Electrode body, lithium ion battery, and method for producing active material for lithium ion battery
By using Si particles with a clathrate type structure and controlled aluminum content, the battery's confining pressure fluctuations are minimized, improving battery stability and efficiency.
Patent Information
- Application Number
- JP2022110771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-08
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-07-08
AI Technical Summary
Silicon (Si) particles used as an active material in batteries experience large volume changes during charging and discharging, leading to fluctuations in confining pressure that can damage the battery.
Incorporating Si particles with a clathrate type structure and adding aluminum (Al) in specific amounts within the negative electrode active material layer to stabilize the Si particles, using a manufacturing method that involves mixing NaSi alloy with AlF3 and heating to form Si particles with a clathrate type structure.
The solution effectively suppresses fluctuations in battery confining pressure during charging and discharging, enhancing the stability and efficiency of the battery.
Smart Images

Figure 0007578647000002 
Figure 0007578647000003 
Figure 0007578647000004
Abstract
Description
Technical Field
[0001] The present disclosure relates to an electrode body, a lithium-ion battery, and a method for manufacturing an active material for a lithium-ion battery.
Background Art
[0002] In recent years, battery development has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles has been promoted. Also, Si is known as an active material used in batteries.
[0003] Si has a large theoretical capacity and is effective for increasing the energy density of batteries. However, Si has a large volume change during charge and discharge.
[0004] From the viewpoint of solving such problems, Si having a class rate structure has been attracting attention.
[0005] x Si 136 Patent Document 1 discloses an active material having a silicon class rate type II crystal phase and having a composition of Na
[0006] Also, Patent Document 2 discloses a method for manufacturing a negative electrode active material containing silicon class rate II, which includes a reaction step of heating a reaction raw material in which a NaSi alloy containing Na and Si and a Na trap agent are contained in a contact state, and reacting Na derived from the NaSi alloy with the Na trap agent to reduce the amount of Na in the NaSi alloy.
Prior Art Documents
Patent Documents
[0007]
Patent Document 1
Patent Document 2
Summary of the Invention
[0008] As described above, while the Si particles as an active material are effective in increasing the energy density of the battery, they undergo a large volume change during charging and discharging. The expansion and contraction of the active material causes fluctuations in the battery's confining pressure. As a means of reducing the fluctuations in the battery's confining pressure, it is considered to suppress the expansion and contraction of the active material that accompanies charging and discharging.
[0009] A primary object of the present disclosure is to provide an electrode assembly capable of suppressing fluctuations in the confining pressure of a battery during charging and discharging. [Means for solving the problem]
[0010] The present inventors have found that the above object can be achieved by the following means: Aspect 1 A negative electrode assembly for a lithium ion battery having a negative electrode current collector layer and a negative electrode active material layer, The negative electrode active material layer contains Si particles having a clathrate structure as a negative electrode active material, The negative electrode active material layer contains 0.850 to 5.000 mass% Al with respect to the mass of the negative electrode active material layer, and The Si particles contain 0.040 to 0.250 mass% Al relative to the mass of the Si particles. Negative electrode body. Aspect 2 The negative electrode body contains 1.500 mass % or more of Al with respect to the total mass of the negative electrode active material layer, and The Si particles contain 0.080 mass% or more of Al relative to the mass of the Si particles. 2. The negative electrode assembly of embodiment 1. Aspect 3 3. The negative electrode body according to aspect 1 or 2, wherein the negative electrode active material layer contains Al-containing particles that are electrochemically inactive under a voltage used in a lithium ion battery. Aspect 4 The negative electrode body according to aspect 3, wherein the Al-containing particles contain F or O. Aspect 5 The Al-containing particles are AlF 3 Or Al 2 O 3 The negative electrode assembly according to embodiment 4, Aspect 6 The negative electrode body according to any one of aspects 1 to 5, wherein the Si particles have a porous structure. Aspect 7 The negative electrode body according to any one of aspects 1 to 6, wherein the Si particles have a clathrate II structure. Aspect 8 A lithium ion battery comprising the negative electrode assembly according to any one of aspects 1 to 7, a solid electrolyte layer, and a positive electrode assembly laminated in this order. Aspect 9: NaSi alloy and AlF 3 and heating the mixture to obtain a mixture containing Si particles having a clathrate structure, NaF, and Al-containing particles; and The mixture was mixed with HNO 3 washing with an aqueous solution followed by filtering and drying; It has A method for producing active materials for lithium-ion batteries. Aspect 10 10. The method of claim 9, comprising mechanically milling Si powder and NaH powder, followed by heating to obtain the NaSi alloy. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide an electrode assembly that can mainly suppress fluctuations in the confining pressure of a battery during charging and discharging. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram of a lithium-ion battery 1 according to one embodiment of the present disclosure. [Diagram 2]1 is an electron image obtained by measuring the negative electrode active material layer of Example 2 by SEM-EDX. [Diagram 3] 1 is an electron image obtained by measuring the negative electrode active material layer of Example 2 by SEM-EDX. [Figure 4] 1 is an electron image obtained by measuring the negative electrode active material layer of Example 2 by SEM-EDX. [Diagram 5] 1 is an electron image obtained by measuring the negative electrode active material layer of Example 2 by SEM-EDX. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0014] Negative electrode body The negative electrode body of the present disclosure has at least a negative electrode current collector and a negative electrode active material layer. Another layer may be interposed between the negative electrode current collector and the negative electrode active material layer. The negative electrode active material layer of the present disclosure contains at least Si particles having a clathrate structure as an active material. The negative electrode active material layer may further contain other than Si particles having a clathrate structure, such as Si particles not having a clathrate structure, as a negative electrode active material, and may contain a solid electrolyte, a conductive assistant, etc. The negative electrode body contains 0.850 to 5.000 mass% Al with respect to the total mass of the negative electrode body, and the Si particles contain 0.040 to 0.250 mass% Al with respect to the total mass of the Si particles.
[0015] When a Si particle having a clathrate structure contains 0.040 to 0.250 mass % Al relative to the total mass of the Si particle, it is believed that the skeletal size of the crystal structure of the Si particle becomes large, and the expansion and contraction of the Si particle itself caused by the introduction of lithium into the cage structure portion of the clathrate structure during charging of the battery is suppressed.
[0016] The Si particles having a clathrate structure may contain Al in an amount of 0.040 mass% or more, 0.060 mass% or more, 0.080 mass% or more, or 0.100 mass% or more, and may contain Al in an amount of 0.250 mass% or less, 0.240 mass% or less, 0.200 mass% or less, or 0.180 mass% or less, based on the total mass of the Si particles.
[0017] When the amount of Al contained in the Si particles is 0.04 mass% or more, the effect of reducing the confining pressure is sufficiently obtained. On the other hand, when the amount of Al contained in the Si particles is 0.250 mass% or less, the reduction ratio of the Si portion of the clathrate structure to the total mass of the Si particles due to the Al content is sufficiently small, and the impact on the energy efficiency per mass of the battery is sufficiently small.
[0018] From the viewpoint of reducing the confining pressure, it is particularly preferable that the amount of Al contained in the Si particles is 0.080 mass % or more based on the total mass of the Si particles.
[0019] In the negative electrode body of the present disclosure, when the Si particles having a clathrate structure contain 0.040 to 0.250 mass % Al with respect to the total mass of the Si particles and the negative electrode active material layer contains 0.850 to 5.000 mass % Al with respect to the total mass of the negative electrode active material layer, Al is not only contained in the Si particles but also present in a predetermined amount in parts of the negative electrode active material layer other than the Si particles as the negative electrode active material.
[0020] Examples of Al present in the negative electrode active material other than Si particles include Al-containing particles and metallic Al, and these may function as a bridge to suppress damage / pulverization of Si particles as an active material due to fluctuations in confining pressure associated with pressing during the manufacture of the negative electrode body and / or battery and with charging / discharging of the battery.
[0021] The negative electrode active material layer may contain Al in an amount of 0.850 mass% or more, 1.000 mass% or more, 1.50 mass% or more, or 2.000 mass% or more, and may contain Al in an amount of 5.000 mass% or less, 4.800 mass% or less, 3.500 mass% or less, or 2.500 mass% or less, based on the total mass of the negative electrode active material layer.
