Differential

A ferritic spheroidal graphite cast iron with controlled chemical composition addresses weldability and cracking issues, ensuring high strength and improved weldability for differential gears, reducing production costs and complexity.

JP7578405B2Active Publication Date: 2024-11-06AISIN TAKAOKA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020051562
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-23
Publication Date
2024-11-06
Estimated Expiration
2040-03-23

AI Technical Summary

Technical Problem

Spheroidal graphite cast iron used in differential gears has poor weldability and is prone to cracking, leading to increased manufacturing costs and reduced mechanical strength, especially in vehicle suspension parts.

Method used

A specific chemical composition for ferritic spheroidal graphite cast iron with controlled amounts of C, Si, Mg, Mn, P, and S, along with a Mg/P ratio of 2.1 or less, ensuring a predominantly ferritic matrix structure, which enhances weldability and reduces cracking.

Benefits of technology

The proposed cast iron composition achieves high mechanical strength and improved weldability, reducing the likelihood of cracks and simplifying production processes while maintaining strength equivalent to FCD600, suitable for differential gear components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578405000003
    Figure 0007578405000003
  • Figure 0007578405000004
    Figure 0007578405000004
  • Figure 0007578405000005
    Figure 0007578405000005
Patent Text Reader

Abstract

To provide a spheroidal graphite cast iron that has high strength and less likely to crack at weld zone.SOLUTION: A ferritic spheroidal graphite cast iron is a ferritic spheroidal cast iron containing C: 3.0 to 3.6 mass%, Si: 4.0 to 5.0 mass%, Mg: 0.020 to 0.10 mass%, Mn: 1.0 mass% or less, P: 0.10 mass% or less, and S: 0.015 mass% or less, and in which the balance is Fe and unavoidable impurities.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention ,difference This relates to operating devices. [Background technology]

[0002] Ductile iron has high toughness and mechanical strength, is inexpensive and easy to mold, and is therefore used in undercarriage and engine parts of vehicles such as automobiles. For example, vehicles are equipped with a differential gear for adjusting the difference in rotation speed between the left and right wheels that occurs when the vehicle turns, and the differential case of this differential gear is manufactured from ductile iron.

[0003] In recent years, in order to reduce weight and improve functionality in differential devices, the ring gear through which power is transmitted and the differential case are joined and integrated by welding instead of the conventional method of bolting. On the other hand, spheroidal graphite cast iron has poor weldability and is prone to cracking. Therefore, various techniques for improving the weldability of spheroidal graphite cast iron have been proposed (for example, see Patent Documents 1 and 2).

[0004] Patent Document 1 discloses that, in laser welding of cast iron and a metal material that can be welded to cast iron, the welded portion is preheated to a predetermined temperature before welding and then laser welding is performed. Patent Document 2 discloses that the weldability of spheroidal graphite cast iron is improved by heat treating pearlite matrix spheroidal graphite cast iron to make the matrix structure of the surface layer of the welded portion a ferrite layer and the matrix structure of the interior a pearlite layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-42748 A [Patent Document 2] JP 2000-63977 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the method described in Patent Document 1 requires a step of preheating the cast iron before laser welding, which may increase manufacturing costs. In addition, the method described in Patent Document 2 requires heat treatment of the cast product to make the base structure of the surface layer of the weld into a ferrite layer. For this reason, there is a concern that costs will increase, as in Patent Document 1. In addition, the method described in Patent Document 2 has low mechanical strength in the surface layer, making it unsuitable for applications in which large stress occurs in the surface layer. In particular, when used as a material for vehicle suspension parts such as differential gears, spheroidal graphite cast iron with high mechanical strength is required.

[0007] The present invention has been made to solve the above problems, and provides a high-strength steel sheet that is less susceptible to cracking at welded portions. Differential device The main purpose is to provide. [Means for solving the problem]

[0008] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by producing spheroidal graphite cast iron having a specific chemical composition. The present invention has been completed based on this knowledge. Specifically, the present invention provides the following means. [1] Ferritic spheroidal graphite cast iron containing 3.0 to 3.6 mass% C, 4.0 to 5.0 mass% Si, 0.020 to 0.10 mass% Mg, 1.0 mass% or less Mn, 0.10 mass% or less P, and 0.015 mass% or less S, with the remainder being Fe and unavoidable impurities. [2] The ferritic spheroidal graphite cast iron according to [1] above, in which the mass ratio of the Mg content to the P content (Mg / P) is 2.1 or less. [3] A differential case formed using the ferritic spheroidal graphite cast iron described above in [1] or [2]. [4] A differential device comprising the differential case of [3] above and a ring gear, the differential case and the ring gear being welded together. Effect of the Invention

