Quantum dot barrier rib structure and preparation method thereof
The quantum dot barrier rib structure, composed of a specific resin composition, addresses the challenge of achieving high light-blocking and low reflectance with uniform thickness, improving resolution and preventing color mixing in quantum dot devices.
Patent Information
- Application Number
- JP2020089318
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-15
- Filing Date
- 2020-05-22
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-05-22
AI Technical Summary
Existing quantum dot devices face challenges in achieving high light-blocking properties and low reflectance while maintaining excellent resolution and pattern properties, with issues such as non-uniform film thickness leading to color mixing and poor resolution.
A quantum dot barrier rib structure formed from a photosensitive resin composition comprising a copolymer, photopolymerizable compound, photopolymerization initiator, and black colorant, with specific optical density and reflectance relationships, allowing for a multilayer cured film with uniform thickness and adjusted reflectance ratios.
The structure achieves high light-blocking properties and low reflectance, preventing color mixing and enhancing resolution in quantum dot displays by ensuring uniform film thickness and appropriate reflectance ratios.
Smart Images

Figure 0007578420000013 
Figure 0007578420000014 
Figure 0007578420000015
Abstract
Description
[Technical field]
[0001] The present invention relates to a quantum dot barrier rib structure that meets the properties of high light shielding and low reflectance, and a method for preparing the same. [Background technology]
[0002] In recent years, there has been growing interest in various electronic devices that use quantum dots (QDs).
[0003] Quantum dots are materials that produce the effect of quantum confinement as nanocrystals of semiconductor materials with diameters of approximately 10 nm or less. They consist of hundreds of thousands of electrons or more, but most of the electrons are tightly bound to atomic nuclei, so that the number of unbound free electrons is limited to about 1-100. In such cases, the energy levels of the electrons are discontinuously limited to exhibit electrical and optical properties different from those of semiconductors in the bulk state forming a continuous band. These quantum dots can produce various colors by generating light wavelengths of different lengths for each particle size even without a change in material type. Since they have the advantages of high color purity and light safety compared to conventional light emitters, they are currently used in various fields such as displays, solar cells, biosensors, and lighting, and are attracting attention as the next generation of light-emitting devices.
[0004] FIG. 1 is a schematic diagram illustrating a typical quantum dot device. Referring to FIG. 1, the substrate structure (100) of the quantum dot device includes a transparent substrate (110) and a barrier rib (120) formed on the transparent substrate (110) to separate areas. Different quantum dot solutions, i.e., a first quantum dot solution (130), a second quantum dot solution (140), and a third quantum dot solution (150), are present in each separate area. The first quantum dot solution (130), the second quantum dot solution (140), and the third quantum dot solution (150) are composed of quantum dots with different energy levels. That is, they are configured to have different emission wavelength bands as the size or material of the quantum dots is manipulated.
[0005] Here, the barrier rib 120 not only functions as a light shielding layer, but also serves to prevent the compositions of different colors poured into the divided areas from mixing together. In general, it can be formed as a film from a photosensitive resin composition.
[0006] In such a case, the photosensitive resin composition used should be able to prevent the deterioration of contrast and color purity caused by light leakage between pixels. In recent years, research on quantum dot devices has been actively conducted, and there is a demand for improved performance in terms of excellent pattern characteristics, low reflectance, and high light blocking. In addition, in order to be applied to quantum dot devices, it is necessary to achieve a uniform film and a suitable film thickness to maintain excellent resolution. For example, if the film is not uniform or the film thickness is too small, it is not suitable for the barrier rib, so the quantum dot solution will overflow the barrier rib, resulting in color mixing or deterioration of resolution. If the film thickness is adjusted by coating the photosensitive resin composition thickly and curing it to solve this problem, there is a problem that it is difficult to achieve a uniform coating, which may cause dirt or contamination. Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, an object of the present invention is to provide a quantum dot barrier rib structure and a preparation method thereof that satisfy properties such as high light shielding property and low reflectance while maintaining excellent resolution and pattern characteristics. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention provides a quantum dot barrier rib structure comprising a cured film formed from a photosensitive resin composition comprising: (A) a copolymer; (B) a photopolymerizable compound; (C) a photopolymerization initiator; and (D) a colorant including a black colorant, The quantum dot barrier rib structure has a total thickness of 6 μm or more and an optical density of 0.05 / μm to 2.0 / μm, and the following relationships, respectively: (Relationship 1) R SCI ≦5.0% (Relationship 2) R SCE ≦0.5% (Relationship 3)2 % ≦R SCE / R SCI <= 10 % The reflectance R measured by the SCI (specular reflection included) method at a wavelength of 550 nm satisfies SCI and reflectance R measured by the SCE (specular reflection not included) method SCE have Provide structures.
[0009] In order to achieve another object, the present invention provides a quantum dot barrier rib structure, comprising a first cured film formed from a first photosensitive resin composition, and a second cured film formed from a second photosensitive resin composition on the first cured film, the first photosensitive resin composition, the second photosensitive resin composition, or both, comprise: (A) a copolymer; (B) a photopolymerizable compound; (C) a photopolymerization initiator; and (D) a colorant, the colorant comprising a black colorant, and the structure has a total thickness of 6 μm or greater. Provide structures.
[0010] In addition, to achieve another object, the present invention provides a method for preparing a quantum dot barrier rib structure, comprising the steps of: coating a first photosensitive resin composition on a substrate and curing it to form a first cured film; coating a second photosensitive resin composition on the first cured film and curing it to form a second cured film; and exposing and developing a multi-layer cured film comprising the first cured film and the second cured film to form a pattern, and then curing it, wherein the first photosensitive resin composition, the second photosensitive resin composition, or both, comprise a colorant, comprising: (A) a copolymer; (B) a photopolymerizable compound; (C) a photopolymerization initiator; and (D) a black colorant.
[0011] Advantageous Effects of the Invention The quantum dot barrier rib structure of the present invention comprises a cured film having a uniform film thickness and a suitable range of film thicknesses, where the reflectance R measured by the SCI (specular reflection included) method is SCI and reflectance R measured by the SCE (specular reflection not included) method SCE decreases, and the ratio between them (R SCE / R SCI ) is appropriately adjusted, so that the resolution and pattern characteristics are maintained excellent while simultaneously satisfying characteristics such as high light blocking property and low reflectance.
[0012] In addition, when the structure of the quantum dot barrier rib is prepared, it is possible to form a multi-layer pattern with a uniform film thickness suitable for the quantum dot barrier rib in a single development process, which can therefore be advantageously used for quantum dot displays. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram illustrating a typical quantum dot device. [Diagram 2] FIG. 2 is a schematic diagram of a quantum dot barrier rib structure comprising a two-layer cured film according to an embodiment of the present invention. [Diagram 3]FIG. 2 is a schematic diagram of a quantum dot barrier rib structure comprising a three-layer cured film according to an embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram of a structure of a quantum dot barrier rib including an n-layer cured film according to an embodiment of the present invention. [Diagram 5] 1 shows photographs of the cross section and side surface of the quantum dot barrier rib structures of Examples 1 to 13 observed with an optical microscope. [Figure 6] 1 shows photographs of the cross sections and side surfaces of the quantum dot barrier rib structures of Comparative Examples 1 to 12 observed with an optical microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention is not limited to the following description, but can be modified in various forms without departing from the spirit of the present invention.
[0015] Throughout this specification, when a portion is said to "comprise" certain elements, it is understood that other elements may be included, rather than excluding other elements, unless otherwise specified. Additionally, all numbers and expressions relating to quantities of ingredients, reaction conditions, and the like used in this specification should be understood to be modified by the term "about," unless otherwise specified.
[0016] The quantum dot barrier rib structure may include a cured film formed from a photosensitive resin composition including (A) a copolymer, (B) a photopolymerizable compound, (C) a photopolymerization initiator, and (D) a colorant including a black colorant. In such a case, the photosensitive resin composition may optionally further include at least one selected from the group consisting of (E) a surfactant, (F) an additive, and (G) a solvent.
[0017] According to an embodiment, the quantum dot barrier rib structure has a total thickness of 6 μm or more and an optical density of 0.05 / μm to 2.0 / μm. The transmittance at 550 nm can be measured using an optical density meter (361T manufactured by Xlite) to obtain the optical density (OD, unit: / μm) based on a thickness of 1 μm of the quantum dot barrier rib structure.
[0018] In addition, in the structure of the quantum dot barrier rib, the reflectance R measured by the SCI (including specular reflection) method at a wavelength of 360 nm to 740 nm or 550 nm is SCI and reflectance R measured by the SCE (specular reflection not included) method SCE may respectively satisfy the following relationships: (Relationship 1) R SCI ≦5.0% (Relationship 2) R SCE ≦0.5% (Relationship 3)2 % ≦R SCE / R SCI <= 10 % .
[0019] R SCI R means the total reflectance, which includes specular reflection of light incident on the surface of an object and reflected at the same angle, and diffuse reflection, which is scattered and reflected in various directions without specular reflection. SCE means diffuse reflection alone, i.e., the total reflectance from which specular reflection has been subtracted.
[0020] Hereinafter, each component of the photosensitive resin composition will be described in detail.
[0021] As used herein, the term "(meth)acrylic" means "acrylic" and / or "methacrylic", and the term "(meth)acrylate" means "acrylate" and / or "methacrylate".
[0022] The weight average molecular weight (g / mol, Da) of each component as described below is determined by gel permeation chromatography (GPC, eluent: tetrahydrofuran) relative to polystyrene standards.
[0023] (A) Copolymer The copolymer (A) used in the present invention may contain at least two structural units selected from the group consisting of (a-1) structural units derived from an ethylenically unsaturated carboxylic acid, an ethylenically unsaturated carboxylic acid anhydride, or a combination thereof, (a-2) structural units derived from an ethylenically unsaturated compound containing an aromatic ring, (a-3) structural units derived from an ethylenically unsaturated compound containing an epoxy group, and (a-4) structural units derived from an ethylenically unsaturated compound different from (a-1), (a-2), and (a-3).
[0024] According to one embodiment, the copolymer (A) may comprise structural units (a-1) and (a-4).
[0025] According to another embodiment, the copolymer (A) may comprise structural units (a-1), (a-2), and (a-4).
[0026] According to another embodiment, the copolymer (A) may comprise structural units (a-1), (a-3), and (a-4).
[0027] According to another embodiment, the copolymer (A) may comprise structural units (a-1), (a-2) and (a-3).
[0028] According to another embodiment, the copolymer (A) may comprise structural units (a-1), (a-2), (a-3), and (a-4).
[0029] The copolymer (A) is an alkali-soluble resin for developability, and can also play the role of a base for forming a film during coating and a structure for forming the final pattern.
[0030] (a-1) Structural units derived from ethylenically unsaturated carboxylic acids, ethylenically unsaturated carboxylic anhydrides, or combinations thereof The structural unit (a-1) is derived from an ethylenically unsaturated carboxylic acid, an ethylenically unsaturated carboxylic anhydride, or a combination thereof. Ethylenically unsaturated carboxylic acids and ethylenically unsaturated carboxylic anhydrides are polymerizable unsaturated monomers containing at least one carboxyl group in the molecule. Specific examples thereof include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, α-chloroacrylic acid, and cinnamic acid; unsaturated dicarboxylic acids and their anhydrides such as maleic acid, maleic anhydride, fumaric acid, itaconic acid, itaconic anhydride, citraconic acid, citraconic anhydride, and mesaconic acid; unsaturated polycarboxylic acids and their anhydrides having three or more valences; and mono[(meth)acryloyloxyalkyl]esters of divalent or higher polycarboxylic acids such as mono[2-(meth)acryloyloxyethyl]succinate and mono[2-(meth)acryloyloxyethyl]phthalate. The structural units derived from the above-exemplified compounds may be contained in the copolymer alone or in combination of two or more.
[0031] The amount of the structural unit (a-1) may be 5 to 65 mol %, or 10 to 50 mol %, based on the total moles of the structural units constituting the copolymer (A). Within the above range, it may have advantageous developability.