[0022] When the amount of Al contained in the negative electrode active material layer is 0.850 mass% or more, the effect of reducing the confining pressure is particularly large. On the other hand, when the amount of Al contained in the negative electrode active material layer is 5.000 mass% or less, the amount of Si particles relative to the total mass of the negative electrode active material layer increases, and the energy efficiency per mass of the battery increases.
[0023] From the viewpoint of reducing the confining pressure, the amount of Al contained in the negative electrode active material layer is particularly preferably 1.500 mass % or more with respect to the total mass of the negative electrode active material layer.
[0024] Without being limited by principle, as described above, in a lithium ion battery constructed using the negative electrode body of the present disclosure, particularly a lithium ion solid state battery having a configuration in which a positive electrode body, a solid electrolyte layer, and the negative electrode body of the present disclosure are stacked in this order, expansion and contraction of the Si particles themselves is suppressed, and damage / crushing, etc. of the Si particles during manufacture of the lithium ion battery or during charging and discharging of the lithium ion battery is suppressed, and therefore it is believed that fluctuations in the confining pressure of the battery due to charging and discharging are reduced.
[0025] The amount of Al (mass %) relative to the total mass of the negative electrode active material layer and the amount of Al (mass %) relative to the total mass of the Si particles can be measured by a conventionally known method such as energy dispersive X-ray spectroscopy (EDX), ICP, GDOES, or XRF.
[0026] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, the material may be stainless steel (SUS), aluminum, copper, nickel, iron, titanium, carbon, a resin current collector, or the like, but is not limited to these.
[0027] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0028] <Negative electrode active material layer> The negative electrode active material layer contains Si particles as a negative electrode active material. The negative electrode active material layer further contains an Al-containing component in addition to the Si particles. The negative electrode active material layer may optionally contain a solid electrolyte, a conductive assistant, and a binder.
[0029] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the Si particles to the solid electrolyte in the negative electrode active material layer (mass of Si particles:mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0030] (Si particles) The Si particles have a clathrate structure.
[0031] The clathrate structure may be a clathrate II structure, because Si having a clathrate II structure can absorb more lithium in its internal cage structure than a clathrate I structure, and tends to expand and contract less during charging and discharging.
[0032] The Si particles may have both clathrate I and clathrate II moieties.
[0033] The mass ratio of the clathrate II type structure portion to the entire Si particles may be 50.00 to 99.05 mass%. The mass ratio of the clathrate II type structure portion to the entire Si particles may be 50.00 mass% or more, 60.00 mass% or more, 70.00 mass% or more, or 80.00 mass% or more, and may be 99.05 mass% or less, 98.00 mass% or less, 95.00 mass% or less, or 90.00 mass% or less.
[0034] More preferably, the Si particles have a porous structure.
[0035] The presence or absence of a porous structure may be confirmed, for example, from an image obtained by a scanning electron microscope (SEM) or the like.
[0036] The porous structure may be a structure having a plurality of pores, more specifically, a nanoporous structure, a mesoporous structure, or a macroporous structure. The nanoporous structure is a porous structure having a pore distribution of, for example, 0.5 to 2.0 nm. The mesoporous structure is a porous structure having a pore distribution of, for example, 2.0 to 50.0 nm. The macroporous structure is a porous structure having a pore distribution of, for example, 50.0 to 1000.0 nm. The pore distribution of Si particles is, for example, 2 It can be measured by gas adsorption method, etc.
[0037] The average particle size (D50) of the Si particles is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the Si particles is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0038] (Components containing Al) The Al-containing component may be, for example, Al-containing particles and / or metallic Al.
