Solid-state battery and method for manufacturing the same
The solid-state battery design with high confining pressures and specific void and surface roughness configurations addresses the fusion and resistance issues in alloy-based negative electrodes, enhancing battery performance by reducing resistance and improving durability.
Patent Information
- Application Number
- JP2022570042
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-10
- Filing Date
- 2021-12-15
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-12-15
AI Technical Summary
When using an alloy-based negative electrode active material in solid-state batteries, low confining pressure during the initial charging process hinders the fusion of the negative electrode active material, leading to difficulty in charging and discharging and increased resistance.
A solid-state battery design with a negative electrode layer containing alloy-based active materials, where voids in the stacking direction account for more than 36% by volume, and initial charging is performed under high confining pressures of 30 MPa or more at the start and 40 MPa or more at the end, along with a negative electrode current collector surface roughness of 0.8 μm to 4.0 μm, promoting fusion and reducing resistance.
The design effectively suppresses the increase in resistance rate by promoting fusion and rearrangement of negative electrode active materials, reducing the impact of voids on electron and ion paths, and enhancing battery durability.
Smart Images

Figure 0007578722000009 
Figure 0007578722000010 
Figure 0007578722000011
Abstract
Description
[Technical field]
[0001] This application relates to solid-state batteries. [Background technology]
[0002] Conventionally, when manufacturing an all-solid-state battery, charging is performed after the battery is assembled. At this time, there is a technique for charging the battery while applying a predetermined pressure to the battery from the viewpoint of improving the battery performance.
[0003] For example, Patent Document 1 discloses a technique for applying a confining pressure of 0.1 MPa to 10 MPa in a constant voltage charging process of an all-solid-state battery from the viewpoint of improving cycle characteristics. Patent Document 2 discloses a technique for charging a battery stack at an initial charging voltage while confining the battery stack at a constant pressure in the stacking direction of the layers constituting the unit cells from the viewpoint of suppressing deterioration of the all-solid-state battery and improving the energy density. Patent Document 3 discloses a technique for sealing a battery stack in a bag-shaped container and then performing preliminary charging and discharging at least once under a predetermined pressure from the viewpoint of improving the contact state of the solid / solid interface and improving the charge / discharge performance under atmospheric pressure. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-81790 A [Patent Document 2] JP 2020-107389 A [Patent Document 3] JP 2010-272210 A Summary of the Invention [Problem to be solved by the invention]
[0005] The inventors have found that when an alloy-based negative electrode active material is used in the negative electrode layer of a solid-state battery, if the battery restraining pressure in the initial charging process is low, fusion of the negative electrode active material is not promoted, and the rate of increase in resistance due to charging and discharging during actual use becomes extremely high.
[0006] In view of the above, an object of the present disclosure is to provide a solid-state battery capable of suppressing an increase in the rate of increase in resistance, and to provide a method for manufacturing the solid-state battery. [Means for solving the problem]
[0007] As one means for solving the above problems, the present application discloses a solid-state battery having a laminate including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer containing an alloy-based negative electrode active material, in which the voids in the stacking direction of the negative electrode layer account for more than 36 volume % of the total voids in the negative electrode layer.
[0008] In the solid-state battery, the voids in the stacking direction may account for 55% by volume or more and 100% by volume or less of the total voids in the negative electrode layer.
[0009] In the solid-state battery, the alloy-based negative electrode active material may contain silicon.
[0010] In the solid-state battery, the silicon may be in the form of particles.
[0011] In the solid-state battery, the particle size D50 of the silicon particles can be set to 1 μm or less.
[0012] In the solid-state battery, silicon may be a thin film.
[0013] In the solid-state battery, the solid electrolyte layer may include a sulfide solid electrolyte.
[0014] In the solid-state battery, the negative electrode layer may further include a negative electrode current collector, and the negative electrode current collector may have a surface roughness Rz of 0.8 μm or more and 4.0 μm or less.
[0015] As one means for solving the above problems, the present application provides a method for manufacturing a solid-state battery, the method comprising: a preparation step of preparing a laminate including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer; and an initial charging step of constraining the laminate in a stacking direction and performing an initial constant-current, constant-voltage charging of the laminate, wherein in the initial charging step, the constraining pressure of the laminate at the start of charging is 30 MPa or more and the constraining pressure of the laminate at the end of charging is 40 MPa or more.
