Resin composition and laminate

A balanced resin composition with ethylene-vinyl acetate copolymer and diglycerin/glycerin fatty acid esters addresses antistatic and seal strength issues, ensuring effective antistatic performance and transparency in packaging materials.

JP7577920B2Active Publication Date: 2024-11-06JAPAN POLYETHYLENE CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020028666
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-21
Publication Date
2024-11-06
Estimated Expiration
2040-02-21

AI Technical Summary

Technical Problem

Ethylene-vinyl acetate copolymers used in packaging materials face challenges in achieving effective antistatic properties without compromising seal strength and transparency, particularly due to the slow action of high molecular weight diglycerin fatty acid esters and the need for large amounts that can lead to bloom and reduced seal strength.

Method used

A resin composition combining ethylene-vinyl acetate copolymer with specific amounts of diglycerin and glycerin fatty acid esters as antistatic agents, balanced to provide excellent antistatic properties without affecting seal strength or transparency, with a surface resistivity of 10 Ω/□ at 500V and a half-life of 60 seconds or less.

Benefits of technology

The resin composition maintains excellent antistatic properties and seal strength, with minimal impact on transparency, suitable for packaging materials like bonito packs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577920000001
    Figure 0007577920000001
  • Figure 0007577920000002
    Figure 0007577920000002
Patent Text Reader

Abstract

To provide a resin composition for extrusion lamination which prevents deterioration in seal strength and transparency while having excellent electrostatic prevention, and a laminate.SOLUTION: A resin composition is obtained by blending 0.05-0.20 wt.% of (A) a diglycerol fatty acid ester and 0.20-0.40 wt.% of (B) a glycerol fatty acid ester as antistatic agents with an ethylene-vinyl acetate copolymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a laminate using the resin composition, and more particularly to a resin composition for extrusion lamination that has excellent antistatic properties without reducing seal strength and transparency, and a laminate using the resin composition. [Background technology]

[0002] Ethylene-vinyl acetate copolymers produced by radical polymerization are characterized by their low-temperature sealing and cutting properties, and are also used as packaging materials for bonito packs. The contents tend to become electrostatically charged and adhere to the sealant layer when filling or removing the contents, so ethylene-vinyl acetate copolymers with antistatic agents kneaded into them are generally used. Ethylene-vinyl acetate copolymers are highly polar, making it difficult for antistatic agents to exert their effects, so the ingredients of the antistatic agent are limited. Diglycerol fatty acid esters, which have a high molecular weight, are relatively commonly used. However, diglycerol fatty acid esters are slow acting, so they deposit on the surface very slowly. For this reason, it is common to use a large amount of antistatic agent. However, if the sealant layer is thick, blooming is likely to occur, and problems such as reduced seal strength and transparency are likely to occur. It was difficult to achieve a balance between the antistatic agent effect and physical properties. Summary of the Invention [Problem to be solved by the invention]

[0003] Therefore, an object of the present invention is to solve the above-mentioned problems of the conventional technology and to provide a resin composition for extrusion lamination containing an ethylene-vinyl acetate copolymer produced by radical polymerization, which has excellent antistatic properties without reducing seal strength and transparency. Another object of the present invention is to provide a laminate using such a resin composition and a packaging material for bonito packs comprising the laminate. [Means for solving the problem]

[0004] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that by combining an ethylene-vinyl acetate copolymer produced by radical polymerization with an appropriate amount of a diglycerol fatty acid ester and a glycerol fatty acid ester, it is possible to provide a resin composition for extrusion lamination which has excellent antistatic properties regardless of the thickness of the sealant layer and which does not reduce seal strength and transparency, and which has thus completed the present invention.

[0005] That is, according to the first aspect of the present invention, there is provided a resin composition comprising an ethylene-vinyl acetate copolymer blended with 0.05 to 0.20 wt % of (A) diglycerol fatty acid ester and 0.20 to 0.40 wt % of (B) glycerol fatty acid ester as an antistatic agent.