[0039] When the component containing Al is an Al-containing particle, the component may be an Al-containing particle that is electrochemically inactive under the operating voltage of a lithium ion battery. Examples of such Al-containing particles include particles that further contain F and / or O in addition to Al, more specifically, AlF 3 Or Al 2 O 3 These include, but are not limited to:
[0040] When the component containing Al is an Al-containing particle, the average particle size (D50) of the Al-containing particle is not particularly limited, but may be, for example, 10 nm or more, and may be, for example, 100 nm or more. On the other hand, the average particle size (D50) of the Al-containing particle is, for example, 50 μm or less, and may be, for example, 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0041] (solid electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in a lithium ion battery can be used. For example, the solid electrolyte may be, but is not limited to, a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer electrolyte.
[0042] Examples of sulfide solid electrolytes include, but are not limited to, sulfide-based amorphous solid electrolytes, sulfide-based crystalline solid electrolytes, and argyrodite-type solid electrolytes.
[0043] As a specific example of a sulfide solid electrolyte, Li 2 SP 2 S 5 System (Li 7 P 3 S 11 , Li 3 P.S. 4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -GeS 2 (Li 13 GeP 3 S 16 , Li 10 GeP2 S 12 etc.), LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.
[0044] An example of an oxide solid electrolyte is Li 7 La 3 Zr 2 O 12、 Li 7-x La 3 Zr 1-x Nb x O 12、 Li 7-3x La 3 Zr 2 Al x O 12 , Li 3x La 2 / 3-x TiO 3 , Li 1+x Al x Ti 2-x (PO 4 ) 3 , Li 1+x Al x Ge 2-x (PO 4 ) 3 , Li 3 PO 4 , or Li 3+x PO 4-x N x (LiPON), but is not limited to these.
[0045] The sulfide solid electrolyte and the oxide solid electrolyte may be glass or crystallized glass (glass ceramic).
[0046] Examples of the polymer electrolyte include, but are not limited to, polyethylene oxide (PEO), polypropylene oxide (PPO), and copolymers thereof.
[0047] (Conductive assistant) The conductive additive is not particularly limited. For example, the conductive additive may be a carbon material such as VGCF (Vapor Grown Carbon Fiber), Ketjen Black (KB), Acetylene Black (AB), and carbon nanofiber, or a metal material, but is not limited thereto.
[0048] (Binder) The binder is not particularly limited. For example, the binder may be, but is not limited to, a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), or styrene butadiene rubber (SBR), or a combination thereof.
[0049] Lithium-ion battery The lithium ion battery of the present disclosure may have, in this order, the electrode assembly of the present disclosure as a negative electrode assembly, a solid electrolyte layer, and a positive electrode assembly layer.
[0050] FIG. 1 is a schematic diagram of a lithium-ion battery 1 according to a first embodiment of the present disclosure.
[0051] As shown in FIG. 1, a lithium ion battery 1 according to the first embodiment of the present disclosure includes an anode electrode body 10 of the present disclosure, a solid electrolyte layer 20 as an electrolyte layer, and a cathode electrode body 30, in this order. Here, the anode electrode body 10 is composed of an anode current collector layer 12 and an anode active material layer 11. Here, the anode current collector layer 12 and the anode active material layer 11 are stacked on each other such that the anode active material layer 11 is in contact with the solid electrolyte layer 20. Similarly, the cathode electrode body 30 is composed of an anode current collector layer 12 and an anode active material layer 11. Here, the cathode current collector layer 32 and the cathode active material layer 31 are stacked on each other such that the cathode active material layer 31 is in contact with the solid electrolyte layer 20.
[0052] The lithium ion battery of the present disclosure may be restrained by restraining members from both sides in the stacking direction, i.e., the direction in which the negative electrode body, electrolyte layer, and positive electrode body layer of the present disclosure are stacked. The restraining members may be, for example, end plates or other restraining members commonly used in lithium ion batteries.
[0053] <Negative electrode body> The lithium ion battery of the present disclosure has the negative electrode assembly of the present disclosure.
[0054] The negative electrode active material layer of the negative electrode body has a thickness of, for example, 0.1 to 1000 μm. The thickness of the negative electrode active material layer is particularly preferably 1 to 100 μm, and further preferably 30 to 100 μm.
