Manufacturing method of superabsorbent resin

By incorporating an aqueous hydrophobic particle dispersion during monomer polymerization, the method enhances the water absorption rate and surface tension of superabsorbent resins, addressing the issues of leakage and property deterioration caused by traditional blowing agents and stabilizers.

JP7578325B2Active Publication Date: 2024-11-06LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023515365
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-16
Filing Date
2021-12-17
Publication Date
2024-11-06
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

Existing superabsorbent resins face challenges in maintaining high water absorption rates and surface areas while avoiding the deterioration of physical properties due to the use of carbonate-based blowing agents and bubble stabilizers, which reduce surface tension and lead to leakage issues.

Method used

A method involving the use of an aqueous hydrophobic particle dispersion during monomer polymerization to capture carbon dioxide bubbles, eliminating the need for separate bubble stabilizers and enhancing the specific surface area of the superabsorbent resin.

Benefits of technology

The method effectively increases the water absorption rate and surface tension of the superabsorbent resin, preventing leakage and maintaining optimal physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578325000001
    Figure 0007578325000001
Patent Text Reader

Abstract

The present invention relates to a method for producing a superabsorbent polymer. More specifically, the method enables the production of a superabsorbent polymer that exhibits high surface tension and improved water absorption rate without a decrease in water absorption properties when a monomer is polymerized in the presence of an aqueous dispersion of hydrophobic particles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0178430 filed on December 18, 2020, and Korean Patent Application No. 10-2021-0180294 filed on December 16, 2021, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a method for producing a superabsorbent resin, more specifically, to a method for producing a superabsorbent resin that can effectively capture carbon dioxide bubbles generated during polymerization of a monomer in the presence of an aqueous dispersion of hydrophobic particles, and that can produce a superabsorbent resin that exhibits high surface tension and improved water absorption speed without reducing water absorption properties. [Background technology]

[0003] Super absorbent polymer (SAP) is a synthetic polymeric material that can absorb 500 to 1,000 times its own weight in water, and is given different names by different developers, such as SAM (Super Absorbency Material) and AGM (Absorbent Gel Material). Such super absorbent polymers were first put to practical use as sanitary products, and are now widely used as materials for gardening soil repair agents, civil engineering and architectural waterproofing materials, seedling sheets, freshness preserving agents in the food distribution field, and for dripping.

[0004] Such superabsorbent polymers are widely used in the field of sanitary materials, such as diapers and sanitary belts. In the sanitary materials, the superabsorbent polymers are generally contained in a state of being spread in the pulp. However, in recent years, there have been ongoing efforts to provide sanitary materials, such as diapers, with thinner thicknesses, and as part of these efforts, the pulp content has been reduced or even no pulp is used at all, so-called pulpless diapers, etc., have been actively developed.

[0005] In the case of sanitary materials in which the pulp content is reduced or no pulp is used, the superabsorbent polymer is contained at a relatively high ratio, and the superabsorbent polymer particles are inevitably contained in multiple layers in the sanitary materials. In order for the overall superabsorbent polymer particles contained in multiple layers to more efficiently absorb a large amount of liquid such as urine, the superabsorbent polymer basically needs to exhibit not only high water absorption performance but also fast water absorption speed.

[0006] In order to manufacture such a superabsorbent resin with improved water absorption speed, a method of increasing the specific surface area by generating pores using a foaming agent in the polymerization step is mainly used. In particular, carbonate-based foaming agents are generally used from the viewpoints of cost and availability, and when the polymerization step is carried out in the presence of such a carbonate-based foaming agent, carbon dioxide bubbles are generated and the specific surface area increases in the crosslinked polymer. In addition, a foam stabilizer is used to minimize the escape of the generated carbon dioxide bubbles out of the crosslinked polymer network, but the use of such a foam stabilizer causes a problem of deteriorating various physical properties of the superabsorbent resin.

[0007] As a result, there is a continuing demand for the development of superabsorbent polymers that exhibit a fast water absorption rate while maintaining the basic water retention capacity (CRC), which is a physical property that indicates the basic water absorption and water retention ability of superabsorbent polymers, and the absorbent capacity under pressure (AUP), which indicates the ability to retain absorbed liquid even when subjected to external pressure. Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, the present invention relates to a method for producing a superabsorbent resin that can exhibit high surface tension while exhibiting improved water absorption speed by adding an aqueous dispersion of hydrophobic particles during the monomer polymerization step to effectively capture bubbles generated by a blowing agent. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention provides A step of preparing a monomer composition including an acrylic acid monomer having an acidic group, at least a portion of which has been neutralized, and an internal crosslinking agent (step 1); a step (2) of cross-linking and polymerizing the monomer composition in the presence of an aqueous dispersion of hydrophobic particles and a carbonate-based foaming agent to prepare a hydrogel polymer; drying and grinding the hydrogel polymer to form a base resin in powder form (Step 3); and Step 4 includes a step of further crosslinking the surface of the base resin in the presence of a surface crosslinking agent to form a surface crosslinked layer, The hydrophobic particle aqueous dispersion is a colloidal solution in which hydrophobic particles are dispersed by a surfactant, The hydrophobic particles contain a metal salt of a fatty acid having 7 to 24 carbon atoms and have an average particle size of 1 μm to 100 μm. A method for producing a superabsorbent resin is provided. Effect of the Invention

[0010] According to the method for producing a superabsorbent polymer of the present invention, when a hydrogel polymer is produced by cross-linking a monomer in the presence of a hydrophobic particle aqueous dispersion and a carbonate-based foaming agent, the carbon dioxide produced can be effectively captured, thereby increasing the specific surface area of ​​the superabsorbent polymer. This can increase the water absorption rate of the superabsorbent polymer produced. In addition, the use of the hydrophobic particle aqueous dispersion does not require the addition of a separate bubble stabilizer, and the surface tension of the superabsorbent polymer is not reduced by the ionic surfactant used as the bubble stabilizer, so that the produced superabsorbent polymer can exhibit high surface tension. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "comprise", "have" and the like are intended to specify the presence of an implemented feature, step, component, or combination thereof, and should be understood not to preclude the presence or additional possibility of one or more other features, steps, components, or combinations thereof.

[0012] The present invention can be modified in various ways and can have various forms, and the following detailed description will be given of specific embodiments by way of example, but it should be understood that the present invention is not limited to the specific disclosed embodiments, but includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.

[0013] Furthermore, the terminology used in this specification is for the purpose of referring to particular embodiments only and is not intended to limit the present invention. Additionally, as used herein, the singular forms "a," "an," and "the" include the plural forms unless the context clearly dictates otherwise.

[0014] The term "polymer" or "polymeric polymer" used in the present specification means a state in which an acrylic acid monomer, which is a water-soluble ethylenically unsaturated monomer, is polymerized, and can include all water content ranges or particle size ranges. Among the above polymers, a polymer in a state after polymerization and before drying and having a water content (water content) of about 40% by weight or more can be called a hydrogel polymer, and particles obtained by crushing and drying such a hydrogel polymer can be called a crosslinked polymer.

[0015] In addition, the term "superabsorbent resin particles" refers to a particulate material including a crosslinked polymer obtained by polymerizing an acrylic acid monomer containing acidic groups and at least a portion of the acidic groups being neutralized, and crosslinking the polymer with an internal crosslinking agent.