[0006] According to the second aspect of the present invention, there is provided a coating film having at least a layer made of the resin composition according to the first aspect of the present invention, and the coating film has a surface resistivity of 10 or less at an applied voltage of 500 V. 13 and an honestometer half-life of 60 seconds or less.

[0007] According to a third aspect of the present invention, there is provided a laminate according to the second aspect, characterized in that it has a layer made of the resin composition on at least one surface side.

[0008] In addition, according to a fourth aspect of the present invention, there is provided a laminate according to the second or third aspect of the present invention, characterized in that the layer made of the resin composition is produced by an extrusion lamination method.

[0009] According to a fifth aspect of the present invention, there is provided a packaging material for bonito packs, comprising the laminate according to any one of the second to fourth aspects of the present invention. Effect of the Invention

[0010] According to the resin composition of the present invention, it is possible to provide a resin composition for extrusion lamination which has excellent antistatic properties while not reducing the seal strength and transparency. Furthermore, according to the laminate and packaging material for bonito packs of the present invention, it is possible to provide a laminate using such a resin composition and a packaging material for bonito packs comprising the laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The resin composition and laminate of the present invention will be described in detail below for each item.

[0012] I. Resin Composition The resin composition of the present invention is a resin composition containing an ethylene-vinyl acetate copolymer and an antistatic agent.

[0013] (i) Ethylene-vinyl acetate copolymer The ethylene-vinyl acetate copolymer used in the resin composition of the present invention is generally produced by radical polymerization. Polymerization methods for ethylene-vinyl acetate copolymer are roughly divided into the autoclave process and the tubular process. The autoclave process uses an autoclave-type reactor (also called a tank type), and the tubular process uses a tubular-type reactor (also called a pipe type). These polymerization methods have different properties due to the difference in reactor shape and polymerization conditions, so the ethylene-vinyl acetate copolymer obtained by the tubular process is clearly distinguishable from that obtained by the autoclave process. The ethylene-vinyl acetate copolymer obtained by the tubular process is known to have a relatively narrow molecular weight distribution and a relatively small melt elasticity.

[0014] 1. Molecular weight distribution of ethylene-vinyl acetate copolymer The ethylene-vinyl acetate copolymer used in the present invention preferably has a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) measured by gel permeation chromatography (GPC) of 3.5 or more, and more preferably 5.5 or less. The conditions for measuring the molecular weight distribution Mw / Mn are as follows: Apparatus: Waters GPC 150C Detector: MIRAN 1A infrared spectrophotometer (measurement wavelength: 3.42 μm) Column: Showa Denko AD806M / S 3 columns (The columns were calibrated by measuring Tosoh monodisperse polystyrene (A500, A2500, F1, F2, F4, F10, F20, F40, F288, each 0.5 mg / ml solution), and approximating the logarithm of the elution volume and molecular weight with a quadratic equation. The molecular weight of the sample was converted to polyethylene using the viscosity equation for polystyrene and polyethylene. Here, the coefficients of the viscosity equation for polystyrene are α=0.723, logK=-3.967, and for polyethylene, α=0.733, logK=-3.407.) Measurement temperature: 140℃ Concentration: 20mg / 10mL Injection amount: 0.2ml Solvent: ortho-dichlorobenzene Flow rate: 1.0ml / min

[0015] 2.Melt flow rate of ethylene-vinyl acetate copolymer From the viewpoint of extrusion lamination processability, the ethylene-vinyl acetate copolymer used in the present invention preferably has a melt flow rate (MFR: 190° C., 21.18 N load) of 5 to 15 g / 10 min, more preferably 7 to 12 g / 10 min. The MFR of ethylene-vinyl acetate copolymer is a value measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18N load).

