Structure, manufacturing method thereof, joined body, and rotor for crusher
By using controlled surface roughness and precise manufacturing methods, the bonded structures of ceramics and metals achieve high bonding strength and airtightness, addressing the issues of breakage and airtightness in existing technologies.
Patent Information
- Application Number
- JP2020218996
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-12-28
AI Technical Summary
Existing bonded bodies of ceramics or ceramics and metal tend to break under perpendicular pressure and suffer from reduced airtightness due to grooves and cutouts, which act as fluid passages.
The structures incorporate columnar recesses or through holes with controlled surface roughness, using ceramics like aluminum oxide, zirconium oxide, and silicon nitride, and a manufacturing process involving firing and precise grinding to enhance bonding strength and airtightness by minimizing unevenness and improving perpendicularity.
The structures achieve high bonding strength and improved airtightness by enhancing the anchoring effect of adhesives and sealing, while maintaining structural integrity under pressure.
Smart Images

Figure 0007578487000002 
Figure 0007578487000003 
Figure 0007578487000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a ceramic structure, a method for producing the same, a joined body, and a rotor for a crusher. [Background technology]
[0002] Conventionally, various manufacturing methods have been considered for obtaining a bonded body between ceramics or between ceramics and metal. For example, Patent Document 1 proposes a method in which a plurality of grooves or notches are formed on at least one of the bonding surfaces of two bonded bodies, an annular bonding agent pellet is placed between both bonding surfaces, and the bonding agent pellet is heated and melted to obtain a bonded body.
[0003] The bonded body proposed in Patent Document 1 had a problem in that it was easily broken between the bonded surfaces when pressure was applied from a direction perpendicular to the axial direction of the two bonded bodies (in other words, a direction parallel to the bonded surfaces).In addition, because it had grooves and notches, when airtightness was required for the bonded body, there was also a problem in that the grooves and notches became passages for fluids, reducing the airtightness. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Utility Model Application Publication No. 63-192441 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present disclosure is to provide a structure having a cylindrical recess or through hole, which, when a joining member such as a pin is inserted into the recess or through hole and sealed, can provide high airtightness in this portion and high joining strength to the joining member, a method for manufacturing the same, and a joined body and a crusher rotor using the structure. [Means for solving the problem]
[0006] A first structure of the present disclosure for solving the above problems comprises a cylindrical recess extending from the surface toward the inside, and is made of ceramics containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component, and one or both of these components other than the main component as a secondary component. The average value of the cut level difference (Rδ), which represents the difference between the cut level at a load length ratio of 25% in the circumferential roughness curve of the first inner circumferential surface forming the recess, and the cut level at a load length ratio of 75% in the roughness curve, is smaller on the opening side of the recess than on the bottom side.
[0007] A second structure of the present disclosure comprises a first surface and a second surface opposite to the first surface, and through holes opening into the first surface and the second surface, and is made of ceramics containing at least one of aluminum oxide, zirconium oxide and silicon nitride as a main component, and one or both of these components other than the main component as a secondary component. The average value of the cut level difference (Rδ), which represents the difference between the cut level at a load length ratio of 25% in the circumferential roughness curve of the second inner circumferential surface surrounding the through holes and the cut level at a load length ratio of 75% in the roughness curve, is smaller in the vicinity of the first surface and in the vicinity of the second surface than in the center of the through holes.
[0008] The first method for producing a structure according to the present disclosure includes: A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; sintering the molded body to obtain a sintered body; The method includes a step of fixing the sintered body, grinding the sintered body with a metal grinding wheel having an axial length shorter than the recess to form a recess in the sintered body, and then performing zero grinding with a part of the metal grinding wheel positioned outside the recess to obtain a structure with a recess. Another method for producing a first structure according to the present disclosure includes the steps of: A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; obtaining a precursor having a first pilot hole formed inward from a surface of the molded body by cutting; sintering the precursor to obtain a sintered body; The method includes a step of fixing the sintered body, grinding the inner surface of the first pilot hole with a metal grinding wheel that is shorter than the axial length of the recess to form a recess in the sintered body, and then performing zero grinding while a part of the metal grinding wheel is positioned outside the recess to obtain a structure with a recess.