[0016] In addition, the term "super absorbent polymer" refers to a crosslinked polymer obtained by polymerizing an acrylic acid monomer containing an acidic group and at least a portion of the acidic group being neutralized, or a powder-form base resin made of super absorbent polymer particles obtained by pulverizing the crosslinked polymer, depending on the context, or is used to encompass all of the crosslinked polymer or base resin that have been subjected to additional processes, such as surface crosslinking, regranulation into fine powder, drying, pulverization, classification, etc., to be in a state suitable for commercialization. Thus, the term "super absorbent polymer" can be interpreted as including a plurality of super absorbent polymer particles.

[0017] In order to produce a superabsorbent resin having a high water absorption rate, the specific surface area of ​​the superabsorbent resin particles must be increased. A foaming agent is usually used as a method for increasing the specific surface area of ​​the superabsorbent resin particles. In order for the bubbles generated by the foaming agent to contribute to the increase in the specific surface area, the bubbles must be trapped inside the crosslinked polymer as soon as they are generated, so that they do not escape to the outside of the polymer. For this reason, a foaming agent and a bubble stabilizer are usually used together. An anionic surfactant, which is mainly used as a bubble stabilizer, can effectively trap bubbles, but it reduces the surface tension of the superabsorbent resin, causing leakage of urine from sanitary products to which the superabsorbent resin is applied.

[0018] Therefore, the present inventors have confirmed that when a superabsorbent resin is prepared by using an aqueous dispersion containing hydrophobic particles as a bubble stabilizer instead of a commonly used bubble stabilizer, the bubbles generated by the foaming agent can be effectively captured and small, uniformly shaped bubbles can be uniformly distributed throughout the entire crosslinked polymer, thereby completing the present invention. In addition, the superabsorbent resin thus prepared has the advantage that the specific surface area is increased by the uniformly distributed bubbles, thereby increasing the water absorption rate, and also has a high surface tension.

[0019] In particular, the method for producing a superabsorbent resin is characterized in that the hydrophobic particles are not used in the form of a powder, but are added to the monomer composition in the form of a dispersion in water. In other words, the hydrophobic particles are added to the monomer composition in the form of a "hydrophobic particle aqueous dispersion", that is, in the form of a colloidal solution in which the hydrophobic particles are stably dispersed without being precipitated or aggregated by a surfactant. This is because, when the hydrophobic particles are added to the monomer composition in the form of a powder and a polymerization process is performed, the hydrophobic particles do not disperse in the monomer composition in the form of an aqueous solution, but aggregate, making it difficult to effectively stabilize the bubbles generated by the foaming agent.

[0020] In addition, the hydrophobic particles are stably dispersed in the aqueous dispersion liquid by the surfactant without inter-particle aggregation. Specifically, the surfactant can form an electric double layer on the surface of the hydrophobic particles to induce electrostatic repulsive force between particles to stabilize the hydrophobic particles, or can be adsorbed to the surface of the hydrophobic particles to induce steric repulsive force between particles to prevent the particles from aggregating with each other. Therefore, if the hydrophobic particle aqueous dispersion liquid does not contain a surfactant, the hydrophobic particles will aggregate with each other or sink due to gravity, and the dispersion stabilization of the hydrophobic particles will not be achieved. Therefore, even if the hydrophobic particle aqueous dispersion liquid not containing a surfactant is used together with a foaming agent in the polymerization step, it is not possible to effectively capture air bubbles and form pores of uniform size in the superabsorbent resin, which makes it difficult to improve the water absorption rate of the superabsorbent resin.

[0021] In addition, the hydrophobic particles dispersed in the aqueous dispersion have an average particle size of 1 μm to 100 μm. If the hydrophobic particles have an average particle size of less than 1 μm, there is a problem that the generated air bubbles are difficult to effectively collect and uniform pores are not formed, and if the hydrophobic particles have an average particle size of more than 100 μm, there is a problem that the viscosity of the monomer composition increases excessively, causing a problem in polymerization stability, and the size of the formed pores is large, making it difficult to improve the water absorption speed of the superabsorbent resin.

[0022] Hereinafter, the steps of the method for producing a superabsorbent polymer will be described in more detail according to a specific embodiment of the present invention.

[0023] (Stage 1) In the method according to one embodiment, step 1 is a step of preparing a monomer composition including an acrylic acid monomer having an acid group, at least a portion of which is neutralized, and an internal crosslinking agent.

[0024] The acrylic acid monomer is a compound represented by the following formula 1:

[0025] [Chemical formula 1] R 1 -COOM 1

[0026] In the above chemical formula 1, R 1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.

[0027] Preferably, the acrylic acid monomer includes at least one selected from the group consisting of acrylic acid, methacrylic acid, and their monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts.

[0028] Here, the acrylic acid monomer may have an acidic group, and at least a part of the acidic group may be neutralized. Preferably, the monomer may be partially neutralized with an alkaline substance such as sodium hydroxide, potassium hydroxide, or ammonium hydroxide. In this case, the neutralization degree of the acrylic acid monomer may be 40 to 95 mol%, 40 to 80 mol%, or 45 to 75 mol%. The range of the neutralization degree may be adjusted according to the final physical properties. However, if the neutralization degree is too high, the neutralized monomer may precipitate, making it difficult to smoothly carry out polymerization, and conversely, if the neutralization degree is too low, the water absorption of the polymer may be greatly reduced and the polymer may exhibit properties similar to elastic rubber, which are difficult to handle.

[0029] The concentration of the acrylic acid monomer may be about 20 to about 60% by weight, preferably about 40 to about 50% by weight, based on the monomer composition including the raw material of the superabsorbent polymer and the solvent, and may be an appropriate concentration in consideration of the polymerization time and reaction conditions, etc. However, if the concentration of the monomer is too low, the yield of the superabsorbent polymer may be low, causing problems in economic efficiency, and conversely, if the concentration is too high, problems may occur in the process, such as a part of the monomer being precipitated or the efficiency of pulverization of the polymerized hydrogel polymer being low, and the physical properties of the superabsorbent polymer may be deteriorated.

[0030] In addition, the term "internal crosslinking agent" used in this specification is a term used to distinguish it from a surface crosslinking agent for crosslinking the surface of the superabsorbent resin particles described below, and plays a role in crosslinking and polymerizing the unsaturated bonds of the water-soluble ethylenically unsaturated monomer described above. The crosslinking in this step is performed regardless of the surface or the inside, but when the surface crosslinking process of the superabsorbent resin particles described below is performed, the particle surface of the finally produced superabsorbent resin has a structure crosslinked by the surface crosslinking agent, and the inside has a structure crosslinked by the internal crosslinking agent.

[0031] As the internal crosslinking agent, any compound can be used as long as it can introduce crosslinking bonds during polymerization of the acrylic unsaturated monomer.Specifically, as the internal crosslinking agent, a crosslinking agent having one or more functional groups capable of reacting with the water-soluble substituent of the acrylic unsaturated monomer and one or more ethylenically unsaturated groups; or a crosslinking agent having two or more functional groups capable of reacting with the water-soluble substituent of the monomer and / or the water-soluble substituent formed by hydrolysis of the monomer can be used.

[0032] Non-limiting examples of the internal crosslinking agent include N,N'-methylenebisacrylamide, trimethylpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di( ... polypropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, poly Multifunctional crosslinkers such as acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, ethylene glycol diglycidyl ether, propylene glycol, glycerin, or ethylene carbonate can be used alone or in combination of two or more, but are not limited thereto.