[0032] (a-2) Structural unit derived from an ethylenically unsaturated compound containing an aromatic ring The structural unit (a-2) is derived from an ethylenically unsaturated compound containing an aromatic ring. Specific examples of the ethylenically unsaturated compound containing an aromatic ring include phenyl (meth)acrylate, benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, p-nonylphenoxypolyethylene glycol (meth)acrylate, p-nonylphenoxypolypropylene glycol (meth)acrylate, tribromophenyl (meth)acrylate; styrene; alkyl styrene such as methylstyrene, dimethylstyrene, trimethylstyrene, ethylstyrene, diethylstyrene, triethylstyrene, propylstyrene, butylstyrene, hexylstyrene, heptylstyrene, and octylstyrene. Examples of the styrene that contains alkyl substituents include styrene that contains halogens such as fluorostyrene, chlorostyrene, bromostyrene, and iodostyrene; styrene that contains alkoxy substituents such as methoxystyrene, ethoxystyrene, and propoxystyrene; 4-hydroxystyrene, p-hydroxy-α-methylstyrene, acetylstyrene; and vinyltoluene, divinylbenzene, vinylphenol, o-vinylbenzyl methyl ether, m-vinylbenzyl methyl ether, p-vinylbenzyl methyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, and the like. The structural unit derived from the above-exemplified compounds can be contained in the copolymer alone or in combination of two or more. In order to obtain the polymerizability of the composition, the structural unit derived from a styrene compound is preferred among these examples.
[0033] The amount of the structural unit (a-2) may be 1-50 mol%, or 3-40 mol%, based on the total moles of the structural units constituting the copolymer (A). Within the above content range, it may be more advantageous in terms of chemical resistance.
[0034] (a-3) Structural unit derived from an ethylenically unsaturated compound containing an epoxy group The structural unit (a-3) is derived from an ethylenically unsaturated compound containing an epoxy group. Specific examples of the ethylenically unsaturated compound containing an epoxy group include glycidyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 4,5-epoxypentyl (meth)acrylate, 5,6-epoxyhexyl (meth)acrylate, 6,7-epoxyheptyl (meth)acrylate, 2,3-epoxycyclopentyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, α-ethylglycidyl acrylate, α-n-propyl acrylate, α ... Examples of the structural units derived from the above-exemplified compounds include glycidyl acrylate, α-n-butyl glycidyl acrylate, N-(4-(2,3-epoxypropoxy)-3,5-dimethylbenzyl)acrylamide, N-(4-(2,3-epoxypropoxy)-3,5-dimethylphenylpropyl)acrylamide, 4-hydroxybutyl(meth)acrylate glycidyl ether, 4-hydroxybutyl acrylate glycidyl ether, allyl glycidyl ether, 2-methylallyl glycidyl ether, and the like. The structural units derived from the above-exemplified compounds may be contained in the copolymer alone or in combination of two or more. Among the above, at least one selected from structural units derived from glycidyl(meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, and 4-hydroxybutyl(meth)acrylate glycidyl ether is more preferred from the viewpoint of improving copolymerizability and strength of the cured film.
[0035] The amount of the structural unit (a-3) may be 1 to 40 mol %, or 5 to 20 mol %, based on the total moles of the structural units constituting the copolymer (A). Within the above range, it may be more advantageous in terms of residues during processing and margins during pre-baking.
[0036] (a-4) A structural unit derived from an ethylenically unsaturated compound different from (a-1), (a-2), and (a-3). The copolymer (A) used in the present invention may further contain, in addition to (a-1), (a-2), and (a-3), structural units derived from an ethylenically unsaturated compound different from (a-1), (a-2), and (a-3).
[0037] Specific examples of structural units derived from ethylenically unsaturated compounds other than the structural units (a-1), (a-2), and (a-3) include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, cyclohexyl (meth)acrylate, ethylhexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, ethylhexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, ethylhexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, ethylhexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, ethylhexyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, ethylhexyl (meth)acrylate, ethylhexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, ethylhex ... (meth)acrylate, 2-hydroxy-3-chloropropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol (meth)acrylate, methyl α-hydroxymethyl acrylate, ethyl α-hydroxymethyl acrylate, propyl α-hydroxymethyl acrylate, butyl α-hydroxymethyl acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate acrylate, methoxytripropylene glycol (meth)acrylate, poly(ethylene glycol) methyl ether (meth)acrylate, trifluoroethyl (meth)acrylate, trifluoro(meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoroisopropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate unsaturated carboxylic acid esters such as N-vinyl ether, dicyclopentanyloxyethyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate; tertiary amines containing an N-vinyl group such as N-vinylpyrrolidone, N-vinylcarbazole, and N-vinylmorpholine; unsaturated ethers such as vinyl methyl ether and vinyl ethyl ether; unsaturated imides such as N-phenylmaleimide, N-(4-chlorophenyl)maleimide, N-(4-hydroxyphenyl)maleimide, and N-cyclohexylmaleimide.The structural units derived from the compounds exemplified above may be contained in the copolymer either alone or in combination of two or more.
[0038] In addition, according to some embodiments, the structural unit (a-4) may include a fluorine-containing compound. For example, it may include at least one selected from trifluoroethyl (meth)acrylate, hexafluoroisopropyl (meth)acrylate, and octafluoropentyl (meth)acrylate.
[0039] The amount of the structural unit (a-4) may be from more than 0 to 80 mol%, or from 30 to 70 mol%, based on the total moles of the structural units constituting the copolymer (A). Within the above range, the storage stability of the photosensitive resin composition can be maintained, and the film retention rate can be more advantageously increased.
[0040] According to an embodiment, examples of copolymers having structural units (a-1) to (a-4) include copolymers of (meth)acrylic acid / styrene / methyl (meth)acrylate / glycidyl (meth)acrylate, copolymers of (meth)acrylic acid / styrene / methyl (meth)acrylate / glycidyl (meth)acrylate / N-phenylmaleimide, copolymers of (meth)acrylic acid / styrene / methyl (meth)acrylate / glycidyl (meth)acrylate / N-cyclohexylmaleimide, copolymers of (meth)acrylic acid / styrene / n-butyl (meth)acrylate / glycidyl (meth)acrylate / N-phenylmaleimide, copolymers of (meth)acrylic acid / styrene / glycidyl (meth)acrylate / N-phenylmaleimide, copolymers of (meth)acrylic acid / styrene / glycidyl (meth)acrylate / N-phenylmaleimide, copolymers of (meth)acrylic acid / styrene / 4-hydroxybutyl acrylate glycidyl ether / N-phenylmaleimide, and the like. One, two or more copolymers may be included in the photosensitive resin composition.
[0041] According to an embodiment, examples of copolymers having structural units (a-1) to (a-4) may include copolymers of (meth)acrylic acid / methyl (meth)acrylate / trifluoro(meth)acrylate / butyl (meth)acrylate, copolymers of (meth)acrylic acid / methyl (meth)acrylate / trifluoroethyl (meth)acrylate / butyl (meth)acrylate, copolymers of (meth)acrylic acid / methyl (meth)acrylate / hexafluoroisopropyl (meth)acrylate / butyl (meth)acrylate, and copolymers of (meth)acrylic acid / methyl (meth)acrylate / octafluoropentyl (meth)acrylate / butyl (meth)acrylate.
[0042] The weight average molecular weight of the copolymer (A) may be 4,000 to 20,000 Da or 6,000 to 15,000 Da. When the weight average molecular weight of the copolymer (A) is within the above range, the process difference due to a lower pattern can be advantageously improved, and the pattern profile during development can be advantageous.
[0043] The amount of copolymer (A) in the entire photosensitive resin composition may be 5-50 wt %, or 10-40 wt %, based on the total weight of the solids content (i.e., the weight excluding the solvent) of the photosensitive resin composition. Within the above ranges, the pattern profile upon development may be favorable, and properties such as film retention and chemical resistance may be improved.
[0044] The copolymer (A) can be prepared by charging a radical polymerization initiator, a solvent, and at least two of the structural units (a-1), (a-2), (a-3), and (a-4) into a reactor, subsequently charging it with nitrogen, and slowly stirring the mixture for polymerization.
[0045] The radical polymerization initiator may be, but is not limited to, an azo compound such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile); or benzoyl peroxide, lauryl peroxide, t-butyl peroxypivalate, 1,1-bis(t-butylperoxy)cyclohexane, etc. The radical polymerization initiator may be used alone or in combination of two or more.
[0046] The solvent may be any conventional solvent commonly used in the preparation of copolymers (A) and may include, for example, propylene glycol monomethyl ether acetate (PGMEA).
[0047] (B) Photopolymerizable compound The photopolymerizable compound (B) used in the present invention can be a monofunctional or polyfunctional ester compound having at least one ethylenically unsaturated double bond. In particular, it can be a polyfunctional compound having at least two functional groups from the viewpoint of chemical resistance.
[0048] The photopolymerizable compound (B) is, for example, dipentaerythritol hexaacrylate, di(trimethylolpropane)tetraacrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, glycerin tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, a monoester of pentaerythritol tri(meth)acrylate and succinic acid ... The acrylate or acrylate copolymer may be selected from the group consisting of, but is not limited to, triethyl acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, monoester of dipentaerythritol penta(meth)acrylate and succinic acid, pentaerythritol triacrylate-hexamethylene diisocyanate (reaction product of pentaerythritol triacrylate and hexamethylene diisocyanate), tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, bisphenol A epoxy acrylate, ethylene glycol monomethyl ether acrylate, and mixtures thereof.
[0049] Examples of commercially available photopolymerizable compounds include (i) monofunctional (meth)acrylates such as Aronix M-101, M-111, and M-114 manufactured by Toagosei Co., Ltd., KAYARAD T4-110S, T-1420, and T4-120S manufactured by Nippon Kayaku Co., Ltd., and V-158 and V-2311 manufactured by Osaka Organic Chemical Industry Co., Ltd.; (ii) difunctional (meth)acrylates such as Aronix M-210, M-240, and M-6200 manufactured by Toagosei Co., Ltd., KAYARAD HDDA, HX-220, and R-604 manufactured by Nippon Kayaku Co., Ltd., and V-260, V-312, and V-335 HP manufactured by Osaka Organic Chemical Industry Co., Ltd., and (iii) difunctional (meth)acrylates such as Aronix M-210, M-240, and M-6200 manufactured by Toagosei Co., Ltd., KAYARAD HDDA, HX-220, and R-604 manufactured by Nippon Kayaku Co., Ltd., and V-260, V-312, and V-335 HP manufactured by Osaka Organic Chemical Industry Co., Ltd. Mention may be made of tri- or higher functional (meth)acrylates such as M-309, M-400, M-403, M-405, M-450, M-7100, M-8030, M-8060, and TO-1382, KAYARAD TMPTA, DPHA, and DPHA-40H manufactured by Nippon Kayaku Co., Ltd., and V-295, V-300, V-360, V-GPT, V-3PA, V-400, and V-802 manufactured by Osaka Organic Chemical Industry Co., Ltd.
[0050] The amount of photopolymerizable compound (B) can be 10-200 parts by weight, 10-150 parts by weight, 15-100 parts by weight, or 15-90 parts by weight based on 100 parts by weight of copolymer (A) based on solid content excluding solvent. When the amount of photopolymerizable compound (B) is within the above range, the pattern developability and coating property can be excellent while keeping the film retention rate constant. When the amount of photopolymerizable compound is less than the above range, the development time will be longer, which may affect the process and residue. When it exceeds the above range, it may cause the problem that the pattern resolution becomes too high.
[0051] (C) Photopolymerization initiator The photoinitiator (C) used in the present invention can be any known photoinitiator.
[0052] The photopolymerization initiator (C) may be selected from the group consisting of acetophenone-based compounds, non-imidazole-based compounds, triazine-based compounds, onium salt-based compounds, benzoin-based compounds, benzophenone-based compounds, polynuclear quinone-based compounds, thioxanthone-based compounds, diazo-based compounds, imide sulfonate-based compounds, oxime-based compounds, carbazole-based compounds, sulfonium borate-based compounds, ketone-based compounds, and mixtures thereof.
[0053] In particular, an oxime-based compound, a triazine-based compound, or a combination thereof may be used as the photopolymerization initiator (C). More particularly, a combination of an oxime-based compound and a triazine-based compound may be used.