[0009] According to the present invention, it is possible to obtain spheroidal graphite cast iron that is high in strength and is less susceptible to cracking at welded portions. In addition, since the differential case of the present invention is formed using the spheroidal graphite cast iron, it has high strength and excellent weldability. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a vertical cross-sectional view showing a schematic configuration of a differential device. [Diagram 2] FIG. 2 is a diagram showing a test piece for evaluating weldability used in the examples and comparative examples. [Diagram 3] FIG. 4 is a diagram showing structure photographs for evaluating the weldability of Examples 1 to 8. [Figure 4] FIG. 2 is a diagram showing structure photographs for evaluating the weldability of Examples 9 to 12 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Matters related to the present invention will be described in detail below. The spheroidal graphite cast iron of the present invention (hereinafter also referred to as "the present cast iron") is a ferritic spheroidal graphite cast iron, and contains 3.0 to 3.6 mass% C, 4.0 to 5.0 mass% Si, 0.020 to 0.10 mass% Mg, 1.0 mass% or less Mn, 0.10 mass% or less P, and 0.015 mass% or less S, with the balance being Fe and unavoidable impurities. The reasons for limiting the chemical composition of the present cast iron are as follows.

[0012] [Chemical composition of spheroidal graphite cast iron] C (carbon) is an element that forms a graphite structure. If the C content is less than 3.0 mass%, the amount of graphite crystallization decreases, and shrinkage cavities are likely to occur. If the C content exceeds 3.6 mass%, dross (floating graphite) is likely to occur. From the viewpoint of effectively strengthening cast iron while suppressing the occurrence of casting defects, the C content is preferably 3.0 to 3.5 mass% with respect to the total mass of the spheroidal graphite cast iron.

[0013] Silicon (Si) is an element that increases the amount of ferrite in the matrix of spheroidal graphite cast iron and dissolves in ferrite to strengthen the matrix. If the Si content is less than 4.0% by mass, the amount of Si dissolved is small, and the tensile strength of the resulting spheroidal graphite cast iron is insufficient. If the Si content is more than 5.0% by mass, the amount of Si dissolved is too large, and the toughness is reduced. From the viewpoint of improving the tensile strength and toughness of the spheroidal graphite cast iron, the Si content is preferably 4.1 to 5.0% by mass, and more preferably 4.2 to 4.9% by mass, based on the total mass of the spheroidal graphite cast iron.

[0014] C and Si are elements involved in the crystallization of graphite. Therefore, it is preferable that the contents of C and Si are comprehensively considered in terms of carbon equivalent (CE value=(C content (mass%))+1 / 3(Si content (mass%))). The CE value is preferably 4.5 to 5.0.

[0015] Mg (magnesium) is an element that affects the spheroidization of graphite. If the Mg content is less than 0.020% by mass, the graphite spheroidization rate is low, resulting in insufficient toughness and reduced tensile strength and elongation. If the Mg content exceeds 0.10% by mass, casting defects such as pinholes are likely to occur. The Mg content is preferably 0.025 to 0.10% by mass, more preferably 0.030 to 0.080% by mass, based on the total mass of the spheroidal graphite cast iron.

[0016] Mn (manganese) is an element that promotes pearlitization. By setting the Mn content to 1.0 mass% or less, the pearlite ratio of the matrix structure can be set to an appropriate range, and spheroidal graphite cast iron mainly composed of ferrite can be obtained. Furthermore, if the Mn content exceeds 1.0 mass%, the toughness decreases. The Mn content is preferably 0.95 mass% or less, more preferably 0.010 to 0.90 mass%, based on the total mass of the spheroidal graphite cast iron.

[0017] This cast iron contains 0.10 mass% or less of P (phosphorus). If the P content exceeds 0.10 mass% of the total mass of the spheroidal graphite cast iron, steadite (Fe3P) will crystallize, causing hot cracking in the weld metal. The P content is preferably 0.080 mass% or less of the total mass of the spheroidal graphite cast iron.