[0055] <Solid electrolyte layer> The solid electrolyte layer includes at least a solid electrolyte. The solid electrolyte layer may include a binder, etc., if necessary, in addition to the solid electrolyte. For the solid electrolyte and the binder, the description of the solid electrolyte and the binder in the above "<Negative electrode active material layer>" can be referred to.
[0056] The solid electrolyte layer may be a layer in which a sheet of resin such as polypropylene is impregnated with an electrolyte solution having lithium ion conductivity.
[0057] The electrolyte preferably contains a supporting salt and a solvent. Examples of the supporting salt (lithium salt) of the electrolyte having lithium ion conductivity include LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 Inorganic lithium salts such as LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(FSO 2 )2 , LiC(CF 3 SO 2 ) 3 Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.
[0058] The thickness of the solid electrolyte layer is, for example, 0.1 to 1000 μm. The thickness of the solid electrolyte layer is preferably 0.1 to 300 μm, and particularly preferably 0.1 to 100 μm.
[0059] <Positive electrode body> The positive electrode body of the present disclosure has at least a positive electrode current collector and a positive electrode active material layer. Another layer may be interposed between the positive electrode current collector and the positive electrode active material layer. The thickness of the positive electrode active material layer of the positive electrode body is, for example, 0.1 to 1000 μm. The thickness of the positive electrode active material layer is particularly preferably 1 to 100 μm, and more preferably 30 to 100 μm.
[0060] (Positive electrode current collector layer) The material and shape of the positive electrode current collector layer are not particularly limited, and the materials and shapes described in the above "Negative electrode current collector layer" may be used. In particular, the material of the positive electrode current collector layer is preferably aluminum. The shape is preferably a foil.
[0061] (Cathode active material layer) The positive electrode active material layer is a layer containing a positive electrode active material, and optionally a solid electrolyte, a conductive assistant, a binder, and the like.
[0062] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0063] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganate (LiMn 2 O 4 ), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li 1+x Mn 2-x-y M y O 4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), or the like, but is not limited thereto.
[0064] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials that constitute the coating layer include LiNbO 3 In addition, Li 4 Ti 5 O 12 , Li 3 PO 4 These include, but are not limited to, the following.
[0065] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0066] For the solid electrolyte, the conductive assistant, and the binder, reference can be made to the above description regarding "<Electrode active material layer>".
[0067] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.
[0068] <Method for producing active material for lithium-ion batteries> The manufacturing method of the present disclosure is a method for manufacturing an active material for a lithium ion battery. The manufacturing method of the present disclosure is a method for manufacturing an active material for a lithium ion battery. 3 and heating the mixture to obtain a mixture containing Si particles having a clathrate structure, NaF, and Al-containing particles, and the mixture is then heated with HNO 3 washing with an aqueous solution followed by filtering and drying; It has.
[0069] NaSi alloy powder and AlF 3 When mixed and heated at a given temperature for a given time, AlF 3 functions as a sodium trapping agent, sodium is released from the NaSi alloy, and Si particles having a clathrate structure, particularly a clathrate II structure, are generated.
[0070] Heating to obtain Si particles having a clathrate structure may be performed at a heating temperature of 250 to 500° C. for a heating time of 30 to 200 hours in an atmosphere inert to Si and Na, for example, a rare gas atmosphere, more specifically, an Ar atmosphere.
[0071] The heating temperature may be 250° C. or more, 300° C. or more, or 350° C. or more, and may be 500° C. or less, 450° C. or less, 400° C. or less, or 350° C. or less.
[0072] The heating time may be 30 hours or more, 40 hours or more, 50 hours or more, or 100 hours or more, and may be 200 hours or less, 180 hours or less, 160 hours or less, or 100 hours or less.
[0073] AlF 3 The average particle size (D50) is not particularly limited, and may be, for example, 10 to 500 μm. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).
[0074] NaSi alloy and AlF 3 The mixing ratio is the molar ratio (NaSi alloy:AlF 3 ) may be 1:0.100 to 1:0.500. This molar ratio (NaSi alloy:AlF 3 ) may be 1:0.150 to 1:0.400, or 1:0.200 to 1:0.3400.