[0054] Specific examples of the photopolymerization initiator (C) include 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), benzoyl peroxide, lauryl peroxide, t-butyl peroxypivalate, 1,1-bis(t-butylperoxy)cyclohexane, p-dimethylaminoacetophenone, 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]phenyl. ]-1-butanone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzil dimethyl ketal, benzophenone, benzoin propyl ether, diethylthioxanthone, 2,4-bis(trichloromethyl)-6-p-methoxyphenyl-s-triazine, 2-trichloromethyl-5-styryl-1,3,4-oxodiazole, 9-phenylacridine, 3-methyl-5-amino-((s-triazin-2-yl)amino) -3-Phenylcoumarin, 2-(o-chlorophenyl)-4,5-diphenylimidazoyl dimer, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-[4-(phenylthio)phenyl]-octane-1,2-dione-2-(o-benzoyloxime), o-benzoyl-4'-(benzmercapto)benzoyl-hexyl-ketoxime, 2,4,6-trimethylphenylcarbonyl-diphenylphospho These may include, but are not limited to, phenyl oxides, hexafluorophosphoro-trialkylphenylsulfonium salts, 2-mercaptobenzimidazole, 2,2'-benzothiazolyl disulfide, 2-(4-styrylphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-ylphenyl)-butan-1-one, and mixtures thereof.
[0055] For reference, examples of commercially available oxime-based photoinitiators include OXE-01 (BASF), OXE-02 (BASF), OXE-03 (BASF), N-1919 (ADEKA), NCI-930 (ADEKA), NCI-831 (ADEKA), and SPI-03 (Samyang). Examples of triazine-based photoinitiators include 2-[4-(2-phenylethenyl)phenyl]-4,6-bis(trichloromethyl)-1,3,5-triazine (Triazine Y, Tronly), etc.
[0056] The photopolymerization initiator (C) can be used in an amount of 0.1 to 10 parts by weight, 0.1 to 8 parts by weight, 0.5 to 8 parts by weight, or 0.5 to 6 parts by weight, based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent.
[0057] In particular, an oxime compound in an amount of 0.05 to 4 parts by weight and / or a triazine compound in an amount of 0.05 to 2 parts by weight based on 100 parts by weight of the copolymer (A) can be used as a photopolymerization initiator.
[0058] More particularly, an oxime compound in an amount of 0.05 to 3.5 parts by weight and / or a triazine compound in an amount of 0.05 to 1.5 parts by weight based on 100 parts by weight of the copolymer (A) can be used as a photopolymerization initiator. When the oxime compound is used in the amount within the above range, it is possible to improve the development property and the coating property as well as the high sensitivity. In addition, when the triazine compound is used in the amount within the above range, it is possible to obtain a cured film having excellent chemical resistance and taper angle during the formation of a pattern as well as high sensitivity.
[0059] (D) Coloring agent The photosensitive resin composition of the present invention may contain a colorant (D) for imparting light-shielding properties to the composition. The colorant (D) may contain a black colorant.
[0060] The black colorant may include at least one selected from the group consisting of a black organic colorant and a black inorganic colorant. In particular, the colorant (D) may include a mixture of a black organic colorant and a black inorganic colorant. In addition, the colorant (D) may include a black organic colorant alone or a black inorganic colorant alone.
[0061] In addition, the colorant (D) may include colorants other than a black colorant.
[0062] In particular, the colorant (D) may comprise a black organic colorant and a colorant other than black. Alternatively, the colorant (D) may comprise a black inorganic colorant and a colorant other than black. Alternatively, the colorant (D) may comprise a black organic colorant, a black inorganic colorant, and a colorant other than black. It is preferred that the colorant (D) has high pigmentation and high heat resistance.
[0063] According to an embodiment, the colorant (D) may comprise a black inorganic colorant and a black organic colorant in a weight ratio of 1-50:50-99.
[0064] According to an embodiment, the colorant (D) may contain a black organic colorant and a non-black colorant in a weight ratio of 60-90:10-40.
[0065] According to an embodiment, the colorant (D) may contain a black inorganic colorant and a non-black colorant in a weight ratio of 1-40:60-99.
[0066] According to an embodiment, the colorant (D) may contain a black inorganic colorant, a black organic colorant, and a non-black colorant in a weight ratio of 1-50:30-80:5-40.
[0067] A specific example of the black organic colorant may be at least one selected from the group consisting of aniline black, lactam black, and perylene black. Specifically, BK-7539 (Tokushiki Co., Ltd.) containing organic black may be used. In this case, low reflectance, high light shielding property, optical density, dielectric constant, etc. may be improved.
[0068] In particular, black organic colorants can lower the energy band gap. The lower the energy band gap, the lower the light reflectance. In addition, black organic colorants can absorb the entire wavelength range in the visible range, which is advantageous for minimizing reflectance.
[0069] Any black inorganic colorant and any non-black colorant known in the art may be used, for example, any compound classified as a pigment in the Color Index (published by the Society of Dye and Color Engineers) and any dye known in the art may be used.
[0070] Specific examples of black inorganic colorants include carbon black, titanium black, metal oxides such as Cu-Fe-Mn oxides, and synthetic iron black.
[0071] The black organic colorant may be used in an amount of 20-100% by weight, or 40-100% by weight, based on the total weight of the solids of the colorant (D) (i.e., the weight excluding the solvent). When the amount of the black organic colorant is within the above range, the pattern profile upon development may be favorable, and properties such as film retention may be improved. However, when the amount of the black organic colorant is less than 20% by weight, based on the total weight of the solids of the colorant (D), the optical density and low reflectance desired in the present invention may not be obtained.
[0072] In addition, the black organic colorant may be used in an amount of 3 to 40 parts by weight, or 5 to 30 parts by weight, based on 100 parts by weight of copolymer (A) based on solids excluding solvent. When the amount of the black organic colorant is within the above range, the pattern profile upon development may be advantageous, and properties such as film retention may be improved.
[0073] According to an embodiment, the black inorganic colorant may be used in an amount of 0 to 20% by weight or 0 to 10% by weight, in particular 0.01 to 20% by weight or 0.01 to 10% by weight, based on the total weight of the solid content (i.e., the weight excluding the solvent) of the colorant (D). If the amount of the black inorganic colorant is excessive, the optical density and low reflectance desired in the present invention may not be obtained.
[0074] In addition, the black inorganic colorant may be used in an amount of 0.01 to 10 parts by weight, or 0.02 to 5 parts by weight, based on 100 parts by weight of copolymer (A) based on solids excluding solvent. When the amount of the black inorganic colorant is within the above range, the pattern profile upon development may be favorable, and properties such as film retention may be improved.
[0075] Specific examples of colorants other than black may include CI Pigment Violet 13, 14, 19, 23, 25, 27, 29, 32, 33, 36, 37, and 38; and CI Pigment Blue 15 (15:3, 15:4, 15:6, etc.), 16, 21, 28, 60, 64, and 76. In particular, the colorant other than black may include at least one colorant selected from the group consisting of blue colorants and violet colorants. Among them, CI Pigment Blue 15:6 and 60, or CI Pigment Violet 23 are preferred from the viewpoint of reducing reflectance.
[0076] According to one embodiment, the blue colorant may be used in an amount of 0 to 50% by weight or 0 to 40% by weight, in particular 0.01 to 50% by weight or 0.01 to 40% by weight, based on the total weight of solids (i.e. weight excluding solvent) of colorant (D).
[0077] In addition, the violet colorant may be used in an amount of 0 to 50% by weight or 0 to 40% by weight, in particular 0.01 to 50% by weight or 0.01 to 40% by weight, based on the total weight of solids (i.e., weight excluding solvent) of colorant (D).
[0078] In addition, the blue colorant may be used in an amount of 0.01 to 10 parts by weight, or 0.01 to 8 parts by weight, based on 100 parts by weight of copolymer (A) based on solids excluding solvent.
[0079] On the other hand, the violet colorant may be used in an amount of 0.01 to 10 parts by weight, or 0.01 to 8 parts by weight, based on 100 parts by weight of copolymer (A) on a solids basis excluding the solvent.
[0080] When the amounts of the blue and violet colorants are within the above ranges, the pattern profile upon development may be favorable, properties such as film retention and optical density may be improved, and the desired total reflectance may be achieved. However, when the amounts of the blue and violet colorants exceed the above respective ranges, the optical density and low reflectance desired in the present invention may not be obtained.
[0081] The colorant (D) may be used in an amount of 1 to 40 parts by weight, or 2 to 30 parts by weight, based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent. When the amount of the colorant (D) is within the above range, the pattern profile during development may be favorable, and properties such as film retention may be improved. When the amount of the colorant (D) exceeds the above range, the optical density and low reflectance desired in the present invention may not be obtained.
[0082] The colorant (D) used in the present invention may be used in a form mixed with a dispersant, a dispersing resin (or binder), a solvent, etc., in order to disperse the colorant in the photosensitive resin composition.
[0083] Examples of dispersants may include any known dispersants for colorants. Specific examples thereof may include cationic surfactants, anionic surfactants, nonionic surfactants, zwitterionic surfactants, silicon-based surfactants, fluorosurfactants, etc. Commercially available dispersants may include Disperbyk-182, -183, -184, -185, -2000, -2150, -2155, -2163, and -2164 manufactured by BYK Co. They may be used alone or in combination of two or more thereof. The dispersant may be pre-added to the colorant by surface treatment of the colorant with the dispersant, or may be added together with the colorant during preparation of the photosensitive resin composition.
[0084] In addition, the colorant (D) may be mixed with a dispersing resin, which may then be used to prepare the photosensitive resin composition. In such a case, the dispersing resin used may be the copolymer (A), a known copolymer, or a mixture thereof.
[0085] That is, the colorant (D) may be in the form of a colored dispersion.
[0086] The color dispersion can be prepared by simultaneously mixing the colorant (D), the dispersing resin, and the dispersing agent and then milling them. Alternatively, it can be prepared by previously mixing the colorant (D) and the dispersing agent as described above, subsequently mixing them with the dispersing resin, and milling them. Here, the milling is carried out until the average diameter of the raw material of the color dispersion is 50-250 nm, 50-150 nm, or 50-110 nm. Within the above ranges, multilayered structures are not formed in the color dispersion, thereby obtaining a more uniform color dispersion.
[0087] The colored dispersion of the present invention can be used in an amount of 20 to 70% by weight, or 30 to 60% by weight, based on the total weight of the solid content of the photosensitive resin composition.
[0088] The quantum dot barrier rib structure obtained from the photosensitive resin composition containing the colorant (D) may be a multi-layer cured film containing two or more cured films and may have a total thickness of 6 μm or more. In addition, the quantum dot barrier rib structure may achieve an optical density of 0.05 / μm to 2.0 / μm. Furthermore, the reflectance R measured by the SCI (specular reflection included) method at a wavelength of 360 nm to 740 nm or 550 nm may be 0.05 / μm to 2.0 / μm. SCI may be 5.0% or less, 4.8% or less, 4.6% or less, 4.0% to 4.8%, or 4.0% to 4.6%, and the reflectance R measured by the SCE (specular reflection not included) method SCE may be 0.5% or less, 0.4% or less, 0.1% to 0.5%, 0.1% to 0.4%, or 0.2% to 0.4%. In addition, R SCI and R SCE The ratio between SCE / R SCI ) is 2 % ~10 % , 2 % ~9 % , 2 % ~8 % , 3 % ~8 % , 4 % ~8 % , or 4 % ~7.5 % Within the above range, the characteristics of low reflectance and high light blocking property can be satisfied, and light leakage of red, green, etc. can be prevented. SCI , R SCE , and R SCE / R SCI If any of the above is outside the above range, the characteristics of low reflectance and high light blocking property may not be satisfied simultaneously.
[0089] (E) Surfactant The photosensitive resin composition of the present invention may further contain a surfactant (E) in order to improve coating properties and prevent the occurrence of defects.
[0090] The type of surfactant (E) is not particularly limited, but for example, a fluorine-based surfactant or a silicon-based surfactant can be used.
