Ink set and image recording method

The use of crosslinked polymer-based pigment dispersants in colored and white inks, combined with a flocculant in the pretreatment liquid, addresses the issue of cracking in recorded images, ensuring uniform aggregation and improved image quality.

JP7577741B2Active Publication Date: 2024-11-05FUJIFILM CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2022522568
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-11
Filing Date
2021-04-12
Publication Date
2024-11-05
Estimated Expiration
2041-04-12

AI Technical Summary

Technical Problem

Existing image recording methods using colored and white inks after applying a pretreatment liquid often result in cracking of the recorded image due to non-uniform aggregation of ink components.

Method used

An ink set comprising colored and white inks with pigment dispersants containing polymers or block polymers having a crosslinked structure, along with a pretreatment liquid containing a flocculant, is used to ensure uniform aggregation and prevent cracking.

Benefits of technology

The ink set effectively suppresses cracking in recorded images by promoting uniform aggregation of ink components, enhancing image quality and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577741000001
    Figure 0007577741000001
  • Figure 0007577741000002
    Figure 0007577741000002
  • Figure 0007577741000003
    Figure 0007577741000003
Patent Text Reader

Abstract

Provided is an ink set comprising: a coloring ink including a coloring pigment that is at least one among a chromatic pigment and a black pigment, a pigment dispersant, and water; and a white ink including a white pigment, a pigment dispersant, and water, wherein the pigment dispersants included in the coloring ink and the white ink each contain a polymer having a crosslinked structure or a block polymer. Also provided is a method for recording an image.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an ink set and an image recording method. [Background technology]

[0002] Conventionally, various studies have been made regarding image recording using a plurality of inks together with a pretreatment liquid.

[0003] For example, JP 2019-167451 A describes an ink set that includes a first ink and a second ink, which are water-based ink compositions, the first ink and the second ink containing a pigment and resin particles, the first ink containing a first pigment, and the second ink containing a second pigment different from the first pigment, and the first ink and the second ink are inks whose volume average particle diameter is increased by mixing with a 5% by mass aqueous solution of magnesium sulfate heptahydrate, the difference between the volume average particle diameters of the inks after mixing being 40% or less, and which is used for recording together with a treatment liquid containing an aggregating agent that aggregates the components of the water-based ink composition. Furthermore, JP 2018-178131 A describes an ink set that includes a reaction liquid containing a coagulant, a first ink containing a colorant, and a second ink containing a colorant, and is used for recording on a non-absorbent recording medium or a low-absorbent recording medium, in which the reaction liquid, the first ink, and the second ink are applied in that order to the recording medium in layers. Summary of the Invention [Problem to be solved by the invention]

[0004] When a pretreatment liquid is applied onto a substrate and then an image is recorded using colored inks and white ink, it is sometimes necessary to suppress cracks in the recorded image.

[0005] The present disclosure has been made in consideration of these circumstances, and according to an embodiment of the present invention, there is provided an ink set and an image recording method that are capable of recording an image in which cracking is suppressed when an image is recorded using colored inks and white ink after a pretreatment liquid is applied. [Means for solving the problem]

[0006] The present disclosure includes the following aspects. <1> An ink set comprising: a colored ink containing a colored pigment, which is at least one of a chromatic pigment and a black pigment, a pigment dispersant, and water; and a white ink containing a white pigment, a pigment dispersant, and water, wherein the colored ink and the pigment dispersant contained in the white ink each contain a polymer having a crosslinked structure or a block polymer. <2> The pigment dispersant contained in the color ink contains a polymer having a crosslinked structure. <1> The ink set according to claim 1. <3> The pigment dispersant contained in the white ink contains a block polymer. <1> or <2> The ink set according to claim 1. <4> The acid value of the pigment dispersant contained in the color ink is 30 mg KOH / g to 180 mg KOH / g. <1> ~ <3> 13. The ink set according to claim 12, <5> The acid value of the pigment dispersant contained in the white ink is 60 mg KOH / g to 150 mg KOH / g. <1> ~ <4> 13. The ink set according to claim 12, <6> The pigment dispersants contained in the color inks and the white ink each contain a structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure, <1> ~ <5> 13. The ink set according to claim 12, <7> The absolute value of the difference between the surface tension of the color ink and the surface tension of the white ink is 0.05 mN / m to 10.0 mN / m. <1> ~ <6> 13. The ink set according to claim 12, <8> Further comprising a pretreatment liquid containing a flocculant; <1> ~ <7> 13. The ink set according to claim 12, <9> The absolute value of the difference between the surface tension of the pretreatment liquid and the surface tension of the color ink is 0.05 mN / m to 10.0 mN / m. <8> The ink set according to claim 1. <10> <1> ~ <7> 2. An image recording method comprising: a colored ink applying step of applying colored inks onto a non-permeable substrate; and a white ink applying step of applying a white ink onto a colored ink film formed by applying the colored inks, the image recording method comprising the steps of: applying the ink set according to any one of the above items; <11> <8> or <9> 2. An image recording method comprising: a pretreatment liquid applying step of applying a pretreatment liquid onto a non-permeable substrate; and an ink applying step of applying color inks and a white ink by an inkjet recording method onto the non-permeable substrate to which the pretreatment liquid has been applied. Effect of the Invention

[0007] According to the present disclosure, there are provided an ink set and an image recording method that are capable of recording an image in which cracking is suppressed when an image is recorded using colored inks and white ink after a pretreatment liquid is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The ink set and image recording method of the present disclosure will be described in detail below.

[0009] In this specification, a numerical range indicated using "to" means a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in a certain numerical range. In addition, in the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0010] In this specification, the amount of each component in a composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. As used herein, a combination of two or more preferred embodiments is a more preferred embodiment. In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0011] In this specification, the term "image" refers to a film formed by applying a pretreatment liquid and an ink in this order, and the term "image recording" refers to the formation of an image (that is, a film). Additionally, the concept of "image" in this specification also includes a solid image.

[0012] In this specification, the term "(meth)acrylate" is a concept that encompasses both acrylate and methacrylate, and the term "(meth)acrylic" is a concept that encompasses both acrylic and methacrylic.

[0013] [Ink set] The ink set of the present disclosure comprises a colored ink containing a colored pigment, which is at least one of a chromatic pigment and a black pigment, a pigment dispersant, and water, and a white ink containing a white pigment, a pigment dispersant, and water, and the pigment dispersants contained in the colored ink and the white ink each contain a polymer having a crosslinked structure or a block polymer.

[0014] Conventionally, a method is known in which a pretreatment liquid is applied to a substrate, and then an image is recorded using a plurality of inks. The pretreatment liquid contains an aggregating agent, and when an ink is applied to the substrate to which the pretreatment liquid has been applied, the components contained in the ink (particularly, the pigment dispersant) are aggregating due to the aggregating agent. It is believed that the occurrence of cracks in the recorded image is due to the fact that this aggregating occurs non-uniformly.

[0015] JP 2019-167451 A describes an ink set that includes a first ink and a second ink that are aqueous ink compositions and is used for recording together with a treatment liquid containing an aggregating agent that aggregates the components of the aqueous ink composition. JP 2019-167451 A describes that the resin dispersant that disperses the pigment contained in the first ink and the second ink can be any of a random copolymer, a block copolymer, an alternating copolymer, and a graft copolymer. That is, JP 2019-167451 A does not focus on the structure of the resin dispersant that disperses the pigment.

[0016] JP 2018-178131 A describes an ink set including a reaction liquid containing an aggregating agent, a first ink containing a coloring material, and a second ink containing a coloring material. JP 2018-178131 A does not focus on the structure of the pigment dispersant that disperses the coloring material.

[0017] In contrast, in the ink set of the present disclosure, the pigment dispersants contained in the colored inks and the white ink each contain a polymer having a crosslinked structure or a block polymer. The reason why cracking of the recorded image is suppressed when the ink set of the present disclosure is used is presumed to be as follows. It is believed that polymers having a crosslinked structure and block polymers have good adsorption properties to the colored pigments and the white pigments, and that there is little free polymer in the colored inks and the white inks. Therefore, it is believed that aggregation by the aggregating agent contained in the pretreatment liquid proceeds relatively uniformly, suppressing cracking of the recorded image.

[0018] Hereinafter, each component contained in the color inks and white ink constituting the ink set of the present disclosure will be described.

[0019] <Colored ink> In the present disclosure, the color ink includes a color pigment, which is at least one of a chromatic pigment and a black pigment, a pigment dispersant, and water.

[0020] (Color pigments) The color ink contains a color pigment that is at least one of a chromatic pigment and a black pigment. The color pigment contained in the color ink may be only one type, or may be two or more types. That is, the color pigment contained in the color ink may be one or more types of chromatic pigments, may be one or more types of black pigments, or may be a combination of one or more types of chromatic pigments and one or more types of black pigments.

[0021] The chromatic pigment is not particularly limited as long as it exhibits a chromatic color. The chromatic pigment is not particularly limited, and examples thereof include cyan pigments, magenta pigments, yellow pigments, blue pigments, red pigments, green pigments, orange pigments, and violet pigments.

[0022] Specific examples of chromatic pigments include organic pigments such as azo pigments, disazo pigments, condensed disazo pigments, phthalocyanine pigments, quinacridone pigments, quinacridonequinone pigments, anthraquinone pigments, aminoanthraquinone pigments, anthranthrone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, perinone pigments, perylene pigments, isoindoline pigments, isoindolinone pigments, isoviolanthrone pigments, benzimidazolone pigments, indanthrone pigments, triarylcarbonium pigments, and diketopyrrolopyrrole pigments.

[0023] More specifically, the chromatic pigments are Perylene pigments such as CI Pigment Red 190, CI Pigment Red 224, CI Pigment Violet 29; Perinone pigments such as CI Pigment Orange 43, CI Pigment Red 194; Quinacridone pigments such as CI Pigment Violet 19, CI Pigment Violet 42, CI Pigment Red 122, CI Pigment Red 192, CI Pigment Red 202, CI Pigment Red 207, Pigment Red 209; Quinacridonequinone pigments such as CI Pigment Red 206, CI Pigment Orange 48, CI Pigment Orange 49; anthraquinone pigments such as CI Pigment Yellow 147; anthanthrone pigments such as CI Pigment Red 168; Benzimidazolone pigments such as CI Pigment Brown 25, CI Pigment Violet 32, CI Pigment Orange 36, CI Pigment Yellow 120, CI Pigment Yellow 180, Pigment Yellow 181, CI Pigment Orange 62, CI Pigment Red 185; Condensed disazo pigments such as CI Pigment Yellow 93, CI Pigment Yellow 94, CI Pigment Yellow 95, CI Pigment Yellow 128, CI Pigment Yellow 166, CI Pigment Orange 34, CI Pigment Orange 13, CI Pigment Orange 31, Pigment Red 144, Pigment Red 166, Pigment Red 220, CI Pigment Red 221, CI Pigment Red 242, Pigment Red 248, CI Pigment Red 262, CI Pigment Brown 23, etc. Disazo pigments such as CI Pigment Yellow 13, CI Pigment Yellow 83, CI Pigment Yellow 188; Azo pigments such as CI Pigment Red 187, CI Pigment Red 170, CI Pigment Yellow 74, CI Pigment Yellow 150, CI Pigment Red 48, Pigment Red 53, CI Pigment Orange 64, CI Pigment Red 247; Indanthrone pigments such as CI Pigment Blue 60; Phthalocyanine pigments such as CI Pigment Green 7, CI Pigment Green 36, CI Pigment Green 37, CI Pigment Green 58, CI Pigment Blue 16, CI Pigment Blue 75, Pigment Blue 15; Triarylcarbonium pigments such as CI Pigment Blue 56, CI Pigment Blue 61; Dioxazine pigments such as CI Pigment Violet 23, CI Pigment Violet 37; Aminoanthraquinone pigments such as CI Pigment Red 177; Diketopyrrolopyrrole pigments such as CI Pigment Red 254, CI Pigment Red 255, CI Pigment Red 264, CI Pigment Red 272, CI Pigment Orange 71, CI Pigment Orange 73; thioindigo pigments such as CI Pigment Red 88; isoindoline pigments such as CI Pigment Yellow 139, Pigment Orange 66; isoindolinone pigments such as CI Pigment Yellow 109 and CI Pigment Orange 61; Pyranthrone pigments such as CI Pigment Orange 40, CI Pigment Red 216; and and isoviolanthrone pigments such as CI Pigment Violet 31.

[0024] The type of black pigment is not particularly limited as long as it exhibits a black color. Examples of black pigments include carbon black and titanium black.

[0025] The average particle size of the chromatic pigment and the black pigment is preferably 10 nm to 200 nm, more preferably 10 nm to 150 nm, and even more preferably 10 nm to 110 nm. When the average particle size is 200 nm or less, the color reproducibility is good, and further, when an image is recorded using an inkjet recording method, the ejection stability is good. On the other hand, when the average particle size is 10 nm or more, the light resistance is good. In addition, the particle size distribution of the pigment may be either a wide particle size distribution or a monodisperse particle size distribution. The average particle size and particle size distribution of the pigment are obtained by measuring the volume average particle size by a dynamic light scattering method using a particle size distribution measuring device, for example, a product name "Nanotrac UPA-EX150" manufactured by Nikkiso Co., Ltd. In addition, when the pigment is covered with a pigment dispersant, the average particle size of the pigment means the average particle size of the pigment covered with the pigment dispersant.

[0026] From the viewpoints of image density and ejection stability, the content of the color pigment is preferably 1% by mass to 15% by mass, and more preferably 2% by mass to 10% by mass, based on the total amount of the color ink.

[0027] (Pigment dispersant) The colored ink of the present disclosure includes a pigment dispersant. The pigment dispersant includes a polymer having a crosslinked structure or a block polymer. In the present disclosure, a polymer refers to a compound having a weight average molecular weight of 1000 or more.