[0016] In the method for producing a solid-state battery, after the initial filling step, the laminate may be restrained under a restraining pressure of 10 MPa or less.
[0017] In the above-described method for producing a solid-state battery, the negative electrode layer may contain an alloy-based negative electrode active material, and the alloy-based negative electrode active material may contain silicon.
[0018] In the method for producing a solid-state battery, the silicon may be in the form of particles.
[0019] In the above method for producing a solid-state battery, the particle size D50 of the silicon particles can be set to 1 μm or less.
[0020] In the method for producing a solid-state battery, silicon may be a thin film.
[0021] In the above-mentioned method for producing a solid-state battery, the solid electrolyte layer may contain a sulfide solid electrolyte.
[0022] In the above-mentioned method for producing a solid-state battery, the negative electrode layer may further include a negative electrode current collector, and the negative electrode current collector may have a surface roughness Rz of 0.8 μm or more and 4.0 μm or less. Effect of the Invention
[0023] According to the present disclosure, it is possible to provide a solid-state battery capable of suppressing an increase in the resistance increase rate. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a flow chart of a manufacturing method 10. [Diagram 2] FIG. 2 is a cross-sectional image of a negative electrode layer including a negative electrode mixture layer (Test A1). [Diagram 3] FIG. 3 is a cross-sectional image of the negative electrode layer including the negative electrode thin film layer (Test A7). [Figure 4] FIG. 4 is a graph showing the relationship between the confining pressure at the end of the first charge and the relative resistance increase rate for Tests A1 to A3 and Tests B1 and B2. [Diagram 5] FIG. 5 is a diagram showing the relationship between Rz and the relative resistance increase rate for Tests A11 to A13 and Tests B11 and B12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] 1. Manufacturing method of solid-state batteries The manufacturing method of the solid-state battery of the present disclosure will be described with reference to a manufacturing method S10 of an all-solid-state battery according to one embodiment (hereinafter, sometimes simply referred to as "manufacturing method S10"). Note that a solid-state battery means a battery that includes a solid electrolyte, and an all-solid-state battery means a solid-state battery that does not include a liquid-based material. FIG. 1 shows a flowchart of the manufacturing method S10. As shown in FIG. 1, the manufacturing method S10 includes a preparation step S11 and an initial charging step S12. Each step will be described below.
[0026] 1.1. Preparation process S11 The preparation step S11 is a step of preparing a laminate in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer containing an alloy-based negative electrode active material are laminated in this order.
[0027] 1.1.1.Positive electrode layer The positive electrode layer includes a positive electrode mixture layer. The positive electrode layer may include a positive electrode current collector on the surface opposite to the surface on which the solid electrolyte layer is laminated.
[0028] The positive electrode mixture layer contains a positive electrode active material. The positive electrode active material is not particularly limited as long as it is a positive electrode active material that can be used in a lithium ion all-solid-state battery. For example, lithium cobalt oxide, lithium nickel cobalt aluminum oxide (NCA-based active material), LiNi 1 / 3 Co 1 / 3 Mn1 / 3 Examples of the positive electrode active material include lithium nickel oxide, lithium manganate, and spinel-based lithium compounds. Among them, it is preferable to use lithium nickel oxide as the positive electrode active material. The particle size of the positive electrode active material is not particularly limited, but is, for example, in the range of 5 μm to 50 μm. The content of the positive electrode active material in the positive electrode mixture layer is, for example, in the range of 50% by weight to 99% by weight. In addition, the surface of the positive electrode active material may be covered with an oxide layer such as a lithium niobate layer, a lithium titanate layer, or a lithium phosphate layer.
[0029] In this specification, the term "particle size" refers to the particle size at 50% cumulative value (D50) in the volume-based particle size distribution measured by a laser diffraction / scattering method.
[0030] The positive electrode mixture layer may optionally include a solid electrolyte. Examples of the solid electrolyte include an oxide solid electrolyte and a sulfide solid electrolyte. A sulfide solid electrolyte is preferable. The oxide solid electrolyte is Li7La3Zr2O 12 , Li 7-x La3Zr 1-x Nb x O 12 , Li 7-3x La3Zr2Al x O 12 , Li 3x La 2 / 3-x TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+x Al x Ge 2-x (PO4)3, Li3PO4, or Li 3+x PO 4-x N x (LiPON), etc. Examples of sulfide solid electrolytes include Li3PS4, Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, and Li2S-P2S5-GeS2. The content of the solid electrolyte in the positive electrode mixture layer is not particularly limited, but is, for example, in the range of 1% by weight to 50% by weight.
