Manufacturing method for all-solid-state batteries

The manufacturing method for all-solid-state batteries with a sublimable filler and voids in the second electrolyte layer addresses durability issues by preventing cracks and short circuits, ensuring efficient battery operation.

JP7578024B2Active Publication Date: 2024-11-06TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021030005
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-26
Publication Date
2024-11-06
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Conventional all-solid-state batteries face issues with durability due to cracks in the solid electrolyte and densification of voids, leading to short circuits and crushing problems.

Method used

A manufacturing method for all-solid-state batteries involving a negative electrode electrolyte layer, a positive electrode electrolyte layer, and a first solid electrolyte layer with a sublimable filler between them, followed by densification and sublimation of the filler to create voids in the second solid electrolyte layer, enhancing durability.

Benefits of technology

The method improves the durability of all-solid-state batteries by preventing cracks and short circuits, allowing efficient charging and discharging while maintaining strong bonding between layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578024000002
    Figure 0007578024000002
  • Figure 0007578024000003
    Figure 0007578024000003
  • Figure 0007578024000001
    Figure 0007578024000001
Patent Text Reader

Abstract

To provide a method for manufacturing an all-solid battery, which enables the enhancement in durability.SOLUTION: A method for manufacturing an all-solid battery comprises the steps of: obtaining a laminate that includes a negative electrode electrolyte layer; a positive electrode electrolyte layer; and a second solid electrolyte layer including a first solid electrolyte layer and a sublimable filler, disposed between the negative and positive electrode electrolyte layers; densifying the laminate; and sublimating the sublimable filler from the second solid electrolyte layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to all-solid-state batteries. [Background technology]

[0002] An all-solid-state battery includes a positive electrode including a positive electrode active material layer, a negative electrode including a negative electrode active material layer, and a solid electrolyte layer including a solid electrolyte disposed therebetween. For example, Patent Document 1 discloses a negative electrode and a negative electrode active material for an all-solid-state battery that are suitable for achieving high energy density and capacity retention rate. Patent Document 2 discloses a solid electrolyte sheet in which a solid electrolyte layer having a porosity of 10% or less and a fragile layer (negative electrode side) having a porosity of 15% or more are laminated, and the fragile layer is manufactured by adjusting the pressing pressure. Patent Document 3 also discloses that the solid electrolyte layer of the all-solid-state battery comprises a powder compact portion formed by compacting a powder of a first solid electrolyte, and a surface deposition film formed by depositing a second solid electrolyte by a vapor phase method on at least one surface of the positive electrode side or the negative electrode side. It is said that the provision of the surface deposition film makes it possible to suppress dendrite growth of metallic lithium and prevent internal short circuits in the battery. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-054720 A [Patent Document 2] JP 2020-107594 A [Patent Document 3] JP 2009-301959 A Summary of the Invention [Problem to be solved by the invention]

[0004] The above-mentioned conventional techniques disclose all-solid-state batteries using alloy-based active materials, but such all-solid-state batteries have problems with durability, such as cracks occurring in the solid electrolyte causing short circuits and voids in the solid electrolyte collapsing due to densification. Therefore, an object of the present disclosure is to provide a method for producing an all-solid-state battery capable of improving durability. [Means for solving the problem]

[0005] As one means for solving the above problems, the present disclosure discloses a method for producing an all-solid-state battery, the method including the steps of obtaining a laminate having a negative electrode electrolyte layer, a positive electrode electrolyte layer, and a second solid electrolyte layer containing a first solid electrolyte layer and a sublimable filler, the second solid electrolyte layer being disposed between the negative electrode electrolyte layer and the positive electrode electrolyte layer, densifying the laminate, and sublimating the sublimable filler from the second solid electrolyte layer. Effect of the Invention

[0006] According to the manufacturing method of an all-solid-state battery of the present disclosure, it is possible to improve the durability of the obtained all-solid-state battery. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a diagram illustrating a layer structure of the all-solid-state battery 10. [Diagram 2] 1 is a diagram illustrating a flow of a manufacturing method S10 for an all-solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1.All-solid-state battery First, an all-solid-state battery produced by the production method of the present disclosure will be described. A schematic cross-sectional view showing an example of an all-solid-state battery is shown in Fig. 1. As shown in Fig. 1, an all-solid-state battery 10 has a positive electrode active material layer 11 containing a positive electrode active material, a negative electrode active material layer 12 containing a negative electrode active material, a first solid electrolyte layer 13 and a second solid electrolyte layer 14 formed between the positive electrode active material layer 11 and the negative electrode active material layer 12, a positive electrode current collector layer 15 that collects current from the positive electrode active material layer 11, and a negative electrode current collector layer 16 that collects current from the negative electrode active material layer 12. The positive electrode active material layer 11 and the positive electrode current collector layer 15 may be collectively referred to as a positive electrode, and the negative electrode active material layer 12 and the negative electrode current collector layer 16 may be collectively referred to as a negative electrode. Each component of the all-solid-state battery 10 will be described below.