[0028] In the present disclosure, the weight average molecular weight means a value measured by gel permeation chromatography (GPC). Measurement by gel permeation chromatography (GPC) is performed using a measuring device, HLC (registered trademark)-8020GPC (manufactured by Tosoh Corporation), three columns, TSKgel (registered trademark) Super Multipore HZ-H (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), and THF (tetrahydrofuran) as an eluent. The measurement is performed using an RI detector with a sample concentration of 0.45 mass%, a flow rate of 0.35 ml / min, a sample injection amount of 10 μl, and a measurement temperature of 40° C. The calibration curve is prepared from eight samples of "Standard sample TSK standard, polystyrene" manufactured by Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".

[0029] In the present disclosure, a pigment dispersant has a function of dispersing a pigment. The pigment dispersant is adsorbed on the surface of the pigment and covers at least a part of the surface of the pigment, thereby enabling the pigment to be dispersed in water.

[0030] The acid value of the pigment dispersant contained in the color ink is preferably 20 mgKOH / g to 205 mgKOH / g, more preferably 30 mgKOH / g to 180 mgKOH / g, and even more preferably 65 mgKOH / g to 140 mgKOH / g. When the acid value of the pigment dispersant is 20 mgKOH / g or more, the image quality of the recorded image is more excellent. Furthermore, when the acid value of the pigment dispersant is 205 mgKOH / g or less, the cracking of the recorded image is further suppressed. In the present disclosure, the acid value is a value measured by the method described in JIS K0070:1992.

[0031] - Polymer with cross-linked structure - The polymer having a crosslinked structure is not particularly limited as long as it has at least one crosslinked structure in the molecule.

[0032] Whether or not the polymer contained in the ink has a crosslinked structure can be determined, for example, by the following method. First, the ink is subjected to a separation method such as solvent extraction to separate the polymer. The separated polymer is analyzed using various analytical methods such as nuclear magnetic resonance (NMR), infrared spectroscopy (IR), and thermal analysis, whereby the presence or absence of a crosslinked structure can be comprehensively determined.

[0033] A polymer having a crosslinked structure (hereinafter referred to as a "crosslinked polymer") is formed, for example, by crosslinking an uncrosslinked polymer with a crosslinking agent. The uncrosslinked polymer is preferably a water-soluble polymer.

[0034] In the present disclosure, "water-soluble" in "water-soluble polymer" means a property in which the amount of the polymer that dissolves in 100 g of distilled water at 25° C. is 2 g or more. The amount of the polymer that dissolves in distilled water at 25° C. is preferably 5 g or more, and more preferably 10 g or more.

[0035] Examples of the uncrosslinked polymer include polyvinyl, polyurethane, and polyester. Of these, the uncrosslinked polymer is preferably polyvinyl.

[0036] The uncrosslinked polymer is preferably a polymer having a functional group that can be crosslinked by a crosslinking agent. Examples of the crosslinkable functional group include a carboxy group or a salt thereof, an isocyanate group, and an epoxy group. Among them, from the viewpoint of improving the dispersibility of the pigment, the crosslinkable functional group is preferably a carboxy group or a salt thereof, and a carboxy group is particularly preferable. That is, the uncrosslinked polymer is preferably a polymer containing a carboxy group.

[0037] The uncrosslinked polymer is preferably a copolymer containing a structural unit derived from a monomer containing a carboxy group (hereinafter referred to as a "carboxy group-containing monomer"). The structural unit derived from the carboxy group-containing monomer contained in the copolymer may be of only one type, or may be of two or more types. The copolymer may be a random copolymer or a block copolymer, but is preferably a random copolymer.

[0038] Examples of carboxy group-containing monomers include (meth)acrylic acid, β-carboxyethyl acrylate, fumaric acid, itaconic acid, maleic acid, and crotonic acid.

[0039] From the viewpoints of crosslinkability and dispersibility, the carboxy group-containing monomer is preferably (meth)acrylic acid or β-carboxyethyl acrylate, and more preferably (meth)acrylic acid.

[0040] The uncrosslinked polymer preferably contains a structural unit derived from a hydrophobic monomer in addition to the structural unit derived from the carboxyl group-containing monomer. The structural unit derived from the hydrophobic monomer contained in the copolymer may be of only one type or of two or more types.

[0041] From the viewpoint of adsorptivity to chromatic pigments and black pigments, the hydrophobic monomer preferably contains an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure, i.e., the crosslinked polymer preferably contains a structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure.

[0042] The structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure is preferably at least one type selected from the group consisting of structural units represented by the following formulas (A) to (F). [ka]

[0043] In formulas (A) to (F), R5 Each independently represents a hydrogen atom or a methyl group. 6 each independently represents an alkyl group, an alkenyl group, or an alkynyl group; m is an integer of 0 to 5; n is an integer of 0 to 11; L 5 represents an alkylene group having 1 to 18 carbon atoms, an arylene group having 6 to 18 carbon atoms, a divalent group which is one type selected from Group 1 consisting of -O-, -NH-, -S-, and -C(=O)-, a divalent group which is a combination of two or more types selected from Group 1, or a single bond.

[0044] [R 6 〕 In formulas (A) to (F), R 6 each independently represents an alkyl group, an alkenyl group, or an alkynyl group.

[0045] The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and further preferably a methyl group or an ethyl group.

[0046] The alkenyl group is preferably an alkenyl group having 2 to 10 carbon atoms, more preferably an alkenyl group having 2 to 4 carbon atoms, and even more preferably an alkenyl group having 2 or 3 carbon atoms.

[0047] The alkynyl group is preferably an alkynyl group having 2 to 10 carbon atoms, more preferably an alkynyl group having 2 to 4 carbon atoms, and even more preferably an alkynyl group having 2 or 3 carbon atoms.

[0048] Also, R 6 R may be an unsubstituted group or a group substituted with a substituent. 6 When is substituted with a substituent, examples of the substituent include a halogen atom (eg, a chlorine atom, a bromine atom, etc.) and an alkyl group (eg, a methyl group, an ethyl group, etc.).

[0049] 〔m〕 In formula (A) and formula (B), m represents a substituent (R 6 )

[0050] m is an integer of 0 to 5, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, and further preferably 0 or 1.

[0051] 〔n〕 In formula (C), n is a substituent (R 6 )

[0052] n is an integer of 0 to 11, preferably an integer of 0 to 6, more preferably an integer of 0 to 2, and further preferably 0 or 1.

[0053] [L 5 〕 In formulas (A) to (F), L 5 represents an alkylene group having 1 to 18 carbon atoms, an arylene group having 6 to 18 carbon atoms, a divalent group which is one type selected from Group 4 consisting of -O-, -NH-, -S-, and -C(=O)-, a divalent group which is a combination of two or more types selected from Group 4, or a single bond.

[0054] L 5 The alkylene group having 1 to 18 carbon atoms may be linear or may have a branched structure and / or a cyclic structure.

[0055] L 5 In the alkylene group having 1 to 18 carbon atoms, the number of carbon atoms is preferably 1 to 12, more preferably 1 to 6, and further preferably 1 or 2.

[0056] Examples of the arylene group having 6 to 18 carbon atoms include a phenylene group, a naphthylene group, and a tolyl group.

[0057] L 5 The arylene group having 6 to 18 carbon atoms in the formula (I) preferably has 6 to 12 carbon atoms, and more preferably has 6 to 10 carbon atoms.

[0058] L 5In the above, the "divalent group formed by combining two or more selected from Group 1" is preferably a divalent group formed by combining at least one of an alkylene group having 1 to 18 carbon atoms and an arylene group having 6 to 18 carbon atoms with at least one of -O-, -NH-, -S-, and -C(=O)-, and is particularly preferably the following group (AO5) or the following group (AO6).

[0059] [ka]

[0060] Group (AO5), R 1A and R 2A each independently represents a hydrogen atom or a methyl group, n represents an integer of 1 to 8 (preferably an integer of 1 to 4, more preferably 1 or 2), *1 represents the bonding position to the carbonyl carbon atom, and *2 represents the bonding position to a non-carbonyl carbon atom.

[0061] R 1A and R 2A When one of these is a methyl group, the other is preferably a hydrogen atom. group (AO6) medium, L 6 represents an alkylene group having 1 to 8 carbon atoms (preferably 1 to 4, more preferably 1 or 2), *1 represents the bonding position to the carbonyl carbon atom, and *2 represents the bonding position to the non-carbonyl carbon atom.

[0062] L 5 is preferably a single bond, -O-, the group (AO5), or the group (AO6), more preferably a single bond or -O-, and even more preferably -O-.

[0063] Specific examples of the structural unit represented by formula (A) are shown below, but the structural unit represented by formula (A) is not limited to the following specific examples.

[0064] [ka]

[0065] Specific examples of the structural unit represented by formula (B) are shown below, but the structural unit represented by formula (B) is not limited to the following specific examples.

[0066] [ka]

[0067] Specific examples of the structural unit represented by formula (C) are shown below, but the structural unit represented by formula (C) is not limited to the following specific examples.

[0068] [ka]

[0069] Specific examples of the structural unit represented by formula (D) are shown below, but the structural unit represented by formula (D) is not limited to the following specific examples.

[0070] [ka]

[0071] Specific examples of the structural unit represented by formula (E) are shown below, but the structural unit represented by formula (E) is not limited to the following specific examples.

[0072] [ka]

[0073] Specific examples of the structural unit represented by formula (F) are shown below, but the structural unit represented by formula (F) is not limited to the following specific examples.

[0074] [ka]

[0075] In the uncrosslinked polymer, the content of the structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure is preferably 35% by mass to 95% by mass, more preferably 50% by mass to 95% by mass, and further preferably 70% by mass to 90% by mass, based on the total amount of the uncrosslinked polymer.

[0076] Similarly, the content of the structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure in the crosslinked polymer is preferably 35% by mass to 95% by mass, more preferably 50% by mass to 95% by mass, and even more preferably 70% by mass to 90% by mass, based on the total amount of the crosslinked polymer (pigment dispersant).

[0077] In addition, the structural unit derived from a hydrophobic monomer may be a (meth)acrylate having an alkyl group having 1 to 20 carbon atoms. The alkyl group may be either linear or branched. Examples of the (meth)acrylate having an alkyl group having 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate.

[0078] The uncrosslinked polymer is preferably a random copolymer containing a structural unit derived from a carboxy group-containing monomer and a structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure, more preferably a random copolymer containing a structural unit derived from (meth)acrylic acid and a structural unit derived from a (meth)acrylate having an aromatic ring structure or an alicyclic structure, and particularly preferably a random copolymer containing a structural unit derived from (meth)acrylic acid and a structural unit derived from benzyl (meth)acrylate.

[0079] The acid value of the uncrosslinked polymer is preferably from 65 mgKOH / g to 220 mgKOH / g, and more preferably from 65 mgKOH / g to 170 mgKOH / g, from the viewpoint of pigment dispersibility.

[0080] In addition, the acid value of the crosslinked polymer is preferably 20 mgKOH / g to 205 mgKOH / g, more preferably 30 mgKOH / g to 180 mgKOH / g, and even more preferably 65 mgKOH / g to 140 mgKOH / g, from the viewpoint of suppressing cracking of the recorded image and improving the quality of the recorded image. When the acid value of the crosslinked polymer is 20 mgKOH / g or more, the quality of the recorded image is more excellent. When the acid value of the crosslinked polymer is 205 mgKOH / g or less, the cracking of the recorded image is further suppressed.

[0081] The weight average molecular weight (Mw) of the uncrosslinked polymer is not particularly limited, but from the viewpoint of pigment dispersibility, it is preferably from 3,000 to 300,000, more preferably from 5,000 to 200,000, and even more preferably from 7,000 to 100,000.

[0082] The preferred range of the weight average molecular weight of the crosslinked polymer is the same as the preferred range of the weight average molecular weight of the uncrosslinked polymer.

[0083] The crosslinking agent used when crosslinking the uncrosslinked polymer is preferably a compound having two or more reactive sites with the uncrosslinked polymer (e.g., a polymer having a carboxy group). Only one type of crosslinking agent may be used, or two or more types may be used.

[0084] A preferred combination of a crosslinking agent and an uncrosslinked polymer is a combination of a compound having two or more epoxy groups (i.e., a bifunctional or higher epoxy compound) and a polymer having a carboxy group. In this combination, a crosslinked structure is formed by the reaction between the epoxy group and the carboxy group. The formation of a crosslinked structure by the crosslinking agent is preferably carried out after the pigment is dispersed by the uncrosslinked polymer.

[0085] Examples of difunctional or higher functional epoxy compounds include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and trimethylolpropane triglycidyl ether.

[0086] Among these, the difunctional or higher epoxy compound is preferably polyethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, or trimethylolpropane triglycidyl ether.

[0087] The crosslinking agent may be a commercially available product. Commercially available products include, for example, Denacol EX-321, EX-821, EX-830, EX-850 and EX-851 (manufactured by Nagase ChemteX Corporation).

[0088] The molar ratio of the reactive site (e.g., epoxy group) in the crosslinking agent to the reactive site (e.g., carboxy group) in the uncrosslinked polymer is preferably 1:1.1 to 1:10, more preferably 1:1.1 to 1:5, and even more preferably 1:1.1 to 1:3, from the viewpoints of the crosslinking reaction rate and the dispersion stability after crosslinking.

[0089] -Block polymer- A block polymer, also known as a block copolymer, is a copolymer in which at least two polymers are bonded together in the molecule.

[0090] The block polymer preferably contains a structural unit derived from a hydrophobic monomer and a structural unit derived from a monomer containing an anionic group (hereinafter, "anionic group-containing monomer").

[0091] The structural unit derived from the hydrophobic monomer contained in the block polymer may be of only one type or of two or more types. The structural unit derived from the anionic group-containing monomer contained in the block polymer may be of only one type or of two or more types.

[0092] Examples of the structural unit derived from a hydrophobic monomer include an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure, and a (meth)acrylate having an alkyl group having 1 to 20 carbon atoms.