[0009] The second method for producing a structure according to the present disclosure includes the steps of: A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; sintering the molded body to obtain a sintered body; The method includes a process of fixing the sintered body and grinding it with a metal grinding wheel that is shorter than the axial length of the through hole to form the through hole, and then zero-grinding at least the vicinity of the first surface and the vicinity of the second surface with a part of the metal grinding wheel positioned outside the through hole to obtain a structure with a through hole. Another method for producing a second structure according to the present disclosure includes the steps of: A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; obtaining a precursor having a second pilot hole formed by cutting the molded body so as to extend from the surface of the molded body toward the inside; sintering the precursor to obtain a sintered body; The method includes a process of fixing the sintered body, inserting a metal grinding wheel having a length shorter than the axial length of the through hole into the second pilot hole that forms a through hole in the sintered body, penetrating the second pilot hole by grinding, and then zero-grinding at least the vicinity of the first surface and the vicinity of the second surface with a portion of the metal grinding wheel positioned outside the through hole, thereby obtaining a structure with a through hole.
[0010] The bonded body of the present disclosure comprises the first or second structure, a pin inserted into the recess or through hole, and a bonding layer interposed between the outer peripheral surface of the pin and the first inner peripheral surface or the second inner peripheral surface. The rotor for a crusher according to the present disclosure includes the above-mentioned joined body. Effect of the Invention
[0011] In the first structure of the present disclosure, the first inner peripheral surface has smaller irregularities on the opening side of the recess than on the bottom side, so that when a joining member such as a pin is inserted into the recess and the opening side of the recess is sealed with an adhesive, airtightness is improved. Also, the inner peripheral surface on the bottom side of the recess has larger irregularities, so that the adhesive has a stronger anchor effect, resulting in high joining strength. In the second structure of the present disclosure, the unevenness of the second inner circumferential surface is smaller near the first surface and near the second surface than in the center of the through hole, so that when a joining member such as a pin is inserted into the through hole and both sides of the through hole (i.e., either or both of the vicinity of the first surface and the vicinity of the second surface) are sealed with an adhesive, airtightness is improved. Also, the unevenness in the center of the second inner circumferential surface is larger, so the anchor effect of the adhesive is enhanced, resulting in high joining strength. Furthermore, according to the first method for manufacturing a structure of the present disclosure, it is possible to improve the perpendicularity of the recess with respect to the surface where the recess opens. According to the second manufacturing method of the present disclosure, the perpendicularity of the through hole with respect to the first surface and the second surface can be improved. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a cross-sectional view illustrating a first structure having a cylindrical recess according to an embodiment of the present disclosure. [Diagram 2] FIG. 11 is a cross-sectional view showing an example of a bonded body using the obtained first structure. [Diagram 3] 5(a) and 5(b) are explanatory views showing a part of a manufacturing process of a first structure according to an embodiment of the present disclosure. [Figure 4] FIG. 2 is a cross-sectional view showing a first structure having a through hole according to an embodiment of the present disclosure. [Diagram 5] 6(a) and 6(b) are explanatory views showing a part of a manufacturing process of the second structure according to the embodiment of the present disclosure. [Figure 6] FIG. 11 is an explanatory view showing an example of inner diameter finishing of the second structure. [Figure 7] 1A and 1B are a cross-sectional view and a plan view, respectively, of a rotor according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A structure according to an embodiment of the present disclosure will now be described. (First structure) FIG. 1 is a cross-sectional view showing a first structure 1 according to this embodiment, and this first structure 1 has a cylindrical recess 2 extending from the surface toward the inside.