[0091] Commercially available silicon-based surfactants may include DC3PA, DC7PA, SH11PA, SH21PA, and SH8400 manufactured by Dow Corning Toray Silicone Co., Ltd., TSF-4440, TSF-4300, TSF-4445, TSF-4446, TSF-4460, and TSF-4452 manufactured by GE Toshiba Silicone Co., Ltd., BYK-333, BYK-307, BYK-3560, BYK UV-3535, BYK-361N, BYK-354, and BYK-399, etc. They may be used alone or in combination of two or more thereof.
[0092] Commercially available fluorosurfactants may include Megaface F-470, F-471, F-475, F-482, F-489, and F-563 manufactured by Dainippon Ink and Chemicals, Inc. (DIC).
[0093] Among these surfactants, BYK-333 and BYK-307 manufactured by BYK and F-563 manufactured by DIC may be preferred from the viewpoint of the coating properties of the composition.
[0094] The surfactant (E) may be used in an amount of 0.01 to 5 parts by weight, 0.1 to 3 parts by weight, or 0.1 to 1 part by weight based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent. When the amount of the surfactant is within the above range, the photosensitive resin composition can be coated smoothly.
[0095] (F) Additives In addition, the photosensitive resin composition of the present invention may further contain at least one additive selected from the group consisting of an epoxy compound, a photobase generator, a thiol compound, and a compound derived from an epoxy resin, so long as it does not adversely affect the physical properties of the photosensitive resin composition.
[0096] The epoxy compound may be an unsaturated monomer containing at least one epoxy group, or a homo- or hetero-oligomer thereof. Examples of the unsaturated monomer containing at least one epoxy group include glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, 3,4-epoxybutyl (meth)acrylate, 4,5-epoxypentyl (meth)acrylate, 5,6-epoxyhexyl (meth)acrylate, 6,7-epoxyheptyl (meth)acrylate, 2,3-epoxycyclopentyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, α-ethyl glycidyl acrylate. , α-n-propyl glycidyl acrylate, α-n-butyl glycidyl acrylate, N-(4-(2,3-epoxypropoxy)-3,5-dimethylbenzyl)acrylamide, N-(4-(2,3-epoxypropoxy)-3,5-dimethylphenylpropyl)acrylamide, allyl glycidyl ether, 2-methylallyl glycidyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, or mixtures thereof. In particular, glycidyl (meth)acrylate may be used.
[0097] An example of a commercially available homo-oligomer of an unsaturated monomer containing at least one epoxy group may include MIPHOTO GHP-03HHP (glycidyl methacrylate, Miwon Commercial Co., Ltd.).
[0098] The epoxy compound may further include the following structural units:
[0099] Specific examples include styrene; styrenes containing alkyl substituents such as methylstyrene, dimethylstyrene, trimethylstyrene, ethylstyrene, diethylstyrene, triethylstyrene, propylstyrene, butylstyrene, hexylstyrene, heptylstyrene, and octylstyrene; styrenes containing halogens such as fluorostyrene, chlorostyrene, bromostyrene, and iodostyrene; styrenes containing alkoxy substituents such as methoxystyrene, ethoxystyrene, and propoxystyrene; p-hydroxy-α-methylstyrene, acetylstyrene; ethylenically unsaturated compounds containing aromatic rings such as divinylbenzene, vinylphenol, o-vinylbenzyl methyl ether, m-vinylbenzyl methyl ether, and p-vinylbenzyl methyl ether;Methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, cyclohexyl (meth)acrylate, ethylhexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-chloropropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate , glycerol (meth)acrylate, methyl α-hydroxymethyl acrylate, ethyl α-hydroxymethyl acrylate, propyl α-hydroxymethyl acrylate, butyl α-hydroxymethyl acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxytripropylene glycol (meth)acrylate, poly(ethylene glycol) methyl ether (meth)acrylate Acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, p-nonylphenoxypolyethylene glycol (meth)acrylate, p-nonylphenoxypolypropylene glycol (meth)acrylate, tetrafluoropropyl (meth)acrylate, 1,1,1,3,3,3-hexafluoroisopropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate unsaturated carboxylic acid esters such as N-vinyl ether, tribromophenyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate; tertiary amines containing an N-vinyl group such as N-vinylpyrrolidone, N-vinylcarbazole, and N-vinylmorpholine; unsaturated ethers such as vinyl methyl ether and vinyl ethyl ether;Examples of structural units derived from unsaturated imides such as N-phenylmaleimide, N-(4-chlorophenyl)maleimide, N-(4-hydroxyphenyl)maleimide, and N-cyclohexylmaleimide are given below. The structural units derived from the compounds exemplified above may be contained in the epoxy compound alone or in combination of two or more thereof.
[0100] The epoxy compound may have a weight average molecular weight of 100 to 30,000 Da. In particular, the epoxy compound may have a weight average molecular weight of 100 to 10,000 Da. When the weight average molecular weight of the epoxy compound is 100 Da or more, the hardness of the cured film may be better. When it is 30,000 Da or less, the thickness of the cured film becomes uniform with smaller step difference, which is more suitable for planarization.
[0101] The epoxy compound may be used in an amount of 0 to 3 parts by weight, 0.01 to 3 parts by weight, or 0.1 to 1 part by weight based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent. Within the above ranges, the pattern profile during development may be advantageous, and chemical resistance and planarization may be enhanced.
[0102] In addition, the photobase generator may include a compound that has the property of generating a base upon irradiation with light (or an activating energy beam). For example, it may include a highly sensitive compound that has a photosensitive range even at wavelengths of 300 nm or more.
[0103] Photobase generator can include crosslinking compound that includes polyamine photobase generator component.Since the present invention includes such photobase generator, when cured film is prepared, it can be cured at low temperature and / or in a short period of time and form fine pattern.In addition, since photobase generator generates base when irradiated with light (e.g. UV), it is not inhibited by oxygen in air, and therefore it is useful for preventing corrosion or deterioration of cured film.
[0104] When the photobase generator is exposed to light, the pendant photobase groups of the polyamine photobase generator component are fragmented or photolyzed to provide amine groups that can react with amine reactive groups of the multifunctional amine reactive component to crosslink the (meth)acrylate copolymer component.
[0105] According to an embodiment, applicable photobase generators include WPBG-018 (Wako, CAS No. 122831-05-7, 9-anthrylmethyl-N,N-diethylcarbamate), WPBG-027 (CAS No. 1203424-93-4, (E)-1-piperidino-3-(2-hydroxyphenyl)-2-propen-1-one), WPBG-266 (CAS No. 1632211-89-2, 1,2-diisopropyl-3-bis(dimethylamino)methylene)guanidinium 2-(3-benzoylphenyl)propionate), WPBG-300 (CAS No. 1801263-71-7, 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidinium n-butyltriphenylborate), and the like. The photobase generators may be used alone or in combination of two or more thereof.
[0106] The photobase generator may be used in an amount of 0 to 10 parts by weight, particularly 0 to 6 parts by weight, more particularly 0.01 to 5 parts by weight, based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent. Within the above range, the pattern profile during development may be advantageous, and the chemical resistance may be excellent.
[0107] The thiol compound can be used as an additive for free radical or catalytic function. It can increase the photocuring conversion rate by UV irradiation or thermal reaction, and it can increase the epoxy conversion rate by lowering the reaction energy by thermal reaction. The thiol compound prevents the disappearance of radicals by oxygen. It also increases the crosslinking degree by crosslinking action with the photopolymerizable compound (B), thereby producing the effect of making the structure denser by improving the crosslinking degree even at low temperature.
[0108] Examples of thiol compounds include compounds having two or more mercapto groups in the molecule, which may be, for example, an aliphatic thiol compound or an aromatic thiol compound.
[0109] Examples of aliphatic thiol compounds include methanedithiol, 1,2-ethanedithiol, 1,2-propanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,2-cyclohexanedithiol, 3,4-dimethoxybutane-1,2-dithiol, 2-methylcyclohexane-2,3-dithiol, 1,2-dimercaptopropyl methyl ether, 2,3-dimercaptopropyl methyl ether, bis(2-methylphenyl)-1,2-dithiol, 1,2-dimethylphenyl ether ... 1,2-bis(mercaptomethylthio)ethane, 1,2-bis(2-mercaptoethylthio)ethane, 1,3-bis(mercaptomethylthio)propane, 1,3-bis(2-mercaptoethylthio)propane, 1,3-bis(2-mercaptoethylthio)propane, 1,3-bis(2-mercaptoethylthio)methane, 1,2-bis(mercaptomethylthio)ethane, 1,2-bis(2-mercaptoethylthio)ethane, 1,3-bis(mercaptomethylthio)propane, 1,3-bis(2-mercaptoethylthio)methane, 1,2-bis(mercaptomethylthio)ethane, 1,3-bis(2-mercaptoethyl ...2-bis(2-mercaptoethylthio)ethane, 1,3- mercaptoethylthio)propane, 1,2,3-tris(mercaptomethylthio)propane, 1,2,3-tris(2-mercaptoethylthio)propane, 1,2,3-tris(3-mercaptopropylthio)propane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-di Mercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, 4,6-bis(mercaptomethylthio)-1,3-dithiane, 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithietane, tetrakis(mercaptomethylthiomethyl)methane, tetrakis(2-mercaptoethylthiomethyl)methane, bis(2,3-dimercaptopropyl)sulfide, 2,5-bismercaptomethyl-1,4-Dithiane, ethylene glycol bis(2-mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), diethylene glycol bis(2-mercaptoacetate), diethylene glycol bis(3-mercaptopropionate), 2,3-dimercapto-1-propanol(3-mercaptopropionate), 3-mercapto-1,2-propanediol bis(2-mercaptoacetate), 3-mercapto-1,2-propanediol di(3-mercaptopropionate), trimethylolpropane tris(2-mercaptoacetate), di-trimethylolpropane tetrakis(2-mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), di-trimethylolpropane tetrakis(3-mercaptopropionate), trimethylolethane tris(2-mercaptoacetate), trimethylolethane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), dipentaerythritol hexa(2-mercaptoacetate), pentaerythritol di(3-mercaptopropionate) , pentaerythritol tris(3-mercaptopropionate), pentaerythritol tetra(3-mercaptopropionate) (PETMP), dipentaerythritol hexa(3-mercaptopropionate), glycerin di(2-mercaptoacetate), glycerin tris(2-mercaptoacetate), glycerin di(3-mercaptopropionate), glycerin tris(3-mercaptopropionate), 1,4-cyclohexanediol bis(2-mercaptoacetate), 1,4-cyclohexanediol bis(3-mercaptopropionate) N,N',propionate), hydroxymethyl sulfide bis(2-mercaptoacetate), hydroxymethyl sulfide bis(3-mercaptopropionate), hydroxyethyl sulfide (2-mercaptoacetate), hydroxyethyl sulfide (3-mercaptopropionate), hydroxymethyl disulfide (2-mercaptoacetate), hydroxymethyl disulfide (3-mercaptopropionate), thioglycolic acid bis(2-mercaptoethyl ester), thiodipropionic acid bis(2-mercaptoethyl ester), and N,N',N''-tris(β-mercaptopropylcarbonyloxyethyl)isocyanurate may be mentioned.
[0110] Examples of aromatic thiol compounds include 1,2-dimercaptobenzene, 1,3-dimercaptobenzene, 1,4-dimercaptobenzene, 1,2-bis(mercaptomethyl)benzene, 1,4-bis(mercaptomethyl)benzene, 1,2-bis(mercaptoethyl)benzene, 1,4-bis(mercaptoethyl)benzene, 1,2,3-trimercaptobenzene, 1,2,4-trimercaptobenzene, 1,3,5-trimercaptobenzene, 1,2,3-tris(mercaptomethyl)benzene, 1,2,4-tris(mercaptomethyl)benzene, 1,3,5-tris(mercaptomethyl)benzene, 1,2,3-tris(mercaptoethyl)benzene, 1,3,5-tris(mercaptoethyl)benzene, 1,2,4-tris(mercaptoethyl)benzene, 2,5-toluenediamine, 1,2,4 ... Thiols that may be mentioned include 3,4-toluenedithiol, 1,4-naphthalenedithiol, 1,5-naphthalenedithiol, 2,6-naphthalenedithiol, 2,7-naphthalenedithiol, 1,2,3,4-tetramercaptobenzene, 1,2,3,5-tetramercaptobenzene, 1,2,4,5-tetramercaptobenzene, 1,2,3,4-tetrakis(mercaptomethyl)benzene, 1,2,3,5-tetrakis(mercaptomethyl)benzene, 1,2,4,5-tetrakis(mercaptomethyl)benzene, 1,2,3,4-tetrakis(mercaptoethyl)benzene, 1,2,3,5-tetrakis(mercaptoethyl)benzene, 1,2,4,5-tetrakis(mercaptoethyl)benzene, 2,2'-dimercaptobiphenyl, and 4,4'-dimercaptobiphenyl.