[0093] The content of the structural unit derived from the hydrophobic monomer is preferably 35% by mass to 95% by mass, more preferably 50% by mass to 95% by mass, and further preferably 70% by mass to 90% by mass, based on the total amount of the block polymer.

[0094] From the viewpoint of adsorption to the pigment, the hydrophobic monomer preferably contains an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure, more preferably contains an ethylenically unsaturated compound having an alicyclic structure, and even more preferably contains an ethylenically unsaturated compound having an alicyclic structure having 6 or more carbon atoms.

[0095] The structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure is preferably at least one selected from the group consisting of structural units represented by formulas (A) to (F) described in the section on the crosslinked polymer above.

[0096] The content of the structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure is preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, even more preferably 30% by mass to 70% by mass, and still more preferably 30% by mass to 60% by mass, based on the total amount of the block polymer.

[0097] It is also preferable that the structural unit derived from a hydrophobic monomer contains a (meth)acrylate having an alkyl group having a carbon number of 1 to 20. The alkyl group may be either linear or branched.

[0098] Examples of (meth)acrylates having an alkyl group having 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate.

[0099] The content of the structural unit derived from a (meth)acrylate having an alkyl group having 1 to 20 carbon atoms is preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, even more preferably 30% by mass to 70% by mass, and particularly preferably 40% by mass to 60% by mass, based on the total amount of the block polymer.

[0100] In the structural unit derived from an anionic group-containing monomer, examples of the anionic group include a carboxy group, a salt of a carboxy group, a sulfo group, a salt of a sulfo group, a phosphoric acid group, a salt of a phosphoric acid group, a phosphonic acid group, and a salt of a phosphonic acid group.

[0101] Examples of counter ions in salts include alkali metal ions such as sodium ion, potassium ion, and lithium ion; alkaline earth metal ions such as calcium ion and magnesium ion; and ammonium ion.

[0102] Among them, the anionic group is preferably a carboxy group or a salt of a carboxy group. Examples of the anionic group-containing monomer include (meth)acrylic acid, β-carboxyethyl acrylate, fumaric acid, itaconic acid, maleic acid, and crotonic acid. Among them, the anionic group-containing monomer is preferably (meth)acrylic acid.

[0103] The content of the structural unit derived from the anionic group-containing monomer is preferably 1 mass % to 30 mass %, more preferably 2 mass % to 25 mass %, and further preferably 3 mass % to 20 mass %, based on the total amount of the block polymer.

[0104] Whether or not the polymer contained in the ink is a block polymer can be determined, for example, by the following method. First, the ink is subjected to a separation method such as solvent extraction to separate the polymer. The separated polymer is analyzed using various analytical methods such as nuclear magnetic resonance (NMR), infrared spectroscopy (IR), and thermal analysis, and physical properties such as the glass transition temperature are measured, allowing a comprehensive determination as to whether or not it is a block polymer.

[0105] From the viewpoint of suppressing cracking of the recorded image and improving the quality of the recorded image, the acid value of the block polymer is preferably 30 mgKOH / g to 170 mgKOH / g, more preferably 60 mgKOH / g to 150 mgKOH / g, and even more preferably 80 mgKOH / g to 120 mgKOH / g. When the acid value of the block polymer is 30 mgKOH / g or more, the quality of the recorded image is more excellent. Also, when the acid value of the block polymer is 170 mgKOH / g or less, the cracking of the recorded image is further suppressed.

[0106] The weight average molecular weight (Mw) of the block polymer is not particularly limited, but from the viewpoint of pigment dispersibility, it is preferably from 3,000 to 100,000, more preferably from 5,000 to 80,000, and even more preferably from 10,000 to 60,000.

[0107] It is believed that the pigment dispersant is present in the ink by being partially adsorbed onto the surface of the pigment and partially detached from the surface of the pigment. In the present disclosure, the pigment dispersant contained in the colored ink is preferably a crosslinked polymer. It is believed that the pigment dispersant is less likely to detach from the surface of the colored pigment because the pigment dispersant is a polymer having a crosslinked structure. As a result, when the colored ink is applied to a substrate to which a pretreatment liquid has been applied, aggregation with the aggregating agent contained in the pretreatment liquid is more uniform, and cracking of the recorded image is more suppressed.

[0108] The mixing ratio of the color pigment to the pigment dispersant is preferably from 1:0.06 to 1:3, more preferably from 1:0.125 to 1:2, and even more preferably from 1:0.125 to 1:1.5, on a mass basis.

[0109] As a dispersing device for dispersing the pigment, a known dispersing device can be used, and examples thereof include a ball mill, a sand mill, a bead mill, a roll mill, a jet mill, a paint shaker, an attritor, an ultrasonic disperser, and a disperser.

[0110] (water) In the present disclosure, the color ink contains water. The amount of water contained is not particularly limited, and is, for example, 40% by mass to 70% by mass.

[0111] (Resin particles) In the present disclosure, the color ink preferably contains at least one type of resin particles from the viewpoint of obtaining scratch resistance of the image. The color ink preferably contains resin particles, which are particles made of a resin, in addition to the pigment dispersant.

[0112] When a color ink is applied onto a substrate to which a pretreatment liquid has been applied, the coagulant contained in the pretreatment liquid comes into contact with the resin particles contained in the color ink, destabilizing the dispersion of the resin particles and increasing the viscosity of the color ink, which causes the color ink to be fixed onto the substrate and improves the quality of the recorded image.

[0113] The resin constituting the resin particles is preferably a water-insoluble polymer. The term "water-insoluble" in the context of a water-insoluble polymer means that the amount of the polymer that dissolves in 100 g of distilled water at 25° C. is less than 2 g.

[0114] The resin particles preferably contain at least one of particles made of acrylic resin (hereinafter referred to as "acrylic resin particles") and particles made of urethane resin (hereinafter also referred to as "urethane resin particles"), and preferably contain acrylic resin particles.

[0115] The resin particles are preferably self-dispersing resin particles. Examples of the self-dispersing resin particles include the resin particles described in paragraphs 0062 to 0076 of JP2016-188345A and paragraphs 0109 to 0140 of WO2013 / 180074A.

[0116] The resin in the resin particles is preferably an acrylic resin containing a structural unit derived from a (meth)acrylate having an aromatic ring structure or an alicyclic structure, a structural unit derived from (meth)acrylic acid, and a structural unit derived from an alkyl (meth)acrylate containing an alkyl group having 1 to 4 carbon atoms.

[0117] The (meth)acrylate having an alicyclic structure is preferably an alkyl (meth)acrylate having a cycloalkyl group having 3 to 10 carbon atoms, and is preferably at least one selected from the group consisting of cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, and dicyclopentanyl (meth)acrylate, and more preferably at least one selected from the group consisting of isobornyl (meth)acrylate, adamantyl (meth)acrylate, and dicyclopentanyl (meth)acrylate. The (meth)acrylate having an aromatic ring structure is preferably phenoxyethyl (meth)acrylate or benzyl (meth)acrylate.

[0118] Examples of the resin in the resin particles include phenoxyethyl acrylate / methyl methacrylate / acrylic acid copolymer (50 / 45 / 5), phenoxyethyl acrylate / benzyl methacrylate / isobutyl methacrylate / methacrylic acid copolymer (30 / 35 / 29 / 6), phenoxyethyl methacrylate / isobutyl methacrylate / methacrylic acid copolymer (50 / 44 / 6), phenoxyethyl acrylate / methyl methacrylate / ethyl acrylate / acrylic acid copolymer (30 / 55 / 10 / 5), benzyl methacrylate acrylate / isobutyl methacrylate / methacrylic acid copolymer (35 / 59 / 6), styrene / phenoxyethyl acrylate / methyl methacrylate / acrylic acid copolymer (10 / 50 / 35 / 5), benzyl acrylate / methyl methacrylate / acrylic acid copolymer (55 / 40 / 5), phenoxyethyl methacrylate / benzyl acrylate / methacrylic acid copolymer (45 / 47 / 8), styrene / phenoxyethyl acrylate / butyl methacrylate / acrylic acid copolymer (5 / 48 / 40 / 7), benzyl methacrylate / isobutyl methacrylate / methacrylic acid copolymer (35 / 59 / 6), styrene / phenoxyethyl acrylate / methyl methacrylate / acrylic acid copolymer (10 / 50 / 35 / 5), benzyl acrylate / methyl methacrylate / acrylic acid copolymer (55 / 40 / 5), phenoxyethyl methacrylate / benzyl acrylate / methacrylic acid copolymer (45 / 47 / 8), styrene / phenoxyethyl acrylate / butyl methacrylate / acrylic acid copolymer (5 / 48 / 40 / 7), ethyl methacrylate / cyclohexyl methacrylate / methacrylic acid copolymer (35 / 30 / 30 / 5), phenoxyethyl acrylate / methyl methacrylate / butyl acrylate / methacrylic acid copolymer (12 / 50 / 30 / 8), benzyl acrylate / isobutyl methacrylate / acrylic acid copolymer (93 / 2 / 5), methyl methacrylate / methoxyethyl acrylate / benzyl methacrylate / acrylic acid copolymer (44 / 15 / 35 / 6), styrene / butyl acrylate / acrylic acid copolymer (62 / 35 / 3), methyl methyl methacrylate / phenoxyethyl acrylate / acrylic acid copolymer (45 / 51 / 4), methyl methacrylate / isobornyl methacrylate / methacrylic acid copolymer (20 / 72 / 8), methyl methacrylate / isobornyl methacrylate / methacrylic acid copolymer (40 / 52 / 8), methyl methacrylate / isobornyl methacrylate / methacrylic acid copolymer (48 / 42 / 10), methyl methacrylate / isobornyl methacrylate / dicyclopentanyl methacrylate / methacrylic acid copolymer (20 / 62 / 10 / 8),Examples include methyl methacrylate / dicyclopentanyl methacrylate / methacrylic acid copolymer (20 / 72 / 8) and methyl methacrylate / isobornyl methacrylate / methacrylic acid / sodium methacrylate (70 / 20 / 5 / 5). The ratio in parentheses indicates the mass ratio of structural units derived from the monomers.

[0119] The acid value of the resin in the resin particles is preferably 25 mgKOH / g to 100 mgKOH / g, more preferably 30 mgKOH / g to 90 mgKOH / g, and further preferably 35 mgKOH / g to 80 mgKOH / g.

[0120] The weight average molecular weight of the resin in the resin particles is preferably from 1,000 to 300,000, more preferably from 2,000 to 200,000, and further preferably from 5,000 to 100,000.

[0121] From the viewpoint of ejection stability, the average particle diameter of the resin particles is preferably 1 nm to 200 nm, more preferably 3 nm to 200 nm, and even more preferably 5 nm to 50 nm. The average particle diameter of the resin particles is determined by measuring the volume average particle diameter by a dynamic light scattering method using a particle size distribution measuring device, for example, a product name "Nanotrac UPA-EX150" manufactured by Nikkiso Co., Ltd.

[0122] When the color ink contains resin particles, the content of the resin particles is preferably 0.1% by mass to 15% by mass, more preferably 0.5% by mass to 10% by mass, even more preferably 1% by mass to 8% by mass, and even more preferably 2% by mass to 5% by mass, relative to the total amount of the color ink.

[0123] (Organic solvent) From the viewpoint of improving ejection stability, the color ink preferably contains at least one type of organic solvent.

[0124] Examples of organic solvents include glycerin, 1,2,6-hexanetriol, trimethylolpropane, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, and alkanediols (polyhydric alcohols) such as 1,3-butanediol and 2,3-butanediol; Alkyl alcohols with 1 to 4 carbon atoms, such as ethanol, methanol, butanol, propanol, and isopropanol; Examples of glycol ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, ethylene glycol mono-iso-propyl ether, diethylene glycol mono-iso-propyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-t-butyl ether, diethylene glycol mono-t-butyl ether, triethylene glycol monoethyl ether, 1-methyl-1-methoxybutanol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-t-butyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-iso-propyl ether, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-iso-propyl ether, and tripropylene glycol monomethyl ether.

[0125] The content of the organic solvent is preferably 5% by mass to 60% by mass, more preferably 10% by mass to 40% by mass, and further preferably 15% by mass to 30% by mass, based on the total amount of the color ink.

[0126] (Surfactant) The color ink may contain at least one type of surfactant from the viewpoint of improving ejection stability.

[0127] Examples of the surfactant include those described in JP-A-62-173463 and JP-A-62-183457. Examples of the surfactant include anionic surfactants such as dialkyl sulfosuccinate, alkyl naphthalene sulfonate, and fatty acid salt; nonionic surfactants such as polyoxyethylene alkyl ether, polyoxyethylene alkyl allyl ether, acetylene glycol, and polyoxyethylene-polyoxypropylene block copolymer; and cationic surfactants such as alkylamine salt and quaternary ammonium salt. The surfactant may be a fluorine-based surfactant or a silicone-based surfactant.

[0128] In the present disclosure, from the viewpoint of further suppressing cracking of a recorded image, the surfactant preferably includes a nonionic surfactant. In particular, the nonionic surfactant is preferably an acetylene glycol derivative (acetylene glycol-based surfactant).

[0129] Examples of acetylene glycol surfactants include 2,4,7,9-tetramethyl-5-decyne-4,7-diol and alkylene oxide adducts of 2,4,7,9-tetramethyl-5-decyne-4,7-diol. Commercially available products include E series such as Olfine E1010 and E1020 from Nissin Chemical Industry Co., Ltd.

[0130] The surfactant preferably contains a fluorine-based surfactant. Commercially available products include Capstone FS-63, Capstone FS-61 (manufactured by Dupont), Ftergent 100, Ftergent 110, Ftergent 150 (manufactured by Neos Co., Ltd.), and CHEMGUARD S-760P (manufactured by Chemguard Inc.).