[0016] 3. Monomers that make up ethylene-vinyl acetate copolymer The ethylene-vinyl acetate copolymer used in the present invention is a copolymer of ethylene and vinyl acetate, and the proportion of ethylene constituting the copolymer is preferably 88 to 95% by weight, and the proportion of vinyl acetate constituting the copolymer is preferably 5 to 12% by weight.

[0017] (ii) Antistatic agent The resin composition of the present invention contains (A) a diglycerol fatty acid ester and (B) a glycerol fatty acid ester as antistatic agents. According to the resin composition of the present invention, by blending a predetermined amount of a diglycerol fatty acid ester and a glycerol fatty acid ester with an ethylene-vinyl acetate copolymer, it is possible to provide a resin composition for extrusion lamination that has excellent antistatic properties regardless of the thickness of the sealant layer and does not reduce the seal strength and transparency.

[0018] 1. Diglycerol fatty acid The diglycerol fatty acid ester used in the present invention is an esterification reaction product of diglycerol and a fatty acid, and is produced by a known method, and a commercially available product can be used.

[0019] Diglycerin used as a raw material for diglycerin fatty acid esters includes a diglycerin mixture having an average degree of polymerization of about 1.5 to 2.4, preferably about 2.0, which is obtained by adding a small amount of acid or alkali as a catalyst to glycerin and heating the mixture at a temperature of, for example, about 180°C or higher under an atmosphere of any inert gas such as nitrogen or carbon dioxide to cause a polycondensation reaction. Diglycerin may also be obtained from glycidol or epichlorohydrin as a raw material. After the reaction is completed, treatment such as neutralization, desalting, and decolorization may be performed if necessary.

[0020] In the present invention, the above diglycerol mixture is purified by a known method such as distillation or column chromatography to obtain high-purity diglycerol having a high concentration of diglycerol consisting of two glycerol molecules of about 50% by mass or more, preferably about 85% by mass or more, and is preferably used.

[0021] The fatty acid used as the raw material of diglycerol fatty acid ester is preferably a fatty acid having 8 to 22 carbon atoms, and examples thereof include saturated fatty acids such as caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, arachidic acid, and behenic acid, and unsaturated fatty acids such as decenoic acid, undecenoic acid, dodecenoic acid, tetradecenoic acid, oleic acid, erucic acid, linoleic acid, linolenic acid, and ricinoleic acid. Among them, lauric acid, myristic acid, palmitic acid, and stearic acid are more preferable from the viewpoint of antistatic performance and color tone. These fatty acids may be used alone or in combination of two or more.

[0022] 2. Glycerin fatty acids The glycerin fatty acid ester used in the present invention may be an esterification reaction product of glycerin and a fatty acid, or an ester exchange product of glycerin and an oil or fat. The glycerin fatty acid ester is produced by a known method, and a commercially available product may be used.

[0023] The fatty acid used as the raw material of the glycerin fatty acid ester is preferably a fatty acid having 8 to 22 carbon atoms, and examples thereof include saturated fatty acids such as caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, arachidic acid, and behenic acid, and unsaturated fatty acids such as decenoic acid, undecenoic acid, dodecenoic acid, tetradecenoic acid, oleic acid, erucic acid, linoleic acid, linolenic acid, and ricinoleic acid. Among them, lauric acid, myristic acid, palmitic acid, and stearic acid are more preferable in terms of antistatic performance and color tone. These fatty acids may be used alone or in combination of two or more.

[0024] 3. Triglycerol fatty acids The resin composition of the present invention may further contain a triglycerol fatty acid ester as an antistatic agent. The triglycerol fatty acid ester that can be used in the present invention is an esterification reaction product of triglycerol and a fatty acid, and is produced by a known method, and a commercially available product can be used.