[0031] The positive electrode mixture layer may optionally include a conductive assistant. Examples of the conductive assistant include carbon materials such as acetylene black, ketjen black, and vapor grown carbon fiber (VGCF), and metal materials such as nickel, aluminum, and stainless steel. The content of the conductive assistant in the positive electrode mixture layer is not particularly limited, but is, for example, in the range of 0.1% by weight to 10% by weight.
[0032] The positive electrode mixture layer may optionally include a binder. Examples of binders include butadiene rubber (BR), butylene rubber (IIR), acrylate butadiene rubber (ABR), polyvinylidene fluoride (PVdF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), etc. The content of the binder in the positive electrode mixture layer is not particularly limited, but is, for example, in the range of 0.1% by weight to 10% by weight.
[0033] The thickness of the positive electrode mixture layer is not particularly limited and may be appropriately set according to the desired battery performance, for example, in the range of 0.1 μm to 1 mm.
[0034] The positive electrode current collector is disposed on the surface opposite to the surface on which the solid electrolyte layer is laminated of the positive electrode composite layer. The material of the positive electrode current collector is not particularly limited, and can be appropriately selected from known materials according to the purpose. For example, Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, etc. can be mentioned. The thickness of the positive electrode current collector is not particularly limited, and can be appropriately set according to the desired battery performance. For example, it is in the range of 0.1 μm to 1 mm.
[0035] The method for producing the positive electrode layer is not particularly limited, and the positive electrode layer can be produced by a known method. For example, the positive electrode layer can be produced by mixing the materials constituting the positive electrode mixture layer with a solvent to form a slurry, applying the slurry to a substrate or a positive electrode current collector, and drying the slurry.
[0036] 1.1.2.Solid electrolyte layer The solid electrolyte layer includes a solid electrolyte. The type of the solid electrolyte may be the same as that of the solid electrolyte used in the positive electrode layer. The solid electrolyte layer may include, for example, a sulfide solid electrolyte. The sulfide solid electrolyte is relatively soft and easily absorbs the volume change caused by the construction of the negative electrode structure in the initial activation. The content of the solid electrolyte in the solid electrolyte layer is, for example, in the range of 50% by weight to 99% by weight.
[0037] The solid electrolyte layer may optionally include a binder. The type of binder may be the same as that used in the positive electrode layer. The content of the binder in the solid electrolyte layer is not particularly limited, but is, for example, in the range of 0.1% by weight to 10% by weight.
[0038] The method for producing the solid electrolyte layer is not particularly limited, and the solid electrolyte layer can be produced by a known method. For example, the solid electrolyte layer can be produced by mixing the materials constituting the solid electrolyte layer with a solvent to form a slurry, applying the slurry to a substrate, and drying the substrate.
[0039] 1.1.3. Negative electrode layer The negative electrode layer includes a negative electrode mixture layer or a negative electrode thin film layer. The negative electrode layer may include a negative electrode current collector on the surface opposite to the surface on which the solid electrolyte layer is laminated.
[0040] The negative electrode mixture layer includes an alloy-based negative electrode active material. The alloy-based negative electrode active material is a metal element capable of bonding with Li, specifically, Si, Sn, Al, Mg, C, Al, Ge, Sb, In, Cu, Mn, or an oxide thereof. Preferably, it is Si or Sn, or an oxide thereof. More preferably, it is Si or an oxide of Si. The negative electrode active material is preferably in a particle shape, and more preferably, its particle size is 1 μm or less. As the particle size of the negative electrode active material becomes smaller, the inactive interface (interface between negative electrode active material and negative electrode active material) in the negative electrode mixture layer increases, while the inactive interface is reduced by fusion between the negative electrode active materials due to charging. The effect of reducing the inactive interface becomes significantly larger when the particle size of the negative electrode active material is 1 μm or less, and as a result, the increase in the resistance increase rate can be suppressed. The content of the negative electrode active material in the negative electrode mixture layer is, for example, in the range of 30% by weight to 90% by weight.