[0033] Preferably, the internal crosslinking agent may be a polyalkylene glycol di(meth)acrylate-based compound such as polyethylene glycol (meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, or polypropylene glycol (meth)acrylate, because when such an internal crosslinking agent is used, foaming by a carbonate-based foaming agent described below is easily performed.

[0034] In the monomer composition, the internal crosslinking agent can be used in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. For example, the internal crosslinking agent can be used in an amount of 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.15 parts by weight or more based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer, and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.7 parts by weight or less. If the content of the upper internal crosslinking agent is too low, crosslinking may not occur sufficiently, making it difficult to achieve a strength above an appropriate level, and if the content of the upper internal crosslinking agent is too high, the internal crosslinking density may increase, making it difficult to achieve the desired water retention ability.

[0035] In addition, the monomer composition may further include a polymerization initiator for initiating a polymerization reaction of the monomer. The polymerization initiator is not particularly limited as long as it is one that is generally used in the production of a highly water-absorbent resin.

[0036] Specifically, the polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator by UV irradiation depending on the polymerization method. However, even in the photopolymerization method, a certain amount of heat is generated by irradiation such as UV irradiation, and a certain amount of heat is generated by the progress of the polymerization reaction, which is an exothermic reaction, so a thermal polymerization initiator may be additionally included.

[0037] The photopolymerization initiator can be any compound capable of forming radicals by the action of light such as ultraviolet light, and is not limited in its composition.

[0038] The photopolymerization initiator may be one or more selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Meanwhile, as a specific example of acylphosphine, commercially available lucirin TPO, i.e., diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, may be used. More various photoinitiators are well described in "UV Coatings: Basics, Recent Developments and New Application" (Elsevier, 2007), p. 115 by Reinhold Schwalm, and are not limited to the above examples.

[0039] The photopolymerization initiator may be contained in a concentration of about 0.01 to about 1.0% by weight based on the monomer composition. If the concentration of the photopolymerization initiator is too low, the polymerization rate may be slow, and if the concentration of the photopolymerization initiator is too high, the molecular weight of the superabsorbent resin may be small, resulting in non-uniform physical properties.

[0040] In addition, the thermal polymerization initiator may be at least one selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid. Specifically, examples of the persulfate initiator include sodium persulfate (Na 2 S 2 O 8 ), potassium persulfate (K 2 S 2 O 8), Ammonium persulfate ((NH 4 ) 2 S 2 O 8 ), and examples of azo initiators include 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, 2-(carbamoylazo)isobutylonitrile, 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), and A wide variety of thermal polymerization initiators are described in detail in Odian's book "Principle of Polymerization (Wiley, 1981)", p. 203, and are not limited to the above examples.

[0041] The thermal polymerization initiator may be included in a concentration of about 0.001 to about 0.5 wt % based on the monomer composition. If the concentration of the thermal polymerization initiator is too low, additional thermal polymerization hardly occurs, and the effect of adding the thermal polymerization initiator may be small, whereas if the concentration of the thermal polymerization initiator is too high, the molecular weight of the superabsorbent resin may be small, resulting in non-uniform physical properties.

[0042] The polymerization initiator can be used in an amount of 2 parts by weight or less based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. That is, if the concentration of the polymerization initiator is too low, the polymerization rate may be slowed down, and a large amount of residual monomer may be extracted in the final product, which is not preferable. On the other hand, if the concentration of the polymerization initiator is higher than the above range, the polymer chains forming the network may become shorter, the content of water-soluble components may increase, and the water absorption capacity under pressure may decrease, which is not preferable, and the physical properties of the resin may decrease.

[0043] The monomer composition may further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.

[0044] The monomer composition including the monomer may be in a solution state dissolved in a solvent such as water, and the solid content in the monomer composition in such a solution state, i.e., the concentration of the monomer, the internal crosslinking agent, and the polymerization initiator, may be appropriately adjusted in consideration of the polymerization time and reaction conditions, etc. For example, the solid content in the monomer composition may be 10 to 80 wt%, or 15 to 60 wt%, or 30 to 50 wt%.

[0045] When the monomer composition has a solid content in the above range, it is possible to eliminate the need to remove unreacted monomers after polymerization by utilizing the gel effect phenomenon that occurs in the polymerization reaction of a high-concentration aqueous solution, and it may be advantageous to adjust the grinding efficiency when grinding the polymer described below.

[0046] The solvent that can be used in this case is not limited in composition as long as it can dissolve the above-mentioned components. For example, one or more selected from water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, and N,N-dimethylacetamide can be used in combination.

[0047] (Stage 2) Next, the monomer composition is cross-linked and polymerized in the presence of a hydrophobic particle aqueous dispersion and a carbonate-based foaming agent to produce a hydrogel polymer. In this step, carbon dioxide bubbles are generated from the carbonate-based foaming agent, and the hydrophobic particles dispersed in water effectively capture these bubbles, thereby increasing the specific surface area of ​​the hydrogel polymer.

[0048] The hydrophobic particles include a metal salt of a fatty acid having 7 to 24 carbon atoms. Here, the metal salt of a fatty acid having 7 to 24 carbon atoms refers to a compound in which a metal cation is bonded instead of a hydrogen ion of a carboxyl group at the end of an unsaturated or saturated fatty acid having a linear structure while having 7 to 24 carbon atoms in the molecule, and in this case, the metal salt may be a monovalent metal salt or a polyvalent metal salt having a valence of 2 or more. In this case, when the hydrophobic particles are metal salts of fatty acids having less than 7 carbon atoms, it is not possible to capture air bubbles that are ionized in an aqueous solution and generated in the form of particles, and when the hydrophobic particles are metal salts of fatty acids having more than 24 carbon atoms, the fatty acid chains are long and dispersion may be difficult.

[0049] Specifically, when the metal salt of the fatty acid is a monovalent metal salt, it has a structure in which one fatty acid carboxylate anion is bound to an alkali ion, which is a monovalent metal cation, and when the metal salt of the fatty acid is a polyvalent metal salt, it has a structure in which fatty acid carboxylate anions are bound to a metal cation in the number equal to the valence of the metal cation.

[0050] In one embodiment, the hydrophobic particles may be a metal salt of a saturated fatty acid having 12 to 20 carbon atoms. For example, the hydrophobic particles may be one or more metal salts of saturated fatty acids selected from the group consisting of a metal salt of lauric acid containing 12 carbon atoms in the molecule, a metal salt of tridecylic acid containing 13 carbon atoms in the molecule, a metal salt of myristic acid containing 14 carbon atoms in the molecule, a metal salt of pentadecanoic acid containing 15 carbon atoms in the molecule, a metal salt of palmitic acid containing 16 carbon atoms in the molecule, a metal salt of margaric acid containing 17 carbon atoms in the molecule, a metal salt of stearic acid containing 18 carbon atoms in the molecule, a metal salt of nonadecylic acid containing 19 carbon atoms in the molecule, and a metal salt of arachidic acid containing 20 carbon atoms in the molecule.

[0051] Preferably, the hydrophobic particles may be a metal stearate, for example, the hydrophobic particles may be one or more metal stearates selected from the group consisting of calcium stearate, magnesium stearate, sodium stearate, zinc stearate, and potassium stearate.