[0131] The content of the surfactant is preferably from 0.01% by mass to 4.0% by mass, more preferably from 0.5% by mass to 3.0% by mass, and even more preferably from 1.2% by mass to 2.0% by mass, based on the total amount of the color ink.

[0132] The surfactant preferably contains an acetylene glycol surfactant and a fluorine-based surfactant. The content of the acetylene glycol surfactant is preferably 0.01% by mass to 3.0% by mass, more preferably 0.1% by mass to 2.0% by mass, and even more preferably 0.8% by mass to 1.5% by mass, based on the total amount of the color ink. The content of the fluorine-based surfactant is preferably 0.01% by mass to 1.0% by mass, more preferably 0.05% by mass to 0.7% by mass, and even more preferably 0.1% by mass to 0.3% by mass, based on the total amount of the color ink.

[0133] (Additives) The color ink may contain additives such as a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, a conductive salt, and a basic compound, as necessary.

[0134] (Physical Properties) From the viewpoint of improving ejection stability, the pH of the color ink is preferably 7 to 10, and more preferably 7.5 to 9.5. The pH is measured at 25° C. using a pH meter, for example, a pH meter manufactured by Toa DKK Corporation (model number "HM-31").

[0135] The viscosity of the color ink is preferably 0.5 mPa·s to 30 mPa·s, more preferably 2 mPa·s to 20 mPa·s, preferably 2 mPa·s to 15 mPa·s, and even more preferably 3 mPa·s to 10 mPa·s. The viscosity is measured at 25°C using a viscometer, for example, a TV-22 viscometer manufactured by Toki Sangyo Co., Ltd.

[0136] The surface tension of the color ink is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The surface tension is measured at 25° C. using a surface tensiometer, for example, an automatic surface tensiometer (product name "CBVP-Z") manufactured by Kyowa Interface Science Co., Ltd., by the plate method.

[0137] <White ink> In the present disclosure, the white ink includes a white pigment, a pigment dispersant, and water.

[0138] (White pigment) The white pigment may be any pigment that exhibits white color, and the type is not particularly limited. Examples of the white pigment include titanium oxide, strontium titanate, barium titanate, zinc oxide, magnesium oxide, zirconium oxide, aluminum oxide, barium sulfate, silica, talc, mica, aluminum hydroxide, calcium silicate, aluminum silicate, and zinc sulfide. The white pigment is preferably a particle having titanium atoms, and more preferably titanium oxide.

[0139] The average particle size of the white pigment is preferably 10 nm to 550 nm, more preferably 100 nm to 450 nm, and even more preferably 150 nm to 400 nm. When the average particle size is 550 nm or less, the color reproducibility is good, and further, when an image is recorded using an inkjet recording method, the ejection stability is good. On the other hand, when the average particle size is 10 nm or more, the light resistance is good. In addition, the particle size distribution of the pigment may be either a wide particle size distribution or a monodisperse particle size distribution. The average particle size and particle size distribution of the pigment are obtained by measuring the volume average particle size by a dynamic light scattering method using a particle size distribution measuring device, for example, a product name "Nanotrac UPA-EX150" manufactured by Nikkiso Co., Ltd. In addition, when the pigment is covered with a pigment dispersant, the average particle size of the pigment means the average particle size of the pigment covered with the pigment dispersant.

[0140] From the viewpoints of image density and ejection stability, the content of the white pigment is preferably 5% by mass to 20% by mass, and more preferably 8% by mass to 15% by mass, relative to the total amount of the color ink.

[0141] (Pigment dispersant) The white ink of the present disclosure includes a pigment dispersant.

[0142] The acid value of the pigment dispersant contained in the white ink is preferably 30 mgKOH / g to 170 mgKOH / g, more preferably 60 mgKOH / g to 150 mgKOH / g, and even more preferably 80 mgKOH / g to 120 mgKOH / g. When the acid value of the pigment dispersant is 30 mgKOH / g or more, the image quality of the recorded image is more excellent. Also, when the acid value of the pigment dispersant is 170 mgKOH / g or less, the cracking of the recorded image is further suppressed.

[0143] The pigment dispersant contains a polymer having a crosslinked structure or a block polymer. Preferred aspects of the polymer having a crosslinked structure and the block polymer contained in the white ink are the same as the preferred aspects of the polymer having a crosslinked structure and the block polymer contained in the colored inks.

[0144] However, in the white ink of the present disclosure, when the pigment dispersant is a block polymer, the acid value of the block polymer is preferably 30 mgKOH / g to 170 mgKOH / g, more preferably 60 mgKOH / g to 150 mgKOH / g, and even more preferably 80 mgKOH / g to 120 mgKOH / g. When the acid value of the block polymer is 30 mgKOH / g or more, the image quality of the recorded image is more excellent. Also, when the acid value of the block polymer is 170 mgKOH / g or less, cracking of the recorded image is further suppressed.

[0145] In the white ink of the present disclosure, when the pigment dispersant is a crosslinked polymer, the acid value of the crosslinked polymer is preferably 45 mgKOH / g to 160 mgKOH / g, more preferably 70 mgKOH / g to 135 mgKOH / g, and even more preferably 95 mgKOH / g to 105 mgKOH / g. When the acid value of the crosslinked polymer is 45 mgKOH / g or more, the image quality of the recorded image is more excellent. In addition, when the acid value of the crosslinked polymer is 160 mgKOH / g or less, the cracking of the recorded image is further suppressed.

[0146] In the present disclosure, the pigment dispersant contained in the white ink is preferably a block polymer. It is believed that the pigment dispersant being a block polymer makes it difficult for the pigment dispersant to detach from the surface of the white pigment. As a result, when the white ink is applied to a substrate to which a pretreatment liquid has been applied, aggregation with the aggregating agent contained in the pretreatment liquid is more uniform, and cracking of the recorded image is more suppressed.

[0147] The mixing ratio of the white pigment to the pigment dispersant is preferably from 1:0.06 to 1:3, more preferably from 1:0.125 to 1:2, and even more preferably from 1:0.125 to 1:1.5, on a mass basis.

[0148] (water) In the present disclosure, the white ink contains water. The amount of water contained is not particularly limited, and is, for example, 40% by mass to 70% by mass.

[0149] (Resin particles) In the present disclosure, the white ink preferably contains at least one type of resin particles from the viewpoint of obtaining scratch resistance of the image. The white ink preferably contains resin particles, which are particles made of a resin, in addition to the pigment dispersant.

[0150] When white ink is applied onto a substrate to which a pretreatment liquid has been applied, the coagulant contained in the pretreatment liquid comes into contact with the resin particles contained in the white ink, destabilizing the dispersion of the resin particles and increasing the viscosity of the white ink, which causes the white ink to be fixed onto the substrate and improves the quality of the recorded image.

[0151] The preferred embodiments of the resin particles contained in the white ink are the same as the preferred embodiments of the resin particles contained in the color inks.

[0152] When the white ink contains resin particles, the content of the resin particles is preferably 0.1% by mass to 15% by mass, more preferably 0.5% by mass to 10% by mass, even more preferably 1% by mass to 8% by mass, and even more preferably 2% by mass to 6% by mass, relative to the total amount of the white ink.

[0153] (Organic solvent) From the viewpoint of improving ejection stability, the white ink preferably contains at least one type of organic solvent.

[0154] The preferred embodiments of the organic solvent contained in the white ink are the same as the preferred embodiments of the organic solvent contained in the color inks.

[0155] The content of the organic solvent is preferably 5% by mass to 60% by mass, more preferably 10% by mass to 40% by mass, and further preferably 20% by mass to 35% by mass, based on the total amount of the white ink.

[0156] (Surfactant) The white ink may contain at least one type of surfactant from the viewpoint of improving ejection stability.

[0157] The preferred embodiments of the surfactant contained in the white ink are the same as the preferred embodiments of the surfactant contained in the color inks.

[0158] The content of the surfactant is preferably 0.01% by mass to 4.0% by mass, more preferably 0.1% by mass to 3.0% by mass, and even more preferably 1.0% by mass to 1.8% by mass, based on the total amount of the white ink. The content of the acetylene glycol surfactant is preferably 0.01% by mass to 3.0% by mass, more preferably 0.1% by mass to 2.0% by mass, and even more preferably 0.8% by mass to 1.5% by mass, based on the total amount of the white ink. The content of the fluorine-based surfactant is preferably 0.01% by mass to 1.0% by mass, more preferably 0.05% by mass to 0.7% by mass, and even more preferably 0.1% by mass to 0.3% by mass, based on the total amount of the white ink.

[0159] (Additives) The white ink may contain additives such as a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, a conductive salt, and a basic compound, as necessary.

[0160] (Physical Properties) From the viewpoint of improving ejection stability, the pH of the white ink is preferably 7 to 10, and more preferably 7.5 to 9.5. The pH is measured at 25° C. using a pH meter, for example, a pH meter manufactured by Toa DKK Corporation (model number "HM-31").

[0161] The viscosity of the white ink is preferably 0.5 mPa·s to 30 mPa·s, more preferably 2 mPa·s to 20 mPa·s, preferably 2 mPa·s to 15 mPa·s, and even more preferably 3 mPa·s to 10 mPa·s. The viscosity is measured at 25°C using a viscometer, for example, a TV-22 viscometer manufactured by Toki Sangyo Co., Ltd.

[0162] The surface tension of the white ink is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The surface tension is measured at 25° C. using a surface tensiometer, for example, an automatic surface tensiometer (product name "CBVP-Z") manufactured by Kyowa Interface Science Co., Ltd., by the plate method.

[0163] The absolute value of the difference between the surface tension of the color ink and the surface tension of the white ink is preferably 0.01 mN / m to 15.0 mN / m, more preferably 0.05 mN / m to 10.0 mN / m, and even more preferably 3.5 mN / m to 7.0 mN / m. If the absolute value of the difference is 0.01 mN / m or more, cracking of the recorded image is further suppressed. Also, if the absolute value of the difference is 15.0 mN / m or less, the image quality of the recorded image is more excellent.

[0164] The ink set of the present disclosure may further include a pretreatment liquid containing a flocculant, in addition to the color inks and the white ink.

[0165] (Flocculant) The flocculant is preferably at least one selected from the group consisting of polyvalent metal compounds, organic acids, metal complexes, and cationic polymers, and more preferably contains an organic acid.

[0166] -Polyvalent metal compounds- Polyvalent metal compounds include salts of alkaline earth metals of Group 2 of the periodic table (e.g., magnesium, calcium), transition metals of Group 3 of the periodic table (e.g., lanthanum), metals of Group 13 of the periodic table (e.g., aluminum), and the lanthanides (e.g., neodymium).

[0167] The salts of these metals are preferably salts of organic acids, nitrates, chlorides, or thiocyanates, as described below.

[0168] Among them, the polyvalent metal compound is preferably a calcium salt or magnesium salt of an organic acid (e.g., formic acid, acetic acid, benzoic acid, etc.); a calcium salt or magnesium salt of nitric acid; calcium chloride, magnesium chloride, or a calcium salt or magnesium salt of thiocyanic acid.

[0169] The polyvalent metal compound is preferably at least partially dissociated into polyvalent metal ions and counter ions in the pretreatment liquid.

[0170] -Organic acid- The organic acid includes an organic compound having an acidic group.

[0171] Acidic groups include phosphate groups, phosphonate groups, phosphinate groups, sulfate groups, sulfonate groups, sulfinate groups, and carboxy groups.

[0172] Among these, from the viewpoint of the aggregation speed of the ink, the acidic group is preferably a phosphoric acid group or a carboxy group, and more preferably a carboxy group.

[0173] It is preferable that the acidic groups are at least partially dissociated in the pretreatment liquid.

[0174] Examples of organic compounds having a carboxy group include (meth)acrylic acid, poly(meth)acrylic acid, acetic acid, formic acid, benzoic acid, glycolic acid, malonic acid, malic acid (preferably DL-malic acid), maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, citric acid, tartaric acid, phthalic acid, 4-methylphthalic acid, lactic acid, pyrrolidone carboxylic acid, pyrone carboxylic acid, pyrrole carboxylic acid, furan carboxylic acid, pyridine carboxylic acid, coumaric acid, thiophene carboxylic acid, and nicotinic acid.

[0175] Among these, from the viewpoint of the aggregation speed of the ink, the organic compound having a carboxy group is preferably a divalent or higher carboxylic acid (hereinafter also referred to as a polyvalent carboxylic acid), and more preferably a dicarboxylic acid.

[0176] Specifically, the polycarboxylic acid is preferably malonic acid, malic acid, maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, tartaric acid, 4-methylphthalic acid, or citric acid, and more preferably malonic acid, malic acid, tartaric acid, succinic acid, glutaric acid, pimelic acid, adipic acid, or citric acid.

[0177] The organic acid preferably has a low pKa (for example, 1.0 to 5.0), which reduces the surface charge of particles such as pigments and resin particles in the ink, which are stabilized in dispersion by weakly acidic functional groups such as carboxy groups, by contacting the particles with an organic acid having a lower pKa, thereby decreasing the dispersion stability.

[0178] The organic acid preferably has a low pKa, high solubility in water, and a valence of at least 2. Furthermore, it is more preferable that the organic acid has a high buffering capacity in a pH range lower than the pKa of the functional group (e.g., carboxy group) that stabilizes the dispersion of the particles in the ink.

[0179] -Metal complexes- The metal complex preferably contains, as a metal element, at least one selected from the group consisting of zirconium, aluminum, and titanium.

[0180] The metal complex is preferably a metal complex containing, as a ligand, at least one selected from the group consisting of acetate, acetylacetonate, methyl acetoacetate, ethyl acetoacetate, octylene glycolate, butoxyacetylacetonate, lactate, lactate ammonium salt, and triethanolamine.

[0181] The metal complex may be a commercially available product. Various organic ligands, particularly various polydentate ligands capable of forming metal chelate catalysts, are commercially available. Therefore, the metal complex may be a metal complex prepared by combining a commercially available organic ligand with a metal.