[0075] In the manufacturing method of the present disclosure, the NaSi alloy powder may be obtained by mechanically milling Si powder and NaH powder, followed by heating. The heating may be performed, for example, at a heating temperature of 250 to 500°C for a heating time of 30 to 200 hours in an atmosphere inert to Si and Na, for example, in a rare gas atmosphere, more specifically, in an Ar atmosphere.
[0076] The heating temperature may be 250° C. or more, 300° C. or more, or 350° C. or more, and may be 500° C. or less, 450° C. or less, 400° C. or less, or 350° C. or less.
[0077] The heating time may be 30 hours or more, 40 hours or more, 50 hours or more, or 100 hours or more, and may be 200 hours or less, 180 hours or less, 160 hours or less, or 100 hours or less.
[0078] The primary particles of the Si powder may have a porous structure.
[0079] A Si powder in which the primary particles have a porous structure can be obtained, for example, by mixing a Si powder raw material with Li in an atmosphere inert to Si and Li, for example, in a rare gas atmosphere, more specifically, in an Ar atmosphere, to obtain a LiSi alloy compound, and then reacting this with, for example, ethanol to remove the Li. EXAMPLES
[0080] Examples 1 to 5 and Comparative Example 1 Example 1 (Synthesis of Si particles) As a Si source, a Si powder (a Si powder having no voids inside the primary particles) was prepared. This Si source and Li metal were weighed out in a molar ratio of Li / Si=4.75 and mixed in a mortar in an Ar atmosphere to obtain an alloy compound. The obtained alloy compound was reacted with ethanol in an Ar atmosphere to obtain a Si powder having voids inside the primary particles, i.e., a porous structure.
[0081] The obtained Si powder and NaH as a Na source were used to produce a NaSi alloy. The NaH used was washed with hexane in advance. The Na source and the Si source were weighed out to a molar ratio of 1.05:1.00, and mixed using a cutter mill. The mixture was heated in a heating furnace under an Ar atmosphere at 400°C for 40 hours to obtain a powdered NaSi alloy.
[0082] The obtained NaSi alloy and AlF 3 The reactants were weighed out to a molar ratio of 1.000:0.200 and mixed using a cutter mill to obtain a reactant. The reactant was placed in a stainless steel reaction vessel and heated in a heating furnace under an Ar atmosphere at 290°C for 120 hours to cause a reaction.
[0083] The reaction product was dissolved in HNO 3 and H 2 The solid matter was dried at 120° C. for 3 hours or more to obtain a powder containing Si particles, Al-containing particles, etc.
[0084] The crystal structure of the obtained Si particles was measured by X-ray crystal diffraction and found to have a clathrate II type structure.
[0085] (Formation of negative electrode body) The polypropylene container was filled with butyl butyrate, a 5 wt% butyl butyrate solution of polyvinylidene fluoride (PVDF) binder, vapor grown carbon fiber (VGCF) as a conductive additive, powder containing synthesized Si particles and Al-containing particles, and Li as a sulfide solid electrolyte. 2 SP 2 S 5 The glass ceramic was added and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.) Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a negative electrode composite slurry.
[0086] The negative electrode mixture was applied onto a Cu foil by a blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100° C. to obtain a negative electrode body.
[0087] (Formation of solid electrolyte layer) A polypropylene container was filled with heptane, a 5 wt% heptane solution of butylene rubber (BR)-based binder, and Li as a sulfide solid electrolyte. 2 SP 2 S 5 The glass ceramic was added and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.) Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry.
[0088] The solid electrolyte slurry was applied onto an Al foil serving as a release sheet by a blade method using an applicator, and dried on a hot plate heated to 100° C. for 30 minutes to form a solid electrolyte layer.
[0089] Three solid electrolyte layers were fabricated.
[0090] (Formation of positive electrode body) A polypropylene container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi with an average particle size of 6 μm as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O 2, Li as sulfide solid electrolyte 2 SP 2 S 5 The glass ceramic and VGCF as a conductive additive were added to the container, and the mixture was stirred for 30 seconds using an ultrasonic disperser (UH-50 manufactured by SMT).