[0025] Triglycerin used as a raw material for triglycerin fatty acid esters includes triglycerin mixtures having an average degree of polymerization of about 2.5 to 3.4, preferably about 3.0, which are usually obtained by adding a small amount of acid (e.g., concentrated sulfuric acid, p-toluenesulfonic acid, etc.) or alkali (e.g., potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, etc.) to glycerin as a catalyst, heating at a temperature of, for example, about 180°C or higher under an atmosphere of any inert gas such as nitrogen or carbon dioxide, and subjecting the mixture to a polycondensation reaction. Triglycerin may also be obtained from glycidol or epichlorohydrin, etc. as a raw material. After the reaction is completed, treatments such as neutralization, desalting, and decolorization may be performed as desired. In the present invention, the above triglycerin mixture is purified using a method known per se, such as distillation or column chromatography, and high-purity triglycerin in which triglycerin consisting of three glycerin molecules is concentrated to about 50% or more, preferably about 80% or more, is preferably used.

[0026] The fatty acid used as the raw material of triglycerol fatty acid ester is preferably a fatty acid having 8 to 22 carbon atoms, and examples thereof include saturated fatty acids such as caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, arachidic acid, and behenic acid, and unsaturated fatty acids such as decenoic acid, undecenoic acid, dodecenoic acid, tetradecenoic acid, oleic acid, erucic acid, linoleic acid, linolenic acid, and ricinoleic acid. Among them, lauric acid, myristic acid, palmitic acid, and stearic acid are more preferable from the viewpoint of antistatic performance and color tone. These fatty acids may be used alone or in combination of two or more.

[0027] (iii) Compounding amount In the resin composition of the present invention, the amount of the diglycerol fatty acid ester (A) as an antistatic agent is 0.05-0.20% by weight, and the amount of the glycerol fatty acid ester (B) as an antistatic agent is 0.20-0.40% by weight, and preferably the amount of the diglycerol fatty acid ester (A) is 0.08-0.18% by weight, and the amount of the glycerol fatty acid ester (B) is 0.25-0.35% by weight. In the resin composition of the present invention, the amount of the ethylene-vinyl acetate copolymer is preferably 99.40-99.75% by weight. Furthermore, in the resin composition of the present invention, when the combined proportion of the diglycerol fatty acid ester (A) and the glycerol fatty acid ester (B) as antistatic agents is less than 0.25% by weight, the antistatic performance of the laminate after extrusion lamination is undesirably reduced. On the other hand, when the combined proportion of the diglycerol fatty acid ester (A) and the glycerol fatty acid ester (B) as antistatic agents exceeds 0.60% by weight, the laminate after extrusion lamination is undesirably whitened and the seal strength is undesirably reduced.

[0028] (iv) Preparation of resin composition The resin composition of the present invention can be prepared by a known method. For example, the resin composition of the present invention may be prepared by melt-mixing an ethylene-vinyl acetate copolymer and an antistatic agent in an extruder, or by dry-blending an ethylene-vinyl acetate copolymer with a master batch in which an antistatic agent has been kneaded into the ethylene-vinyl acetate copolymer.

[0029] (v) Other ingredients Furthermore, the resin composition of the present invention may contain additives, such as lubricants, neutralizing agents, antioxidants, etc., which are usually used in polyethylene, as required.

[0030] II. Laminate The laminate of the present invention has at least a layer made of the above-mentioned resin composition of the present invention, and preferably has a layer made of the resin composition on at least one surface. The layer made of the above-mentioned resin composition of the present invention is preferably used as a sealant layer, and its thickness is preferably 15 to 40 μm. Hereinafter, the layer made of the resin composition of the present invention is also referred to as a sealant layer.

[0031] (i) Surface resistivity The laminate of the present invention has excellent antistatic properties, and the layer made of the resin composition has a surface resistivity of, for example, 10 at an applied voltage of 500 V. 13 Below 10, preferably 11 ~10 12 It is. In this specification, the surface resistivity is a value measured by applying a charge of 500 V for 1 minute using a surface resistivity meter (for example, Mitsubishi Petrochemical's surface resistivity meter MCP-HT250), and the unit is Ω / □.