[0009] 1.1. Positive electrode active material layer The positive electrode active material layer 11 is a layer containing a positive electrode active material, and may further contain at least one of a solid electrolyte material, a conductive material, and a binder, as necessary. The positive electrode active material may be a known active material. For example, cobalt-based (LiCoO2, etc.), nickel-based (LiNiO2, etc.), manganese-based (LiMn2O4, Li2Mn2O3, etc.), iron phosphate-based (LiFePO4, Li2FeP2O7, etc.), NCA-based (nickel, cobalt, aluminum compound), NMC-based (nickel, manganese, cobalt compound), etc. are listed. More specifically, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc. The surface of the positive electrode active material may be covered with an oxide layer such as a lithium niobate layer, a lithium titanate layer, or a lithium phosphate layer.

[0010] The solid electrolyte is preferably an inorganic solid electrolyte, since it has higher ionic conductivity and superior heat resistance compared to organic polymer electrolytes. Examples of inorganic solid electrolytes include sulfide solid electrolytes and oxide solid electrolytes. Examples of sulfide solid electrolyte materials having Li ion conductivity include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S- Examples of the sulfide include SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-ZmSn (where m and n are positive numbers. Z is any of Ge, Zn, and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, and Li2S-SiS2-LixMOy (where x and y are positive numbers. M is any of P, Si, Ge, B, Al, Ga, and In). The above description of "Li2S-P2S5" refers to a sulfide solid electrolyte material made using a raw material composition containing Li2S and P2S5, and the same applies to other descriptions.

[0011] On the other hand, examples of oxide solid electrolyte materials having Li ion conductivity include compounds having a NASICON structure. An example of a compound having a NASICON structure is a compound represented by the general formula Li 1+x Al x Ge 2-x Compounds represented by the formula (PO4)3 (0≦x≦2) (LAGP), general formula Li 1+x Al x Ti 2-x (PO4)3 (0≦x≦2) (LATP) and the like. Another example of the oxide solid electrolyte material is LiLaTiO (for example, Li 0.34 La 0.51 TiO3), LiPON (e.g., Li 2.9 PO 3.3 N 0.46 ), LiLaZrO (e.g., Li7La3Zr2O 12 ) etc.

[0012] The binder is not particularly limited as long as it is chemically and electrically stable, and examples thereof include fluorine-based binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE), rubber-based binders such as styrene butadiene rubber (SBR), olefin-based binders such as polypropylene (PP) and polyethylene (PE), and cellulose-based binders such as carboxymethylcellulose (CMC). As the conductive material, carbon materials such as acetylene black and ketjen black, and metal materials such as nickel, aluminum, and stainless steel can be used.

[0013] The content of each component in the positive electrode active material layer 11 and the shape of the positive electrode active material layer 11 may be the same as in the past. In particular, a sheet-shaped positive electrode active material layer 11 is preferable from the viewpoint of easily configuring the all-solid-state battery 10. In this case, the thickness of the positive electrode active material layer 11 is preferably, for example, 0.1 μm or more and 1 mm or less, and more preferably 1 μm or more and 150 μm or less.

[0014] 1.2.Negative electrode active material layer The negative electrode active material layer 12 is a layer containing at least a negative electrode active material, and may contain at least one of a solid electrolyte material, a conductive material, and a binder, as necessary. The solid electrolyte material, the conductive material, and the binder can be considered to be the same as those of the positive electrode active material layer 11.

[0015] The negative electrode active material is not particularly limited. In the case of forming a lithium ion battery, examples of the negative electrode active material include carbon materials such as graphite and hard carbon, various oxides such as lithium titanate, Si and Si alloys, metallic lithium and lithium alloys, and the like.

[0016] 1.3.First solid electrolyte layer In this embodiment, the first solid electrolyte layer 13 is a solid electrolyte layer disposed on the positive electrode active material layer 11 side between the positive electrode active material layer 11 and the negative electrode active material layer 12. The first solid electrolyte layer 13 contains at least a solid electrolyte material. The solid electrolyte material can be considered to be the same as the solid electrolyte material described for the positive electrode active material layer 11.

[0017] 1.4.Second solid electrolyte layer In this embodiment, the second solid electrolyte layer 14 is a solid electrolyte layer disposed on the negative electrode active material layer 12 side between the positive electrode active material layer 11 and the negative electrode active material layer 12. That is, in this embodiment, the second solid electrolyte layer 14 is disposed between the first solid electrolyte 13 and the negative electrode active material layer 12. The second solid electrolyte layer 14 contains at least a solid electrolyte material. The solid electrolyte material can be considered to be similar to the solid electrolyte material described for the positive electrode active material layer 11.