[0091] Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.), further stirred with an ultrasonic dispersing device for 30 seconds, and then shaken with the shaker for 3 minutes to obtain a positive electrode composite slurry.
[0092] The positive electrode mixture slurry was applied onto an Al foil by a blade method using an applicator, and dried for 30 minutes on a hot plate heated to 100° C. to form a positive electrode body.
[0093] (Battery Assembly) The positive electrode body and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. to obtain a positive electrode laminate.
[0094] The negative electrode body and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. to obtain a negative electrode laminate.
[0095] Furthermore, the Al foil as a release sheet was peeled off from the surfaces of the solid electrolyte layers of the positive electrode laminate and the negative electrode laminate, and then the Al foil as a release sheet was peeled off from the third solid electrolyte layer.
[0096] The positive electrode laminate and the negative electrode laminate were laminated on each other so that the solid electrolyte layer sides of each were facing the third solid electrolyte layer, and the laminate was set in a flat uniaxial press and pre-pressed at 100 MPa and 25° C. for 10 seconds, and finally the laminate was set in a flat uniaxial press and pressed for 1 minute at a pressure of 200 MPa and a press temperature of 120° C. This produced an all-solid-state battery.
[0097] Example 2 NaSi alloy and AlF 3 The Si particles of Example 2 were obtained in the same manner as in Example 1, except that the heating conditions were changed to 310° C. and 60 hours. Using these Si particles, an all-solid-state battery was obtained in the same manner as in Example 1.
[0098] Example 3 NaSi alloy and AlF 3 The Si particles of Example 3 were obtained in the same manner as in Example 2, except that the molar ratio of was 1.000:0.210. Using these Si particles, an all-solid-state battery was obtained in the same manner as in Example 2.
[0099] Example 4 NaSi alloy and AlF 3 The molar ratio of AlF to AlF was 1.000:0.336, and fine particles were removed using a metal sieve (mesh size 20 μm). 3 The Si particles of Example 4 were obtained in the same manner as in Example 2, except that the above was used. An all-solid-state battery was obtained in the same manner as in Example 2 using these Si particles.
[0100] Example 5 NaSi alloy and AlF 3 The Si particles of Example 5 were obtained in the same manner as in Example 2, except that the molar ratio of was 1.000:0.336. Using these Si particles, an all-solid-state battery was obtained in the same manner as in Example 2.
[0101] Comparative Example 1 Si particles were used as the Si source, and Na particles were used as the Na source. The Si particles and Na particles were mixed in a molar ratio of 1:1, placed in a crucible, sealed under an Ar atmosphere, and heated at 700°C to obtain a NaSi alloy. The obtained NaSi alloy was heated under vacuum (about 1 Pa) and 340°C to remove Na, and an intermediate having a silicon clathrate II crystal phase was obtained. The obtained intermediate and Li metal were weighed in a molar ratio of Li / Si=1.7 and mixed in a mortar in an Ar atmosphere to obtain an alloy compound. The obtained alloy compound was reacted with ethanol in an Ar atmosphere to obtain Si particles with voids formed inside the primary particles.
[0102] An all-solid-state battery was obtained in the same manner as in Example 1 using the obtained Si particles.
[0103] <Measurement of Al content> The Al amount (mass %) in the negative electrode active material layer similar to that formed during the production of the all-solid-state battery of each example was measured by SEM-EDX, and the Al amount (mass %) in the Si particles was measured by TEM-EDX.
[0104] <Measurement of confining pressure fluctuation> The all-solid-state battery of each example was restrained at a predetermined restraining pressure using a restraining jig, and the amount of restraining pressure fluctuation was measured when the battery was charged at a constant current and constant voltage at a 10-hour rate (1 / 10C) up to 4.55 V. The amount of restraining pressure fluctuation is the difference between the maximum and minimum values of the restraining pressure.
[0105] <result> The manufacturing conditions of the Si particles used in the all-solid-state batteries of each example, the Al content (mass%) in the Si particles, and Negative electrode active material layer The Al content (mass%) in the negative electrode active material layer and the amount of change in the confining pressure during charging and discharging are shown in Table 1. Electron images of the negative electrode active material layer of Example 2 measured by SEM-EDX are shown in Figs. 2 to 5. 3 "Classification by metal sieve" indicates the presence or absence of classification using a metal sieve and the mesh size of the metal sieve. The fluctuation amount of the confining pressure is a relative value with the value in Comparative Example 1 taken as 100.