[0111] The thiol-based compound may be an aliphatic thiol compound. Specifically, it may include pentaerythritol tetra(3-mercaptopropionate) (PETMP), SIRIUS-501 (SUBARU-501, Osaka Organic Chemical Industry Co., Ltd.), and glycoluril derivatives (TS-G, Shikoku Chemical Industry Co., Ltd.).
[0112] The thiol compound may be used in an amount ranging from 0 to 10 parts by weight, 0 to 6 parts by weight, or 0.01 to 5 parts by weight based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent. When the amount of the thiol compound is within the above range, the pattern profile during development may be advantageous and the chemical resistance may be excellent.
[0113] The photosensitive resin composition of the present invention may further comprise a compound derived from an epoxy resin, which has at least one double bond and may have a cardo main chain structure, may be a novolac resin, or may be an acrylic resin containing a double bond in its side chain.
[0114] The weight average molecular weight (Mw) of the compound derived from the epoxy resin, as measured by gel permeation chromatography using polystyrene as a standard, may be in the range of 3,000 to 18,000 Da, or 5,000 to 10,000 D. When the molecular weight of the compound derived from the epoxy resin is within the above range, the pattern profile during development may be advantageous, and properties such as chemical resistance and elastic recovery may be improved.
[0115] Specifically, the compound derived from the epoxy resin has the following formula 1: [Formula 1] [ka] The compound may have a cardo backbone structure such as represented by:
[0116] In the above formula 1, Each X is independently [ka] and each L1 is independently C 1~10 Alkylene group, C 3~20 Cycloalkylene group, or C 1~10an alkyleneoxy group; R1 to R7 each independently represent H, C 1~10 Alkyl group, C 1~10 Alkoxy group, C 2~10 Alkenyl group, or C 6~14 is an aryl group; R8 is H, methyl, ethyl, CH3CHCl-, CH3CHOH-, CH2=CHCH2-, or phenyl; and n is an integer from 0 to 10.
[0117] C 1~10 Specific examples of alkylene groups may include methylene, ethylene, propylene, isopropylene, butylene, isobutylene, sec-butylene, t-butylene, pentylene, isopentylene, t-pentylene, hexylene, heptylene, octylene, isooctylene, t-octylene, 2-ethylhexylene, nonylene, isononylene, decylene, isodecylene, and the like. 3~20 Specific examples of cycloalkylene groups can include cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, cycloheptylene, decalinylene, adamantylene, and the like. 1~10 Specific examples of alkyleneoxy groups may include methyleneoxy, ethyleneoxy, propyleneoxy, butyleneoxy, sec-butyleneoxy, t-butyleneoxy, pentyleneoxy, hexyleneoxy, heptyleneoxy, octyleneoxy, 2-ethyl-hexyleneoxy, and the like. 1~10 Specific examples of alkyl groups may include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, t-butyl, pentyl, isopentyl, t-pentyl, hexyl, heptyl, octyl, isooctyl, t-octyl, 2-ethylhexyl, nonyl, isononyl, decyl, isodecyl, and the like. 1~10 Specific examples of alkoxy groups can include methoxy, ethoxy, propoxy, butyloxy, sec-butoxy, t-butoxy, pentoxy, hexyloxy, heptoxy, octyloxy, 2-ethyl-hexyloxy, and the like. 2~10 Specific examples of alkenyl groups may include vinyl, allyl, butenyl, propenyl, and the like. 6~14Particular examples of aryl groups can include phenyl, tolyl, xylyl, naphthyl, and the like.
[0118] As an example, a compound derived from an epoxy resin having a cardo backbone structure can be prepared by the following synthetic route as represented by Reaction Scheme 1. [Reaction Scheme 1] [ka]
[0119] In the above Reaction Scheme 1, Hal is a halogen; X, R1, R2, and L1 are the same as defined in formula 1 above.
[0120] Compounds derived from epoxy resins having a cardo backbone structure can be obtained by reacting an epoxy resin having a cardo backbone structure with an unsaturated basic acid to produce an epoxy adduct, and then reacting the epoxy adduct thus obtained with a polybasic acid anhydride, or by further reacting the product thus obtained with a monofunctional or polyfunctional epoxy compound. Any unsaturated basic acid known in the art can be used, such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, sorbic acid, etc. Any polybasic acid anhydride known in the art can be used, such as succinic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, hexahydrophthalic anhydride, etc. Any mono- or polyfunctional epoxy compound known in the art may be used, such as glycidyl methacrylate, methyl glycidyl ether, ethyl glycidyl ether, propyl glycidyl ether, isopropyl glycidyl ether, butyl glycidyl ether, isobutyl glycidyl ether, bisphenol Z glycidyl ether, and the like.
[0121] As an example, a compound derived from an epoxy resin having a cardo backbone structure can be prepared by the following synthetic route as represented by Reaction Scheme 2. [Reaction Scheme 2] [ka]
[0122] In the above Reaction Scheme 2, R9 is independently H, C 1~10 Alkyl group, C 1~10 Alkoxy group, C 2~10 Alkenyl group, or C 6~14 is an aryl group; R 10 and R 11 are each independently a saturated or unsaturated C6 aliphatic or aromatic ring; n is an integer from 1 to 10; and X, R1, R2, and L1 are the same as defined in formula 1 above.
[0123] When a compound derived from an epoxy resin having a cardo backbone structure is used, the cardo backbone structure can improve the adhesion of the cured material to the substrate, alkali resistance, processability, strength, etc. Furthermore, images with fine resolution can be formed in the pattern once the uncured parts are removed during development.
[0124] The compound derived from an epoxy resin may be used in an amount of 0 to 50 parts by weight, particularly 0 to 40 parts by weight, more particularly 0.01 to 50 parts by weight, 0.01 to 40 parts by weight, or 0.01 to 30 parts by weight, based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent. When the compound derived from an epoxy resin is used within the above amount range, the developability and pattern profile during development may be advantageous.
[0125] (G) Solvent The photosensitive resin composition of the present invention can be prepared as a liquid composition in which the above-mentioned components are mixed with a solvent. Any solvent known in the art that is compatible but non-reactive with the components in the photosensitive resin composition can be used as the solvent (G) in the preparation of the photosensitive resin composition.
[0126] Examples of the solvent (G) include glycol ethers such as ethylene glycol monoethyl ether; ethylene glycol alkyl ether acetates such as ethyl cellosolve acetate; esters such as ethyl 2-hydroxypropionate; diethylene glycols such as diethylene glycol monomethyl ether; propylene glycol alkyl ether acetates such as propylene glycol monomethyl ether acetate and propylene glycol propyl ether acetate; and alkoxy alkyl acetates such as 3-methoxybutyl acetate. The solvent (G) may be used alone or in combination of two or more.
[0127] The amount of the solvent (G) is not particularly limited, but may be 50 to 200 parts by weight, or 80 to 150 parts by weight, based on 100 parts by weight of the copolymer (A) based on the solid content excluding the solvent, from the viewpoint of the coating property and stability of the finally obtained photosensitive resin composition. When the amount of the solvent is within the above range, the resin composition is smoothly coated, and the delay margin that may occur in the work process is small.
[0128] In addition, the photosensitive resin composition of the present invention may further contain other additives such as antioxidants and stabilizers, so long as they do not adversely affect the physical properties of the photosensitive resin composition.
[0129] The photosensitive resin composition containing the above components can be prepared as a liquid composition by a conventional method. For example, the colorant is mixed with the dispersion resin, dispersant, and solvent in advance, and dispersed therein by using a bead mill until the average particle diameter of the colorant reaches a desired value, thereby preparing a colored dispersion. In such a case, the surfactant and / or copolymer can be partially or completely blended. The remainder of the copolymer and surfactant, the photopolymerizable compound, and the photopolymerization initiator are added to the dispersion. If necessary, additives such as epoxy compounds or additional solvents are further blended to a certain concentration, and then they are thoroughly stirred to prepare a liquid photosensitive resin composition.
[0130] The present invention can provide a quantum dot barrier rib structure in the form of a cured film by coating such a photosensitive resin composition on a substrate and curing it. The quantum dot barrier rib structure can include a multilayer cured film of two or more layers.
[0131] Specifically, the present invention provides a quantum dot barrier rib structure comprising a first cured film formed from a first photosensitive resin composition and a second cured film formed from a second photosensitive resin composition on the first cured film, the first photosensitive resin composition, the second photosensitive resin composition, or both, comprise: (A) a copolymer; (B) a photopolymerizable compound; (C) a photopolymerization initiator; and (D) a colorant, the colorant comprising a black colorant, and the structure has a total thickness of 6 μm or greater. The structure may be provided.
[0132] The first photosensitive resin composition and the second photosensitive resin composition may be the same or different.
[0133] In addition, according to some embodiments, the first photosensitive resin composition and the second photosensitive resin composition may or may not contain fluorine.
[0134] For example, the first photosensitive resin composition may not contain fluorine, and the second photosensitive resin composition may contain fluorine.
[0135] In addition, neither the first photosensitive resin composition nor the second photosensitive resin composition may contain fluorine.
[0136] When the first photosensitive resin composition or the second photosensitive resin composition contains fluorine, the structural unit (a-4) may contain a fluorine-containing compound when the copolymer (A) used in the photosensitive resin composition is prepared.For example, the structural unit (a-4) may contain at least one selected from the group consisting of trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, pentafluorobenzyl (meth)acrylate, hexafluoroisopropyl (meth)acrylate, heptadecafluoro-1-nonyl (meth)acrylate, octafluoropentyl (meth)acrylate, 4-trifluoromethyl-4-hydroxy-5,5,5-trifluoro-2-pentyl (meth)acrylate, and trimethoxysilylpropyl methacrylate.
[0137] On the other hand, the quantum dot barrier rib structure according to an embodiment can be a multi-layered cured film consisting of two layers including a first cured film and a second cured film.
[0138] Specifically, the multi-layer cured film may be a two-layer cured film including a first cured film formed by coating a first photosensitive resin composition on a substrate and curing it; and a second cured film formed by coating a second photosensitive resin composition on the first cured film and curing it.
[0139] In the multilayer cured film consisting of two layers, the first cured film and the second cured film each may have a thickness of 10 μm or less, particularly 4 μm to 9 μm, more particularly 5 μm to 9 μm. In addition, the multilayer cured film consisting of two layers may have a total thickness, i.e., the total thickness of the first cured film and the second cured film, of 6 μm to 20 μm, particularly 6 μm to 18 μm, more particularly 10 μm to 18 μm.
[0140] According to another embodiment, the quantum dot barrier rib structure can be a multi-layer cured film consisting of three layers including a first cured film, a second cured film, and a third cured film.
[0141] In the three-layer multilayer cured film, the first cured film, the second cured film, and the third cured film may each have a thickness of 8 μm or less, particularly 2 μm to 8 μm, and more particularly 3 μm to 8 μm. In addition, the three-layer multilayer cured film may have a total thickness, i.e., the total thickness of the first cured film, the second cured film, and the third cured film, of 6 μm to 24 μm, particularly 9 μm to 24 μm, and more particularly 12 μm to 24 μm.
[0142] According to another embodiment, the quantum dot barrier rib structure includes a first cured film, a second cured film, and a n 番目の The cured film may be a multilayer cured film consisting of n layers including the cured film, where n is 4 or more, and in particular 4 to 10, 4 to 8, 4 to 6, or 4 to 5.