[0052] As described above, the hydrophobic particles dispersed in the aqueous dispersion have an average particle size of 1 μm to 100 μm. As an example, the hydrophobic particles may have an average particle size of 1 μm to 20 μm. For example, the hydrophobic particles may have an average particle size (μm) of 1 or more, but 100 or less, 50 or less, 40 or less, 30 or less, or 20 or less.

[0053] Here, the average particle size of the hydrophobic particles means D50, and the "particle size Dn" means the particle size at n% of the cumulative particle number distribution according to particle size. That is, D50 is the particle size at 50% of the cumulative particle number distribution according to particle size, D90 is the particle size at 90% of the cumulative particle number distribution according to particle size, and D10 is the particle size at 10% of the cumulative particle number distribution according to particle size. The Dn can be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and when the particles pass through a laser beam, the diffraction pattern difference according to the particle size is measured to calculate the particle size distribution. D10, D50, and D90 can be measured by calculating the particle diameter at 10%, 50%, and 90% of the cumulative particle number distribution according to particle size in the measuring device.

[0054] In addition, the hydrophobic particles may be contained in the aqueous dispersion in an amount of 10 to 70 wt % based on the total weight of the aqueous dispersion. If the content of the hydrophobic particles in the aqueous dispersion is too low or too high, the hydrophobic particles may not be dispersed and may aggregate with each other or settle due to gravity.

[0055] In addition, as the surfactant that serves to disperse the hydrophobic particles in the hydrophobic particle aqueous dispersion, any surfactant known in the art that can stabilize the dispersion of the hydrophobic particles can be used without limitation. For example, the surfactant can be one or more surfactants selected from the group consisting of cationic surfactants, anionic surfactants, amphoteric surfactants, and nonionic surfactants. Preferably, two or more surfactants can be used in terms of stabilizing the dispersion of the hydrophobic particles. More specifically, in consideration of the form of the hydrophobic particles, for example, the form of a metal salt of a saturated fatty acid, a nonionic surfactant and an anionic surfactant, for example, a nonionic surfactant bonded to a long-chain hydrocarbon having 10 or more carbon atoms and a sulfate-based anionic surfactant, can be used together to more effectively disperse the hydrophobic particles in water.

[0056] As an example, the cationic surfactant may include dialkyldimethylammonium salts, alkylbenzylmethylammonium salts, etc., the anionic surfactant may include alkyl polyoxyethylene sulfates, monoalkyl sulfates, alkylbenzene sulfonates, monoalkyl phosphates, sulfates having a functional group containing a long chain hydrocarbon or a sodium salt thereof, such as sodium lauryl sulfate, sodium dodecyl sulfate, or sodium laureth sulfate, etc., the amphoteric surfactant may include alkyl sulfobetaines, alkyl carboxybetaines, etc., and the nonionic surfactant may include polyoxyethylene alkyl ethers such as polyethylene glycol, polyoxyalkylene alkylphenyl ethers, polyoxyethylene arylphenyl ethers, fatty acid esters such as sorbitan monopalmitate, fatty acid sorbitan esters, or glyceryl monostearate, alkyl monoglyceryl ethers, alkanolamides, alkyl polyglucosides, etc., but is not limited thereto.

[0057] The hydrophobic particle aqueous dispersion may have a pH of at least 7. If the hydrophobic particle aqueous dispersion has a pH of less than 7, it will be acidic, making it difficult to stabilize the hydrophobic particles, which are metal salts of fatty acids, and is therefore unsuitable.

[0058] Meanwhile, the hydrophobic particles are used in an amount of 0.01 to 0.5 parts by weight based on 100 parts by weight of the acrylic acid monomer. If the content of the hydrophobic particles is too low, the bubble stabilizing effect may be insufficient, and the water absorption speed may be slowed down. If the content of the hydrophobic particles is too high, the amount of surfactant used to stabilize the hydrophobic particles in the hydrophobic particle aqueous dispersion may increase, and the surface tension may be reduced. For example, the hydrophobic particles may be used in an amount of 0.01 or more, 0.03 or more, 0.05 or more, or 0.08 or more, but not more than 0.5 parts by weight, not more than 0.4 parts by weight, not more than 0.3 parts by weight, or not more than 0.2 parts by weight based on 100 parts by weight of the acrylic acid monomer.

[0059] In addition, the carbonate-based foaming agent foams during polymerization to form pores in the hydrogel polymer, thereby increasing the surface area. For example, one or more types selected from the group consisting of sodium bicarbonate, sodium carbonate, potassium bicarbonate, potassium carbonate, calcium bicarbonate, calcium carbonate, magnesium bicarbonate, and magnesium carbonate can be used.

[0060] The carbonate-based blowing agent can be used in an amount of 0.005 to 1 part by weight based on 100 parts by weight of the acrylic acid-based monomer. If the amount of the blowing agent is less than 0.005 parts by weight, the role of the blowing agent may be insignificant, and if the amount of the blowing agent is more than 1 part by weight, the crosslinked polymer may have too many pores, resulting in a decrease in gel strength and density of the produced superabsorbent resin, which may cause problems in distribution and storage. For example, the carbonate-based blowing agent may be 0.01 parts by weight or more, 0.05 parts by weight or more, but 0.5 parts by weight or less, 0.3 parts by weight or less, or 0.2 parts by weight or less based on 100 parts by weight of the acrylic acid-based monomer.

[0061] In addition, the carbonate foaming agent and the hydrophobic particles can be used in a weight ratio of 1:0.1 to 1:2. If the hydrophobic particles are used in an amount that is too low compared to the carbonate foaming agent, it is difficult to effectively capture the generated bubbles, and if the hydrophobic particles are used in an amount that is too high compared to the foaming agent, various physical properties such as water retention capacity and water absorption rate may decrease. Specifically, the carbonate foaming agent and the hydrophobic particles can be used in a weight ratio of 1:0.4 or more, 1:0.6 or more, or 1:0.8 or more, but not more than 1:1.7, 1:1.5 or less, or 1:1.2 or less. For example, the carbonate foaming agent and the hydrophobic particles can be used in a weight ratio of 1:1.

[0062] Also, surfactants such as alkyl sulfate compounds and polyoxyethylene alkyl ether compounds, which are generally used as foam stabilizers, may not be used in steps 1 and 2. For example, cationic surfactants such as quaternary ammonium compounds such as dodecyltrimethylammonium chloride and dodecyltrimethylammonium bromide; anionic surfactants such as alkyl sulfate compounds such as sodium dodecyl sulfate, ammonium lauryl sulfate, sodium lauryl ether sulfate, and sodium myreth sulfate; or nonionic surfactants such as alkyl ether sulfate compounds such as polyoxyethylene lauryl ether may not be used in steps 1 and 2. This can prevent the problem of the surface tension of the superabsorbent resin decreasing due to the use of the surfactants.

[0063] On the other hand, the polymerization of the monomer composition in the presence of such an aqueous dispersion of hydrophobic particles and a carbonate-based blowing agent is not particularly limited as long as it is a commonly used polymerization method.

[0064] Specifically, polymerization methods are broadly divided into thermal polymerization and photopolymerization depending on the polymerization energy source. Typically, thermal polymerization can be carried out in a reactor having a stirring shaft such as a kneader, and photopolymerization can be carried out in a reactor equipped with a movable conveyor belt. However, the above-mentioned polymerization methods are merely examples, and the present invention is not limited to the above-mentioned polymerization methods.