[0018] This cast iron contains 0.015% by mass or less of S (sulfur). If the S content exceeds 0.015% by mass relative to the total mass of the spheroidal graphite cast iron, the graphite spheroidization rate decreases and the toughness decreases. The S content is preferably 0.010% by mass or less relative to the total mass of the spheroidal graphite cast iron.

[0019] In the present cast iron, the mass ratio (Mg / P) of the Mg content to the P content is preferably 2.1 or less. In ferritic spheroidal graphite cast iron, intermediate temperature embrittlement occurs, in which ductility (elongation) decreases at around 400°C. In response to this, by adding P and Mg so that the Mg / P ratio is 2.1 or less, it is possible to suppress the decrease in elongation at around 400°C. The Mg / P ratio is more preferably 2.0 or less, and further preferably 1.1 to 2.0.

[0020] This cast iron contains the above components, with the remainder being Fe (iron) and unavoidable impurities. The chemical components of the spheroidal graphite cast iron are C and S, which are measured using a CS meter based on JIS G 1211, and the other components are measured using ICP atomic emission spectrometry based on JIS 1258:2014.

[0021] [Manufacturing of spheroidal graphite cast iron] The present cast iron can be manufactured according to a known method. To explain an example of the manufacturing method, first, raw materials such as iron scraps and pig iron are charged into a melting furnace, and the raw materials are melted at, for example, 1500 to 1600°C to prepare a molten metal (melting process). Here, the type and amount of inoculant are selected so as to obtain the present cast iron, and the molten metal before pouring is prepared by performing a known spheroidizing process and inoculation process. Next, the molten metal set to a predetermined pouring temperature is poured into a mold, and the molten metal is cooled (casting process). After that, the casting is removed from the mold (flask removal process). In this way, a casting as the present cast iron is obtained. The obtained casting is subjected to various processes such as cutting as necessary to obtain a cast product having a desired shape.

[0022] [Physical properties of spheroidal graphite cast iron] This cast iron is a spheroidal graphite cast iron whose matrix structure excluding the graphite structure is mainly ferrite. In cast iron, the ratio of ferrite structure in the matrix structure is expressed by the ratio of the area occupied by pearlite structure to the area of ​​the spheroidal graphite cast iron excluding the graphite structure (hereinafter referred to as "pearlite ratio"). In this case, it can be said that the lower the pearlite ratio, the higher the ratio of ferrite structure in the matrix structure.

[0023] Specifically, the pearlite ratio of the present cast iron is preferably 40% or less, more preferably 20% or less, and even more preferably 10% or less, from the viewpoint of obtaining a cast iron that is less likely to crack at the welded portion and has excellent weldability. In this specification, the "pearlite ratio" is a value calculated by the following formula (1) by image processing of a structural photograph taken by an optical microscope of a cross section of the cast iron, with the structure excluding graphite being the "area of ​​pearlite + ferrite" and the structure excluding graphite and ferrite being the "area of ​​pearlite". Details of the method for measuring the pearlite ratio follow the procedure described in the examples below. Pearlite ratio = [(area of ​​pearlite) / (area of ​​pearlite + ferrite)] x 100 …(1)

[0024] In general, the higher the pearlite ratio of the matrix structure of spheroidal graphite cast iron, the higher the tensile strength. In contrast, the present cast iron has a low pearlite ratio but high tensile strength. In other words, with the present cast iron having a chemical composition within the above range, a cast iron material with high tensile strength can be obtained, even though the metal structure of the matrix is ​​mainly ferrite. Specifically, the present cast iron has a tensile strength of, for example, 550 N / mm 2 or more, preferably 580N / mm 2 The upper limit of the tensile strength of the present cast iron is not particularly limited, but is, for example, 700 N / mm 2 The tensile strength is a value measured in accordance with JIS Z 2241:2011.

[0025] In addition, the 0.2% yield strength of this cast iron is, for example, 420N / mm 2 More than 450N / mm 2 The 0.2% proof stress is a value measured by the offset method in accordance with JIS Z 2241:2011.

[0026] The hardness of the present cast iron is, for example, 180HV20 or more in Vickers hardness (HV20), preferably 200HV20 or more, from the viewpoint of obtaining a cast iron material suitable for a differential case of a differential device. The upper limit of the Vickers hardness of the present cast iron is not particularly limited, but is, for example, 250HV20 or less from the viewpoint of improving machinability. The Vickers hardness is a value measured in accordance with JIS Z 2244:2009. The details of the measurement method of the tensile strength, 0.2% proof stress and Vickers hardness are in accordance with the method described in the examples below.