[0041] The negative electrode mixture layer may optionally include a solid electrolyte. The solid electrolyte may be the same type as the solid electrolyte used in the positive electrode layer. The content of the solid electrolyte in the negative electrode mixture layer is not particularly limited, but is, for example, in the range of 10% by weight to 70% by weight.
[0042] The negative electrode mixture layer may optionally contain a conductive assistant. The conductive assistant may be the same type as the conductive assistant used in the positive electrode layer. The content of the conductive assistant in the negative electrode mixture layer is not particularly limited, but is, for example, in the range of 0.1% by weight to 20% by weight.
[0043] The negative electrode mixture layer may optionally include a binder. The binder may be the same type as the conductive assistant used in the positive electrode layer. The content of the binder in the negative electrode mixture layer is not particularly limited, but is, for example, in the range of 0.1% by weight to 10% by weight.
[0044] The thickness of the negative electrode mixture layer is not particularly limited and may be appropriately set according to the desired battery performance, for example, in the range of 0.1 μm to 1 mm.
[0045] The negative electrode thin film layer is a thin film containing an alloy-based negative electrode active material. The content of the alloy-based negative electrode active material in the negative electrode thin film layer is preferably 90% by weight or more, more preferably 95% by weight or more, and particularly preferably 100% by weight (consisting of the alloy-based negative electrode active material). The types of alloy-based negative electrode active material that can be used are as described above. The thickness of the negative electrode thin film layer is not particularly limited. For example, it is in the range of 1 μm to 10 μm. From the viewpoint of ensuring energy density, the lower limit is set to 1 μm. Also, in consideration of the battery performance and the expansion rate due to charging and discharging, the upper limit is set to 10 μm.
[0046] The negative electrode current collector is a member disposed on the surface of the negative electrode composite layer or the negative electrode thin film layer opposite to the surface on which the solid electrolyte layer is laminated. The material constituting the negative electrode current collector can be appropriately selected from known materials according to the purpose. For example, Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, etc. can be mentioned. The thickness of the negative electrode current collector is not particularly limited and may be appropriately set according to the desired battery performance. For example, it is in the range of 0.1 μm to 1 mm.
[0047] In addition, the surface roughness of the negative electrode current collector, at least on the side in contact with the negative electrode composite layer or the negative electrode thin film layer, is preferably 0.8 μm or more and 4.0 μm or less in terms of maximum height Rz according to JIS B 0601:2013 (ISO 4287:1997). This enhances the adhesion between the negative electrode current collector and the negative electrode composite layer or the negative electrode thin film layer, as described later, and suppresses expansion in the planar direction by the strength of the negative electrode current collector, thereby facilitating fusion of the negative electrode active material and enabling suppression of the rate of increase in resistance.
[0048] The method for producing the negative electrode layer is not particularly limited, and the layer can be produced by a known method. When manufacturing a negative electrode layer including a negative electrode composite layer, for example, materials constituting the negative electrode composite layer are mixed with a solvent to form a slurry, and the slurry is applied to a substrate or a negative electrode current collector, and then dried, thereby manufacturing a negative electrode layer including a negative electrode composite layer. When producing a negative electrode layer including a negative electrode thin film layer, for example, a negative electrode active material can be sputtered onto a substrate or a negative electrode current collector to produce a negative electrode layer including a negative electrode thin film layer. The sputtering conditions can be appropriately set depending on the thickness of the negative electrode thin film layer, etc.
[0049] Laminate The laminate is a laminate in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer containing an alloy-based active material are laminated in this order. In the laminate, the capacity ratio of the negative electrode layer to the positive electrode layer is preferably 5 or less. The "capacity ratio" is a value calculated from the theoretical capacity (mAh) of the negative electrode layer / theoretical capacity (mAh) of the positive electrode layer. The softness of the negative electrode active material changes as it absorbs Li during charging. By setting the capacity ratio of the negative electrode layer to the positive electrode layer in the laminate to 5 or less, the softness of the negative electrode active material can be adjusted to make it more likely to fuse together during charging.