[0182] Examples of the metal complex include zirconium tetraacetylacetonate (e.g., "Orgatix ZC-150" manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium monoacetylacetonate (e.g., "Orgatix ZC-540" manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium bisacetylacetonate (e.g., "Orgatix ZC-550" manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium monoethylacetoacetate (e.g., "Orgatix ZC-560" manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium acetate (e.g., "Orgatix ZC-115" manufactured by Matsumoto Fine Chemical Co., Ltd.), and titanium diisopropoxybis(acetylacetonate) (e.g., "Orgatix ZC-550" manufactured by Matsumoto Fine Chemical Co., Ltd.). TC-100"), titanium tetraacetylacetonate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatics TC-401"), titanium dioctyloxybis(octylene glycolate) (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatics TC-200"), titanium diisopropoxybis(ethylacetoacetate) (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatics TC-750"), zirconium tetraacetylacetonate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatics ZC-700"), zirconium tributoxymonoacetylacetonate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatics ZC-540"), zirconium monobutoxyacetylacetonate bis(ethylacetoacetate) (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatics Zirconium dibutoxy bis(ethylacetoacetate) (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix ZC-580"), aluminum trisacetylacetonate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix AL-80"), titanium lactate ammonium salt (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix TC-300"), titanium lactate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix TC-310, 315"), titanium triethanolamine (Matsumoto Fine Chemical Co., Ltd.'s "OrgatixTC-400"), and zirconyl chloride compounds (for example, Orgatix ZC-126 manufactured by Matsumoto Fine Chemical Co., Ltd.).

[0183] Among them, the metal complex is preferably a titanium lactate ammonium salt (e.g., "Orgatix TC-300" manufactured by Matsumoto Fine Chemical Co., Ltd.), a titanium lactate (e.g., "Orgatix TC-310, 315" manufactured by Matsumoto Fine Chemical Co., Ltd.), a titanium triethanolamine (e.g., "Orgatix TC-400" manufactured by Matsumoto Fine Chemical Co., Ltd.), or a zirconyl chloride compound (e.g., "Orgatix ZC-126" manufactured by Matsumoto Fine Chemical Co., Ltd.).

[0184] -Cationic polymer- The pretreatment liquid may also be in a form containing one or more cationic polymers as an aggregating component. The cationic polymer is preferably a homopolymer of a cationic monomer having a primary to tertiary amino group or a quaternary ammonium salt group, or a copolymer or condensation polymer of a cationic monomer and a non-cationic monomer. The cationic polymer may be used in the form of either a water-soluble polymer or a water-dispersible latex particle. Examples of the cationic polymer include polyvinylpyridine salts, polyalkylaminoethyl acrylates, polyalkylaminoethyl methacrylates, polyvinylimidazoles, polyethyleneimines, polybiguanides, polyguanides, polyallylamine, and derivatives thereof.

[0185] The weight-average molecular weight of the cationic polymer is preferably small from the viewpoint of viscosity of the pretreatment liquid. When the pretreatment liquid is applied to a recording medium by an inkjet recording method, the weight-average molecular weight is preferably 1,000 to 500,000, more preferably 1,500 to 200,000, and even more preferably 2,000 to 100,000. A weight-average molecular weight of 1000 or more is advantageous from the viewpoint of aggregation speed. A weight-average molecular weight of 500,000 or less is advantageous from the viewpoint of ejection reliability. However, this does not apply when the pretreatment liquid is applied to a recording medium by a method other than the inkjet recording method.

[0186] The pretreatment liquid according to the present disclosure may contain only one type of flocculant, or may contain two or more types of flocculants.

[0187] The content of the flocculant is preferably 0.1% by mass to 40% by mass, more preferably 0.1% by mass to 30% by mass, even more preferably 1% by mass to 20% by mass, and particularly preferably 1% by mass to 10% by mass, relative to the total amount of the pretreatment liquid.

[0188] (Other Ingredients) The pretreatment liquid may contain other components other than the flocculant as necessary. Examples of other components that may be contained in the pretreatment liquid include known additives such as organic solvents, resin particles, surfactants, solid wetting agents, colloidal silica, inorganic salts, anti-fading agents, emulsion stabilizers, penetration enhancers, UV absorbers, preservatives, antifungal agents, pH adjusters, viscosity adjusters, rust inhibitors, chelating agents, and water-soluble polymer compounds (for example, the water-soluble polymer compounds described in paragraphs 0026 to 0080 of JP2013-001854A).

[0189] (Physical Properties) From the viewpoint of the ink aggregation speed, the pH of the pretreatment liquid is preferably 0.1 to 4.5, and more preferably 0.2 to 4.0. The pH is measured at 25° C. using a pH meter, for example, a pH meter manufactured by Toa DKK Corporation (model number "HM-31").

[0190] From the viewpoint of the ink aggregation speed, the viscosity of the pretreatment liquid is preferably 0.5 mPa·s to 10 mPa·s, and more preferably 1 mPa·s to 5 mPa·s. The viscosity is a value measured at 25°C using a viscometer. The viscosity is measured at 25°C using a viscometer, for example, a TV-22 type viscometer manufactured by Toki Sangyo Co., Ltd.

[0191] The surface tension of the pretreatment liquid is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The surface tension is a value measured at a temperature of 25° C. The surface tension is measured at 25° C. using a surface tensiometer, for example, an automatic surface tensiometer (product name "CBVP-Z") manufactured by Kyowa Interface Science Co., Ltd., by a plate method.

[0192] The absolute value of the difference between the surface tension of the pretreatment liquid and the surface tension of the color ink is preferably 0.05 mN / m to 10.0 mN / m. The absolute value of the difference between the surface tension of the pretreatment liquid and the surface tension of the white ink is preferably 0.05 mN / m to 10.0 mN / m. When the absolute value of the difference is 0.05 mN / m or more, cracking of the recorded image is further suppressed. When the absolute value of the difference is 10.0 mN / m or less, the image quality of the recorded image is more excellent.

[0193] [Image recording method] The image recording method of the present disclosure includes a pretreatment liquid applying step of applying a pretreatment liquid onto a non-permeable substrate, and an ink applying step of applying the color inks and the white ink by an inkjet recording method onto the non-permeable substrate to which the pretreatment liquid has been applied.

[0194] (Pretreatment liquid application step) The pretreatment liquid can be applied by a known application method such as a coating method, an inkjet recording method, or a dipping method in the pretreatment liquid application step.

[0195] Examples of the coating method include known coating methods using a bar coater, an extrusion die coater, an air doctor coater, a blade coater, a rod coater, a knife coater, a squeeze coater, a reverse roll coater, and the like.

[0196] Details of the inkjet recording method are the same as those of the inkjet recording method in the ink application step described below.

[0197] The amount of pretreatment liquid applied was 0.5 g / m 2 ~2.5g / m 2 It is preferable that the thickness is 1.0 g / m 2 ~2.0g / m 2 It is more preferable that:

[0198] The non-permeable substrate may be heated before the pretreatment liquid is applied. The heating temperature may be appropriately set depending on the type of non-permeable substrate and the composition of the pretreatment liquid, but the temperature of the non-permeable substrate is preferably 30°C to 70°C, and more preferably 30°C to 60°C.

[0199] The non-permeable substrate may be a non-permeable substrate that has been surface-treated in advance. Alternatively, a non-permeable substrate that has not been surface-treated may be used, and the surface of the non-permeable substrate may be treated before the application of the pretreatment liquid in the pretreatment application step. Examples of surface treatments include, but are not limited to, corona treatment, plasma treatment, frame treatment, heat treatment, abrasion treatment, light irradiation treatment (e.g., UV treatment), and flame treatment. Corona treatment may be performed using, for example, Corona Master (product name "PS-10S", manufactured by Shinko Electrical Instruments Co., Ltd.). Conditions for corona treatment may be appropriately selected depending on the type of non-permeable substrate, etc.

[0200] In the pretreatment liquid application step, the pretreatment liquid applied to the non-permeable substrate may be dried by heating. Examples of a means for drying the pretreatment liquid by heating include a known heating means such as a heater, a known air blowing means such as a dryer, and a combination of these.

[0201] Examples of methods for drying the pretreatment liquid by heating include a method of applying heat with a heater or the like from the side opposite to the side of the non-permeable substrate to which the pretreatment liquid has been applied, a method of applying warm or hot air to the side of the non-permeable substrate to which the pretreatment liquid has been applied, a method of applying heat with an infrared heater from the side of the non-permeable substrate to which the pretreatment liquid has been applied or the side opposite to the side to which the pretreatment liquid has been applied, and a combination of two or more of these methods.

[0202] The heating temperature during drying of the pretreatment liquid is preferably 35° C. or higher, and more preferably 40° C. or higher. There is no particular upper limit to the heating temperature, but it is preferably 100° C., more preferably 90° C., and even more preferably 70° C.

[0203] The time for heat drying is not particularly limited, but is preferably 0.5 seconds to 60 seconds, more preferably 0.5 seconds to 20 seconds, and even more preferably 0.5 seconds to 10 seconds.

[0204] (Ink application process) The ink application step is a step of applying color inks and white ink by an inkjet recording method onto a non-permeable substrate to which a pretreatment liquid has been applied. The color inks may be applied and then the white ink may be applied, or the color inks may be applied and then the white ink may be applied, onto a non-permeable substrate to which a pretreatment liquid has been applied. When the non-permeable substrate is transparent and used for reverse printing, it is preferable to apply the color inks and then the white ink onto a non-permeable substrate to which a pretreatment liquid has been applied. When applying the white ink after applying the color inks, it is preferable to apply the white ink onto a color ink film formed by applying the color inks.

[0205] The difference between the surface tension of the ink to be applied first onto the non-permeable substrate to which the pretreatment liquid has been applied and the surface tension of the pretreatment liquid is preferably 0.05 mN / m to 10 mN / m. For example, when a colored ink and a white ink are applied onto a non-permeable substrate to which the pretreatment liquid has been applied in the order of the colored ink and the white ink, the difference between the surface tension of the colored ink and the surface tension of the pretreatment liquid is preferably 0.05 mN / m to 10 mN / m. Furthermore, when the white ink and the colored ink are applied in the order of the white ink and the colored ink, the difference between the surface tension of the white ink and the surface tension of the pretreatment liquid is preferably 0.05 mN / m to 10 mN / m.

[0206] The ink ejection method in the inkjet recording method is not particularly limited, and may be any of the well-known methods, such as a charge control method that uses electrostatic attraction to eject ink, a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element, an acoustic inkjet method in which an electric signal is converted into an acoustic beam and irradiated onto the ink to eject ink using radiation pressure, and a thermal inkjet (Bubble Jet (registered trademark)) method in which ink is heated to form bubbles and the resulting pressure is utilized.

[0207] As the inkjet recording method, in particular, the method described in JP-A-54-59936 can be effectively used, in which ink subjected to the action of thermal energy undergoes a sudden volume change, and the ink is ejected from the nozzle by the action force caused by this state change. As the inkjet recording method, the method described in paragraphs 0093 to 0105 of JP-A-2003-306623 can also be applied.

[0208] Application of ink by inkjet recording onto the non-permeable substrate to which the pretreatment liquid has been applied is performed by ejecting the ink from the nozzles of an inkjet head.

[0209] Inkjet head methods include the shuttle method, in which a short serial head is scanned across the width of the recording medium to perform recording, and the line method, which uses a line head in which recording elements are arranged to cover the entire area of ​​one side of the recording medium.

[0210] In the line method, an image can be recorded on the entire surface of a recording medium by scanning the recording medium in a direction intersecting the arrangement direction of the recording elements. The line method does not require a transport system such as a carriage that scans a short head in the shuttle method. Furthermore, compared to the shuttle method, the line method does not require complex scanning control of the carriage movement and the recording medium, and only the recording medium moves. Therefore, the line method achieves faster image recording speeds than the shuttle method.

[0211] The ink is preferably applied using an inkjet head having a resolution of 300 dpi or more (more preferably 600 dpi or more, and even more preferably 800 dpi or more), where dpi is an abbreviation for dots per inch, and 1 inch is 2.54 cm.

[0212] The amount of ink droplets discharged from the nozzles of the inkjet head is preferably 1 pL (picoliter) to 10 pL, more preferably 1.5 pL to 6 pL, from the viewpoint of obtaining a high-definition image. Also, from the viewpoint of improving image unevenness and continuous gradation, it is effective to discharge a combination of different droplet amounts.

[0213] The total amount of the color ink and the white ink applied to the non-permeable substrate to which the pretreatment liquid was applied was 3.0 g / m 2 ~35.0g / m 2 It is preferable that the thickness is 9.0 g / m 2 ~25.0g / m 2 More preferably, it is 12.0 g / m 2 ~20.0g / m 2 It is more preferable that the total amount of application is 3.0 g / m 2When the total amount of the toner applied is 35.0 g / m or more, the image quality of the recorded image is superior. 2 When it is equal to or less than this, cracking of the recorded image is further suppressed, and the image quality of the recorded image is further improved.

[0214] In the ink application step, the ratio of the total amount of color pigment and white pigment applied to the amount of aggregating agent applied is, by mass, preferably 5 to 400, more preferably 20 to 300, and even more preferably 50 to 150. When the ratio is 5 or more, cracking of the recorded image is further suppressed. Also, when the ratio is 400 or less, the image quality of the recorded image is superior.

[0215] Here, the amount of the flocculant and the total amount of the color pigment and the white pigment are set to 1000g per 1 m2 of area. 2 Mass per unit (g / m 2 )

[0216] The amount of flocculant applied was determined based on the amount of pretreatment liquid applied (g / m 2 ) and the content (mass %) of the flocculant contained in the pretreatment liquid, and can be adjusted by adjusting at least one of them.

[0217] The amount of color pigment applied is the amount of color pigment applied (g / m 2 ) and the content (mass %) of the color pigment contained in the color ink, and can be adjusted by adjusting at least one of them.