[0032] (ii) Half-life In the laminate of the present invention, the layer made of the resin composition has excellent antistatic properties, for example, an Honestometer half-life of 60 seconds or less, preferably 30 seconds or less. In this specification, the honestometer half-life is a value measured by applying a charge of 10 KV for 2 minutes using an honestometer (for example, static honestometer H-0110 manufactured by Shishido Electrostatic) and measuring the time it takes for the initial charged voltage to decay to half.

[0033] (iii) Heat seal strength In the laminate of the present invention, the layer made of the resin composition has excellent antistatic properties while suppressing a decrease in seal strength. For example, the decrease in heat seal strength compared to an additive-free product is preferably 3N / 15mm or less. In this specification, the heat seal strength is measured by cutting a laminated film into a width of 15 mm, placing the sealant sides together, setting the upper seal bar of a heat sealer (e.g., a hot platen heat sealer manufactured by Tester Sangyo) at 120°C and the lower seal bar at 30°C, and sealing pressure of 2 kg / cm. 2The strength of the heat-sealed portion was measured at a tensile tester (for example, a Toyo Seiki tensile tester) at a tensile speed of 300 mm / min after heat sealing for a sealing time of 1 second.

[0034] (iv) Haze In the laminate of the present invention, the layer made of the resin composition has excellent antistatic properties, while suppressing a decrease in transparency. For example, the decrease in haze compared to an additive-free product is preferably 0.5% or less. In this specification, the haze (cloudiness) is measured with a haze meter (for example, HM-150 haze meter manufactured by Murakami Color Research Laboratory).

[0035] (v) Laminated body configuration The laminate of the present invention usually has a substrate layer. Examples of substrate layers that can be used in the laminate of the present invention include paper such as fine paper, craft paper, tissue paper, and Kent paper, metal foils such as aluminum foil, cellophane, woven fabric, nonwoven fabric, nylon substrates such as stretched nylon, non-stretched nylon, special nylon (MXD6, etc.), and K-nylon (polyvinylidene fluoride coated), PET (polyethylene terephthalate) substrates such as stretched PET, non-stretched PET, K-PET, and aluminum-deposited PET (VMPET), polypropylene substrates such as stretched PP (OPP), non-stretched PP (CPP), aluminum-deposited PP, K-PP, and co-extruded PP film, and synthetic resin film substrates such as LDPE film, LLDPE film, EVA film, stretched LDPE film, stretched HDPE film, and polystyrene film, and these may be printed. In addition, various pretreatments such as corona treatment, frame treatment, plasma treatment, ultraviolet treatment, and anchor coat treatment may be performed as necessary.

[0036] In the laminate of the present invention, the sealant layer and the substrate layer may be disposed adjacent to each other, but it is desirable to provide a barrier material layer between the substrate layer and the sealant layer as necessary. The barrier material layer is composed of a material that blocks gases such as oxygen or water vapor to prevent deterioration of the contents, and depending on the application, it may be made of a polyamide film, a polyethylene terephthalate film, a polyvinyl alcohol film, an aluminum-deposited film, a metal foil such as aluminum foil, a saponified ethylene-vinyl acetate copolymer, or the like. In particular, aluminum foil with low gas permeability and water vapor permeability, and a saponified ethylene-vinyl acetate copolymer with low gas permeability are preferred. These materials may be overlapped with the substrate layer described above, for example, a substrate layer having barrier properties such as aluminum-deposited PET or aluminum-deposited PP. In addition, when the adhesion to the substrate layer is poor, secondary processability may be improved by surface treatment such as ozone treatment, corona discharge treatment, and application of a surfactant.

[0037] The laminate of the present invention is not limited thereto, and for example, a layer made of a polyolefin such as polyethylene, an ionomer resin, an acid-modified polyolefin and / or rubber obtained by graft-modifying various polyolefins and / or rubbers with an unsaturated carboxylic acid or a derivative thereof may be further provided between the substrate layer and the sealant layer, between the substrate layer and the barrier material layer, between the barrier material layer and the sealant layer, or on the outside of the substrate layer.