[0014] The first structure 1 is made of ceramics containing at least one of aluminum oxide Al2O3, zirconium oxide ZrO2, and silicon nitride Si3N4 as a main component, and containing one or both of the above components other than the main component as a secondary component. This ceramic is usually classified as a difficult-to-cut material. Here, the main component refers to a component that accounts for 50 mass% or more of the total amount, and the secondary component refers to a component that accounts for less than 50 mass%.
[0015] Specifically, for example, the ceramic contains 65% to 96% by mass of Al2O3, 4% to 34.4% by mass of ZrO2, 0.2% or more by mass of SiO2, 0.22% or more by mass of TiO2, and 0.12% or more by mass of MgO, with the combined content of SiO2, TiO2, and MgO being 0.6% to 4.5% by mass. In this ceramic, the main component is Al2O3. Alternatively, the ceramic may contain 20% to 60% by mass of Si3N4, 25% to 70% by mass of ZrO2, and 5% to 15% by mass of at least one selected from MgO, Y2O3, CeO2, CaO, HfO2, TiO2, Al2O3, SiO2, MoO3, CrO, CoO, ZnO, Ga2O3, Ta2O5, NiO, and V2O5. In this ceramic, the main component is either Si3N4 or ZrO2 depending on the blending amount. The components constituting the ceramics can be identified by an X-ray diffractometer using CuKα radiation. The content of each component can be determined, for example, by an ICP (Inductively Coupled Plasma) emission spectrometer or a fluorescent X-ray analyzer.
[0016] The cylindrical recess 2 formed in the first structure 1 is formed so that the average value of the cut level difference (Rδ), which represents the difference between the cut level at a load length ratio of 25% on the circumferential roughness curve of the first inner surface 9 and the cut level at a load length ratio of 75% on the roughness curve, is smaller on the opening side (indicated by arrow B) of the recess 2 than on the bottom side (indicated by arrow A). Here, the bottom side of the recess 2 refers to an area that is 25% or less from the bottom of the recess 2 when the axial length of the first inner circumferential surface 9 is taken as 100%. Also, the opening side refers to an area that is 25% or less from the opening end of the recess 2 when the axial length of the first inner circumferential surface 9 is taken as 100%.
[0017] As shown in Fig. 2, a pin 3 is inserted into a recess 2 of a first structure 1, and a bonding layer 4 (adhesive or the like) is interposed between the outer peripheral surface of the pin 3 and the inner peripheral surface of the recess 2 to produce a bonded body 5. At this time, since the average value of the cut level difference (Rδ) on the opening side is small, the airtightness of the opening side of the recess 2 sealed with the bonding agent is improved. In addition, since the inner peripheral surface on the bottom side of the closed recess 2 has relatively large irregularities, the anchor effect of the bonding agent is enhanced, and high bonding strength is obtained. The bonding agent may be, for example, an epoxy adhesive, sealing glass, etc. The pin 3 may be made of, for example, S45C free-cutting steel, SUS303 free-cutting steel, etc.
[0018] It is preferable that the average value of the cut level difference (Rδ) on the first inner circumferential surface 9 of the recess 2 decreases exponentially or linearly from the bottom side toward the opening side of the recess 2. This makes the recess 2 more airtight than in a state in which the cut level difference (Rδ) on the first inner circumferential surface 9 is not controlled.
[0019] It is preferable that the average value of the cut level difference (Rδ) on the bottom side of the closed recess 2 be 1.5 μm or less. This improves the surface properties of the bottom side to be closed and reduces the likelihood of ceramic particles detaching during the joining operation, thereby maintaining high joining strength.