[0018] Here, the second solid electrolyte layer 14 has a larger porosity than the first solid electrolyte layer 13. This can increase durability (suppress self-discharge voltage after cycling). This is because the porosity of the second solid electrolyte layer 14 is made larger than that of the first solid electrolyte 13, and the voids in the second solid electrolyte layer 14 relieve stress caused by a change in the volume of the negative electrode during charging and discharging, preventing the first solid electrolyte layer from cracking and short-circuiting. In addition, even if cracks occur in the second solid electrolyte layer 14, it is possible to suppress the cracks from reaching the positive electrode active material layer and short-circuiting. The above-mentioned effects are achieved so long as second solid electrolyte layer 14 has a larger porosity than first solid electrolyte layer 13, but the above-mentioned effects become more pronounced when the ratio (b / a) of the porosity b of second solid electrolyte layer 14 to the porosity a of first solid electrolyte layer 13 is 2 or greater.

[0019] The difference in thickness between second solid electrolyte layer 14 and first solid electrolyte layer 13 is not particularly limited, but the above-mentioned effect can be made more remarkable when the ratio (d / c) of the thickness d of second solid electrolyte layer 14 to the thickness c of first solid electrolyte layer 13 is in the range of 0.25 or more and 4 or less.

[0020] 1.5.Current collector layer The current collectors are a positive electrode current collector layer 15 that collects current from the positive electrode active material layer 11, and a negative electrode current collector layer 16 that collects current from the negative electrode active material layer 12. Examples of materials constituting the positive electrode current collector layer 15 include stainless steel, aluminum, nickel, iron, titanium, and carbon. On the other hand, examples of materials constituting the negative electrode current collector layer 16 include stainless steel, copper, nickel, and carbon.

[0021] 1.6.Battery case The all-solid-state battery may include a battery case (not shown) for housing each component, and may be, for example, a stainless steel battery case.

[0022] 2. Manufacturing method of all-solid-state batteries The manufacturing method of the all-solid-state battery will be described below. Fig. 2 shows the flow of the manufacturing method S10 of the all-solid-state battery according to one embodiment (sometimes referred to as "manufacturing method S10"). As can be seen from Fig. 2, the manufacturing method S10 includes steps of preparing a positive electrode side member (preparing a positive electrode paste S11, applying a positive electrode paste S12, preparing a first solid electrolyte layer paste S13, applying a first solid electrolyte layer paste S14), steps of preparing a negative electrode side member (preparing a negative electrode paste S15, applying a negative electrode paste S16, preparing a second solid electrolyte layer paste S17, applying a second solid electrolyte layer paste S18), a lamination and densification step S19, and a sublimable filler removal step S20. Each step will be described below. For ease of understanding, each layer is denoted by the same reference numeral as in the all-solid-state battery 10. However, the manufacturing method S10 can also be applied to the manufacture of all-solid-state batteries other than the all-solid-state battery 10.

[0023] 2.1. Process for producing the positive electrode component In the process of producing the positive electrode side member in this embodiment, a layer that will become the positive electrode active material layer 11 and a layer that will become the first solid electrolyte layer 13 are sequentially applied to a layer that will become the positive electrode current collector layer 15. More specifically, the process includes the steps of preparing a positive electrode paste S11, applying a positive electrode paste S12, preparing a first solid electrolyte layer paste S13, and applying a first solid electrolyte layer paste S14.

[0024] Specifically, a positive electrode active material is prepared, and necessary materials (solid electrolyte, binder, conductive material, etc.) are mixed with this positive electrode active material to obtain a positive electrode paste (positive electrode paste preparation S11). Next, the positive electrode paste obtained in positive electrode paste preparation S11 is applied to a layer that will become the positive electrode current collector layer 15 to a predetermined thickness, and dried to form a layer that will become the positive electrode active material layer 11 (positive electrode paste application S12).

[0025] A first solid electrolyte material (e.g., a sulfide solid electrolyte material) is prepared, and necessary materials (such as a binder) are mixed with it to obtain a first solid electrolyte layer paste (first solid electrolyte layer paste preparation S13). Thereafter, the first solid electrolyte paste obtained in first solid electrolyte layer paste preparation S13 is applied to a predetermined thickness on the layer that will become the positive electrode active material layer 11 formed in positive electrode paste application S12, and dried to obtain a layer that will become the first solid electrolyte layer 13 (first solid electrolyte layer paste application S14).

[0026] This results in a positive electrode side member (laminate) in which the layer that will become the positive electrode current collector layer 15, the layer that will become the positive electrode active material layer 11, and the layer that will become the first solid electrolyte layer 13 are laminated.