[0065] For example, the hydrogel polymer obtained by thermal polymerization by supplying hot air to a reactor such as a kneader equipped with an agitator shaft or by heating the reactor as described above may be several centimeters to several millimeters in size when discharged from the reactor outlet, depending on the type of the agitator shaft equipped in the reactor. Specifically, the size of the obtained hydrogel polymer varies depending on the concentration of the monomer composition injected and the injection speed, and a hydrogel polymer having a weight average particle size of 2 to 50 mm is usually obtained.

[0066] In addition, when photopolymerization is performed in a reactor equipped with a movable conveyor belt as described above, the form of the obtained hydrogel polymer may be a sheet-like hydrogel polymer having the width of the belt. In this case, the thickness of the polymer sheet varies depending on the concentration and injection speed of the monomer composition injected, but it is preferable to supply the monomer composition so that a sheet-like polymer having a thickness of about 0.5 to about 5 cm is obtained. If the monomer composition is supplied so that the thickness of the sheet-like polymer is too thin, the production efficiency is low, which is undesirable, and if the thickness of the sheet-like polymer exceeds 5 cm, the polymerization reaction may not occur uniformly over the entire thickness due to the excessive thickness.

[0067] The water content of the hydrogel polymer obtained by this method may be about 40 to about 80% by weight. Meanwhile, throughout this specification, the "water content" refers to the water content relative to the total polymer weight, and means the weight of the polymer minus the weight of the polymer in a dry state. Specifically, it is defined as a value calculated by measuring the weight loss due to the evaporation of water in the polymer during the process of drying by increasing the temperature of the polymer through infrared heating. Here, the drying conditions are a method of increasing the temperature from room temperature to about 180°C and then maintaining it at 180°C, and the total drying time is set to 20 minutes, including 5 minutes for the temperature increase stage, and the water content is measured.

[0068] (Stage 3) Then, the hydrogel polymer is dried and pulverized to form a powder-type base resin, and if necessary, a coarse pulverization step may be performed before the drying step to increase the efficiency of the drying step.

[0069] In this case, the crusher used is not limited in structure, and specifically may include any one selected from the group of crushing equipment consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, and a disc cutter, but is not limited to the above examples.

[0070] In this case, the pulverization step can be performed so that the polymer has a particle size of about 2 to about 10 mm. It is technically difficult to pulverize the polymer to a particle size of less than 2 mm due to the high water content of the hydrogel polymer, and the pulverized particles may aggregate with each other. On the other hand, when the polymer is pulverized to a particle size of more than 10 mm, the efficiency of the subsequent drying step is not increased significantly.

[0071] The polymer immediately after polymerization, which is either pulverized as described above or not pulverized, is dried. In this case, the drying temperature in the drying step may be about 150 to about 250°C. If the drying temperature is less than 150°C, the drying time may be too long, and the physical properties of the superabsorbent resin finally formed may be deteriorated. If the drying temperature exceeds 250°C, only the polymer surface may be dried excessively, and fine powder may be generated in the subsequent pulverization process, and the physical properties of the superabsorbent resin finally formed may be deteriorated. Therefore, the drying may be preferably performed at a temperature of about 150 to about 200°C, more preferably at a temperature of about 160 to about 180°C.

[0072] On the other hand, the drying time can be about 20 to about 90 minutes in consideration of process efficiency, but is not limited thereto.

[0073] The drying method in the drying step can be selected and used without any limitation on its configuration as long as it is a method commonly used for drying hydrogel polymers. Specifically, the drying step can be performed by a method such as hot air supply, infrared radiation, ultrashort wave radiation, or ultraviolet radiation. The water content of the polymer after the drying step may be about 0.1 to about 5% by weight.

[0074] Then, the dried polymer obtained through the drying step is pulverized.

[0075] The base resin, which is a polymer powder obtained after the pulverization step, may have a particle size of about 150 to about 850 μm. Specific examples of the pulverizer used to pulverize to such a particle size include a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, and a jog mill, but the present invention is not limited to the above examples.

[0076] After the pulverization step, the base resin obtained after pulverization is classified according to particle size in order to control the physical properties of the superabsorbent resin powder that is the final product. Preferably, polymers having a particle size of about 150 to about 850 μm are classified, and only the base resin having such a particle size may be subjected to the surface crosslinking reaction step. Such particle size can be measured according to the EDANA WSP 220.3 method of the European Disposables and Nonwovens Association (EDANA) standard.

[0077] (Stage 4) Next, a step of forming a surface cross-linked layer by additionally cross-linking the surface of the base resin in the presence of a surface cross-linking agent is carried out, whereby a superabsorbent resin having a surface cross-linked layer formed on the surface of the base resin, more specifically, on at least a portion of the surface of each base resin particle, is produced.

[0078] Surface cross-linking is a step that increases the cross-link density near the surface of superabsorbent polymer particles relative to the cross-link density inside the particle. Generally, a surface cross-linking agent is applied to the surface of the superabsorbent polymer particles. Thus, the reaction occurs on the surface of the superabsorbent polymer particles, which improves the cross-linking on the surface of the particles while leaving the inside of the particles substantially unaffected. Thus, surface cross-linked superabsorbent polymer particles have a higher degree of cross-linking near the surface than inside.

[0079] The surface cross-linking agent may be any surface cross-linking agent used in the manufacture of existing superabsorbent resins without any particular limitation. For example, the surface cross-linking agent may include one or more polyols selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,2-hexanediol, 1,3-hexanediol, 2-methyl-1,3-propanediol, 2,5-hexanediol, 2-methyl-1,3-pentanediol, 2-methyl-2,4-pentanediol, tripropylene glycol, and glycerol; one or more carbonate-based compounds selected from the group consisting of ethylene carbonate, propylene carbonate, and glycerol carbonate; epoxy compounds such as ethylene glycol diglycidyl ether; oxazoline compounds such as oxazolidinone; polyamine compounds; mono-, di-, or polyoxazolidinone compounds; or cyclic urea compounds; etc. Specifically, one or more of the above-mentioned surface cross-linking agents may be used as the surface cross-linking agent, or two or more of the above-mentioned surface cross-linking agents may be used as the surface cross-linking agent. For example, ethylene carbonate may be used as the surface cross-linking agent.

[0080] There is no limitation on the constitution of the method for mixing the surface crosslinking agent with the base resin. A method of mixing the surface crosslinking agent and the base resin powder in a reaction tank, a method of spraying the surface crosslinking agent onto the base resin powder, a method of continuously supplying the base resin and the surface crosslinking agent to a continuously operated mixer, and the like can be used.

[0081] When the surface crosslinking agent is added, it may be added in the form of a surface crosslinking solution by mixing with water. When water is added, it is advantageous that the surface crosslinking agent can be uniformly dispersed in the polymer. At this time, the content of the added water is preferably about 1 to about 10 parts by weight per 100 parts by weight of the base resin for the purpose of inducing uniform dispersion of the surface crosslinking agent, preventing the polymer powder from clumping, and optimizing the surface penetration depth of the surface crosslinking agent.

[0082] The base resin to which the surface crosslinking solution containing the surface crosslinking agent and the solvent has been added is heated at a temperature of about 100 to about 150° C., preferably about 110 to about 140° C., for about 15 to about 80 minutes, preferably about 20 to about 70 minutes, to thereby carry out a surface crosslinking reaction.