[0050] The method of stacking the positive electrode layer, the solid electrolyte layer, and the negative electrode layer is not particularly limited, and a known method can be adopted. For example, the positive electrode layer, the solid electrolyte layer, and the negative electrode layer are separately prepared, and the positive electrode layer and the solid electrolyte layer are stacked by pressing them at a predetermined pressure, and the negative electrode layer is stacked by pressing them at a predetermined pressure on the surface of the solid electrolyte layer opposite to the positive electrode layer, to produce a stacked body. In addition, a slurry constituting the positive electrode layer, the solid electrolyte layer, and the negative electrode layer is separately prepared, and the positive electrode layer, the solid electrolyte layer, and the negative electrode layer are stacked in this order, and then dried, to produce a stacked body.
[0051] 1.2. Initial charging process S12 The initial charging step S12 is a step performed after the preparation step S11, in which the laminate produced in the preparation step S11 is restrained in the stacking direction and the battery is initially charged at a constant current and constant voltage. In the initial charging step S12, the restraining pressure of the laminate at the start of charging is 30 MPa or more, and the restraining pressure at the end of charging is 40 MPa or more.
[0052] During normal use, from the viewpoint of handling the all-solid-state battery, it is difficult to increase the confining pressure of the laminate to the confining pressure in the initial charging step S12.
[0053] The conditions for the initial constant-current constant-voltage charging are not particularly limited and may be the same as those in the past, that is, may be appropriately set depending on the battery performance of the laminate.
[0054] The restraining pressure of the laminate at the start of charging may be 30 MPa or more. Preferably, it is 40 MPa or more. On the other hand, it may be 70 MPa or less in consideration of the durability of the laminate. Also, the restraining pressure of the laminate at the end of charging may be 40 MPa or more. Preferably, it is 50 MPa or more. On the other hand, it may be 80 MPa or less in consideration of the durability of the laminate. Here, since the negative electrode active material expands by absorbing Li during charging, the restraining pressure at the end of charging is greater than that at the start of charging. Therefore, it is assumed that the restraining pressure of the laminate at the end of charging is greater than that at the start of charging.
[0055] 1.3. Effects etc. The manufacturing method of the all-solid-state battery of the present disclosure has been described above with reference to the manufacturing method S10. In the manufacturing method of the all-solid-state battery of the present disclosure, a larger confining pressure than that during normal use is applied to the laminate in the initial charging step to perform the initial charging, thereby making it possible to suppress an increase in the resistance increase rate of the all-solid-state battery manufactured using the laminate. More specifically, by performing the initial charge under conditions where the confining pressure at the start of charge is 30 MPa or more and the confining pressure at the end of charge is 40 MPa or more, it is possible to suppress a decrease in the relative resistance increase rate, i.e., deterioration of the battery stack due to durability. In order to reduce the relative resistance increase rate, it is necessary to promote the fusion of the negative electrode active materials, and in order to promote the fusion of the negative electrode active materials, it is important to grow the active materials in the thickness direction where the confining pressure is applied. By promoting the fusion of the negative electrode active materials, the inactive interface (interface between the negative electrode active materials) is reduced, and rearrangement of the negative electrode active materials in the negative electrode layer occurs. Then, when the negative electrode active material shrinks (for example, during discharge), voids in the negative electrode layer are likely to occur in the stacking direction. The voids in the stacking direction are unlikely to obstruct the electron path and ion path. Therefore, the arrangement of voids generated in the negative electrode layer can be controlled by the initial charging process, and as a result, the increase in the resistance increase rate can be suppressed.
[0056] Furthermore, by setting the surface roughness of the negative electrode current collector within a predetermined range, that is, by setting the surface roughness Rz of the negative electrode current collector to 0.8 μm or more and 4.0 μm or less, the above effect becomes more remarkable. In order to concentrate the expansion and contraction of the alloy-based active material caused by the absorption and release of Li in the thickness direction of the electrode, the above-mentioned constraints are used to increase the adhesion between the negative electrode current collector and the layer containing the negative electrode active material, and by setting the surface roughness of the negative electrode current collector within a specified range, the expansion of the layer containing the negative electrode active material in the planar direction is suppressed by the strength of the negative electrode current collector, promoting the fusion of the negative electrode active material and making it possible to further suppress the rate of increase in resistance.
[0057] After the above-mentioned initial filling step, the laminate may be restrained at a restraining pressure of 10 MPa or less. Furthermore, after the initial charging step S12, a step of housing the laminate in a case equipped with terminals necessary for a battery, such as electrodes, may be included.