[0027] 2.2. Process for preparing the negative electrode component In this embodiment, the process of preparing the negative electrode side member is a process parallel to the process of preparing the positive electrode side member, and a layer that will become the negative electrode active material layer 12 and a layer that will become the second solid electrolyte layer 14 are sequentially applied to a layer that will become the negative electrode current collector layer 15. More specifically, the process includes the processes of preparing a negative electrode paste S15, applying a negative electrode paste S16, preparing a second solid electrolyte layer paste S17, and applying a second solid electrolyte layer paste S18.

[0028] Specifically, a negative electrode active material is prepared, and necessary materials (solid electrolyte, binder, conductive material, etc.) are mixed with this negative electrode active material to obtain a negative electrode paste (negative electrode paste preparation S15). Next, the negative electrode paste obtained in negative electrode paste preparation S15 is applied to a layer that will become the negative electrode current collector layer 16 to a predetermined thickness, and dried to form a layer that will become the negative electrode active material layer 12 (negative electrode paste application S16).

[0029] In addition, a second solid electrolyte material (for example, a sulfide solid electrolyte) is prepared, and necessary materials are prepared and mixed with this to obtain a second solid electrolyte layer paste (preparation of second solid electrolyte layer paste S17). As described above, second solid electrolyte layer 14 is configured to have a higher porosity than first solid electrolyte layer 13. Therefore, in second solid electrolyte layer paste preparation S17, a sublimable filler is included as a necessary material for forming the voids. The sublimable filler is a material that can be sublimated, is in a solid state in the second solid electrolyte layer paste preparation S17, and can be vaporized (sublimated) in the sublimable filler removal S20 described later. Such a material is not particularly limited, but may be, for example, sulfur. The amount of sublimable filler contained in the second solid electrolyte layer paste is determined so as to satisfy the porosity that is to be formed in second solid electrolyte layer 14 .

[0030] Thereafter, the second solid electrolyte paste obtained in second solid electrolyte layer paste preparation S17 is applied to a predetermined thickness on the layer that will become the negative electrode active material layer 12 formed in negative electrode paste application S16, and dried to obtain a layer that will become the second solid electrolyte layer 14 (second solid electrolyte layer paste application S18).

[0031] This results in a negative electrode member (laminate) in which the layer that will become the negative electrode current collector layer 16, the layer that will become the negative electrode active material layer 12, and the layer that will become the second solid electrolyte layer 14 are laminated.

[0032] 2.3.Layering and densification In the lamination and densification step S19, the layer that will become the first solid electrolyte layer 13 of the positive electrode side component and the layer that will become the second solid electrolyte layer 14 of the negative electrode side component that have been prepared up to this point are overlapped and pressed to densify them into a laminated electrode body.

[0033] 2.4. Sublimable filler removal In the step of removing the sublimable filler S20, the laminated electrode body obtained in the lamination and densification S19 is placed in an exterior body, and the sublimable filler contained in the layer that will become the second solid electrolyte layer 14 is removed. Any appropriate method may be selected as a means for removing the sublimable filler, and examples of the method include reduced pressure (heat) drying.

[0034] 2.5. Effects etc. According to the manufacturing method of the present disclosure, pressing is performed in a state in which the sublimable filler is contained before voids are formed, and therefore the restraining force is prevented from being absorbed by the voids during pressing and is efficiently transmitted to each layer, so that even with a low restraining pressure, the layers are firmly bonded together, making the material chargeable and dischargeable, and providing excellent cycle characteristics. In addition, since the sublimable filler is removed after pressing to form voids, the voids are not crushed and remain in the second solid electrolyte layer, and therefore, as described above, the change in the expansion and contraction of the electrodes due to charging and discharging when used as an all-solid-state battery can be efficiently absorbed.

[0035] 3.Other In the above description, an example was described in which the solid electrolyte layer is a first and a second solid electrolyte layer, but three or more solid electrolyte layers may be provided. In this case, at least one of the solid electrolyte layers should contain a sublimable filler and have a higher porosity than the other solid electrolyte layers. In the above description, the solid electrolyte layer on the cathode side has a higher porosity than the solid electrolyte layer on the cathode side, but the reverse may be true. However, since the cathode experiences a larger change in expansion and contraction during charging and discharging, it is preferable to place the second solid electrolyte layer on the cathode side as in this embodiment. In the above description, in the manufacturing process, all of the layers are laminated and then pressed (densified). However, the positive electrode side laminate including the first solid electrolyte layer and the negative electrode side laminate including the second solid electrolyte may be pressed (densified) separately and then the two laminates may be joined together.

[0036] 4. Test Example 4.1. Preparation of all-solid-state batteries for Tests 1 to 11

[0037] [Test 1] Example 1 is a method for producing an all-solid-state battery in which a sublimable filler is mixed in the second solid electrolyte layer (negative electrode side solid electrolyte layer) and the sublimable filler is sublimated after lamination and densification (pressing), forming voids in the second solid electrolyte layer, which is referred to as Production Method A here. It will be described in detail below.