[0106] [Table 1]
[0107] As shown in Table 1, the Al content in the Si particles is 0.043 mass%. Negative electrode active material layer The all-solid-state battery of Example 1, in which the Al content was 0.850 mass %, exhibited a smaller change in confining pressure during charging and discharging than the all-solid-state battery of Comparative Example 1. Specifically, the change in confining pressure was 84% of the change in confining pressure in Comparative Example 1.
[0108] Similarly, the all-solid-state batteries of Examples 2 to 5 also showed a smaller fluctuation in confining pressure during charging and discharging than the all-solid-state battery of Comparative Example 1.
[0109] In addition, the Al content and Negative electrode active material layer The Al content in the powder is considered to be the amount of Al contained as an impurity in the raw materials such as silicon powder.
[0110] Fig. 2 is an SEM image of the negative electrode active material layer. Fig. 3 shows the distribution of O, Fig. 4 shows the distribution of Al, and Fig. 5 shows the distribution of F. As shown in Figs. 2 to 5, the Al element in the negative electrode active material layer is detected at the same position as the O element as in (1), or at the same position as the F element as in (2). In other words, it can be said that the negative electrode active material layer of Example 2 contains particles containing Al and O, and particles containing Al and F. In addition, stable substances containing Al and O elements are Al. 2 O 3 The most stable substance containing Al and F is AlF 3 Therefore, the negative electrode active material layer of Example 2 is Al 2 O 3 and AlF 3 It is believed that this includes: [Explanation of symbols]
[0111] 1 Lithium-ion battery 10 Negative electrode body 11 Negative electrode active material layer 12 Negative electrode current collector layer 20 Solid electrolyte layer 30 Positive electrode body 31 Positive electrode active material layer 32 Positive electrode current collector layer
Claims
1. A negative electrode assembly for a lithium ion battery having a negative electrode current collector layer and a negative electrode active material layer, The negative electrode active material layer contains Si particles having a clathrate structure as a negative electrode active material, The negative electrode active material layer contains 0.850 to 5.000 mass% of Al relative to the mass of the negative electrode active material layer, and The Si particles contain 0.040 to 0.250 mass% Al relative to the mass of the Si particles. Negative electrode body.
2. The negative electrode body contains 1.500 mass % or more of Al with respect to the total mass of the negative electrode active material layer, and The Si particles contain 0.080 mass% or more of Al relative to the mass of the Si particles. The negative electrode assembly according to claim 1 .
3. 3. The negative electrode body according to claim 1, wherein the negative electrode active material layer contains Al-containing particles that are electrochemically inactive under a voltage used in a lithium ion battery.
4. The negative electrode body according to claim 3 , wherein the Al-containing particles contain F or O.
5. The Al-containing particles are AlF 3 Or Al 2 O 3 The negative electrode body according to claim 3 ,
6. The negative electrode body according to claim 1 , wherein the Si particles have a porous structure.
7. The negative electrode body according to claim 1 , wherein the Si particles have a clathrate II structure.
8. A lithium ion battery comprising the negative electrode body according to claim 7, a solid electrolyte layer, and a positive electrode body stacked in this order.
9. NaSi alloy and AlF 3 and heating the mixture to obtain a mixture containing Si particles having a clathrate structure, NaF, and Al-containing particles; and The mixture was mixed with HNO 3 washing with an aqueous solution followed by filtering and drying; It has A method for producing active materials for lithium-ion batteries.
10. 10. The method of claim 9, comprising mechanically milling Si powder and NaH powder, followed by heating to obtain the NaSi alloy.
Citation Information
Patent Citations
Active material, negative electrode layer, battery and these manufacturing methods
JP2021158003A
Active material, battery, and manufacturing method thereof
JP2021192348A
Method for producing negative electrode active material
JP2022034998A