[0083] The temperature raising means for the surface crosslinking reaction is not particularly limited. Heating can be performed by supplying a heat medium or directly supplying a heat source. At this time, the type of heat medium that can be used can be a heated fluid such as steam, hot air, hot oil, etc., but the present invention is not limited thereto, and the temperature of the heat medium to be supplied can be appropriately selected in consideration of the means of the heat medium, the heating rate, and the target temperature of the heat raising. On the other hand, examples of the heat source to be directly supplied include heating by electricity and heating by gas, but the present invention is not limited to the above examples.

[0084] After the surface cross-linked layer is formed on the surface of the base resin as described above, an inorganic material may be further mixed.

[0085] The inorganic material may be, for example, one or more selected from the group consisting of silica, clay, alumina, a silica-alumina composite material, and titania, and preferably, silica.

[0086] Such inorganic substances can be used in an amount of 0.01 parts by weight or more, or 0.05 parts by weight or more, or 0.1 parts by weight or more, but not more than 5 parts by weight, or not more than 3 parts by weight, or not more than 1 part by weight, based on 100 parts by weight of the superabsorbent resin.

[0087] Meanwhile, in order to control the physical properties of the superabsorbent polymer to be manufactured as a final product, a step of classifying the superabsorbent polymer obtained after the surface cross-linking reaction step according to particle size can be additionally carried out. Preferably, polymers having a particle size of about 150 to about 850 μm are classified, and only the superabsorbent polymer having such a particle size can be used as the final product.

[0088] The highly absorbent resin obtained by the above-mentioned production method has a well-balanced water absorption rate and water absorption properties, and can satisfy the following properties.

[0089] 1) Water absorption rate (vortex time) at 24.0°C is 55 seconds or less; 2) Surface tension of 65mN / m or more; 3) Centrifugation retention capacity (CRC) of 25-30 g / g, as measured by the EDANA method WSP241.3; and 4) The water absorption capacity under pressure (AUP) measured by EDANA method WSP242.3 is 20-26g / g at 0.7 psi.

[0090] More specifically, the superabsorbent polymer produced by the above-mentioned production method may have a water absorption rate (vortex time) of 50 seconds or less, 48 ​​seconds or less, 46 seconds or less, or 45 seconds or less, measured by a vortex method at 24° C. The smaller the water absorption rate, the better, and the lower limit of the water absorption rate is theoretically 0 seconds, but may be, for example, 10 seconds or more, 20 seconds or more, 30 seconds or more, or 35 seconds or more. At this time, the method for measuring the water absorption rate of the superabsorbent polymer will be described in more detail in the Examples below.

[0091] In addition, the surface tension of the superabsorbent polymer may be 65 mN / m or more, 66 mN / m or more, or 68 mN / m or more, but 72 mN / m or less. In this case, a method for measuring the surface tension of the superabsorbent polymer will be described in more detail in the Examples below.

[0092] In addition, the superabsorbent polymer may have a centrifuge retention capacity (CRC) of 25 g / g or more, 26 g / g or more, or 27 g / g or more, but 30 g / g or less, or 29.5 g / g or less, as measured by EDANA method WSP241.3.

[0093] The superabsorbent polymer may also have an absorbency under pressure (AUP) at 0.7 psi, measured by the EDANA method WSP242.3, of 20 g / g or more, 22 g / g or more, or 23 g / g or more, but 26 g / g or less, or 25.5 g / g or less.

[0094] The present invention will be described in more detail with reference to the following examples, but the following examples are merely illustrative of the present invention and are not intended to limit the scope of the present invention. EXAMPLES

[0095] <Production Example> The hydrophobic particle aqueous dispersions used in the following examples were prepared in the following manner.

[0096] Production Example 1: Production of calcium stearate aqueous dispersion Ca-st (5) First, 50 g of water containing two or more surfactants (including sulfate-based anionic surfactants and fatty acid ester-based nonionic surfactants) was added to a high shear mixer and heated to 165°C, and then 50 g of calcium stearate powder was added. Then, the mixture was stirred at 4000 rpm at normal pressure for 30 minutes to thoroughly pulverize the calcium stearate, thereby obtaining an aqueous dispersion Ca-st(5) in which 50% by weight of calcium stearate having an average particle size of 5 μm was dispersed. At this time, the pH of the aqueous dispersion was 9.5. After the preparation of Ca-st(5), its average particle size (D50) was measured / calculated as the particle size at the 50% point of the cumulative particle number distribution using a laser diffraction particle size measuring device (Microtrac S3500).

[0097] Production Example 2: Production of calcium stearate aqueous dispersion Ca-st (20) An aqueous dispersion Ca-st(20) in which 50% by weight of calcium stearate having an average particle size of 20 μm was dispersed was obtained using the same method as in Preparation Example 1, except that the stirring conditions were different. At this time, the pH of the aqueous dispersion was 9.5, and the average particle size of Ca-st(20) was measured / calculated using the same method as in Preparation Example 1.

[0098] Production Example 3: Production of magnesium stearate aqueous dispersion Mg-st (1) First, 50 g of water containing two or more surfactants (including sulfate-based anionic surfactants and fatty acid ester-based nonionic surfactants) was added to a high shear mixer and heated to 150°C, and then 10 g of magnesium stearate powder was added. Next, the mixture was stirred at 4000 rpm at normal pressure for 30 minutes to thoroughly pulverize the magnesium stearate, thereby obtaining an aqueous dispersion Mg-st(1) in which 17% by weight of magnesium stearate having an average particle size of 1 μm was dispersed. At this time, the pH of the aqueous dispersion was 9, and the average particle size of Mg-st(1) was measured / calculated in the same manner as in Preparation Example 1.

[0099] Production Example 4: Production of magnesium stearate aqueous dispersion Mg-st (5) A water dispersion Mg-st(5) in which 17% by weight of magnesium stearate having an average particle size of 5 μm was dispersed was obtained using the same method as in Preparation Example 3, except that the stirring conditions were different. At this time, the pH of the water dispersion was 9, and the average particle size of Mg-st(5) was measured / calculated using the same method as in Preparation Example 1.

[0100] Production Example 5: Production of sodium stearate aqueous dispersion Na-st (5) First, 50 g of water containing two or more surfactants (including sulfate-based anionic surfactants and fatty acid ester-based nonionic surfactants) was placed in a high shear mixer, and 50 g of sodium stearate powder was added at room temperature. Then, the mixture was stirred at 2000 rpm under normal pressure for 5 minutes to thoroughly pulverize the sodium stearate, thereby obtaining an aqueous dispersion Na-st(5) in which 50% by weight of sodium stearate having an average particle size of 5 μm was dispersed. At this time, the pH of the aqueous dispersion was 9, and the average particle size of Na-st(5) was measured / calculated in the same manner as in Preparation Example 1.

[0101] Production Example 6: Production of potassium stearate aqueous dispersion K-st (5) First, 50 g of water containing two or more surfactants (including sulfate-based anionic surfactants and fatty acid ester-based nonionic surfactants) was added to a high shear mixer, and 20 g of potassium stearate powder was added at room temperature. Then, the mixture was stirred at 4000 rpm under normal pressure for 30 minutes to thoroughly pulverize the potassium stearate, thereby obtaining an aqueous dispersion K-st(5) in which 29% by weight of potassium stearate having an average particle size of 5 μm was dispersed. At this time, the pH of the aqueous dispersion was 9, and the average particle size of K-st(5) was measured / calculated in the same manner as in Preparation Example 1.