[0218] The amount of white pigment applied is the amount of white ink applied (g / m 2 ) and the content (mass %) of the color pigment contained in the white ink, and can be adjusted by adjusting at least one of them.

[0219] (Other processes) The image recording method of the present disclosure may have, after the ink application step, a drying step of heating and drying the applied ink.

[0220] Means for heating and drying the ink include known heating means such as a heater, known air blowing means such as a dryer, and a combination of these.

[0221] Methods for heating and drying the ink include, for example, a method of applying heat using a heater or the like from the side opposite to the ink-applied side of the non-permeable substrate, a method of applying warm or hot air to the ink-applied side of the non-permeable substrate, a method of applying heat using an infrared heater from the ink-applied side or the side opposite to the ink-applied side of the non-permeable substrate, and a combination of two or more of these methods.

[0222] The heating temperature during drying by heating is preferably 55° C. or higher, more preferably 60° C. or higher, and particularly preferably 65° C. or higher. There is no particular upper limit to the heating temperature, but it is, for example, 100° C., and preferably 90° C.

[0223] The time for heating and drying the ink is not particularly limited, but is preferably 3 to 60 seconds, more preferably 5 to 60 seconds, and particularly preferably 10 to 45 seconds.

[0224] In addition, the image recording method of the present disclosure may be a method including: a colored ink applying step of applying the colored ink onto a non-permeable substrate; and a white ink applying step of applying a white ink onto the colored ink film formed by applying the colored ink.

[0225] The details of the color ink application process and the white ink application process are similar to those of the ink application process described above, and therefore will not be described here.

[0226] The image recording method of the present disclosure may include a drying step of heating and drying the applied ink after the white ink application step. Details of the drying step are the same as those of the above-mentioned drying step, and therefore will not be described here. EXAMPLES

[0227] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples as long as it does not exceed the gist of the disclosure. In the examples, the surface tension was measured by the plate method using an automatic surface tensiometer (product name "CBVP-Z") manufactured by Kyowa Interface Science Co., Ltd. The acid value was measured by the method described in JIS K0070:1992.

[0228] <Examples 1 to 30, Comparative Examples 1 and 2> First, a magenta pigment dispersion and a white pigment dispersion were prepared, and various additives were added to the prepared magenta pigment dispersion and white pigment dispersion, respectively, to prepare a magenta ink and a white ink.

[0229] The pigment dispersants P1 to P4 and the pigment dispersants Q1 to Q8 used in the preparation of the magenta pigment dispersion and the white pigment dispersion were prepared by the following method.

[0230] (Pigment Dispersant P1) 965g of dipropylene glycol was added to a 5000mL three-neck flask equipped with a stirrer and a cooling tube, and heated to 85°C under a nitrogen atmosphere. 640g of benzyl methacrylate, 340g of methacrylic acid, and 19.94g of 2-mercaptopropionic acid were dissolved in 370.28g of dipropylene glycol to prepare solution I, and 17.69g of t-butylperoxy-2-ethylhexanoate (product name "Perbutyl O", NOF Chemicals) was dissolved in 221.17g of dipropylene glycol to prepare solution II. Solution I was added dropwise to the three-neck flask over 4 hours, and solution II was added dropwise over 5 hours. After the dropwise addition, the mixture was allowed to react for another 2 hours. The disappearance of the monomer was confirmed by 1H-NMR. The obtained reaction solution was heated to 70°C, and 248.02g of 50% by mass potassium hydroxide aqueous solution was added, followed by adding 107.48g of dipropylene glycol and 75.52g of pure water and stirring to obtain a 37% by mass solution of random polymer. This random polymer was designated as pigment dispersant P1. The structural units constituting the obtained random polymer were confirmed by 1H-NMR. In addition, the weight average molecular weight (Mw) was determined by GPC. The weight average molecular weight (Mw) of the obtained pigment dispersant P1 was 8400, and the acid value was 221.7mgKOH / g.

[0231] (Pigment Dispersant P2) Pigment dispersant P2 was obtained in the same manner as pigment dispersant P1, except that the amounts of benzyl methacrylate, methyl methacrylate, and methacrylic acid contained in solution I were changed. Specifically, it was prepared by dissolving 456 g of benzyl methacrylate, 329 g of methyl methacrylate, 215 g of methacrylic acid, and 19.94 g of 2-mercatopropionic acid in 370.28 g of dipropylene glycol. The obtained pigment dispersant P2 was a random polymer, had a weight average molecular weight (Mw) of 9000, and an acid value of 145.3 mgKOH / g.

[0232] (Pigment Dispersant P3) Pigment dispersant P3 was obtained in the same manner as pigment dispersant P1, except that the amounts of benzyl methacrylate, methyl methacrylate, and methacrylic acid contained in solution I were changed. Specifically, it was prepared by dissolving 838.9 g of benzyl methacrylate, 161.1 g of methacrylic acid, and 19.94 g of 2-mercaptopropionic acid in 370.28 g of dipropylene glycol. The obtained pigment dispersant P3 was a random polymer, had a weight average molecular weight (Mw) of 9200, and an acid value of 100.5 mgKOH / g.

[0233] (Pigment Dispersant P4) A 500 ml separable flask equipped with a reflux tube, a gas introduction device, a thermometer and a stirrer was charged with 198.2 parts by mass of diethylene glycol monobutyl ether (hereinafter abbreviated as "BC"), 1.0 part by mass of iodine, 3.7 parts by mass of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (hereinafter abbreviated as "V-70"), 107.8 parts by mass of tricyclodecyl methacrylate (trade name "FA-513M", Hitachi Chemical Co., Ltd., homopolymer Tg = 173 ° C., hereinafter abbreviated as "TCDMA"), 19.5 parts by mass of methacrylic acid (hereinafter abbreviated as "MAA"), and 0.17 parts by mass of diphenylmethane as a catalyst. The mixture was polymerized at 45 ° C. for 5 hours while flowing nitrogen, to obtain a solution of a random polymer. The polymerization rate (yield) of the random polymer calculated from the solid content of the solution was 96.2%. The Mn measured by GPC was 9,800. The solid content of the obtained random polymer solution was 41.4%. After cooling the random polymer solution, 66.1 parts by mass of BC was added to adjust the solid content to 33.3% by mass. This random polymer was used as pigment dispersant P4. The acid value of pigment dispersant P4 was 100 mg KOH / g.

[0234] (Pigment Dispersant Q1) In a 500 ml separable flask equipped with a reflux tube, a gas introduction device, a thermometer and a stirrer, 198.2 parts by mass of BC, 1.0 parts by mass of iodine, 3.7 parts by mass of V-70, 66.1 parts by mass of TCDMA, and 0.17 parts by mass of diphenylmethane as a catalyst were charged. The mixture was polymerized at 45° C. for 5 hours while flowing nitrogen, to obtain a solution of A polymer block. The polymerization rate (yield) of A polymer block calculated from the solid content of the solution was 96.2%. In addition, the number average molecular weight (Mn) measured using GPC was 4900, the molecular weight distribution (hereinafter abbreviated as "PDI") was 1.20, and the peak top molecular weight was 6000. Next, the polymerization temperature was lowered to 40° C., and 41.7 parts by mass of TCDMA, 19.5 parts by mass of MAA, and 1.2 parts by mass of V-70 were added to the obtained solution of A polymer block. Then, the mixture was polymerized for 4 hours, and then heated to 70° C. and polymerized for 1 hour to form a B polymer block, thereby obtaining a solution of an AB block copolymer. The solid content of the obtained AB block copolymer solution was 41.2%, and the polymerization rate of the B polymer block calculated from the solid content was almost 100%. After cooling the AB block copolymer solution, 66.1 parts by mass of BC was added to adjust the solid content to 33.3% by mass. This AB block copolymer was used as pigment dispersant Q1. The Mn of pigment dispersant Q1 was 9500 and the acid value was 100.0 mgKOH / g. The acid value was calculated by titration using a 0.1 mol / L potassium hydroxide solution containing ethanol and toluene as a solvent and phenolphthalein as an indicator.

[0235] (Pigment Dispersant Q2) Pigment dispersant Q2 was obtained in the same manner as pigment dispersant Q1, except that the amounts of TCDMA and MAA added to the solution of A polymer block were changed. Specifically, 47.2 parts by mass of TCDMA, 14.1 parts by mass of MAA, and 1.2 parts by mass of V-70 were added to the solution of A polymer block. Pigment dispersant Q2 was a block polymer, with Mn of 10,500 and acid value of 72 mgKOH / g.

[0236] (Pigment Dispersant Q3) Pigment dispersant Q3 was obtained in the same manner as pigment dispersant Q1, except that the amounts of TCDMA and MAA added to the solution of A polymer block were changed. Specifically, 54.4 parts by mass of TCDMA, 6.8 parts by mass of MAA, and 1.2 parts by mass of V-70 were added to the solution of A polymer block. Pigment dispersant Q3 was a block polymer, with Mn of 10,500 and acid value of 35 mgKOH / g.

[0237] (Pigment Dispersant Q4) Pigment dispersant Q4 was obtained in the same manner as pigment dispersant Q1, except that the amounts of TCDMA and MAA added to the solution of A polymer block were changed. Specifically, 38.6 parts by mass of TCDMA, 22.7 parts by mass of MAA, and 1.2 parts by mass of V-70 were added to the solution of A polymer block. Pigment dispersant Q4 was a block polymer, with an Mn of 10,500 and an acid value of 116 mgKOH / g.

[0238] (Pigment Dispersant Q5) Pigment dispersant Q5 was obtained in the same manner as pigment dispersant Q1, except that the amount of TCDMA and MAA added to the solution of A polymer block was changed. Specifically, 34.3 parts by mass of TCDMA, 27.0 parts by mass of MAA, and 1.2 parts by mass of V-70 were added to the solution of A polymer block. Pigment dispersant Q5 was a block polymer, with Mn of 10,500 and acid value of 138 mgKOH / g.

[0239] (Pigment Dispersant Q6) Pigment dispersant Q6 was obtained in the same manner as pigment dispersant Q1, except that the amounts of TCDMA and MAA added to the solution of A polymer block were changed. Specifically, 29.0 parts by mass of TCDMA, 32.2 parts by mass of MAA, and 1.2 parts by mass of V-70 were added to the solution of A polymer block. Pigment dispersant Q6 was a block polymer, with Mn of 11,500 and acid value of 165 mgKOH / g.

[0240] (Pigment Dispersant Q7) Pigment dispersant Q7 was obtained in the same manner as pigment dispersant Q1, except that the amount of TCDMA added in the formation of the A polymer block and the amount of TCDMA and MAA added to the solution of the A polymer block were changed. Specifically, the amount of TCDMA added in the formation of the A polymer block was 27.2 parts by mass. In addition, 65.2 parts by mass of TCDMA, 13.5 parts by mass of MAA, and 1.2 parts by mass of V-70 were added to the solution of the A polymer block. Pigment dispersant Q7 was a block polymer, had an Mn of 9300, and an acid value of 88 mgKOH / g.

[0241] (Pigment Dispersant Q8) A pigment dispersant Q8, which is a block polymer, was synthesized with reference to Synthesis Example 8 of JP2015-83688A. The details are shown below. A 1L separable flask reactor equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube was charged with 266 parts by mass of diethylene glycol dimethyl ether, 6.2 parts by mass of 2-iodo-2-cyanopropane, 120 parts by mass of methyl methacrylate (MMA), 28.8 parts by mass of acrylic acid (AA), 67.2 parts by mass of cyclohexyl methacrylate (CHMA), 7.9 parts by mass of azobisdimethylisovaleronitrile (hereinafter abbreviated as "V-65"), and 0.7 parts by mass of 2-t-butyl-4,6-dimethylphenol, and stirred while flowing nitrogen. Next, the temperature (reaction temperature) of the mixture in the reactor was raised to 70°C, and polymerization was carried out for 3 hours to obtain a polymerization solution A containing an MMA / AA / CHMA copolymer. After 3 hours, a portion of the polymerization solution A was sampled and the solid content was measured, which was 42.0% by mass, confirming that most of the monomers had polymerized. Furthermore, the weight average molecular weight (Mw) of the MMA / AA / CHMA copolymer was measured by GPC and found to be 7500. The acid value of this MMA / AA / CHMA copolymer was 101.0 mgKOH / g.

[0242] Next, a mixture of benzyl methacrylate (BzMA) (35.2 parts by mass) and V-65 (0.3 parts by mass) was added to the above polymerization solution A, and polymerization was carried out at 70°C for 3 hours to obtain a polymerization solution B containing a block polymer. The obtained block polymer is a block polymer containing an A block that is an MMA / AA / CHMA copolymer and a B block that is a BzMA homopolymer. The obtained block polymer was designated as pigment dispersant Q8. The solid content of polymerization solution B was measured to be 43.2% by mass, and it was confirmed that most of the monomers had polymerized. The Mw of pigment dispersant Q8 was 8,500, and the acid value was 89.3 mgKOH / g.

[0243] (Magenta ink M1) -Preparation of magenta pigment dispersion MA1- 150 parts by mass of pigment dispersant P1 was dissolved in water to prepare a polymer aqueous solution so that the concentration of pigment dispersant P1 was about 25% by mass. 180 parts by mass of the polymer aqueous solution, 90 parts by mass of magenta pigment PR-122 (FUJI Fast Red (registered trademark), Fuji Color Co., Ltd.), and 171.9 parts by mass of water were mixed to obtain a mixed solution. A potassium hydroxide aqueous solution was added to the obtained mixed solution, and the pH after neutralization was adjusted to 8.7. The pH was measured at 25°C using a pH meter (model name: WM-50EG, manufactured by Toa DDK Co., Ltd.). Next, the mixed solution after neutralization was subjected to a dispersion treatment for 3 hours using a bead mill (bead diameter: 0.1 mmφ, zirconia beads). As a result, a magenta pigment dispersion (uncrosslinked dispersion) in which the magenta pigment was dispersed by the pigment dispersant P1 was obtained. The pigment concentration of the uncrosslinked dispersion was 15% by mass.