[0038] <Preparation of coated positive electrode active material> The positive electrode active material is LiNi with an average particle diameter (D50) of 6 μm as measured by the laser diffraction / scattering method. 1 / 3 Mn 1 / 3 Co 1 / 3 The surface of the positive electrode active material was coated with LiNbO3 by a sol-gel method using O2 powder. Specifically, an equal number of moles of LiOC2H5 and Nb(OC2H5)5 were dissolved in an ethanol solvent to prepare a metal alkoxide liquid for coating. Then, the metal alkoxide liquid for coating was coated on the surface of the positive electrode active material using a rolling fluidized coating device (model: SFP-01, product of Powrex Corporation) under atmospheric pressure. At that time, the treatment time was adjusted so that the thickness of the coating film was about 5 nm. Next, the coated positive electrode active material was heat-treated at 350°C under atmospheric pressure for 1 hour to obtain LiNi whose surface was coated with LiNbO3. 1 / 3 Mn 1 / 3 Co 1 / 3 A positive electrode active material consisting of O2 was obtained.

[0039] <Preparation of the layer that will become the positive electrode> A positive electrode was fabricated using the positive electrode active material obtained above and 15LiBr 10LiI 75 (0.75Li2S 0.25P2S5) glass ceramics with an average particle size (D50) of 2.5 μm measured based on the laser diffraction / scattering method as a sulfide solid electrolyte. Specifically, the positive electrode active material and the sulfide solid electrolyte were weighed out so that the weight ratio of the positive electrode active material:sulfide solid electrolyte was 75:25. Furthermore, 4 parts by weight of a PVDF-based binder and 6 parts by weight of a conductive material (acetylene black) were weighed out per 100 parts by weight of the positive electrode active material. These were mixed with butyl butyrate to give a solid content of 70% by weight and kneaded with a stirrer to obtain a composition for forming a positive electrode active material layer (positive electrode paste). The obtained positive electrode paste was then applied by blade coating using a commercially available applicator onto a positive electrode current collector made of aluminum foil having a thickness of 15 μm in an amount of 26 mg / cm2. 2 The coating was then dried at 120° C. for 3 minutes to obtain a layer that would become a positive electrode, in which a layer that would become a positive electrode active material layer was formed on a layer that would become a positive electrode current collector made of aluminum foil.

[0040] <Preparation of the negative electrode layer> A negative electrode was prepared by using Si (silicon) powder with an average particle size (D50) of 6 μm measured based on a laser diffraction / scattering method as the negative electrode active material, and the same sulfide solid electrolyte as the positive electrode as the solid electrolyte. Specifically, the negative electrode active material and the sulfide solid electrolyte were weighed out so that the weight ratio of the negative electrode active material to the sulfide solid electrolyte was negative electrode active material:sulfide solid electrolyte=55:45, and 6 parts by weight of a PVDF-based binder and 6 parts by weight of a conductive material (acetylene black) were weighed out for 100 parts by weight of the negative electrode active material, and these were mixed with butyl butyrate to a solid content of 70% by weight, and kneaded with a stirrer to obtain a composition for forming a negative electrode active material layer (negative electrode paste). Next, the obtained negative electrode paste was applied by blade coating using a commercially available applicator to a layer that would become a negative electrode current collector layer made of copper foil with a thickness of 15 μm in an amount of 4.0 mg / cm 2 The coating was then dried at 120° C. for about 3 minutes to obtain a layer that would become a negative electrode, in which a layer that would become a negative electrode active material layer was formed on a layer that would become a negative electrode current collector made of copper foil.

[0041] <Preparation of Layer to Become First Solid Electrolyte Layer> Using the sulfide solid electrolyte used in the preparation of the layer to become the positive electrode and the layer to become the negative electrode, a layer to become a first solid electrolyte layer was prepared on the layer to become the positive electrode. First, a layer to become the positive electrode active material layer was covered with stainless steel (SUS) foil, and pressure was applied using a press (25° C., 15 MPa, 30 seconds). Next, 99.0 parts by weight of a sulfide solid electrolyte and 1.0 part by weight of an SBR (styrene-butadiene rubber)-based binder were weighed out, mixed with butyl butyrate to give a solid content of 60% by weight, and subjected to ultrasonic dispersion treatment for about 2 minutes using an ultrasonic dispersion device (model: UH-50, product of SMT Corporation) to obtain a composition for forming a first solid electrolyte layer (first solid electrolyte paste). Thereafter, the obtained first solid electrolyte paste was applied to the layer that would become the positive electrode active material layer in a manner similar to that used for producing the positive electrode, with a basis weight of 8.0 mg / cm2. 2 After uniformly applying the coating to a thickness of 40 μm, the coating was naturally dried and then further dried at 120° C. for about 3 minutes to laminate the layer that would become the first solid electrolyte layer on the layer that would become the positive electrode active material layer.