[0020] The cut level difference (Rδc) can be measured using a shape analysis laser microscope (Keyence Corporation, VK-X1100 or its successor model) in accordance with JIS B 0601:2001. The measurement conditions are as follows: first, the illumination method is a coaxial epi-illumination method, the magnification is 480x, the cutoff value λs is none, the cutoff value λc is 0.08mm, the cutoff value λf is none, and the end effect is corrected. The measurement points are the bottom side and the opening side of the first inner circumferential surface 9 of the recess 2. The measurement method is to draw four lines to be measured at approximately equal intervals along the circumferential direction, measure the surface roughness of each line, and calculate the average value based on the measured values for each line. The measurement range per point is 710μm×533μm, and the length of each line to be measured is 560μm. When setting an approximation function (such as an exponential function or a linear function) that indicates a gradual decrease in the average value of the cut level difference (Rδ), the cut level difference (Rδ) is measured every 10% in the range of 10% to 90% of the axial length from the bottom surface of the recess 2 toward the opening end of the recess 2, and the average value is calculated. An approximation function (exponential function, linear function, etc.) showing the gradual decrease in the average value of the amputation level difference (Rδ) is set using a graph tool provided in Excel (registered trademark, Microsoft Corporation), and then the correlation coefficient R is calculated. Then, using an r table (correlation coefficient test table), the correlation coefficient R is tested at a significance level of 5% (two-sided probability), and if significant, an approximation function (exponential function, linear function, etc.) showing the gradual decrease in the average value of the amputation level difference (Rδ) is determined.
[0021] Next, a method for manufacturing the first structure 1 will be described. First, a molded body is obtained that contains at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component, and one or both of these components other than the main component as a sub-component. That is, after weighing each of the above components, they are put into a grinding mill together with a solvent (ion-exchanged water) and ground until the average particle size (D50) of the powder is 1.5 μm or less, and then an organic binder is added and mixed to obtain a slurry. Examples of the organic binder include acrylic emulsion, polyvinyl alcohol, polyethylene glycol, and polyethylene oxide. The slurry is spray-granulated to obtain granules, which are then pressed at a molding pressure of 78 MPa to 128 MPa using a uniaxial press molding device or a cold isostatic press molding device to obtain a green body.
[0022] Next, a first pilot hole is formed from the surface of the obtained molded body toward the inside by cutting to obtain a precursor. The opening diameter of the pilot hole is preferably 70% to 95% of the opening diameter of the recess 2. When the thickness of the molded body is thin, for example, between 1 mm and 30 mm, the first pilot hole does not need to be formed at the precursor stage, and after obtaining the sintered body described below, the formation of the recess and zero grinding can be performed with a metal grinding wheel. Alternatively, when the recess 2 is small, for example when the opening diameter of the recess 2 is 1 mm or more and 10 mm or less and the depth of the recess 2 is 1 mm or more and 30 mm or less, the first pilot hole does not need to be formed at the precursor stage, and after obtaining the sintered body described below, the recess may be formed and zero grinding may be performed with a metal grinding wheel.
[0023] Next, the obtained precursor is fired to obtain a sintered body. In the case of a molded body mainly composed of aluminum oxide or zirconium oxide, firing is suitably performed in an air atmosphere at 1400°C to 1700°C for 1 hour to 6 hours. In the case of a molded body mainly composed of silicon nitride, the molded body is heated from room temperature to 300 to 1000°C in a vacuum atmosphere, and then nitrogen gas is introduced to maintain the nitrogen partial pressure at 10 to 100 kPa. Then, the temperature is continued to be raised, and the temperature is held at 1750°C for 1 to 2 hours to obtain a fine crystal structure. Thereafter, the temperature is further raised and the temperature is held at 1800°C to 1860°C for 1 hour to 6 hours.