[0244] Next, 3.00 parts by mass of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", Nagase ChemteX Corporation) as a crosslinking agent and 32.8 parts by mass of an aqueous boric acid solution (boric acid concentration: 4% by mass) were added to 136 parts by mass of the uncrosslinked dispersion, and the mixture was reacted at 70°C for 6 hours, and then cooled to 25°C. As a result, a magenta pigment dispersion (crosslinked dispersion) in which the pigment dispersant P1 was crosslinked and the magenta pigment was dispersed by the pigment dispersant P1a was obtained. The pigment dispersant P1a is a polymer in which the pigment dispersant P1 is crosslinked by a crosslinking agent. Ion-exchanged water was added to the crosslinked dispersion so that the pigment concentration was 15% by mass. The crosslinked dispersion was passed through an ultrafiltration device (crossflow type ultrafilter (UF), manufactured by Sartorius) equipped with a polyethersulfone (PESU) membrane (micropore size: 0.1 μm) at a flow rate of 600 mL per minute to perform ultrafiltration. The liquid temperature was adjusted to 25°C, and ultrafiltration was performed 10 times, with one time being the volumetric magnification of the charged liquid. Ion-exchanged water was added so that the pigment concentration was 15% by mass. This resulted in the production of magenta pigment dispersion MA1. The acid value of the pigment dispersant P1a (crosslinked polymer) contained in magenta pigment dispersion MA1 was 105 mgKOH / g.

[0245] -Preparation of magenta ink M1- Magenta ink M1 was prepared by mixing the following components. The above magenta pigment dispersion MA1 (pigment concentration: 15% by mass) ... 46.7% by mass Dispersion of resin particles A (solid content: 23% by mass) ... 12.9% by mass Propylene glycol: 26.0% by mass Olfine E1010 (manufactured by Nissin Chemical Industry Co., Ltd.) ... 0.25% by mass Olfin E1020 (manufactured by Nissin Chemical Industry Co., Ltd.) ... 1.0 mass% ·Capstone FS 63 (solid content concentration: 35% by mass, manufactured by Dupont) …0.7% by mass Water: The remaining amount that makes up 100% of the ink by weight

[0246] The resin particles A were prepared by the following method. A 2-liter three-neck flask (reaction vessel) equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube was charged with 560.0 g of methyl ethyl ketone and heated to 87°C. Next, while maintaining the reflux state in the reaction vessel, a mixed solution consisting of 220.4 g of methyl methacrylate, 301.6 g of isobornyl methacrylate, 58.0 g of methacrylic acid, 108 g of methyl ethyl ketone, and 2.32 g of dimethyl 2,2'-azobis(2-methylpropionate) (product name "V-601", Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator was added dropwise at a constant rate so that the drop was completed in 2 hours. The reflux state was maintained until the end of the reaction. After the dropwise addition was completed, the mixture was stirred for 1 hour, and then the operation of the following step (1) was performed on the reaction solution. Step (1): A solution consisting of 1.16 g of "V-601" and 6.4 g of methyl ethyl ketone was added and stirred for 2 hours. Next, the above step (1) was repeated four times, and then a solution consisting of 1.16 g of "V-601" and 6.4 g of methyl ethyl ketone was added and the mixture was stirred for 3 hours. After the reaction was completed, the temperature of the solution was lowered to 65° C., 163.0 g of isopropanol was added, and the mixture was allowed to cool to obtain a polymerization solution containing a copolymer (solid content concentration: 41.0% by mass). Next, 317.3 g of the obtained polymerization solution was weighed out, and 46.4 g of isopropanol, 1.65 g of a 20 mass% aqueous maleic anhydride solution (corresponding to 0.3 mass% of maleic acid relative to the copolymer), and 40.77 g of a 2 mol / L aqueous sodium hydroxide solution were added thereto, and the temperature of the liquid in the reaction vessel was raised to 70°C. Next, 380 g of distilled water was added dropwise to the liquid heated to 70°C at a rate of 10 mL / min. After that, the temperature of the liquid in the reaction vessel was kept at 70°C for 1.5 hours under reduced pressure, and a total of 287.0 g of isopropanol, methyl ethyl ketone, and distilled water was distilled off. 0.278 g of Proxel GXL(S) (Arch Chemicals Japan) (440 ppm as benzoisothiazolin-3-one relative to the polymer solid content) was added to the obtained liquid. The resulting liquid was filtered through a 1 μm filter, and the filtrate was collected to obtain an aqueous dispersion (solid content concentration 23.2% by mass) of resin particles A, which is a copolymer of methyl methacrylate / isobornyl methacrylate / methacrylic acid / sodium methacrylate (=70 / 20 / 5 / 5 [mass ratio]). The volume average particle size of resin particles A was 5.0 nm, and the weight average molecular weight (Mw) was 60,000.

[0247] (Magenta ink M2~M8) -Preparation of magenta pigment dispersion MA2- 150 parts by mass of pigment dispersant Q1 was dissolved in water to prepare a polymer aqueous solution so that the concentration of pigment dispersant Q1 was about 25% by mass. 180 parts by mass of the polymer aqueous solution, 90 parts by mass of magenta pigment PR-122 (FUJI Fast Red (registered trademark), Fuji Color Co., Ltd.), and 171.9 parts by mass of water were mixed to obtain a mixed liquid. A potassium hydroxide aqueous solution was added to the obtained mixed liquid, and the pH after neutralization was adjusted to 8.7. Next, the neutralized mixed liquid was subjected to a dispersion treatment for 3 hours using a bead mill (bead diameter: 0.1 mmφ, zirconia beads). As a result, a magenta pigment dispersion in which the magenta pigment was dispersed by pigment dispersant Q1 was obtained. The pigment concentration was 15% by mass.

[0248] -Preparation of magenta pigment dispersion MA3- Magenta pigment dispersion MA3 was obtained in the same manner as for magenta pigment dispersion MA1, except that the amount of the crosslinking agent was changed to 4.28 parts by mass and the amount of the boric acid aqueous solution was changed to 47.1 parts by mass. The acid value of the pigment dispersant P1b (crosslinked polymer) contained in the magenta pigment dispersion MA3 was 54 mgKOH / g.

[0249] -Preparation of magenta pigment dispersion MA4- Magenta pigment dispersion MA4 was obtained in the same manner as for Magenta pigment dispersion MA1, except that the amount of the crosslinking agent was changed to 5.03 parts by mass and the amount of the boric acid aqueous solution was changed to 55.5 parts by mass. The acid value of the pigment dispersant P1c (crosslinked polymer) contained in Magenta pigment dispersion MA4 was 24 mgKOH / g.

[0250] -Preparation of magenta pigment dispersion MA5- Magenta pigment dispersion MA5 was obtained in the same manner as for Magenta pigment dispersion MA1, except that the amount of the crosslinking agent was changed to 2.21 parts by mass and the amount of the boric acid aqueous solution was changed to 24.3 parts by mass. The acid value of P1d (crosslinked polymer) contained in Magenta pigment dispersion MA5 was 135 mgKOH / g.

[0251] -Preparation of magenta pigment dispersion MA6- Magenta pigment dispersion MA6 was obtained in the same manner as for Magenta pigment dispersion MA1, except that the amount of the crosslinking agent was changed to 1.57 parts by mass and the amount of the boric acid aqueous solution was changed to 17.3 parts by mass. The acid value of P1e (crosslinked polymer) contained in Magenta pigment dispersion MA6 was 160 mgKOH / g.

[0252] -Preparation of magenta pigment dispersion MA7- Magenta pigment dispersion MA7 was obtained in the same manner as for Magenta pigment dispersion MA1, except that the amount of the crosslinking agent was changed to 0.55 parts by mass and the amount of the boric acid aqueous solution was changed to 6.08 parts by mass. The acid value of P1f (crosslinked polymer) contained in Magenta pigment dispersion MA7 was 200 mgKOH / g.

[0253] -Preparation of magenta pigment dispersion MA8- Magenta pigment dispersion MA8 was obtained in the same manner as for magenta pigment dispersion MA1, except that pigment dispersant P1 was changed to pigment dispersant P2, the amount of crosslinker was changed to 2.07 parts by mass, and the amount of boric acid aqueous solution was changed to 22.84 parts by mass. The acid value of pigment dispersant P2a (crosslinked polymer) contained in magenta pigment dispersion MA8 was 84.2 mgKOH / g.

[0254] -Preparation of magenta inks M2 to M8- Magenta inks M2 to M8 were prepared in the same manner as for magenta ink M1, except that the above magenta pigment dispersions MA2 to MA8 were used.

[0255] (Magenta ink M9, M10) Magenta inks M9 and M10 were prepared in the same manner as Magenta ink M1, except that the contents (mass %) of the organic solvent and surfactant were changed as shown in Table 2.

[0256] (Magenta ink M11) -Preparation of magenta pigment dispersion MA11- The pigment dispersant P1 was changed to the pigment dispersant P3, and a magenta pigment dispersion (uncrosslinked dispersion) in which the magenta pigment was dispersed by the pigment dispersant P3 was obtained. The obtained uncrosslinked dispersion was named magenta pigment dispersion MA11. -Preparation of magenta ink M11- Magenta ink M11 was prepared in the same manner as Magenta ink M1, except that the above magenta pigment dispersion MA11 was used.

[0257] In Tables 1 and 2, the content (mass %) of the pigment, resin particles, organic solvent, and surfactant relative to the total amount of the magenta ink is shown. Additionally, in Tables 1 and 2, the type and form of the pigment dispersant contained in each magenta ink is shown. In the form column, "crosslinked" means crosslinked polymer, "block" means block polymer, and "random" means random polymer.

[0258] [Table 1]

[0259] [Table 2]

[0260] (White ink W1) -Preparation of white pigment dispersion WA1- 136.4 parts by mass of pigment dispersant Q1, 163.6 parts by mass of butyl carbitol, and 450 parts by mass of CI Pigment White 6 (trade name "JR-405", titanium oxide, manufactured by Teika Co., Ltd.) as a white pigment were mixed and stirred with a disperser. Next, the white pigment was thoroughly dispersed using a horizontal media disperser to obtain an oil-based pigment dispersion. The average particle diameter of the white pigment dispersed in the oil-based pigment dispersion was 290 nm. The viscosity of the oil-based pigment dispersion was 86.3 m3a·s. Next, while stirring 700 parts by mass of the oil-based pigment dispersion using a disperser, a mixed liquid consisting of 4.0 parts by mass of potassium hydroxide and 341 parts by mass of water was gradually added to neutralize and cause phase inversion. Then, the white pigment was thoroughly dispersed using a horizontal media disperser to obtain an aqueous pigment dispersion. Coarse particles were removed from the obtained aqueous pigment dispersion using a 10 μm filter and a 5 μm filter. At this time, no clogging of the filters was observed. The average particle size of the white pigment dispersed in the aqueous pigment dispersion was 266 nm. The viscosity of the aqueous pigment dispersion was 14.5 mPa s, and the pH was 9.8. The average particle size of the white pigment was measured using a particle size distribution analyzer that uses light scattering (product name "UPA-EX150", manufactured by Nikkiso Co., Ltd.).

[0261] -Preparation of white ink W1- The following components were mixed to prepare a white ink W1. The above white pigment dispersion WA1 (pigment concentration: 45% by mass) ... 26.7% by mass Dispersion of resin particles A (solid content: 23% by mass) ... 17.2% by mass Propylene glycol: 27.0% by mass Olfine E1010 (manufactured by Nissin Chemical Industry Co., Ltd.) ... 0.25% by mass Olfin E1020 (manufactured by Nissin Chemical Industry Co., Ltd.) ... 1.0 mass% ·Capstone FS-63 (solid content concentration: 35% by mass, manufactured by DuPont) …0.7% by mass Water: The remaining amount that makes up 100% of the ink by weight

[0262] (White ink W2) -Preparation of white pigment dispersion WA2- White pigment dispersion WA2 was obtained in the same manner as for magenta pigment dispersion MA1, except that a white pigment, CI Pigment White 6 (product name: JR-405, manufactured by Teika Co., Ltd.), was used instead of the magenta pigment. White pigment dispersion WA2 is a dispersion in which a white pigment is dispersed by pigment dispersant P1a (crosslinked polymer). -Preparation of white ink W2- White ink W2 was prepared in the same manner as white ink W1, except that white pigment dispersion WA2 was used.

[0263] (White ink W3~W8, W13 and W14) -Preparation of white pigment dispersions WA3 to WA8, WA13 and WA14- White pigment dispersions WA3 to WA8, WA13 and WA14 were obtained in the same manner as for white pigment dispersion WA1, except that pigment dispersants Q2 to Q8 and P4 were used instead of pigment dispersant Q1. -Preparation of White Inks W3 to W8, W13 and W14- White inks W3 to W8 and W13 were prepared in the same manner as white ink W1, except that the above white pigment dispersions WA3 to WA8, WA13 and WA14 were used.

[0264] (White ink W9~W12) White inks W9 to W12 were prepared in the same manner as white ink W1, except that the contents (mass %) of the organic solvent and surfactant were changed as shown in Table 4.

[0265] In Tables 3 and 4, the content (mass %) of the pigment, resin particles, organic solvent, and surfactant relative to the total amount of the white ink is shown. Additionally, in Tables 3 and 4, the type and form of the pigment dispersant contained in each white ink is shown. In the form column, "crosslinked" means crosslinked polymer, "block" means block polymer, and "random" means random polymer.

