table 5] TIFF0007577733000005.tif234153
[0224] [Table 6] TIFF0007577733000006.tif179153 [Industrial Applicability]
[0225] The polymer particles of the present invention can be dissolved in a dissolution medium without forming splices, and can uniformly improve the viscosity of the composition. By using such polymer particles, it is possible to provide a composition capable of forming a coating film having a uniform thickness and composition and greatly reducing the occurrence of defective appearance.
[0226] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to Japanese Patent Application No. 2020-60220, filed on March 30, 2020, the disclosure of which is incorporated herein by reference in its entirety. [Explanation of symbols]
[0227] 10 Test Pieces J Horizontal platform X One edge L1 tangent L2 tangent
Claims
1. Polymer particles having a number-average particle diameter of 1 to 50 μm and a coefficient of variation in number-based particle size distribution of 30% or more and 80% or less, The weight average molecular weight of the entire polymer particles is A, the weight average molecular weight of small particles, the cumulative percentage of which from the small diameter side in the number-based particle size distribution of the polymer particles is 5% or less, is defined as B; When the weight average molecular weight of the large particles having a particle diameter 5 times or more the number average particle diameter of the polymer particles is C, The following formulas (1) and (2) are satisfied, 0.90≦(B / A)<1.0...Formula (1) 1<(C / B)<1.25...Formula (2) The polymer particles contain a polymer of a raw material monomer, and the content of a polyfunctional monomer in the raw material monomer is 0 mass % or 1.0 mass % or less relative to the total amount of the raw material monomer.
2. The polymer particle according to claim 1, which satisfies the following formula (3): 1.0<(C / A)≦1.10...Formula (3)
3. 3. The polymer particles according to claim 1, wherein the content of large particles having a particle diameter of 5 times or more the number average particle diameter of the polymer particles is 0.1% or less on a number basis.
4. 4. The polymer particle according to claim 1, wherein the polymer comprises an acrylic polymer.
5. A thickener comprising the polymer particles according to any one of claims 1 to 4.
6. A composition comprising a dissolution medium and a solution of the polymer particles according to any one of claims 1 to 4.
7. The composition of claim 6, further comprising a photoinitiator.
Citation Information
Patent Citations
Production of polymerized toner having small particle size
JP1994043693A
Resin composition for toner and toner
JP1995092729A
Optical sheet and back light unit using the same
JP2004198743A
Heat shrinkable film
JP2009096182A
White reflective film
JP2010033053A