[0102] <Example> Example 1 (Step 1) 450 g of acrylic acid, 3 g of PEGDA400 (polyethylene glycol diacrylate 400) as an internal crosslinking agent, and 0.04 g of diphenyl(2,4,6-trimethylbenzoyl)-phosphine oxide as a photoinitiator were added to a 3 L glass container equipped with a stirrer and a thermometer and dissolved, and then 580 g of 31.5% sodium hydroxide solution was added to prepare a monomer composition (neutralization degree: 70 mol%; solid content: 41 wt%).

[0103] (Step 2) A calcium stearate aqueous dispersion Ca-st(5) was added to the monomer composition so that 0.1 g of calcium stearate was added per 100 g of acrylic acid, and 0.1 g of carbonate-based foaming agent sodium bicarbonate (SBC) was added per 100 g of acrylic acid. 1000 g of the prepared aqueous solution was placed in a stainless steel container with a width of 250 mm, a length of 250 mm, and a height of 30 mm, and irradiated with ultraviolet light (irradiation dose: 10 mV / cm 2 ) and UV polymerization was carried out for 90 seconds to obtain a hydrogel polymer. The obtained hydrogel polymer was crushed into pieces of 2 mm x 2 mm, and the water content was measured, which was 40.1%.

[0104] (Step 3) Next, the sheet-shaped hydrogel polymer was cut into pieces of about 5cm x 5cm, and then put into a meat chopper to crush the polymer, obtaining hydrogel particle powder (crumb) with a size of 1mm to 10mm. The powder (crumb) was then dried in an oven capable of shifting the air flow up and down. Hot air of 180°C or more was blown from bottom to top for 15 minutes, then from top to bottom for another 15 minutes to dry uniformly, so that the moisture content of the dried material after drying was 1% or less. After drying, the product was crushed in a grinder and classified to select a size of 150 to 850μm to prepare a base resin.

[0105] (Step 4) 6 parts by weight of a surface cross-linking agent aqueous solution containing 3 parts by weight of ethylene carbonate was sprayed onto 100 parts by weight of the prepared base resin powder, and the mixture was stirred at room temperature to uniformly distribute the surface cross-linking liquid on the base resin powder. Then, the base resin powder mixed with the surface cross-linking liquid was placed in a surface cross-linking reactor to carry out a surface cross-linking reaction.

[0106] In the surface crosslinking reactor, the base resin powder was gradually heated from an initial temperature of about 80°C, and was operated so as to reach a maximum reaction temperature of 190°C after 30 minutes. After reaching the maximum reaction temperature, the reaction was continued for an additional 15 minutes, and then a final superabsorbent resin sample was taken. After the surface crosslinking process, the superabsorbent resin of Example 1 having a particle size of 150μm to 850μm was produced by classifying the particles using a standard mesh sieve according to the ASTM standard.

[0107] Example 2 A superabsorbent resin was prepared in the same manner as in Example 1, except that magnesium stearate aqueous dispersion Mg-st(5) was used in place of calcium stearate aqueous dispersion Ca-st(5) as the hydrophobic particle aqueous dispersion in Example 1, so that 0.1 g of magnesium stearate was added per 100 g of acrylic acid.

[0108] Example 3 A superabsorbent resin was prepared in the same manner as in Example 1, except that sodium stearate aqueous dispersion Na-st(5) was added in an amount of 0.1 g per 100 g of acrylic acid instead of calcium stearate aqueous dispersion Ca-st(5) as the hydrophobic particle aqueous dispersion in Example 1.

[0109] Example 4 A superabsorbent resin was prepared in the same manner as in Example 1, except that potassium stearate aqueous dispersion K-st(5) was used as the hydrophobic particle aqueous dispersion in place of calcium stearate aqueous dispersion Ca-st(5) in such a manner that 0.1 g of potassium stearate was added per 100 g of acrylic acid.

[0110] Example 5 A superabsorbent resin was prepared in the same manner as in Example 1, except that calcium stearate aqueous dispersion Ca-st(20) was used as the hydrophobic particle aqueous dispersion instead of calcium stearate aqueous dispersion Ca-st(5).

[0111] Example 6 A superabsorbent resin was prepared in the same manner as in Example 1, except that magnesium stearate aqueous dispersion Mg-st(1) was used in place of calcium stearate aqueous dispersion Ca-st(5) as the hydrophobic particle aqueous dispersion in Example 1, so that 0.1 g of magnesium stearate was added per 100 g of acrylic acid.

[0112] Comparative Example 1 A superabsorbent resin was prepared in the same manner as in Example 1, except that the aqueous dispersion of hydrophobic particles was not used.

[0113] Comparative Example 2 A superabsorbent resin was prepared in the same manner as in Example 1, except that 0.02 g of 25 wt % sodium dodecyl sulfate solution (SDS, manufactured by Sigma Aldrich) was added instead of the calcium stearate aqueous dispersion Ca-st(5) in Example 1.

[0114] Comparative Example 3 A superabsorbent resin was prepared in the same manner as in Example 1, except that 0.02 g of dodecyltrimethylammonium chloride (DTAC) was added instead of the calcium stearate aqueous dispersion Ca-st(5) in Example 1.

[0115] Comparative Example 4 A superabsorbent resin was prepared in the same manner as in Example 1, except that 0.2 g of SBC and 0.05 g of 25 wt % sodium dodecyl sulfate solution (SDS) were added instead of 0.1 g of SBC and calcium stearate aqueous dispersion Ca-st(5) in Example 1.

[0116] Comparative Example 5 A superabsorbent resin was prepared in the same manner as in Example 1, except that neither the hydrophobic particle aqueous dispersion nor sodium bicarbonate (SBC) was used.

[0117] Comparative Example 6 A superabsorbent resin was prepared in the same manner as in Example 1, except that calcium stearate in powder form having an average particle size of 5 μm was used in an amount of 0.1 g per 100 g of acrylic acid instead of Ca-st(5) in the form of a hydrophobic particle aqueous dispersion in Example 1. However, it was confirmed that calcium stearate in powder form did not disperse in the monomer composition and coagulated in the neutralization solution.

[0118] <Experimental Example> The superabsorbent resins prepared in the above examples and comparative examples were evaluated for physical properties by the following methods, and the results are shown in Table 1 below. Unless otherwise indicated, all the processes for evaluating the physical properties below were carried out in a constant temperature and humidity room (23±0.5°C, relative humidity 45±0.5%), and the average value of three measurements was used to prevent measurement errors. In addition, in the following physical property evaluations, saline or salt water refers to a 0.9 wt% sodium chloride (NaCl) aqueous solution.

[0119] (1)Centrifuge Retention Capacity (CRC) The water retention capacity of each resin was measured by the water absorption capacity under no load using EDANA WSP241.3.

[0120] Specifically, the highly water-absorbent resin W 0 (g) (about 0.2 g) was evenly placed in a nonwoven envelope, sealed, and then immersed in physiological saline (0.9 wt%) at room temperature. After 30 minutes, the envelope was centrifuged at 250 G for 3 minutes to remove water, and the mass of the envelope W 2 The mass W (g) was measured after the same procedure was performed without using resin. 1 The mass (g) was measured. The CRC (g / g) was calculated using the obtained masses according to the following formula.