[0024] Next, the obtained sintered body 6 is fixed, and as shown in Figure 3(a), the inner surface of the first pilot hole 7 is ground with a metal grinding wheel 8 that is shorter than the axial length of the pilot hole, and then, as shown in Figure 3(b), zero grinding is performed with a part of the metal grinding wheel 8 positioned outside the first pilot hole 7, to obtain a first structure 1 having a recess 2. The metal grinding wheel is a grinding wheel made of abrasive grains and a metal binder, and for example, a product name "Solotel" manufactured by Asahi Diamond Industrial Co., Ltd. can be used. The same metal grinding wheel may be used for both grinding and zero grinding, or different metal grinding wheels may be used. In particular, among metal grinding wheels, electroplated grinding wheels are preferable. As described above, since the sintered body 6 is a difficult-to-cut material, when it is cut, the machining resistance is large, so the tool is bent when cutting, resulting in a tapered shape and the recess 2 being prone to becoming an inverted truncated cone. In contrast, since the metal grindstone described above has high rigidity, the hole diameter difference between the bottom side A and the opening side B of the recess 2 can be made 0.025 mm or less when grinding is performed with a metal grindstone that is shorter than the axial length of the pilot hole. This makes it possible to improve the perpendicularity of the first inner peripheral surface 9 with respect to the surface where the recess 2 opens.
[0025] Zero grinding, which is performed after grinding, is, so to speak, the inner diameter finishing of the opening side B of the recess 2. Here, zero grinding means that no infeed is performed at the end of the grinding process, and only the feed is applied, and is also called spark out or zero cut. Therefore, in zero grinding, grinding is performed with no part of the metal grinding wheel inserted into the recess 2. At this time, since the sintered body 6 is a difficult-to-cut material and has a large processing resistance, by performing zero grinding with part of the metal grinding wheel positioned outside the recess 2, the unevenness of the first inner surface 9 can be made smaller on the opening side B of the recess 2 than on the bottom side A. The shape of the first structure 1 is not particularly limited, and in addition to a rotor-like shape described below, shapes such as a flat plate, a cylindrical body, a flat plate, a housing, and a polyhedron are possible.
[0026] (Second structure) Next, the second structure according to the present disclosure will be described. Fig. 4 is a cross-sectional view showing the second structure 10. As shown in the figure, the second structure 10 has a first surface 10a and a second surface 10b opposite to the first surface 10a, and has a through hole 11 opening to the first surface 10a and the second surface 10b. The second structure 10 is made of ceramics containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component, and one or both of these components other than the main component as a secondary component, similar to the first structure 1. This ceramic is a difficult-to-cut material.
[0027] The average value of the cut level difference (Rδ), which represents the difference between the cut level at a load length ratio of 25% on the circumferential roughness curve of the second inner surface 12 surrounding the through hole 11 and the cut level at a load length ratio of 75% on the same roughness curve, is configured to be smaller near the first surface 10a and near the second surface 10b than in the central portion of the through hole 11.
[0028] As a result, the unevenness of the second inner circumferential surface 12 is smaller near the first surface 10a and near the second surface 10b than in the center of the through hole 11, so that when a joining member such as a pin is inserted into the through hole 11 and both sides of the through hole 11 are sealed with an adhesive, as with the first structure 1 shown in Fig. 2, airtightness is improved. Also, since the unevenness of the second inner circumferential surface 12 in the center is larger, the anchor effect of the adhesive is enhanced, and high joining strength is obtained. Here, the vicinity of the first surface 10a and the vicinity of the second surface 10b refer to regions that are 25% or less of the total length from the first surface 10a and the second surface 10b, respectively, in the axial direction of the through hole 11. The central portion of the through hole 11 refers to the region sandwiched between the vicinity of the first surface 10a and the vicinity of the second surface 10b. The overall length of the through hole 11 is preferably 10 mm or more and 30 mm or less.
[0029] The average value of the cutting level difference (Rδ) preferably decreases exponentially or linearly from the center of the through hole 11 toward at least one of the first surface 10a side and the second surface 10b side. The average value of the cutting level difference (Rδ) at the center of the through hole 11 is preferably 1.5 μm or less. The rest is the same as that of the first structure 1. The measuring device, measuring conditions, and measuring method used for measuring the cut level difference (Rδc) of the second inner circumferential surface 12 are the same as those used for measuring the first inner circumferential surface 9. The measurement locations are the vicinity of the first surface 10a of the second inner circumferential surface 12, the second surface 10b, and the center.