[0027] [Differential case and differential gear] This cast iron is suitable as a material for forming a differential case of a differential gear. Fig. 1 shows an example of the configuration of a differential gear 10. Fig. 1 shows a cross section including a rotation axis L1 of a differential case 20 and a ring gear 30, and a rotation axis L2 of a pinion gear 42. The differential gear 10 of this embodiment is a device that is attached to a drive shaft of a vehicle and enables left and right drive wheels to rotate at different speeds.

[0028] As shown in FIG. 1, the differential device 10 includes a differential case 20, a ring gear 30, a side gear 41, and a pinion gear 42. The differential case 20 is hollow and is formed by casting using cast iron. The interior of the differential case 20 is an accommodation chamber 21, in which the side gear 41 and the pinion gear 42 are accommodated. An annular flange portion 22 is formed and extends from the outer periphery of the lower portion of the differential case 20. In the differential device 10, the ring gear 30 is assembled to the outer periphery of the flange portion 22, thereby integrating the differential case 20 and the ring gear 30.

[0029] The ring gear 30 has an annular shape, and has teeth 31 formed on the entire outer circumferential surface thereof. In this embodiment, the ring gear 30 is formed of a helical gear, and a plurality of teeth constituting the teeth 31 are formed obliquely with respect to the rotation axis L1. The ring gear 30 is formed of, for example, carbon steel or alloy steel (such as chrome molybdenum steel (SCM)) in order to ensure the strength of the teeth 31 and the accuracy of meshing of the tooth surfaces. The side gears 41 and the pinion gears 42 are incorporated into the accommodation chamber 21 of the differential case 20 so as to form pairs.

[0030] In the differential gear 10 mounted on a vehicle, when power from a power source (e.g., an engine) is input to the ring gear 30, the differential case 20 rotates about the rotation axis L1 together with the ring gear 30. Accordingly, power is distributed to the left and right drive shafts via the pinion gears 42 and the side gears 41 while allowing differential rotation. Note that the differential mechanism of the pinion gears 42 and the side gears 41 is well known, so a detailed description thereof will be omitted here.

[0031] In the differential device 10, the ring gear 30 is joined to the flange portion 22 of the differential case 20 by fusion welding. In this embodiment, the ring gear 30 and the differential case 20 are joined by laser welding, and the ring gear 30 and the differential case 20 are integrated. The welding process is performed according to a well-known method. For example, in a state where the flange portion 22 of the differential case 20 and the inner peripheral portion of the ring gear 30 are in contact with each other, a laser is continuously irradiated from the outer peripheral side to the contact surface in the circumferential direction. In this case, a welded portion W is formed in the differential device 10 over the entire circumference of the contact portion between the inner peripheral portion of the ring gear 30 and the outer peripheral portion of the differential case 20.

[0032] The method for welding the ring gear 30 and the differential case 20 is not limited to laser welding, and may be, for example, electron beam welding, arc welding, etc. The shape of the contact surface between the flange portion 22 and the inner periphery of the ring gear 30 is not particularly limited, and may be an oblique shape, a stepped shape, or the like.

[0033] Here, when spheroidal graphite cast iron (FCD) is welded, the welded portion W is easily hardened, and the weldability tends to be poor. According to the inventor's investigation, among conventional FCDs used as the material for the differential case 20, those with a tensile strength of about 500 MPa are relatively unlikely to crack at the welded portion W. However, FCDs with a tensile strength of about 500 MPa are inferior in mechanical strength as a material for the differential case 20.

[0034] Meanwhile, among conventional FCDs used as materials for the differential case 20, FCDs with a relatively high pearlite ratio in the base and a tensile strength of 550 MPa or more are excellent in terms of mechanical strength, but the inventors' investigations have revealed that, when welded, they are more likely to crack in the welded zone W (more specifically, the heat-affected zone (HAZ)) than FCDs with a tensile strength of about 500 MPa. This is thought to be due to the transformation of pearlite in the FCD into hard and brittle martensite due to the thermal history during welding, i.e., the thermal change associated with heating cast iron to a temperature above the A1 transformation point during welding and then quenching it.