[0038] For example, the layer structure is as follows: PET base material / PE laminate / sealant layer, PET base material / PE laminate / Al / sealant layer, PET base material / PE laminate / Al / PE laminate / sealant layer, PET base material / acid-modified PE / EVOH / PE laminate / sealant layer, PET base material / Al / PE laminate / sealant layer, Nylon-based substrate / PE laminate / sealant layer, Nylon-based substrate / PE laminate / Al / sealant layer, Nylon-based substrate / PE laminate / Al / PE laminate / sealant layer, Nylon-based substrate / acid-modified PE / EVOH / sealant layer, Examples include paper / PE laminate / sealant layer, paper / PE laminate / Al / sealant layer, paper / PE laminate / Al / PE laminate / sealant layer, paper / acid-modified PE / EVOH / sealant layer, OPP / PE laminate / sealant layer, OPP / PE laminate / Al / sealant layer, K-nylon / acid-modified PE / EVOH / sealant layer, stretched HDPE / acid-modified PE / EVOH / PE laminate / sealant layer, nonwoven fabric / acid-modified PE / EVOH / PE laminate / sealant layer, etc. Aluminum vapor deposition film or silica vapor deposition film may be used instead of Al. (Here, PE laminate: laminate layer of polyethylene resin, Al: aluminum foil, acid-modified PE: maleic anhydride-modified polyethylene).

[0039] (vi) Use of the laminate The laminate of the present invention has at least a layer made of the resin composition of the present invention described above, and therefore can be suitably used as a packaging material. In particular, the laminate of the present invention is suitable as a packaging material for contents that tend to be easily charged, specifically as a packaging material for bonito packs.

[0040] (vii) Method for producing laminate In the laminate of the present invention, the layer made of the resin composition of the present invention is preferably produced by an extrusion lamination method. The extrusion lamination method is a method in which a molten resin composition is extruded from a die into a film shape, and a layer made of the resin composition is laminated on a substrate layer or the like. For example, there is a method in which a resin such as LDPE or LLDPE is laminated to a base layer by extrusion lamination, and then a sealant layer is laminated by extrusion lamination, or a method in which a resin such as LDPE or LLDPE is laminated to a base layer by extrusion lamination, and at the same time an aluminum base is sandwiched between them, and then a sealant layer is laminated by extrusion lamination. Various methods may be used, including a method in which an adhesive is interposed between the base layer and the resin such as LDPE or LLDPE. EXAMPLES

[0041] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating physical properties and processability, and the resins, substrates, and additives used in the examples and comparative examples are as follows.

[0042] 1. Evaluation method of physical properties (1)Melt flow rate (MFR): Measurements were performed in accordance with JIS K7210 test condition 4 (190°C, 21.18N load). (2) Density: Measurements were performed in accordance with JIS K7112. (3) Molecular weight distribution (Mw / Mn): The measurement was performed by gel permeation chromatography (GPC) under the following conditions: Apparatus: Waters GPC 150C Detector: MIRAN 1A infrared spectrophotometer (measurement wavelength: 3.42 μm) Column: Showa Denko AD806M / S 3 columns (The columns were calibrated by measuring Tosoh monodisperse polystyrene (A500, A2500, F1, F2, F4, F10, F20, F40, F288, each 0.5 mg / ml solution), and approximating the logarithm of the elution volume and molecular weight with a quadratic equation. The molecular weight of the sample was converted to polyethylene using the viscosity equation for polystyrene and polyethylene. Here, the coefficients of the viscosity equation for polystyrene are α=0.723, logK=-3.967, and for polyethylene, α=0.733, logK=-3.407.) Measurement temperature: 140℃ Concentration: 20mg / 10mL Injection amount: 0.2ml Solvent: ortho-dichlorobenzene Flow rate: 1.0ml / min