[0143] In a multi-layer cured film consisting of n layers, a first cured film, a second cured film, and a n 番目の The cured films may each have a thickness of 8 μm or less, particularly 1.5 μm to 8 μm, more particularly 2 μm to 8 μm. In addition, a multilayer cured film consisting of n layers may have a total thickness of 6 μm to 80 μm, particularly 6 μm to 40 μm, more particularly 6 μm to 30 μm.
[0144] The quantum dot barrier rib structure according to some embodiments has a large total film thickness as described above, so that it can achieve excellent optical density (i.e., high light blocking) and low reflectance even when the amount of colorant is less than that in the prior art.
[0145] In the quantum dot barrier rib structure, the thickness and optical density of each cured film of the multi-layered cured film may be the same or different. For example, the thickness of the first cured film may be the same or different from the thickness of the second cured film. In addition, the optical density of the first cured film may be the same or different from the optical density of the second cured film.
[0146] The cured film is measured for height difference due to vertical movement of the instrument probe tip using an Alpha-Step instrument (SCAN PLUS). The thickness of the cured film is obtained from these results. The thickness of the multilayer cured film is the initial film thickness. It means the thickness of the multilayer cured film as formed, i.e., the thickness of the film prepared during pre-baking before exposure and development in the preparation of the quantum dot barrier ribs.
[0147] When a single-layer cured film is obtained from the photosensitive resin composition, there is a problem that the cured film is only performed as a thin film. In addition, when a single-layer cured film is used for a quantum dot barrier rib, its thickness is thin. Therefore, when the quantum dot solution is dripped, it may overflow the barrier rib. If it overflows the barrier rib, staining due to color mixing may occur or reliability may be reduced. In addition, when the composition is coated thickly in a single layer and then cured, it is difficult to achieve a uniformly cured film, and staining may occur due to thickness fluctuation, or the quantum dot solution is likely to overthrow the barrier rib with a thin thickness. There is a limitation in being used for a quantum dot barrier rib.
[0148] However, the multi-layered cured film (or quantum dot barrier rib structure) according to one embodiment has a minimum film thickness of 6 μm. In addition, since a colorant is applied, when the quantum dots emit various colors of light, there is an advantage of light shielding by the barrier ribs. In addition, it is possible to form a multi-layered pattern with a uniform film thickness by adjusting the number and thickness of layers of each cured film. The fluorine-containing cured film is the final n-th layer. 番目の When applied in layers, it is possible to prevent drainage of the quantum dot solution by overflowing into adjacent areas when the quantum dot solution is applied by inkjet method.
[0149] The present invention can prepare a quantum dot barrier rib structure in the form of a multi-layer cured film by the following method: When the quantum dot barrier rib structure is formed, a multi-layer pattern with a uniform film thickness suitable for the quantum dot barrier rib can be formed in a single development process.
[0150] Specifically, the method for preparing the quantum dot barrier rib structure includes the steps of: (S1) coating a first photosensitive resin composition on a substrate and curing the first photosensitive resin composition to form a first cured film; (S2) coating a second photosensitive resin composition on the first cured film and curing the second photosensitive resin composition to form a second cured film; and (S3) exposing and developing a multi-layered cured film including the first cured film and the second cured film to form a pattern, and then curing the multi-layered cured film. Here, the first photosensitive resin composition, the second photosensitive resin composition, or both may contain (A) a copolymer; (B) a photopolymerizable compound; (C) a photopolymerization initiator; and (D) a colorant, including a black colorant.
[0151] More specifically, a method for preparing a quantum dot barrier rib structure according to an embodiment may include a step (S1) of coating a first photosensitive resin composition onto a substrate and curing it to form a first cured film.
[0152] In the step of forming a first cured film, the photosensitive resin composition according to the present invention is coated on a pretreated substrate by a spin coating method, a slit coating method, a roll coating method, a screen printing method, an applicator method, etc., to a desired thickness, for example, 4 μm to 8 μm, which is cured by removing the solvent therefrom to form a first cured film.
[0153] Glass substrate, ITO deposition substrate, SiN x Deposition substrate and SiON x Various inorganic substrates such as deposition substrates can be used as the substrate. Any material can be used for the substrate as long as it can be used to form the structure of the quantum dot barrier rib.
[0154] Curing to form the first cured film may be carried out for 100 to 800 seconds at 70° C. to 140° C. Curing may be carried out in one step or in two or more steps.
[0155] If curing is carried out in one step, it may be carried out at 70°C to 140°C for 100 seconds to 800 seconds, particularly at 80°C to 130°C for 150 seconds to 600 seconds, and particularly at 90°C to 130°C for 150 seconds to 500 seconds.
[0156] When curing is carried out in two or more steps, it may be carried out, for example, as a pre-bake at 70°C to 100°C for 50 seconds to 400 seconds, particularly at 70°C to 90°C for 100 seconds to 300 seconds, and then as a mid-bake at 80°C to 140°C for 100 seconds to 500 seconds, particularly at 90°C to 130°C for 100 seconds to 300 seconds.
[0157] A method for preparing a quantum dot barrier rib structure according to an embodiment may include a step (S2) of coating a second photosensitive resin composition onto the first cured film and curing it to form a second cured film.
[0158] In the step of forming a second cured film, a second photosensitive resin composition is coated onto the first cured film obtained in the above step S1 in a desired thickness, for example, 4 μm to 8 μm, which is cured by removing the solvent therefrom to form a second cured film.
[0159] Curing to form the second cured film may be carried out for 100 to 800 seconds at 70° C. to 140° C. Curing may be carried out in one step or in two or more steps.
[0160] Specifically, when curing is carried out in one step, it may be carried out at 70°C to 140°C for 100 seconds to 800 seconds, particularly at 80°C to 130°C for 150 seconds to 600 seconds, and more particularly at 90°C to 130°C for 150 seconds to 500 seconds.
[0161] When curing is carried out, for example, in two or more steps, it may be carried out as a pre-bake at 70°C to 100°C for 50 to 400 seconds, particularly at 70°C to 90°C for 100 to 300 seconds, and then as a mid-bake at 80°C to 140°C for 100 to 500 seconds, particularly at 90°C to 130°C for 100 to 300 seconds.
[0162] The curing conditions for the first and second cured films may be the same or different.
[0163] In the method for preparing the structure of quantum dot barrier ribs according to an embodiment, a multi-layer cured film consisting of two layers is exposed and developed. When a cured film having three or more layers is prepared, a cured film having one or more layers can be further formed on the second cured film, followed by exposure and development thereof. In such a case, the photosensitive resin composition used to prepare one or more cured films formed on the second cured film can be the same or different from the photosensitive resin composition used to prepare the first cured film and the second cured film. In addition, the optical density of each cured film can vary with the components and contents of the photosensitive resin composition used to prepare the first cured film and the second cured film.
[0164] A method for preparing a quantum dot barrier rib structure according to an embodiment may include exposing and developing a multi-layer cured film including a first cured film and a second cured film to form a pattern, and then curing it (S3).
[0165] In step S3, in order to form a pattern on the multilayer cured film thus obtained, a mask having a predetermined shape is placed thereon, which is then irradiated with actinic rays of 200 to 500 nm. As the light source used for irradiation, a low pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, an argon gas laser, etc. may be used. If necessary, X-rays, electron beams, etc. may also be used. The exposure dose of light for exposure may vary depending on the type and composition ratio of the components of the composition and the thickness of the dried coating. When a high pressure mercury lamp is used, the exposure dose is 500 mJ / cm. 2 or less (at a wavelength of 365 nm).
[0166] After the exposure step, the unnecessary parts are dissolved and removed using an aqueous alkaline solution such as sodium carbonate, sodium hydroxide, potassium hydroxide, tetramethylammonium hydroxide, etc. as a developer, so that only the exposed parts remain to form a pattern. The image pattern obtained by development is cooled to room temperature and post-baked in a hot air circulation type drying oven, thereby obtaining the final pattern.
[0167] The exposure can be carried out by arranging a mask so that the intervals between each pattern are 10 μm to 30 μm, and irradiating it with actinic rays.
[0168] The development may be carried out for 50 seconds to 300 seconds, particularly 100 seconds to 300 seconds.
[0169] Curing during pattern formation, ie, post-baking, is carried out at 150° C. to 300° C. for 10 to 60 minutes, particularly at 180° C. to 280° C. for 20 to 50 minutes, and more particularly at 200° C. to 260° C. for 20 to 40 minutes.
[0170] The method for preparing quantum dot barrier ribs according to certain embodiments allows for the formation of multi-layer patterns with uniform film thickness suitable for quantum dot barrier ribs in a single development process.
[0171] The present invention provides a quantum dot barrier rib structure prepared by the quantum dot barrier rib preparation method according to the above embodiment.
[0172] In the structure of the quantum dot barrier rib according to an embodiment, the pattern is formed at regular intervals as shown in Figures 2 to 4. It can be a multi-layer structure having two or more layers.
[0173] As shown in FIG. 2, the quantum dot barrier rib structure (200) according to one embodiment may be a multi-layer structure (200) of quantum dot barrier ribs consisting of two layers including a first cured film (211) and a second cured film (212) formed on a substrate (210).
[0174] Specifically, the quantum dot barrier rib structure (200) can be a two-layer structure (200) of quantum dot barrier ribs prepared by exposing and developing a two-layer cured film to form a pattern and then post-baking it, where the two-layer cured film includes a first cured film (211) formed by coating a first photosensitive resin composition on a substrate (210) and curing it; and a second cured film (212) formed by coating a second photosensitive resin composition on the first cured film (211) and curing it.
[0175] According to another embodiment, the quantum dot barrier rib structure (300) may be a multi-layer structure (300) of quantum dot barrier ribs consisting of three layers including a first cured film (311), a second cured film (312), and a third cured film (313), as illustrated in FIG.
[0176] Specifically, the quantum dot barrier rib structure (300) can be a three-layer structure (300) of quantum dot barrier ribs prepared by exposing and developing a three-layer cured film to form a pattern and then post-baking it, where the three-layer cured film includes a first cured film (311) formed by coating a first photosensitive resin composition on a substrate (310) and curing it; a second cured film (312) formed by coating a second photosensitive resin composition on the first cured film (311) and curing it; and a third cured film (313) formed by coating a third photosensitive resin composition on the second cured film (312) and curing it.
[0177] Another embodiment of the quantum dot barrier rib structure (400) includes a first cured film (411), a second cured film (412), a third cured film (413), and an n-th cured film (414), as illustrated in FIG. 番目の It may be a multi-layer structure (400) of quantum dot barrier ribs consisting of n layers including a cured film (nn).
[0178] Specifically, the quantum dot barrier rib structure (400) can be an n-layer structure of quantum dot barrier ribs (400) prepared by exposing and developing an n-layer cured film to form a pattern and then post-baking it, where the n-layer cured film includes a first cured film (411) formed by coating a first photosensitive resin composition on a substrate (410) and curing it; a second cured film (412) formed by coating a second photosensitive resin composition on the first cured film (411) and curing it; a third cured film (413) formed by coating a third photosensitive resin composition on the second cured film (412) and curing it; and 番目の The nth cured film (413) is formed by coating a photosensitive resin composition on the third cured film (413) and curing it. 番目の Cured films (nn) where n can be 4 or more, particularly 4-10, 4-8, 4-6, or 4-5.
[0179] In the quantum dot barrier rib structure, the thickness and optical density of each cured film may be the same or different.
[0180] The quantum dot barrier rib structure may have an optical density of 0.05 / μm to 2.0 / μm, 0.05 / μm to 1.5 / μm, 0.05 / μm to 1.0 / μm, 0.05 / μm to 0.5 / μm, or 0.1 / μm to 0.2 / μm. Here, the transmittance at 550 nm may be measured using an optical density meter (361T manufactured by Xlite) to obtain an optical density (OD, unit: / μm) based on a thickness of 1 μm. From this, the quantum dot barrier rib structure may have a total optical density of 0.5 to 10.0, 1.0 to 6.0, or 1.0 to 4.0. The total optical density is a value obtained by multiplying the unit optical density by the total thickness of the quantum dot barrier rib structure.
[0181] When the optical density and total optical density are in the above ranges, the resolution of the display screen can be further increased.