[0035] It is known that the structure of the heat-affected zone in cast iron turns white in the area in contact with the weld metal (weld bead), and this whitened area is prone to cracking due to hardening. However, the whitening of the heat-affected zone can be suppressed by a known method such as using a welding wire containing Ni.

[0036] In contrast, the present cast iron having the above-mentioned chemical composition has a base structure mainly composed of ferrite, so that it is difficult to transform into martensite during welding, and cracks are unlikely to occur in the welded part W even when welding is performed. In addition, the present cast iron has a high tensile strength, and has a tensile strength equivalent to that of FCD600 specified in JIS G5502. Thus, the present cast iron, which has excellent mechanical strength and weldability, is suitable as a material for the differential case 20 that is integrated with the ring gear 30 by welding.

[0037] Moreover, with this cast iron, cracks are unlikely to occur in the welded portion W, and the strength of the welded portion is highly reliable, so that it is possible to simplify the inspection process of the welded portion W using an ultrasonic flaw detector or the like. Furthermore, since the weldability of this cast iron is improved by the chemical components of the base structure, there is no need to perform special heat treatment on the cast article to improve the weldability of the cast iron. This makes it possible to suppress an increase in the number of steps in the production line and an increase in production costs. EXAMPLES

[0038] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are based on mass unless otherwise specified. Chemical components and physical properties were measured as follows.

[0039] [Measurement of chemical composition]: The chemical composition of the spheroidal graphite cast iron was measured using a CS meter based on JIS G 1211 for C and S, and using ICP atomic emission spectrometry based on JIS 1258:2014 for other components. [Tensile strength and elongation]: In accordance with JIS Z 2241:2011, No. 4 test pieces were prepared and the tensile strength (maximum stress) and elongation (elongation at break) were measured at room temperature from a stress-strain diagram. [0.2% yield strength]: Measured according to JIS Z 2241:2011 using the offset method. [Hardness]: Vickers hardness was measured in accordance with JIS Z2244:2009 with a test force of 196.1 N at room temperature. [Pearlite ratio]: The cross section of the cast iron was photographed at 100x magnification using an optical microscope (Olympus Corporation). The photographed structure was processed to extract the structure excluding graphite as the "area of ​​pearlite + ferrite," and the structure excluding graphite and ferrite as the "area of ​​pearlite." The pearlite ratio [%] was calculated using the above formula (1).

[0040] [Example 1] 1. Manufacturing of spheroidal graphite cast iron Scrap iron was added to a high-frequency induction melting furnace and heated to melt the material. An inoculant and a spheroidizing agent were added to the obtained molten metal, and the molten metal was poured into a Y-block shaped mold. After that, the molten metal was cooled in the mold to the dismantling temperature, and the cast iron was removed from the mold. The chemical composition of the obtained spheroidal graphite cast iron is shown in Table 1. However, the remainder omitted from Table 1 is Fe and unavoidable impurities. In Table 1, "-" indicates that the component is not contained. For the spheroidal graphite cast iron of Example 1, the mass ratio of the Mg content to the P content (Mg / P) was 2.0.

[0041] 2. Evaluation The spheroidal graphite cast iron produced in 1 above was measured for tensile strength (MPa), breaking elongation (%), 0.2% yield strength (MPa), hardness (HV20), and pearlite ratio (%). The evaluation results are shown in Table 2. The spheroidal graphite cast iron of Example 1 had a pearlite ratio of 1% and was a ferrite matrix.

[0042] 3. Evaluation of weldability The evaluation test piece 50 shown in FIG. 2 was made using the spheroidal graphite cast iron produced in the above 1. and steel (SCM420). The evaluation test piece 50 is formed by stacking an FCD plate 52 made of spheroidal graphite cast iron on an annular gear material 51 made of steel (SCM420). The FCD plate 52 is a circular plate corresponding to the upper surface shape of the gear material 51. For this evaluation test piece 50, a laser was irradiated from the side to an abutment portion 53 between the gear material 51 and the FCD plate 52, and the gear material 51 and the FCD plate 52 were integrated by laser welding. The laser welding was performed using a Ni-containing welding wire under the conditions of a laser output of 3.8 kW and a welding speed of 1.5 m / min. The cross section of the welded portion of the evaluation test piece 50 was photographed with an optical microscope (manufactured by Olympus) at a magnification of 100 times to evaluate the weldability. A structural photograph of the cross section of the welded portion is shown in FIG. 3. 3, "FCD" corresponds to the FCD plate 52 of the evaluation test piece 50, and "SCM" corresponds to the gear material 51. "Bead" represents a weld bead (the same applies to FIG. 4).