[0266] [Table 3]

[0267] [Table 4]

[0268] (Pretreatment solution) A pretreatment liquid to be applied in advance to a substrate was prepared by mixing the resin particles, flocculant, organic solvent, and surfactant shown in Table 5 with water to the contents (mass %) shown in Table 5. The pretreatment liquid contains water in addition to the components shown in Table 5 so that the total pretreatment liquid is 100 mass %. Details of the resin particles, flocculant, organic solvent, and surfactant used in preparing the pretreatment liquid are as follows. -Resin particles- - PES RESIN A124GP (polyester resin, manufactured by Takamatsu Oil Co., Ltd.) -Flocculant- Malonic Acid Calcium chloride (CaCl 2 ) TC-310 (Titanium Lactate, Matsumoto Fine Chemical Co., Ltd.) -Organic solvents- Propylene glycol -Surfactants- W-13T (Sodium dodecylbenzenesulfonate (hard type), manufactured by Tokyo Chemical Industry Co., Ltd.)

[0269] [Table 5]

[0270] [Image recording] Using the ink and the pretreatment liquid, an image was recorded by the following method. A GELJET (registered trademark) GX5000 printer head (manufactured by Ricoh Co., Ltd.) was prepared as an inkjet head. The inkjet head was a line head with 96 nozzles arranged. The inkjet head was arranged by fixing it to an inkjet recording device. At this time, the direction in which the 96 nozzles were arranged was inclined at 75.7° with respect to the direction perpendicular to the moving direction of the stage of the inkjet recording device on the same plane. A polyethylene terephthalate (PET) substrate (product name "FE2001", thickness 12 μm, manufactured by Futamura Chemical Co., Ltd.) was prepared as a substrate, and the following pretreatment liquid application process and image recording process were sequentially performed using this PET substrate.

[0271] (Pretreatment liquid application step) The substrate was fixed on the stage of an inkjet recording apparatus, and the stage on which the substrate was fixed was then moved in a linear direction at a constant speed of 500 mm / sec while the pretreatment liquid was applied onto the substrate using a wire bar coater. The amount of the pretreatment liquid applied was 1.5 g / m 2 At the location where application of the pretreatment liquid was completed, drying of the pretreatment liquid was started using a dryer at 50°C 1.5 seconds after application of the pretreatment liquid to this location was completed. Drying was completed 3.5 seconds after application of the pretreatment liquid was completed. In other words, the drying time was 2 seconds.

[0272] (Image recording process) While the substrate on which the pretreatment liquid had been dried was moved at a constant stage speed of 50 mm / sec, magenta ink was ejected from the inkjet head onto the surface of the substrate on which the pretreatment liquid had been applied. After ejection of the magenta ink, white ink was ejected to record a solid image, thereby obtaining an image recording. A sample piece measuring 4 cm in length and 15 cm in width was cut out from the obtained image recording. The ejection of the magenta ink was started within 2 seconds after the pretreatment liquid had been dried. The ink ejection conditions were an ejection frequency of 24 kHz and a resolution of 1200 dpi x 1200 dpi (dot per inch). The total amount of the magenta ink and the white ink applied was 17.9 g / m 2The magenta ink and the white ink were deaerated through a degassing filter before being ejected, and the temperature was adjusted to 30°C.

[0273] [evaluation] For each of the examples and comparative examples, the obtained sample pieces (solid images) were used to evaluate image cracking and image quality. The evaluation methods were as follows.

[0274] -Cracked image- The obtained sample pieces were visually observed and evaluated for cracks according to the following criteria. 7: No visible cracks in the image 6: One or more but less than five cracks in the image are visible in the transport direction of the substrate. 5: Five or more but less than 10 cracks in the image are visible in the transport direction of the substrate. 4: 10 or more but less than 15 cracks in the image are visible in the transport direction of the substrate. 3: 15 or more but less than 20 cracks in the image are visible in the transport direction of the substrate. 2: 20 or more cracks in the image are visible in the transport direction of the substrate. 1: Image cracks are visible with no particular direction.

[0275] -image quality- The obtained sample pieces were visually observed, and the image quality was evaluated based on the unevenness in density of the solid image. The evaluation criteria were as follows: 5: When a solid image is observed from a distance of 5 cm, no density unevenness is observed. 4: When a solid image is observed from a distance of 5 cm, density unevenness is observed, but when observed from a distance of 10 cm, no density unevenness is observed. 3: When a solid image is observed from a distance of 10 cm, density unevenness is observed, but when observed from a distance of 15 cm, no density unevenness is observed. 2: When a solid image is observed from a distance of 15 cm, density unevenness is noticeable, but when observed from a distance of 20 cm, no density unevenness is noticeable. 1: Even when observing a solid image from a distance of 20 cm, uneven density can be seen.

[0276] The evaluation results are shown in Tables 6 to 8 below. In Tables 6 to 8, "|Tm-Tw|" means the absolute value of the difference between the surface tension of the magenta ink and the surface tension of the white ink. "|Tm-Tp|" means the absolute value of the difference between the surface tension of the magenta ink and the surface tension of the pre-treatment liquid.

[0277] [Table 6]

[0278] [Table 7]

[0279] [Table 8]

[0280] [Table 9]

[0281] As shown in Tables 6 to 8, in Examples 1 to 30, the pigment dispersants contained in the magenta ink and white ink each contain a polymer having a cross-linked structure or a block polymer, and therefore it was found that cracking of the recorded image was suppressed.

[0282] On the other hand, in Comparative Example 1, the pigment dispersant contained in the white ink was neither a polymer having a crosslinked structure nor a block polymer, and therefore cracks occurred in the recorded image.

[0283] In Comparative Example 2, the pigment dispersant contained in the magenta ink and the pigment dispersant contained in the white ink were neither a polymer having a cross-linked structure nor a block polymer, and therefore cracks occurred in the recorded image.

[0284] It was found that in Example 1, the pigment dispersant contained in the magenta ink was a polymer having a crosslinked structure, and therefore, compared to Example 28, cracking of the recorded image was further suppressed.

[0285] In Example 1, since the pigment dispersant contained in the white ink is a block polymer, it was found that cracking of the recorded image was more suppressed than in Example 29.

[0286] In Example 1, since the acid value of the pigment dispersant contained in the magenta ink is 30 mgKOH / g to 180 mgKOH / g, it was found that the image quality of the recorded image is superior to that of Example 4. Furthermore, since the acid value of the pigment dispersant contained in the magenta ink is 30 mgKOH / g to 180 mgKOH / g, it was found that cracking of the recorded image is further suppressed in Example 1 compared to Example 7.

[0287] In Example 1, since the acid value of the pigment dispersant contained in the white ink is 60 mgKOH / g to 150 mgKOH / g, it was found that the image quality of the recorded image is superior to that of Example 9. In addition, since the acid value of the pigment dispersant contained in the white ink is 60 mgKOH / g to 150 mgKOH / g, it was found that cracking of the recorded image is further suppressed compared to Example 12.

[0288] In Example 1, the absolute value of the difference between the surface tension of the magenta ink and the surface tension of the white ink is 0.05 mN / m to 10.0 mN / m, and therefore it was found that cracking of the recorded image was more suppressed compared to Example 17. Furthermore, it was found that Example 1 had superior image quality of the recorded image compared to Example 19.

[0289] In Example 1, since the absolute value of the difference between the surface tension of the magenta ink and the surface tension of the pretreatment liquid was 0.05 mN / m to 10.0 mN / m, it was found that cracking of the recorded image was further suppressed compared to Example 21.

[0290] In Example 1, the absolute value of the difference between the surface tension of the magenta ink and the surface tension of the pretreatment liquid was 0.05 mN / m to 10.0 mN / m, so it was found that the quality of the recorded image was superior to that of Example 23.

[0291] <Example 31 to Example 37> Next, using magenta ink M1 and white ink W1, image recording was performed in the same manner as in Example 1, with the application amount of the pretreatment liquid and the total application amount of the magenta ink and white ink (in Table 10, "total application amount of ink") being as shown in Table 10. In addition, the application amount (g / m 2 ) is the total amount of magenta pigment contained in the magenta ink and the white pigment contained in the white ink (g / m 2 The amounts of magenta ink and white ink applied were adjusted so that the ratio of the total amount of pigment applied to the amount of flocculant applied (in Table 10, "ratio of the total amount of pigment applied to the amount of flocculant applied") would be the value shown in Table 10.

[0292] [Table 10]

[0293] As shown in Table 10, in Example 1, the ratio of the total amount of magenta pigment and white pigment applied to the amount of flocculant applied was 20 to 300, and therefore it was found that the image quality of the recorded image was superior to that of Example 31. In addition, it was found that in Example 1, cracking of the recorded image was further suppressed to a greater extent than in Example 33.

[0294] In Example 1, the amount of the pretreatment liquid applied was 1.0 g / m 2 ~2.0g / m 2 Therefore, it was found that the image quality of the recorded image was superior to that of Example 34. Moreover, it was found that the cracking of the recorded image was more suppressed in Example 1 than in Example 35.

[0295] In Example 1, the total amount of magenta ink and white ink applied was 9.0 g / m 2 ~25.0g / m 2Therefore, it was found that the quality of the recorded image was superior to that of Example 36. Moreover, it was found that the quality of the recorded image was superior to that of Example 37, and cracks in the recorded image were further suppressed.

[0296] <Example 38> Image recording was performed in the same manner as in Example 1, except that the ejection order of the magenta ink and the white ink was reversed. That is, in Example 38, a white ink was ejected onto the surface of the substrate to which the pretreatment liquid had been applied, and after the ejection of the white ink, a magenta ink was ejected successively to record a solid image, thereby obtaining an image recording matter.

[0297] <Comparative Example 3> Image recording was performed in the same manner as in Comparative Example 1, except that the ejection order of the magenta ink and the white ink was reversed. That is, in Comparative Example 3, the white ink was ejected onto the surface of the substrate to which the pretreatment liquid had been applied, and after the ejection of the white ink, the magenta ink was ejected successively to record a solid image, thereby obtaining an image recording material.

[0298] The same evaluation as in Example 1 was performed for Example 38 and Comparative Example 3. It was found that the image quality of the recorded image was superior in Example 38 compared to Comparative Example 3, and that cracking of the recorded image was further suppressed.

[0299] The disclosure of Japanese Patent Application No. 2020-083140, filed on May 11, 2020, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. a color ink including a color pigment, which is at least one of a chromatic pigment and a black pigment, a pigment dispersant, and water; a white ink containing a white pigment, a pigment dispersant, and water; Equipped with The pigment dispersant contained in the white ink contains a polymer or a block polymer having a crosslinked structure, the pigment dispersant contained in the color ink contains a structural unit derived from a (meth)acrylate having an aromatic ring structure or an alicyclic structure, and contains a polymer having a crosslinked structure; Ink set.

2. a color ink including a color pigment, which is at least one of a chromatic pigment and a black pigment, a pigment dispersant, and water; a white ink containing a white pigment, a pigment dispersant, and water; Equipped with The pigment dispersant contained in the white ink contains a polymer or a block polymer having a crosslinked structure, the pigment dispersant contained in the color ink contains a structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure, and contains a polymer having a crosslinked structure; the content of the structural unit derived from the ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure is 35% by mass to 95% by mass based on the total amount of the pigment dispersant contained in the color ink; Ink set.

3. a color ink including a color pigment, which is at least one of a chromatic pigment and a black pigment, a pigment dispersant, and water; a white ink containing a white pigment, a pigment dispersant, and water; Equipped with The pigment dispersant contained in the white ink contains a polymer having a crosslinked structure or a block polymer, The pigment dispersant contained in the color ink contains a block polymer, The ink set, wherein the acid value of the pigment dispersant contained in the white ink is 60 mgKOH / g to 150 mgKOH / g.

4. a color ink including a color pigment, which is at least one of a chromatic pigment and a black pigment, a pigment dispersant, and water; a white ink containing a white pigment, a pigment dispersant, and water; Equipped with The pigment dispersant contained in the white ink contains a block polymer, The pigment dispersant contained in the color ink contains a polymer having a crosslinked structure or a block polymer, The ink set, wherein the acid value of the pigment dispersant contained in the white ink is 60 mgKOH / g to 150 mgKOH / g.

5. 3. The ink set according to claim 1, wherein the acid value of the pigment dispersant contained in the white ink is 60 mgKOH / g to 150 mgKOH / g.

6. The ink set according to claim 4 , wherein the pigment dispersant contained in the color inks contains a polymer having a crosslinked structure.

7. The ink set according to any one of claims 1 to 3, wherein the pigment dispersant contained in the white ink contains a block polymer.

8. The ink set according to any one of claims 1 to 7, wherein the acid value of the pigment dispersant contained in the color ink is 30 mgKOH / g to 180 mgKOH / g.

9. The ink set according to claim 3 or claim 4, wherein the pigment dispersants contained in the color inks and the white ink each contain a structural unit derived from an ethylenically unsaturated compound having an aromatic ring structure or an alicyclic structure.

10. 10. The ink set according to claim 1, wherein an absolute value of a difference between the surface tension of the color inks and the surface tension of the white ink is 0.05 mN / m to 10.0 mN / m.

11. The ink set according to any one of claims 1 to 10, further comprising a pretreatment liquid containing a flocculant.

12. 12. The ink set according to claim 11, wherein an absolute value of a difference between the surface tension of the pretreatment liquid and the surface tension of the color ink is 0.05 mN / m to 10.0 mN / m.

13. The ink set according to any one of claims 1 to 10 is used, a color ink application step of applying the color ink onto a non-permeable substrate; and applying the white ink onto the colored ink film formed by applying the colored ink.

14. The ink set according to claim 11 or 12 is used, a pretreatment liquid application step of applying the pretreatment liquid onto a non-permeable substrate; an ink applying step of applying the color inks and the white ink by an ink jet recording method onto the non-permeable substrate to which the pretreatment liquid has been applied.

Citation Information

Patent Citations

  • Ink composition, ink set, and image forming method

    JP2009190379A

  • Inkjet recording method and ink set

    JP2010046945A

  • Ink composition, method of producing the same, ink set, and image forming method

    JP2011231315A

  • Aqueous white ink for inkjet recording, white pigment paste, and aqueous ink set for inkjet recording

    JP2013082885A

  • White ink composition, ink set for forming multi-layer, image forming method and printed material

    JP2014185235A