[0030] The following describes a method for producing the second structure 10. Note that the manufacturing conditions and other matters not described below are the same as those in the manufacturing method for the first structure 1, and therefore should be considered as equivalent thereto. First, a molded body is prepared which contains at least one of aluminum oxide, zirconium oxide and silicon nitride as a main component and one or both of these components other than the main component as a secondary component.
[0031] 5(a), a second pilot hole 14 extending from the surface of the obtained molded body 13 toward the inside is cut with a tool 20 to obtain a precursor 15. The second pilot hole 14 preferably penetrates from one surface to the other surface. When the thickness of the molded body is thin, for example, between 1 mm and 30 mm, the second pilot holes 14 do not need to be formed at the precursor stage, and after obtaining the sintered body described below, the formation of through holes and zero grinding can be performed with a metal grinding wheel. Alternatively, when the through hole 2 is small, for example when the opening diameter is 1 mm or more and 10 mm or less, the second pilot hole 14 does not need to be formed at the precursor stage, and after obtaining the sintered body described below, the formation of the through hole and zero grinding can be performed with a metal grinding wheel.
[0032] Next, the precursor 15 is fired to obtain a sintered body. The obtained sintered body 16 is fixed, and as shown in Fig. 5(b), a metal grindstone 17 shorter than the axial length of the through hole is inserted into the second pilot hole 14 to perform grinding. At this time, in consideration of the processing resistance, it is preferable that the diameter of the metal grindstone 17 is approximately the same as the diameter of the second pilot hole 14.
[0033] Next, the inner diameter is finished as shown in Fig. 6. That is, zero grinding is performed on at least the vicinity of the first surface and the vicinity of the second surface with a part of the metal grinding wheel 17' positioned outside the through hole to obtain a structure with a through hole. At this time, the grinding amount of the inner diameter is preferably about 2 to 0.05 mm. In the inner diameter finishing, it is preferable to process the through hole in stages in the axial direction from the first surface to the second surface. For example, when forming a through hole with a total length of 22 mm in a structure, the inner diameter is finished to a depth of 0 to 2.5 mm in the first stage, and to a depth of 2.5 to 5.0 mm in the second stage, and grinding is performed every 5 mm in sequence. This concentrates stress on a smaller area on the side surface of the metal grinding wheel 17', improving the accuracy of the inner diameter. Also, if necessary, only the vicinity of the first surface and the vicinity of the second surface may be zero-ground with the metal grindstone 17'.
[0034] In the second structure 10 thus obtained, the average value of the cutting level difference (Rδ) is smaller in the vicinity of the first surface 10a and in the vicinity of the second surface 10b than in the central portion of the through-hole 11.
[0035] Next, the measurement results of the average value of the cut level difference (Rδ) for the second structure 10 manufactured as described above will be described. The cut level difference (Rδ) was measured along the circumferential direction at three locations, namely, near the first surface 10a, the center, and near the second surface 10b on the second inner circumferential surface 12 of the through hole 11, and the average value was calculated. The measuring device, measuring conditions, and measuring method were the same as those described above. The results are shown in Table 1. In Table 1, the second structure 10 according to the present disclosure (through hole 11 total length 22 mm, finished inner diameter 8.1 mm) is taken as an example. As a comparative example, a structure of the same dimensions obtained by finishing the inner diameter using a metal grindstone longer than the total length (22 mm) of through hole 11 was also evaluated in the same manner.
[0036] [Table 1]
[0037] From Table 1, it can be seen that the second structure 10, which is an embodiment, differs from the comparative example in that the average value of the cutting level difference (Rδ) is smaller near the first surface 10a and near the second surface 10b than in the center of the through hole 11.
[0038] A bonded body using the second structure 10 according to the present disclosure has a structure, similar to the first structure 1, in which a pin inserted into a through hole 11 is bonded with a bonding layer interposed between the outer peripheral surface of the pin and a second inner peripheral surface 12.