[0043] [Examples 2 to 12] The tensile strength, fracture elongation, 0.2% yield strength, hardness and pearlite rate were measured and the weldability was evaluated in the same manner as in Example 1, except that the spheroidal graphite cast iron used was changed to spheroidal graphite cast iron having the chemical composition shown in Table 1. The evaluation results are shown in Table 2, Figures 3 and 4. The Mg / P ratios of the spheroidal graphite cast irons of Examples 2 to 12 were 2.0, 1.7, 1.2, 1.2, 1.1, 1.1, 1.7, 1.4, 0.95, 1.9 and 1.1, respectively.

[0044] [Comparative Example 1] The tensile strength, fracture elongation, 0.2% yield strength, hardness and pearlite ratio were measured and the weldability was evaluated in the same manner as in Example 1, except that the spheroidal graphite cast iron used was changed to spheroidal graphite cast iron equivalent to FCD450 having the chemical composition shown in Table 1. The evaluation results are shown in Table 2 and Figure 4. The spheroidal graphite cast iron of Comparative Example 1 had an Mg / P ratio of 2.3. [Comparative Example 2] The tensile strength, fracture elongation, 0.2% yield strength, hardness and pearlite rate were measured and the weldability was evaluated in the same manner as in Example 1, except that the spheroidal graphite cast iron used was changed to spheroidal graphite cast iron equivalent to FCD600 having the chemical composition shown in Table 1. The evaluation results are shown in Table 2 and Figure 4. The spheroidal graphite cast iron of Comparative Example 2 had Mg / P = 2.0.

[0045] [Table 1]

[0046] [Table 2]

[0047] Comparing the mechanical properties of spheroidal graphite cast iron between Examples 1 to 12 and Comparative Examples 1 and 2, as shown in Table 2, the FCDs of Examples 1 to 12 had pearlite ratios lower or similar to those of Comparative Example 1 (FCD450), but showed tensile strengths 110 MPa or more higher than Comparative Example 1 and values ​​comparable to those of Comparative Example 2 (FCD600). In addition, the FCDs of Examples 1 to 12 showed values ​​equivalent to or higher than those of Comparative Example 2 (FCD600) in terms of 0.2% yield strength and elongation. The FCDs of Examples 1 to 12 also showed hardness equivalent to that of Comparative Example 2 (FCD600).

[0048] 3 and 4, in Examples 1 to 12 and Comparative Example 1 (FCD450), no cracks were observed in the welded portion between the gear material 51 and the FCD plate 52. In contrast, in Comparative Example 2 (FCD600), cracks occurred throughout the entire welded portion between the gear material 51 and the FCD plate 52. From the above results, it is clear that the spheroidal graphite cast iron of the present invention has excellent weldability while having high mechanical strength equivalent to that of FCD600. [Explanation of symbols]

[0049] 10...differential device, 20...differential case, 21...accommodation chamber, 22...flange portion, 30...ring gear, 41...side gear, 42...pinion gear, 50...evaluation test piece, W...welded portion.

Claims

1. A differential device comprising a differential case and a ring gear, the differential case and the ring gear being welded together, The differential case contains 3.0 to 3.5 mass% C, 4.6 to 5.0 mass% Si, 0.020 to 0.10 mass% Mg, 1.0 mass% or less Mn, 0.10 mass% or less P, and 0.015 mass% or less S, with the balance being Fe and unavoidable impurities. A differential device formed using ferritic spheroidal graphite cast iron.

2. 2. The differential gear according to claim 1, wherein a mass ratio (Mg / P) of the Mg content to the P content in the ferritic spheroidal graphite cast iron is 2.1 or less.

Citation Information

Patent Citations

  • JP1975124817A

  • Spheroidal graphite cast iron excellent in wear resistance and oxidation resistance

    JP1988072850A

  • Spheroidal graphite cast iron and its production

    JP1990166257A

  • Casting made of spheroidal graphite cast iron

    JP2000063977A

  • Manufacturing method of spheroidal graphite cast iron casting

    JP2008229640A