[0042] <Preparation of Layer to Become Second Solid Electrolyte Layer> Using the sulfide solid electrolyte used in the preparation of the layer to become the positive electrode and the layer to become the negative electrode, a layer to become a second solid electrolyte layer was prepared on the layer to become the negative electrode. First, a layer to become the negative electrode active material layer was covered with stainless steel SUS foil, and pressure was applied using a press (25° C., 15 MPa, 30 seconds). Next, 88.6 parts by weight of the sulfide solid electrolyte, 1.0 part by weight of an SBR (styrene-butadiene rubber)-based binder, and 10.4 parts by weight of sulfur as a sublimable filler were weighed out, mixed with butyl butyrate to give a solid content of 60% by weight, and subjected to ultrasonic dispersion treatment for about 2 minutes using an ultrasonic dispersion device (model: UH-50, product of SMT Co., Ltd.) to obtain a composition for forming a second solid electrolyte (second solid electrolyte paste). Thereafter, the obtained second solid electrolyte paste was applied to the layer that becomes the negative electrode active material layer in a manner similar to that for producing the layer that becomes the positive electrode described above, so as to have a basis weight of 2.0 mg / cm 2After uniformly applying the coating to a thickness of 10 μm, the coating was naturally dried and then further dried at 120° C. for about 3 minutes to laminate the layer that would become the second solid electrolyte layer on the layer that would become the negative electrode active material layer.

[0043] <Fabrication of all-solid-state batteries (battery assemblies) and formation of voids> The layer to become the positive electrode and the layer to become the first solid electrolyte layer were punched out together with the aluminum foil into a square shape measuring 3 cm in length and 3 cm in width, and placed on top of the layer to become the negative electrode and the layer to become the second solid electrolyte layer that had been punched out into the same shape. The mixture was pressed at 25°C and a pressure of 300 MPa for 1 minute to obtain a laminated electrode body. The laminated electrode body thus obtained was placed in an exterior body made of an aluminum laminate film to which positive and negative electrode terminals had been previously attached, and subjected to a process of vacuum drying at 140°C for 12 hours to remove sulfur from the second solid electrolyte layer on the negative electrode side, followed by sealing, thereby obtaining an all-solid-state battery (all-solid-state lithium ion secondary battery) according to Example 1 having voids in the solid electrolyte layer after electrode body joining and densification.

[0044] [Test 2] In preparing the second solid electrolyte paste, the compounding ratio was 78 parts by weight of the sulfide solid electrolyte, 1.0 part by weight of an SBR (styrene-butadiene rubber)-based binder, and 21 parts by weight of sulfur, but the same materials and steps as those in Example 1 were used to obtain an all-solid-state battery (all-solid-state lithium ion secondary battery) of Example 2.

[0045] [Test 3] In preparing the second solid electrolyte paste, the compounding ratio was 67.2 parts by weight of the sulfide solid electrolyte, 1.0 part by weight of an SBR (styrene-butadiene rubber)-based binder, and 31.8 parts by weight of sulfur, but the same materials and steps as those in Example 1 were used to obtain an all-solid-state battery (all-solid-state lithium ion secondary battery) of Example 3.

[0046] [Test 4] In preparing the second solid electrolyte paste, the compounding ratio was 56.2 parts by weight of the sulfide solid electrolyte, 1.0 part by weight of an SBR (styrene-butadiene rubber)-based binder, and 42.8 parts by weight of sulfur, but the same materials and steps as those in Example 1 were used to obtain an all-solid-state battery (all-solid-state lithium ion secondary battery) of Example 4.

[0047] [Test 5] The weight of the first solid electrolyte layer is 5.0 mg / cm 2 (Thickness 25μm), weight of the second solid electrolyte layer is 5.0mg / cm 2 An all-solid-state battery (all-solid-state lithium ion secondary battery) of Example 5 was obtained using the same materials and steps as in Example 2, except that the coating was uniformly applied to a thickness of 25 μm.

[0048] [Test 6] The weight of the first solid electrolyte layer is 2.0 mg / cm 2 (Thickness 10μm), weight of the second solid electrolyte layer is 8.0mg / cm 2 An all-solid-state battery (all-solid-state lithium ion secondary battery) of Example 6 was obtained using the same materials and steps as in Example 2, except that the coating was uniformly applied to a thickness of 40 μm.

[0049] [Test 7] In preparing the second solid electrolyte layer paste, the compounding ratio was 93.9 parts by weight of sulfide solid electrolyte, 1.0 part by weight of SBR (styrene-butadiene rubber)-based binder, and 5.1 parts by weight of sulfur as a sublimable filler. Except for this, an all-solid-state battery (all-solid-state lithium-ion secondary battery) of Test 7 was obtained using the same materials and processes as Test 1.