[0043] 2. Evaluation method of resin composition and laminate (1)Surface resistivity: The surface resistivity was measured using a Mitsubishi Petrochemical Co., Ltd. MCP-HT250 surface resistivity tester by applying a charge of 500V for 1 minute. The unit is Ω / □. (2)Half-life: A charge of 10 kV was applied for 2 minutes using a Shishido Electrostatic Static Honest Meter H-0110, and the time it took for the initial charged voltage to decay to half was measured. (3) Heat seal strength: The laminated film was cut to a width of 15 mm, and the sealant surfaces were aligned together. The upper seal bar of a Tester Sangyo hot platen heat sealer was set at 120°C, the lower seal bar at 30°C, and the sealing pressure was 2kg / cm. 2 The strength of the heat-sealed portion was measured at a tensile speed of 300 mm / min using a tensile tester manufactured by Toyo Seiki Co., Ltd. The heat-seal strength was evaluated based on the measured values ​​according to the following criteria. 〇: The decrease is 3N or less compared to the additive-free product △: Reduction is more than 3N and less than 10N compared to additive-free product ×: 10N or more decrease compared to additive-free product (4) Haze Haze was measured using a Haze Meter HM-150 manufactured by Murakami Color Research Laboratory. Haze was evaluated based on the measured value according to the following criteria. 〇: Less than 0.5% decrease compared to additive-free product △: Decrease is more than 0.5% and less than 2% compared to additive-free product ×: 2% or more decrease compared to additive-free product

[0044] 3. Raw materials (1)Resin used: The following polyethylene resins were used: (i) Ethylene-vinyl acetate copolymer produced by radical polymerization (MFR: 10 g / 10 min, VA: 7 wt%, Mw / Mn: 5.36, brand: EVA LV271, manufactured by Japan Polyethylene Co., Ltd.) (ii) Ethylene-1-hexene copolymer (density: 0.919 g / cm 3 , MFR: 10g / 10min, Brand: Kernel KC581, made by Japan Polyethylene Co., Ltd.)

[0045] (2) Antistatic agents The following antistatic agents were used: (A): Diglycerol fatty acid ester (Rikemal S-71-D, manufactured by Riken Vitamin Co., Ltd.) (B): Glycerin monostearate (Kao Corporation, TS-5BS)

[0046] (3) Base material: The following substrates were used: (i) ASOPP (brand P2241: manufactured by Toyobo Co., Ltd.) (ii) EVOH (brand: manufactured by Kuraray Co., Ltd.)

[0047] 4.Processing conditions and equipment The laminate was processed using the following equipment and conditions. Equipment: Modern, 90mmφ single laminating machine Die width: 500mm Machining speed: 100m / min Anchor coating agent: A3210 / A3075 (manufactured by Mitsui Chemicals Polyurethanes, Inc.)

[0048] [Example 1] A master batch was prepared by kneading and pelletizing (A) 5 wt% diglycerol fatty acid ester with an ethylene-vinyl acetate copolymer resin (brand: EVA LV271, manufactured by Japan Polyethylene Co., Ltd.) with a melt flow rate (MFR) of 10g / 10min and VA of 7% using a twin-screw extruder manufactured by Toshiba Machine Co., Ltd. Additionally, (B) glycerol monostearate ester (manufactured by Kao Corporation, TS-5B) as a glycerol fatty acid ester was kneaded and pelletized in the same manner to prepare a master batch. Again, 1.6 wt% of (A) diglycerol fatty acid ester masterbatch and 4.8 wt% of (B) glycerol fatty acid ester masterbatch were added to LV271 manufactured by Japan Polyethylene Corporation, and the mixture was mixed so that the diglycerol fatty acid ester (A) and the glycerol fatty acid ester (B) were 0.12 wt% and 0.35 wt%, respectively. The base material was an OPP (25μ, Toyobo Co., Ltd., brand P2241) containing an antistatic agent and an EVOH film (12μ, Kuraray Co., Ltd., brand EF-XL) laminated in advance by dry lamination on the EVOH#12 surface, on which a linear low-density polyethylene resin (density: 0.919 g / cm3 A laminate was prepared by extrusion laminating an LLDPE film having a thickness of 30 μm using an anchor coating agent (Takelac A3210 / A3075 (aromatic ester), manufactured by Mitsui Chemicals Polyurethanes, Inc.) with an LLDPE film having a thickness of 30 μm. Next, the prepared pellets were fed to a 90 mmφ single laminator manufactured by Modern Co., Ltd., and laminated onto the LLDPE side of the laminate to a thickness of 40 μm to obtain a laminate. The obtained laminate was used to evaluate the heat seal strength between the sealant layers, antistatic performance (surface resistivity, half-life), and transparency after one month of storage. The evaluation results are shown in Table 1.