[0121] [Formula 1] CRC(g / g) = {[W 2 (g)-W 1 (g)] / W 0 (g)}-1

[0122] (2) Absorbtion Under Pressure (AUP) The water absorption capacity of each resin at 0.7 psi was measured by EDANA method WSP242.3.

[0123] Specifically, a 400 mesh stainless steel iron net was attached to the bottom of a plastic cylinder with an inner diameter of 60 mm. The highly water-absorbent resin W was placed on the iron net under conditions of room temperature and 50% humidity. 0 The piston is slightly smaller than 60 mm in outer diameter and has no gap with the inner wall of the cylinder so that the vertical movement is not hindered. At this time, the weight of the device is W 3 (g) was measured.

[0124] A glass filter with a diameter of 90 mm and a thickness of 5 mm was placed inside a Petri dish with a diameter of 150 mm, and physiological saline composed of 0.9% by weight of sodium chloride was placed at the same level as the upper surface of the glass filter. A sheet of filter paper with a diameter of 90 mm was placed on top of the glass filter. The measuring device was placed on the filter paper, and the liquid was absorbed under a load for one hour. After one hour, the measuring device was lifted up and its weight W 4 (g) was measured.

[0125] The obtained masses were used to calculate the water absorption capacity under pressure (g / g) according to the following formula.

[0126] [Formula 2] AUP(g / g) = [W 4 (g)-W 3 (g)] / W 0 (g)

[0127] (3) Water absorption rate (Vortex time) The water absorption rate (vortex time) of the superabsorbent resins of the above examples and comparative examples was measured by the following method.

[0128] (i) First, 50 mL of 0.9% salt water was poured into a 100 mL beaker with a flat bottom using a 100 mL measuring cylinder. (ii) Next, the beaker was placed so that it was positioned at the center of a magnetic stirrer, and then a magnetic bar (diameter 30 mm) was placed in the beaker. (iii) The stirrer was then operated so that the magnetic bar was stirring at 600 rpm, and the lowest part of the vortex generated by the stirring was touching the top of the magnetic bar. (iv) After confirming that the temperature of the salt water in the beaker had reached 24.0°C, 2±0.01 g of the superabsorbent resin sample was added while simultaneously starting a stopwatch, and the time until the liquid surface became completely horizontal while the vortex disappeared was measured in seconds, and this was regarded as the water absorption speed.

[0129] (4) Surface tension (S / T) The surface tension of the superabsorbent resins of the above Examples and Comparative Examples was measured as follows.

[0130] (i) First, 40 g of physiological saline solution composed of 0.9 wt % sodium chloride was placed in a 50 mL beaker and then stirred at 350 rpm for 3 minutes. (ii) Next, 0.5 g of superabsorbent resin was added to the stirred solution and further stirred for 3 minutes, after which the stirring was stopped and the solution was left to stand for 2 minutes to allow the swollen superabsorbent resin to sink to the bottom. (iii) The supernatant (the solution just below the surface) was then extracted with a pipette and transferred to another clean cup, after which the surface tension was measured using a surface tension meter (Force Tensiometer-K11 / K100, manufactured by Kruss).

[0131] [Table 1]

[0132] As shown in Table 1 above, the superabsorbent resins of the Examples, which were prepared by polymerization of monomers in the presence of a hydrophobic particle aqueous dispersion, exhibited a high water absorption rate and high surface tension without any reduction in water absorption performance, as compared to the superabsorbent resins of the Comparative Examples.

[0133] Specifically, the superabsorbent resins of the above examples have a water absorption rate at the same level as the superabsorbent resins of Comparative Examples 2 to 4, which use sodium dodecyl sulfate (SDS) and dodecyltrimethylammonium chloride (DTAC), which are conventionally used as foam stabilizers, but have a significantly higher surface tension.

[0134] In addition, the superabsorbent resins of the above examples have a significantly improved water absorption rate compared to the superabsorbent resin of Comparative Example 1, which does not use a bubble stabilizer, and the superabsorbent resin of Comparative Example 6, in which hydrophobic particles are added in powder form.

[0135] Therefore, when a hydrogel polymer is produced by cross-linking monomers in the presence of an aqueous dispersion of hydrophobic particles, it is confirmed that the specific surface area of ​​the superabsorbent resin can be increased without decreasing the surface tension by effectively capturing carbon dioxide generated by the foaming agent.

Claims

1. Step 1: preparing a monomer composition including an acrylic acid monomer having an acidic group, at least a portion of which has been neutralized, and an internal crosslinking agent; Step 2: preparing a hydrogel polymer by cross-linking the monomer composition in the presence of an aqueous dispersion of hydrophobic particles and a carbonate-based foaming agent; drying and grinding the hydrogel polymer to form a base resin in powder form (Step 3); and and (4) further cross-linking the surface of the base resin in the presence of a surface cross-linking agent to form a surface cross-linked layer. The hydrophobic particle aqueous dispersion is a colloidal solution in which hydrophobic particles are dispersed by a surfactant, the hydrophobic particles contain a metal salt of a fatty acid having 7 to 24 carbon atoms and have an average particle size of 1 μm to 100 μm; The hydrophobic particles are used in an amount of 0.01 to 0.5 parts by weight based on 100 parts by weight of the acrylic acid monomer. A method for producing a superabsorbent resin.

2. 2. The method for producing a highly absorbent resin according to claim 1, wherein the hydrophobic particles are one or more metal salts of stearic acid selected from the group consisting of calcium stearate, magnesium stearate, sodium stearate, zinc stearate, and potassium stearate.

3. 3. The method for producing a highly water-absorbent resin according to claim 1, wherein the hydrophobic particles have an average particle size of 1 μm to 20 μm.

4. The method for producing a superabsorbent resin according to any one of claims 1 to 3, wherein the carbonate-based foaming agent is at least one selected from the group consisting of sodium bicarbonate, sodium carbonate, potassium bicarbonate, potassium carbonate, calcium bicarbonate, calcium carbonate, magnesium bicarbonate, and magnesium carbonate.

5. The method for producing a highly absorbent resin according to any one of claims 1 to 4, wherein the carbonate-based foaming agent and the hydrophobic particles are used in a weight ratio of 1:0.1 to 1:

2.

6. The method for producing a superabsorbent resin according to claim 1 , wherein the surfactant includes a nonionic surfactant and an anionic surfactant.

7. The method for producing a superabsorbent polymer according to any one of claims 1 to 6, wherein the superabsorbent polymer has an absorption speed (vortex time) of 55 seconds or less at 24.0°C.

8. The method for producing a superabsorbent polymer according to claim 1 , wherein the superabsorbent polymer has a surface tension of 65 mN / m or more.

9. The method for producing a superabsorbent polymer according to any one of claims 1 to 8, wherein the superabsorbent polymer has a centrifugation retention capacity (CRC) of 25 to 30 g / g as measured by EDANA method WSP 241.

3.

10. The method for producing a superabsorbent polymer according to any one of claims 1 to 9, wherein the superabsorbent polymer has a water absorption capacity under pressure (AUP) of 20 to 26 g / g at 0.7 psi measured by EDANA method WSP 242.3.

Citation Information

Patent Citations

  • Production method of water-absorbent resin

    JP2002265528A

  • Method for producing absorbing resin particle

    JP2011252080A

  • Particulate water absorbent and process for production thereof

    US20120184670A1

  • Particulate water absorbent and process for production thereof

    WO2011040472A1

  • Superabsorbent polymer and preparation method therefor

    WO2019117541A1