[0039] (rotor) Next, the rotor for the pulverizer of the present disclosure will be described. As an example of the pulverizer, a wet medium disperser is used, which contains a dispersion medium (beads) in a treatment tank, and the material to be treated supplied to the treatment tank is stirred together with the dispersion medium by a rotor, and the material to be treated is finely divided by the shear force generated between the dispersion medium, and dispersed in a liquid.
[0040] 7(a) and (b) are a cross-sectional view and a plan view showing the rotor. The rotor 18 is cylindrical, and a protrusion plate 19 consisting of a large number of small protrusions is integrally formed on the outer circumferential surface. The rotor 18 is made of the above-mentioned ceramics, and a plurality of through holes 11 are formed in the circumferential direction at both ends. Therefore, the rotor 18 is the second structure 10 described above.
[0041] The crusher rotor 18 according to the present disclosure is obtained by joining the above-mentioned pins to these through holes 11. The above-mentioned pins are for attaching the rotor 18 to a rotating shaft (not shown) or the like. When the recess 2 is provided instead of the through hole 11, the rotor 18 is the first structure 1 described above.
[0042] Although the embodiment of the present disclosure has been described above, the structure of the present disclosure is not limited to the above embodiment. For example, the structure of the present disclosure can be applied to other uses in addition to the rotor for a crusher. [Explanation of symbols]
[0043] 1 First structure 2 Recess 3-pin 4 Bonding layer 5 Zygote 6 Sintered body 7 First pilot hole 8 Metal grinding wheels 9 First inner surface 10 Second structure 10a 1st page 10b 2nd side 11 Through hole 12 Second inner surface 13 Molded body 14 Second pilot hole 15 Precursors 16 Sintered body 17, 17´ Metal grinding wheel 18 Rotor 19 Protrusion plate 20 Tools
Claims
1. A ceramic structure having a cylindrical recess extending from a surface toward the inside, the ceramic structure containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component, and containing one or both of these components other than the main component as a secondary component, a structure in which an average value of a cut level difference (Rδ) representing the difference between a cut level at a load length rate of 25% in a circumferential roughness curve of a first inner surface forming the recess and a cut level at a load length rate of 75% in the roughness curve is smaller on the opening side of the recess than on the bottom side of the recess (wherein, when the axial length of the first inner surface is taken as 100%, the bottom side refers to a region that is 25% or less from the bottom of the recess, and the opening side refers to a region that is 25% or less from the opening of the recess).
2. 2. The structure according to claim 1, wherein an average value of the cut level difference (Rδ) on the first inner circumferential surface decreases exponentially or linearly from a bottom side toward an opening side of the recess.
3. 3. The structure according to claim 1, wherein an average value of the cut level difference (Rδ) on the bottom side of the recess is 1.5 μm or less.
4. A ceramic structure comprising a first surface and a second surface opposed to the first surface, a through hole opening to the first surface and the second surface, the ceramic structure comprising at least one of aluminum oxide, zirconium oxide and silicon nitride as a main component, and one or both of these components other than the main component as a secondary component, a structure in which an average value of a cut level difference (Rδ) representing the difference between a cut level at a load length rate of 25% in a circumferential roughness curve of a second inner surface surrounding the through hole and a cut level at a load length rate of 75% in the roughness curve is smaller in the vicinity of the first surface and in the vicinity of the second surface than in the central portion of the through hole (wherein, the vicinity of the first surface and the vicinity of the second surface refer to regions that are 25% or less of the total length from the first surface and the second surface, respectively, in the axial direction of the through hole, and the central portion of the through hole refers to a region sandwiched between the vicinity of the first surface and the vicinity of the second surface).
5. The structure according to claim 4, wherein an average value of the cut level difference (Rδ) decreases exponentially or linearly from the central portion toward at least one of the first surface side and the second surface side.