[0182] The cured film of the quantum dot barrier rib structure is measured for height difference by vertical movement of the instrument probe tip using SCAN PLUS, an Alpha-Step instrument (Alpha-Step Profilometer). The thickness of the cured film is obtained from these results. The final film thickness is obtained by measuring the final film of the quantum dot barrier rib structure prepared by forming a pattern by exposure and development, and then post-baking it. It includes the entire multi-layer cured film, and the final film thickness can be 6 μm to 20 μm.
[0183] In addition, in the structure of the quantum dot barrier rib, the reflectance R measured by the SCI (including specular reflection) method at a wavelength of 360 nm to 740 nm or 550 nm is SCI and reflectance R measured by the SCE (specular reflection not included) method SCE are related as follows: (Relationship 1) R SCI≦5.0% (Relationship 2) R SCE ≦0.5% (Relationship 3)2 % ≦R SCE / R SCI <= 10 % can be satisfied.
[0184] Specifically, R SCI R may be 5.0% or less, 4.8% or less, 4.6% or less, 4.0% to 4.8%, or 4.0% to 4.6%. SCE can be 0.5% or less, 0.4% or less, 0.1% to 0.5%, 0.1% to 0.4%, or 0.2% to 0.4%. The ratio therebetween (i.e. SCE / R SCI ) is 2 % ~10 % , 2 % ~9 % , 2 % ~8 % , 3 % ~8 % , 4 % ~8 % , or 4 % ~7.5 % In this way, the characteristics of low reflectance and high light blocking can be satisfied, and light leakage of red, green, etc. can be prevented.
[0185] Since the quantum dot barrier rib structure thus prepared has excellent properties, it can be advantageously used for quantum dot displays. EXAMPLES
[0186] The present invention will now be described in more detail with reference to the following examples, which are provided to illustrate the present invention and are not intended to limit the scope of the present invention thereto.
[0187] In the following synthesis examples, weight average molecular weights are determined by gel permeation chromatography (GPC, eluent: tetrahydrofuran) relative to polystyrene standards.
[0188] Synthesis Example 1: Preparation of Copolymer (A-1) A 500 ml round-bottom flask equipped with a reflux condenser and stirrer was charged with 100 g of a mixture consisting of 50 mol% N-phenylmaleimide (PMI), 6 mol% styrene (Sty), 10 mol% 4-hydroxybutyl acrylate glycidyl ether (4-HBAGE), and 34 mol% (meth)acrylic acid (MAA), together with 300 g of propylene glycol monomethyl ether acetate (PGMEA) as a solvent and 2 g of 2,2'-azobis(2,4-dimethylvaleronitrile) as a radical polymerization initiator. The mixture was then heated to 70°C and stirred for 5 hours to obtain a copolymer (A-1) solution having a solid content of 31 wt%. The copolymer thus prepared had an acid value of 100 mg KOH / g and a weight average molecular weight (Mw) based on polystyrene standards of 7,000 Da measured by gel permeation chromatography.
[0189] Synthesis Example 2: Preparation of Copolymer (A-2) 30g of a monomer mixture consisting of 30mol% methyl (meth)acrylate, 20mol% (meth)acrylic acid, 30mol% hexafluoroisopropyl (meth)acrylate, and 20mol% butyl (meth)acrylate, and a mixture of 2.74g of V-59 as a radical polymerization initiator dissolved in 30g of propylene glycol methyl ether acetate (PGMEA) as a solvent, were added dropwise over 4 hours to the solvent heated to 80°C in a nitrogen atmosphere in a 250ml round-bottom flask equipped with a reflux condenser and a stirrer. It was then polymerized for 20 hours to obtain copolymer (A-2). The copolymer thus prepared had an acid value of 85mg KOH / g, a weight average molecular weight (Mw) of 9,053 Da based on polystyrene, a solid content of 30.5wt%, and a polydispersity (Mw / Mn) of 2.3, as measured by gel permeation chromatography.
[0190] Synthesis Example 3: Preparation of copolymer (A-3) 30g of a monomer mixture consisting of 30mol% methyl (meth)acrylate, 20mol% (meth)acrylic acid, 30mol% octafluoropentyl (meth)acrylate, and 20mol% butyl (meth)acrylate, and a mixture of 2.74g of V-59 as a radical polymerization initiator dissolved in 30g of propylene glycol methyl ether acetate (PGMEA) as a solvent, were added dropwise over 4 hours to the solvent heated to 80°C in a nitrogen atmosphere in a 250ml round-bottom flask equipped with a reflux condenser and a stirrer. It was then polymerized for 20 hours to obtain copolymer (A-3). The copolymer thus prepared had an acid value of 66mg KOH / g, a weight average molecular weight (Mw) of 14,968Da based on polystyrene, a solid content of 31.2wt%, and a polydispersity (Mw / Mn) of 2.3, as measured by gel permeation chromatography.
[0191] Synthesis Example 4: Preparation of copolymer (A-4) 30g of a monomer mixture consisting of 30mol% methyl (meth)acrylate, 20mol% (meth)acrylic acid, 30mol% trifluoroethyl (meth)acrylate, and 20mol% butyl (meth)acrylate, and a mixture of 2.74g of V-59 as a radical polymerization initiator dissolved in 30g of propylene glycol methyl ether acetate (PGMEA) as a solvent, were added dropwise over 4 hours to the solvent heated to 80°C in a nitrogen atmosphere in a 250ml round-bottom flask equipped with a reflux condenser and a stirrer. It was then polymerized for 20 hours to obtain copolymer (A-4). The copolymer thus prepared had an acid value of 98mg KOH / g, a weight average molecular weight (Mw) of 7,551Da based on polystyrene, a solid content of 31.6wt%, and a polydispersity (Mw / Mn) of 2.04, as measured by gel permeation chromatography.
[0192] The structural units used in the preparation of the copolymers of Synthesis Examples 1 to 4 and their contents are shown in Table 1 below.
[0193] [Table 1]
[0194] Preparation Example: Preparation of Photosensitive Resin Composition The photosensitive resin compositions of the following Preparation Examples were prepared using the copolymers prepared in the Synthesis Examples above.
[0195] The ingredients used in the following preparation examples are shown in Table 2 below.
[0196] [Table 2]
[0197] Preparation Example <Preparation of Photosensitive Resin Composition> Preparation Example 1-1: First photosensitive resin composition The copolymer (A-1) was 100 parts by weight (solid content) of the copolymer obtained in Synthesis Example 1 as the copolymer, 40 parts by weight of 6-functional dipentaerythritol hexaacrylate (DPHA) (B-1, Nippon Kayaku Co., Ltd.) as the photopolymerizable compound (B), 40 parts by weight of 4-functional di(trimethylolpropane)tetraacrylate (B-2, trade name T-1420, Nippon Kayaku Co., Ltd.) as the photoinitiator (C), 2.0 parts by weight of N-1919, oxime-based photoinitiator 1 (C-1 ), 1.0 parts by weight of SPI-03, oxime photoinitiator 2 (C-2), and 0.4 parts by weight of (E)-2-(4-styrylphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, triazine photoinitiator 3 (C-3), 6.8 parts by weight of BK-7539 (Tokushiki Co., Ltd.) as black organic colorant (D-2), 0.2 parts by weight of F563 (DIC) as surfactant (E), and 0.5 parts by weight of MIPHOTO GHP03HHP (Miwon) as additive, epoxy hardener (F-1) were uniformly mixed. Propylene glycol monomethyl ether acetate (PGMEA) was added to the mixture so that the solid content of the mixture was 25% by weight. The resultant was mixed using a shaker for 2 hours to prepare a liquid-phase photosensitive resin composition.
[0198] Preparation example 1-2: Second photosensitive resin composition A photosensitive resin composition was prepared in the same manner as in Preparation Example 1-1, except that 0.6 parts by weight of SPI-03, oxime photoinitiator 2 (C-2), and 0.4 parts by weight of (E)-2-(4-styrylphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, triazine photoinitiator 3 (C-3) were used as the photopolymerization initiator (C), 12.7 parts by weight of BK-7539 (Tokushiki Co., Ltd.), which was uniformly mixed without the addition of any additives, was used as the organic colorant (D-2), and a mixture of propylene glycol monomethyl ether acetate (PGMEA) (G-1) and 3-methoxybutyl acetate (3BMA) (G-2) was added so that the solid content of the mixture was 25% by weight.
[0199] Preparation Examples 2-1 to 25-2 Photosensitive resin compositions were prepared in the same manner as in Preparation Example 1-1, except that the type and / or content of each component was changed as shown in Table 3 below.
[0200] [Table 3]
[0201] [Table 4]
[0202] <Preparation of quantum dot barrier rib structure> Example 1 The photosensitive resin composition obtained in Preparation Example 1-1 as the first photosensitive resin composition was coated on a glass substrate immersed in distilled water using a spin coater, and then dried. It was pre-baked at 90°C for 150 seconds to form a coated film with a thickness of 6.0 μm or more. The coated film was further mid-baked at 130°C for 300 seconds to remove the solvent and form a first cured film (i.e., the lower film).
[0203] The photosensitive resin composition obtained in Preparation Example 1-2 as the second photosensitive resin composition was coated on the first cured film, which was then prebaked at 90° C. for 150 seconds to form a second cured film (i.e., upper film) having a thickness of 6.0 μm or more, thereby preparing a multi-layered cured film having two layers.
[0204] Then, a mask was placed on the multilayer cured film so that a 5 cm x 5 cm area of it was 100% exposed and had minimal gap contact with the substrate. It was then irradiated with light having a wavelength of 200 nm to 450 nm at 150 mJ / cm based on a wavelength of 365 nm for a certain period of time using an aligner (model name: MA6) that emits light having a wavelength of 200 nm to 450 nm. 2 It was then developed at 23° C. with an aqueous solution of potassium hydroxide diluted to a concentration of 0.04% by weight until the unexposed parts were completely washed away. The pattern thus formed was post-baked in an oven at 230° C. for 30 minutes to prepare a quantum dot barrier rib structure.
[0205] Examples 2 to 13 A quantum dot barrier rib structure including a multilayer cured film was prepared in the same manner as in Example 1, except that the first photosensitive resin composition and the second photosensitive resin composition (Preparation Examples 2-1 to 13-2) having the components and contents shown in Table 3 above were used, and the development time and film thickness were changed as shown in Tables 4 and 6 below.
[0206] Comparative Example 1 to Comparative Example 11 A quantum dot barrier rib structure including a single-layer cured film was prepared in the same manner as in Example 1, except that a first cured film was formed using a photosensitive resin composition (Preparation Examples 14 to 24) having the components and contents shown in Table 3 above, and the development time and film thickness were changed as shown in Tables 4 and 6 below to prepare a single-layer cured film.
[0207] Comparative Example 12 A quantum dot barrier rib structure including a multilayer cured film was prepared in the same manner as in Example 1, except that the first photosensitive resin composition (Preparation Example 25-1) and the second photosensitive resin composition (Preparation Example 25-2) having the components and contents shown in Table 3 above were used, and the development time and film thickness were changed as shown in Tables 4 and 6 below.
[0208] Evaluation Example 1: Development Time In the methods for preparing the quantum dot barrier rib structures of the examples and comparative examples, the time taken for the unexposed portions to be completely washed away (to the stage where the O-ring portion of the developing device can be completely seen behind the substrate) was measured during development with an aqueous solution of 0.04 wt % potassium hydroxide. - If the development time was 300 seconds or less, it was evaluated as ○. If it was more than 300 seconds, it was evaluated as ×.
[0209] Evaluation Example 2: Resolution and Critical Dimensions of Line Patterns To measure the pattern resolution and critical dimension (CD; unit: μm) of the line patterns in the quantum dot barrier rib structures of the examples and comparative examples, the line CD was observed with a micro-optical microscope (STM6-LM, manufacturer: Olympus) and an X-ray scanning electron microscope (SEM; S4300). The results are shown in Figures 5 and 6.
[0210] In addition, the size of the 13 μm line pattern of the photomask was observed to measure the resolution. 2 The pattern dimensions of the line pattern after curing were measured at 13 μm below. The smaller this value, the better the resolution because a smaller pattern can be formed. - If the resolution was greater than 0 to 20 μm, it was evaluated as ○. If it exceeded 20 μm, it was evaluated as ×.