[0049] [Examples 2 to 5] In Examples 2 to 5, laminates were produced and evaluated in the same manner as in Example 1, except that the blending amounts of the antistatic agents (A) and (B) were changed to the ratios shown in Table 1. The evaluation results are shown in Table 1.

[0050] [Example 6] In Example 6, the blending amounts of the antistatic agents (A) and (B) were changed to the ratios shown in Table 1, and the laminate thickness of the linear low density polyethylene resin was set to 15 μm, and the EVA thickness was also set to 15 μm. Except for this, a laminate was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0051] [Example 7] In Example 7, the blending amounts of the antistatic agents (A) and (B) were changed to the ratios shown in Table 1, and the laminate thickness of the linear low density polyethylene resin was set to 20 μm, and the EVA thickness was set to 30 μm. Except for this, a laminate was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0052] [Comparative Example 1] In Comparative Example 1, except that no antistatic agent was used, a laminate was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0053] [Comparative Examples 2 to 5] In Comparative Examples 2 to 5, laminates were produced and evaluated in the same manner as in Examples 2 to 5, except that the blending amounts of the antistatic agents (A) and (B) were changed to the ratios shown in Table 2. The evaluation results are shown in Table 2.

[0054] [Comparative Example 6] In Comparative Example 6, a laminate was produced and evaluated in the same manner as in Example 6, except that the blending amounts of the antistatic agents (A) and (B) were changed to the ratios shown in Table 2. The evaluation results are shown in Table 2.

[0055] [Comparative Example 7] In Comparative Example 7, a laminate was produced and evaluated in the same manner as in Example 7, except that the blending amounts of the antistatic agents (A) and (B) were changed to the ratios shown in Table 2. The evaluation results are shown in Table 2.

[0056] [Table 1]

[0057] [Table 2]

Claims

1. The antistatic layer has a layer on at least one surface thereof made of a resin composition (excluding compositions containing sorbitan aliphatic esters and compositions containing liquid polyolefins) in which 0.05 to 0.20% by weight of (A) diglycerol fatty acid ester and 0.20 to 0.40% by weight of (B) glycerol fatty acid ester are blended with an ethylene-vinyl acetate copolymer as an antistatic agent, and has a surface resistivity of 10 or more at an applied voltage of 500 V. 13 The packaging material for bonito packs is characterized by comprising a laminate having a half-life of 60 seconds or less and an honestometer half-life of 60 seconds or less.

2. 2. The packaging material for bonito packs according to claim 1, wherein the layer made of the resin composition is produced by an extrusion lamination method.

Citation Information

Patent Citations

  • Polyolefine resin multi-layer stretched film for packaging

    JP1998244638A

  • Antistatic agent for olefinic resin and olefinic resin composition containing the same

    JP1999071482A

  • Polyolefinic resin laminated film

    JP2000343655A

  • Anti-fogging film

    JP2003321613A

  • Laminated body for dispensing packaging and packaging bag for dispensing packaging using the same

    JP2005305830A