[0050] [Test 8] The weight of the first solid electrolyte layer is 9.0 mg / cm 2 (Thickness 45μm), weight of the second solid electrolyte layer is 1.0mg / cm 2 An all-solid-state battery (all-solid-state lithium ion secondary battery) of Test 8 was obtained using the same materials and steps as in Example 2, except that the coating was uniformly applied to a thickness of 5 μm.

[0051] [Test 9] The weight of the first solid electrolyte layer is 1.6 mg / cm 2 (thickness 8μm), weight of the second solid electrolyte layer is 8.4mg / cm 2 An all-solid-state battery (all-solid-state lithium ion secondary battery) of Test 9 was obtained using the same materials and steps as in Example 2, except that the coating was uniformly applied to a thickness of 42 μm.

[0052] [Test 10] The layers that would become the solid electrolyte layer were pressed separately to adjust the porosity, and then the positive electrode and negative electrode components were joined to produce an all-solid-state battery. This is called manufacturing method B. In test 10, the positive electrode was the same as that produced by manufacturing method A, and the negative electrode was produced by manufacturing method B.

[0053] <Preparation of the first solid electrolyte layer> The sulfide solid electrolyte used in the preparation of the positive and negative electrodes was used to form a layer that would become a first solid electrolyte layer on the layer that would become the positive electrode. First, the positive electrode active material layer was covered with stainless steel (SUS) foil and pressed with a press (25°C, 15 MPa, 30 seconds). Next, 99.0 parts by weight of the sulfide solid electrolyte and 1.0 part by weight of an SBR (styrene-butadiene rubber)-based binder were weighed out, mixed with butyl butyrate to give a solid content of 60% by weight, and subjected to ultrasonic dispersion treatment for about 2 minutes using an ultrasonic dispersion device (model: UH-50, product of SMT Corporation) to obtain a composition for forming a first solid electrolyte (first solid electrolyte paste). The obtained first solid electrolyte paste was applied to a layer that would become a positive electrode active material layer in a manner similar to that used for producing the positive electrode, with a basis weight of 8.0 mg / cm2. 2 (thickness 40 μm), which was then naturally dried and further dried at 120° C. for about 3 minutes to produce a layer that would become a first solid electrolyte layer on the layer that would become the positive electrode active material layer.

[0054] <Preparation of second solid electrolyte layer> The second solid electrolyte layer was prepared on the negative electrode using the sulfide solid electrolyte used in the preparation of the positive and negative electrodes. First, the negative electrode active material layer was covered with stainless steel (SUS) foil and pressed with a press (25°C, 300 MPa, 1 minute). Next, 99.0 parts by weight of the sulfide solid electrolyte and 1.0 part by weight of an SBR (styrene-butadiene rubber)-based binder were weighed out and mixed with butyl butyrate to give a solid content of 60% by weight. The mixture was subjected to ultrasonic dispersion treatment for about 2 minutes using an ultrasonic dispersion device (model: UH-50, manufactured by SMT Corporation) to obtain a composition for forming a second solid electrolyte (second solid electrolyte paste). The obtained second solid electrolyte paste was then applied to the layer that would become the negative electrode active material layer in a manner similar to that used for producing the positive electrode, with a basis weight of 2.0 mg / cm2. 2 (thickness 10 μm), and then naturally dried and dried for about 3 minutes at 120° C. Furthermore, the layer to become the negative electrode coated with the layer to become the second solid electrolyte layer was pressed with a press (25° C., 24 MPa, 30 seconds) to obtain a layer to become the second solid electrolyte layer having voids on the layer to become the negative electrode active material layer.

[0055] <Production of all-solid-state battery (battery assembly)> The positive electrode and the first solid electrolyte layer were punched together with the aluminum foil into a square shape of 3 cm in length and 3 cm in width, and pressed at 25°C and 300 MPa for 1 minute. Next, the layer to become the negative electrode and the layer to become the second solid electrolyte layer punched into the same shape were superimposed on the layer to become the positive electrode and the layer to become the first solid electrolyte, and pressed at 25°C and 24 MPa for 30 seconds to obtain a laminated electrode body. This laminated electrode body was placed in an exterior body made of an aluminum laminate film to which positive and negative electrode terminals were previously attached, and sealed, and a void was formed in the layer to become the second solid electrolyte layer, and then the all-solid-state battery (all-solid-state lithium-ion secondary battery) of Test 10 was obtained.