6. 6. The structure according to claim 4, wherein an average value of the cut level difference (Rδ) in the central portion is 1.5 μm or less.
7. The ceramic is Al 2 O 3 65% by mass to 96% by mass of ZrO 2 4% by mass to 34.4% by mass, SiO 2 0.2 mass% or more, TiO 2 and 0.12 mass% or more of MgO, 2 , TiO 2 The structure according to any one of claims 1 to 6, wherein the combined content of MgO is 0.6 mass% to 4.5 mass%.
8. The ceramic is Si 3 N 4 20% by mass to 60% by mass of ZrO 2 25% by mass to 70% by mass of MgO, Y 2 O 3 , CeO 2 , CaO, HfO 2 , TiO 2 , Al 2 O 3 , SiO 2 , MoO 3 , CrO, CoO, ZnO, Ga 2 O 3 , Ta 2 O 5 , NiO and V 2 O 5 The structure according to any one of claims 1 to 6, comprising 5 mass % to 15 mass % of at least one selected from the following:
9. A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; sintering the molded body to obtain a sintered body; a step of fixing the sintered body, grinding the sintered body with a metal grindstone having an axial length shorter than the recessed portion to form a recessed portion in the sintered body, and then performing zero grinding in a state in which a part of the metal grindstone is positioned outside the recessed portion to obtain a structure having a recessed portion; A method for producing a structure according to any one of claims 1 to 3, and claims 7 and 8 which refer to claims 1 to 3.
10. A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; obtaining a precursor having a first pilot hole formed inward from a surface of the molded body by cutting; sintering the precursor to obtain a sintered body; a step of fixing the sintered body, grinding the inner peripheral surface of the first pilot hole with a metal grindstone having a length shorter than the axial length of the recess to form a recess in the sintered body, and then performing zero grinding in a state in which a part of the metal grindstone is positioned outside the recess to obtain a structure having a recess; A method for producing a structure according to any one of claims 1 to 3, and claims 7 and 8 which refer to claims 1 to 3.
11. A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; sintering the molded body to obtain a sintered body; a step of fixing the sintered body, grinding the sintered body with a metal grindstone having a length shorter than the axial length of the through hole to form the through hole, and then zero-grinding at least the vicinity of the first surface and the vicinity of the second surface in a state where a part of the metal grindstone is positioned outside the through hole to obtain a structure having a through hole; A method for producing a structure according to any one of claims 4 to 6, and claims 7 and 8 which refer to claims 4 to 6.
12. A step of obtaining a molded body containing at least one of aluminum oxide, zirconium oxide, and silicon nitride as a main component and one or both of these components other than the main component as a secondary component; obtaining a precursor having a second pilot hole formed by cutting the molded body so as to extend from a surface of the molded body toward the inside; sintering the precursor to obtain a sintered body; a step of fixing the sintered body, inserting a metal grindstone having a length shorter than the axial length of the through hole into the second pilot hole that forms a through hole in the sintered body, penetrating the second pilot hole by grinding, and then zero-grinding at least the vicinity of the first surface and the vicinity of the second surface in a state in which a part of the metal grindstone is positioned outside the through hole, thereby obtaining a structure having a through hole; A method for producing a structure according to any one of claims 4 to 6, and claims 7 and 8 which refer to claims 4 to 6.
13. A bonded body comprising: a structure according to any one of claims 1 to 8; a pin inserted into the recess or the through hole; and a bonding layer interposed between an outer peripheral surface of the pin and the first inner peripheral surface or the second inner peripheral surface.
14. A rotor for a crusher, comprising the joined body according to claim 13.
Citation Information
Patent Citations
Engine part
JP1982191274A
JP1988192441U
Method for foil decoration simultaneously with injection molding and foil decoration mold therefor
JP2000263598A
Pigment-dispersing device and pigment-dispersing method
JP2000351916A
Ceramic sintered compact, method for producing the same, and biomaterial
JP2005075659A