[0058] 2. Solid state battery An all-solid-state battery, which is one embodiment of a solid-state battery manufactured by the manufacturing method of a solid-state battery of the present disclosure, includes a laminate in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated in this order, and the ratio of voids in the stacking direction to the total voids present in the negative electrode layer can be greater than 36 volume %, more preferably 55 volume % or more, while the upper limit is 100 volume %. Here, "voids in the stacking direction" refers to voids whose major axis is at an angle of 45° or less to the stacking direction, whose major axis length is 0.5 μm or more, and whose minor axis length is 2 μm or less.
[0059] The method for calculating the ratio of voids in the stacking direction to all voids present in the negative electrode layer (vertical crack ratio) is, for example, as follows. First, the laminate is cut in the stacking direction, and a cross-sectional image of the negative electrode layer is obtained using a scanning electron microscope. The cross-sectional image is one that shows a predetermined range of the negative electrode cross section. From the viewpoint of ensuring the accuracy of the vertical crack rate, the cross-sectional image is one that shows at least a 15 μm × 15 μm range of the negative electrode cross section. Next, image analysis is performed on the obtained cross-sectional image, and the volume ratio of voids in the image (=porosity) is calculated. In addition, in the above voids, the direction viewed from the top and bottom surfaces with respect to the stacking direction is taken as the horizontal plane, and a longitudinal crack is defined as a crack whose long axis is 45° or more with respect to the horizontal plane, whose length is 0.5 μm or more, and whose short axis is 2 μm or less. The volume ratio of voids in the stacking direction to the volume of all voids is calculated as the longitudinal crack ratio (volume %).
[0060] The voids in the stacking direction are less likely to obstruct the electron path and ion path in the negative electrode layer than the other voids. Therefore, according to the all-solid-state battery of the present disclosure in which the ratio of the voids in the stacking direction in the negative electrode layer (vertical crack ratio) is greater than 36 volume %, preferably 55 volume % or more, the increase in the resistance increase rate can be suppressed. In particular, even in the case of silicon, which expands and contracts greatly, the increase in resistance during cycling can be suppressed.
[0061] 3. Testing 3.1. Testing for binding force 3.1.1.Laminate preparation Laminates for evaluation in Tests A1 to A7 and Tests B1 to B5 were prepared as follows.
[0062] 3.1.1a. Preparation of the positive electrode layer The raw material is NCA-based positive electrode active material (LiNi 0.8 Co 0.15 Al 0.05A positive electrode slurry was prepared by stirring a positive electrode mixture containing NCA, sulfide-based solid electrolyte (Li2S-P2S5), vapor-grown carbon fiber, PVdF-based binder, and butyl butyrate using an ultrasonic disperser. The weight ratio of NCA-based positive electrode active material: sulfide-based solid electrolyte: vapor-grown carbon fiber: PVdF-based binder in the positive electrode slurry was adjusted to 88.2:9.8:1.3:0.7. This positive electrode slurry was applied onto a positive electrode current collector (Al foil) by the blade method, and the positive electrode layer was obtained by drying the coated material at 100°C on a hot plate for 30 minutes.
[0063] 3.1.1b. Preparation of the negative electrode layer including the negative electrode mixture layer A negative electrode slurry was prepared by stirring the negative electrode mixture containing powdered Si particles, sulfide-based solid electrolyte (Li2S-P2S5), vapor-grown carbon fiber, PVdF-based binder, and butyl butyrate as raw materials using an ultrasonic dispersion device. The particle size of the Si particles is as shown in Tables 2 to 4. Here, the weight ratio of powdered Si particles: sulfide-based solid electrolyte: vapor-grown carbon fiber: PVdF-based binder in the negative electrode slurry was adjusted to 47.0:44.6:7.0:1.4. This negative electrode slurry was applied onto a negative electrode current collector foil (Ni foil) by the blade method, and this was dried at 100°C on a hot plate for 30 minutes to obtain a negative electrode layer.
[0064] 3.1.1c. Preparation of the negative electrode layer including the negative electrode thin film layer An electrolytic copper foil with a roughened surface obtained by electrolytically depositing copper was used as the negative electrode current collector. A RF sputtering device was used to form a thin Si film on the surface of the negative electrode current collector to obtain a negative electrode layer. The conditions for forming the thin Si film are shown in Table 1. In Table 1, the thickness of the thin Si film was calculated by calculating the surface density of Si by inductively coupled plasma optical emission spectrometry, and this surface density value was used as the true density of Si (2.3 gcm -3 ) The Si content in the negative electrode layer was 95 mass % or more.