[0056] [Test 11] In Test 11, an all-solid-state battery was produced in which a layer to become a solid electrolyte layer, which was not mixed with a sublimable filler (sulfur in Test 1) in the layer to become the second solid electrolyte layer produced in Test 1, was formed only on the negative electrode side. Specifically, the layer to become the first solid electrolyte layer described in Test 1 was not provided, and the mixture ratio was 99 parts by weight of sulfide solid electrolyte, 1.0 part by weight of SBR (styrene-butadiene rubber)-based binder, and the basis weight was 10.0 mg / cm in the same manner as in the production of the second solid electrolyte paste. 2(thickness 50 μm). Otherwise, the same materials and processes as those in Test 1 were used to obtain an all-solid-state battery (all-solid-state lithium-ion secondary battery) for Test 11.

[0057] Evaluation [Measurement of thickness and porosity of solid electrolyte layer] The actual thickness of the solid electrolyte layer was read from the cross-sectional SEM image of the laminated all-solid-state battery. The thickness at 100% packing rate was calculated from the specific gravity, composition ratio, and basis weight of each material, and the porosity was calculated from the difference with the actual thickness.

[0058] [Cell resistance measurement] After restraining the all-solid-state battery of each test at a fixed size in the lamination direction of the electrode body at 1 MPa, it was charged and discharged at 4.5 V-CCCV charge, current rate 15 mA, current cut 1 mA, and discharged at 3.5 V-CCCV discharge, current rate 15 mA, current cut 1 mA, and left for 1 hour. It was then discharged at CC discharge, current rate 100 mA, current cut 10 seconds, and the cell resistance was measured according to Ohm's law. These results are shown in the corresponding columns of Table 1 as a ratio to Test 11.

[0059] [Durability test] After measuring the cell resistance, each solid-state battery was charged at 4.5V-CCCV, with a current rate of 15mA and a current cut of 1mA, and discharged at 2.5V-CCCV, with a current rate of 15mA and a current cut of 1mA, and then charged again at 4.5V-CCCV, with a current rate of 15mA and a current cut of 1mA, and the voltage drop after 24 hours was taken as the self-discharge voltage and used as an index of the durability of the solid electrolyte layer. These results are shown in the corresponding columns of Table 1 as a ratio to Test 11.

[0060] 4.3.Results Table 1 shows the main conditions and results of each test.

[0061] [Table 1]

[0062] Comparing Test 11 with Tests 1 to 10, it is clear that durability can be increased (self-discharge voltage after cycling can be suppressed) by providing a second solid electrolyte layer and making its porosity larger than that of the first solid electrolyte layer. Furthermore, among these, a larger porosity reduces stress caused by volumetric changes in the negative electrode during charging and discharging, preventing the solid electrolyte layer on the positive electrode side from cracking and short-circuiting. More specifically, a comparison of Tests 1 to 4 with Test 7 revealed that the self-discharge suppression effect is more pronounced when the ratio b / a, which is the ratio of the porosity a of the first solid electrolyte layer to the porosity b of the second solid electrolyte layer, is 2 or more. This is thought to be because the stress relaxation effect is enhanced by making the pores in the second solid electrolyte layer sufficiently large. Furthermore, by comparing Tests 2, 5, and 6 with Tests 8 and 9, it was found that the effect of suppressing the self-discharge voltage was significant when d / c, which is the ratio of the thickness c of the first solid electrolyte layer to the thickness d of the second solid electrolyte layer, was in the range of 0.25 to 4. This is thought to be because, by setting the ratio in this range, the thicknesses of the first solid electrolyte layer and the second solid electrolyte layer are balanced, making it possible to suppress cracking of either solid electrolyte layer.

[0063] A comparison of Test 1 and Test 10 also revealed the effect of reducing cell resistance due to the difference in process. As in Test 1, by pressing after bonding the positive electrode, solid electrolyte layer, and negative electrode, the interface was maintained even after the formation of voids, making it difficult for ion conduction to be hindered, and the increase in resistance could be suppressed. [Explanation of symbols]

[0064] 10 All-solid-state battery 11 Cathode active material layer 12 Negative electrode active material layer 13 First solid electrolyte layer 14 Second solid electrolyte layer 15 Positive electrode current collector layer 16 Negative electrode current collector layer

Claims

[Claim 1] A method for producing an all-solid-state battery, comprising: obtaining a laminate having a negative electrode active material layer, a positive electrode active material layer, and a second solid electrolyte layer including a first solid electrolyte layer and a sublimable filler, the second solid electrolyte layer being disposed between the negative electrode active material layer and the positive electrode active material layer; densifying the laminate; and sublimating the sublimable filler from the second solid electrolyte layer after the densifying step. How solid-state batteries are manufactured.

Citation Information

Patent Citations

  • Production of electrochemical cell

    JP1985135756A

  • All-solid lithium secondary battery

    JP2009301959A

  • Negative electrode for all-solid battery

    JP2017054720A

  • All-solid battery

    JP2018206727A

  • Manufacturing method of sulfide solid electrolyte

    JP2019192598A