[0211] Evaluation Example 3: Thickness of Cured Film Before and After Post-baking The quantum dot barrier rib structures of the example and comparative example were measured for height difference due to vertical movement of the device probe tip using an alpha-step profilometer, SCAN PLUS, and their thicknesses were obtained from these results.
[0212] Initial film thickness refers to the thickness of the film formed during pre-baking prior to the exposure and development steps in preparing the quantum dot barrier rib structures (ie, the film thickness prior to post-baking).
[0213] The final film thickness refers to the final film thickness of the quantum dot barrier rib structure formed during the exposure and development steps for forming a pattern in the preparation of the quantum dot barrier rib structure and its post-baking (i.e., the film thickness after post-baking). - If the initial film thickness and the final film thickness were multi-layered, they were evaluated as ◯. If they were mono-layered, they were evaluated as ×.
[0214] Evaluation Example 4: Optical Density The transmittance at 550 nm of the cured films of the quantum dot barrier rib structures of the examples and comparative examples was measured using an optical density meter (361T manufactured by Xlite). The optical density (OD, unit: / μm) based on a thickness of 1 μm and the optical density of the final film thickness were measured. The total optical density was obtained by multiplying the optical density based on 1 μm by the final film thickness (in the case of Comparative Examples 11 and 12, the total optical density was calculated based on the film thickness before post-baking). Total optical density = optical density based on 1 μm ( / μm) × final film thickness (μm)
[0215] Evaluation Example 5: Reflectance The cured films of the quantum dot barrier rib structures of the examples and comparative examples were each measured using a spectrophotometer device (CM-3700A) at a wavelength of 550 nm. SCI and R SCE The ratio between them (R SCE / RSCI ) was then calculated. - R SCI If it was 5.0% or less, it was evaluated as ○. If it exceeded 5.0%, it was evaluated as ×. - R SCE If it was 0.5% or less, it was evaluated as ○. If it exceeded 0.5%, it was evaluated as ×. - R SCE / R SCI If it was between 2% and 10%, it was evaluated as ○. If it was less than 2.0% or more than 10%, it was evaluated as ×.
[0216] Evaluation Example 6: Contact angle The cured films of the quantum dot barrier rib structures of the examples and comparative examples were each measured for contact angle using 2-ethoxyethanol, a polar solvent, and a contact angle measuring device (DM300, Kyowa). It was confirmed that the cured film containing no fluorine-containing copolymer had a contact angle of 0°, and the cured film containing the fluorine-containing copolymer had a contact angle of 10° to 20°.
[0217] The results of the evaluation examples are shown in Tables 4 to 7 below.
[0218] [Table 5]
[0219] [Table 6]
[0220] [Table 7]
[0221] [Table 8]
[0222] As shown in Tables 4 to 7, the quantum dot barrier rib structures of Examples 1 to 13 prepared from the multilayer cured films using the photosensitive resin compositions of Preparation Examples 1-1 to 13-2 had a total thickness that satisfied the range of 6 μm to 20 μm. It was possible to form a sufficient thickness that can be used for the quantum dot barrier rib. When the multilayer cured film having a thickness within the above range is used as the quantum dot barrier rib, when the quantum dot solution is dripped, it does not overflow the barrier rib. Therefore, the colored composition is not mixed, and it is possible to prevent deterioration of the resolution.
[0223] Furthermore, the quantum dot barrier rib structures of Examples 1 to 13 have an R of 5% or less. SCI , R less than 0.5% SCE , and 2 % ~10 % R SCE / R SCI Therefore, it was confirmed that they met the low reflectance characteristics. In addition, it was confirmed that they could achieve high light blocking properties since the total optical density for the final film thickness after post-baking fell within the range of the present invention. The resolution was excellent at the level of 12 μm to 16 μm.
[0224] In contrast, the quantum dot barrier rib structures of Comparative Examples 1 to 11 prepared from single-layer cured films using the photosensitive resin compositions of Preparation Examples 14 to 24 had total thicknesses of less than 3 μm to 6 μm. If structures having such thickness ranges are used as quantum dot barrier ribs, the quantum dot solution may overflow the barrier rib, resulting in difficulty in color separation, which is likely to be contaminated, and resulting in deterioration of resolution.
[0225] In particular, the quantum dot barrier rib structures of Comparative Examples 3 and 4 had poor light blocking properties because they had a total optical density of 0.7. SCI , R exceeding 0.5% SCE , and 10 % Exceeds R SCE / R SCIIt was suggested that they have a higher reflectance than the quantum dot barrier rib structures of Examples 1 to 13. Therefore, they cannot achieve the low reflectance and high light shielding property desired in the present invention.
[0226] 5 and 6 are photographs of the cross section and side surface of the quantum dot barrier rib structures of Examples 1 to 13 and Comparative Examples 1 to 12 observed with an optical microscope.
[0227] As can be seen from FIG. 5, the cured films of the quantum dot barrier rib structures of Examples 1-13 are all clear and distinct in terms of line width, and uniform and thick in terms of film thickness.
[0228] In contrast, as can be seen from FIG. 6, the cured films of the quantum dot barrier rib structures of Comparative Examples 1 to 12 were not suitable for quantum dot barrier ribs because they had small thicknesses. In particular, in Comparative Examples 11 and 12, the film was detached, so the pattern was not formed; or it was not clear. In particular, the quantum dot barrier rib structure of Comparative Example 12 was prepared as a multi-layer cured film, but the content of the colorant was high, and as a result, the optimal exposure dose condition (150 mJ / cm2) was not achieved. 2 ) the film detached, resulting in a resolution of 0 μm; and the pattern was not clear. [Explanation of symbols]
[0229] 100 Base structure 110 Transparent substrate 120 Barrier Rib 130 First quantum dot solution 140 2nd quantum dot solution 150 3rd quantum dot solution 200, 300, 400 Quantum dot barrier rib structure 210, 310, 410 base material 211, 311, 411 First hardening film 212, 312, 412 Second hardening film 313, 413 3rd hardening film nn nth 番目の Hardened Film
Claims
1. (A) a copolymer comprising (a-1) structural units derived from an ethylenically unsaturated carboxylic acid, an ethylenically unsaturated carboxylic acid anhydride, or a combination thereof, (a-2) structural units derived from an ethylenically unsaturated compound containing an aromatic ring, (a-3) structural units derived from an ethylenically unsaturated compound containing an epoxy group, and (a-4) structural units derived from an ethylenically unsaturated compound different from (a-1), (a-2), and (a-3); (B) photopolymerizable compound; (C) a photopolymerization initiator, and (D) Coloring agent including a black coloring agent A quantum dot barrier rib structure comprising a cured film formed from a photosensitive resin composition comprising: The structure of quantum dot barrier ribs has a total thickness of 6 μm or more, an optical density of 0.05 / μm to 2.0 / μm, and The following relationships, respectively: (Relationship 1) R SCI ≦5.0% (Relationship 2) R SCE ≦0.5% (Relationship 3) 2% ≤ R SCE / R SCI ≦10% The reflectance R measured by the SCI (specular reflection included) method at a wavelength of 550 nm satisfies SCI and reflectance R measured by the SCE (specular reflection not included) method SCE A structure having the above structure.
2. 2. The quantum dot barrier rib structure of claim 1, wherein the black colorant comprises at least one selected from the group consisting of a black organic colorant and a black inorganic colorant.
3. 3. The quantum dot barrier rib structure according to claim 2, wherein the black organic colorant is used in an amount of 3 to 40 parts by weight based on 100 parts by weight of the copolymer (A).
4. 3. The quantum dot barrier rib structure according to claim 2, wherein the black inorganic colorant is used in an amount of 0.01 to 10 parts by weight based on 100 parts by weight of the copolymer (A).
5. 2. The quantum dot barrier rib structure of claim 1, wherein the colorant (D) further comprises at least one colorant selected from the group consisting of a blue colorant and a violet colorant.
6. The quantum dot barrier rib structure of claim 5, wherein the blue colorant and the violet colorant are each used in an amount of 0.01 to 10 parts by weight based on 100 parts by weight of the copolymer (A).
7. The quantum dot barrier rib structure according to claim 1, wherein the colorant (D) is used in an amount of 1 to 40 parts by weight based on 100 parts by weight of the copolymer (A).
8. The quantum dot barrier rib structure according to claim 1, wherein the photosensitive resin composition further comprises at least one selected from the group consisting of an epoxy compound, a photobase generator, a thiol compound, and a compound derived from an epoxy resin.
9. A quantum dot barrier rib structure comprising a first cured film formed from a first photosensitive resin composition and a second cured film formed from a second photosensitive resin composition on the first cured film, the first photosensitive resin composition, the second photosensitive resin composition, or both of them, (A) comprises a copolymer including (a-1) a structural unit derived from an ethylenically unsaturated carboxylic acid, an ethylenically unsaturated carboxylic acid anhydride, or a combination thereof, (a-2) a structural unit derived from an ethylenically unsaturated compound containing an aromatic ring, (a-3) a structural unit derived from an ethylenically unsaturated compound containing an epoxy group, and (a-4) a structural unit derived from an ethylenically unsaturated compound different from (a-1), (a-2), and (a-3); (B) a photopolymerizable compound; (C) a photopolymerization initiator; and (D) a colorant including a black colorant; The structure has a total thickness of 6 μm or greater.
10. 10. The quantum dot barrier rib structure of claim 9, wherein the first hardened film and the second hardened film each have a thickness of 10 μm or less.
11. 10. The quantum dot barrier rib structure of claim 9, wherein the multilayer cured film has a total thickness of 6 μm to 20 μm.
12. 10. The quantum dot barrier rib structure of claim 9 having an optical density of 0.05 / μm to 2.0 / μm.
13. coating a first photosensitive resin composition onto a substrate and curing it to form a first cured film; coating a second photosensitive resin composition onto the first cured film and curing it to form a second cured film; exposing and developing the multi-layer cured film including the first cured film and the second cured film to form a pattern, and then curing it; A method for preparing a quantum dot barrier rib structure, comprising: The first photosensitive resin composition, the second photosensitive resin composition, or both of them comprise: (A) a copolymer including (a-1) a structural unit derived from an ethylenically unsaturated carboxylic acid, an ethylenically unsaturated carboxylic acid anhydride, or a combination thereof, (a-2) a structural unit derived from an ethylenically unsaturated compound containing an aromatic ring, (a-3) a structural unit derived from an ethylenically unsaturated compound containing an epoxy group, and (a-4) a structural unit derived from an ethylenically unsaturated compound different from (a-1), (a-2), and (a-3); (B) a photopolymerizable compound; (C) a photopolymerization initiator; and (D) a colorant including a black colorant.
14. 14. The method for preparing a quantum dot barrier rib structure according to claim 13, wherein the curing to form the first cured film and the second cured film is carried out at 70°C to 140°C for 100 seconds to 800 seconds, respectively.
15. 15. The method for preparing the quantum dot barrier rib structure according to claim 14, wherein the curing to form the first cured film and the second cured film is carried out as a pre-bake at 70°C to 100°C for 50 seconds to 400 seconds and a mid-bake at 80°C to 140°C for 100 seconds to 500 seconds, respectively.
16. The method for preparing the structure of quantum dot barrier ribs as claimed in claim 13, wherein the curing after forming the pattern is carried out at 150°C to 300°C for 10 minutes to 60 minutes.
17. The method for preparing a quantum dot barrier rib structure according to claim 13, wherein the exposure is carried out by arranging a mask so that the interval between each pattern is 10 μm to 30 μm, and irradiating with active light.
18. The method for preparing a quantum dot barrier rib structure according to claim 13, wherein the developing is carried out for 50 seconds to 300 seconds.
19. The method for preparing a quantum dot barrier rib structure according to claim 13, wherein one or more cured films are further formed on the second cured film.
20. 20. The method for preparing a quantum dot barrier rib structure according to claim 19, wherein each cured film in the multi-layer cured film has a thickness of 8 μm or less, and the multi-layer cured film has a total thickness of 6 μm to 20 μm.
Citation Information
Patent Citations
Color filter formed substrate, manufacturing method for the same, and display device
JP2014025986A
Curable composition, light-shielding film, solid-state imaging device, and color filter
WO2017141723A1