[0065] [Table 1]
[0066] 3.1.1d. Preparation of solid electrolyte layer A solid electrolyte slurry was prepared by stirring a solid electrolyte mixture containing a sulfide-based solid electrolyte (Li2S-P2S5), a PVdF-based binder, and butyl butyrate as raw materials using an ultrasonic disperser. The weight ratio of the sulfide-based solid electrolyte to the PVdF-based binder in the solid electrolyte slurry was adjusted to 99.6:0.4. This solid electrolyte slurry was applied onto an Al foil by the blade method, and then dried at 100°C on a hot plate for 30 minutes to obtain a peelable solid electrolyte layer.
[0067] 3.1.1e. Preparation of the laminate The prepared positive electrode layer and solid electrolyte layer were laminated so that the composite surfaces overlapped. After pressing with a roll press at a pressure of 50 kN / cm and a temperature of 160°C, the Al foil of the solid electrolyte layer was peeled off and the laminate was cut into 1 cm pieces. 2 A positive electrode laminate was obtained by punching out the material into a size of 10 mm.
[0068] The prepared negative electrode layer and solid electrolyte layer were laminated so that their composite surfaces overlapped each other or the thin film surface and the composite surface overlapped each other. After pressing with a roll press at a pressure of 50 kN / cm and a temperature of 160°C, the Al foil of the solid electrolyte layer was peeled off to obtain a negative electrode laminate A. Furthermore, a solid electrolyte layer was further laminated on the solid electrolyte layer side of the negative electrode laminate A so that the composite surfaces overlapped. This laminate was pre-pressed with a flat uniaxial press at a pressure of 100 MPa and a temperature of 25°C, after which the Al foil of the solid electrolyte layer was peeled off and a 1.08 cm 2 A negative electrode laminate B was obtained by punching out the laminate into a size of 10 mm.
[0069] The prepared positive electrode laminate and negative electrode laminate B were laminated so that the composite surfaces overlapped. This laminate was pressed with a flat uniaxial press at a pressure of 200 MPa and a temperature of 120° C. to obtain a laminate. The capacity ratio of the negative electrode layer to the positive electrode layer of the prepared laminate is shown in Tables 2 to 5.
[0070] 3.1.2. First charge evaluation The laminate obtained as described above was sandwiched between two restraining plates, and these two restraining plates were fastened by a fastener to the restraining pressure at the start of charging shown in Tables 2 to 5, to fix the distance between these two restraining plates. Next, the laminate was subjected to a constant current charge of 1 / 10C to 4.2V, and then to a constant voltage charge of 4.2V to a cut-off current of 1 / 100C. The restraining pressure at the end of charging was recorded. Furthermore, a constant current discharge of 1 / 10C to 2.5V was performed, and then a constant voltage discharge of 2.5V to a cut-off current of 1 / 100C was performed.
[0071] 3.1.3. Evaluation of longitudinal crack rate The longitudinal cracking rate was evaluated for Test A1, Test A3, Test A7, Test B1, and Test B5. Specifically, the laminate after the initial charge evaluation was first disassembled, and the laminate was cut in the stacking direction by an ion milling device. Next, a cross-sectional image of the cut laminate in the range of 15 μm × 15 μm was obtained using a scanning electron microscope. The obtained cross-sectional image was color-coded into four elements, namely, the negative electrode active material, the solid electrolyte, the carbon fiber, and the voids, by image analysis, and the volume ratio of the voids in the image (= void ratio) was calculated. In addition, in the above voids, the direction viewed from the top and bottom surfaces with respect to the stacking direction is taken as the horizontal plane, and the long axis is 45° or more with respect to the horizontal plane, the length is 0.5 μm or more, and the length of the short axis is 2 μm or less is defined as a longitudinal crack, and the volume ratio of the voids in the stacking direction to the volume of all voids was calculated as the longitudinal cracking rate (volume %). The results are shown in Tables 2 and 5. Moreover, a cross-sectional image (Test A1) of a negative electrode including a negative electrode mixture layer is shown in Fig. 2. A cross-sectional image (Test A7) of a negative electrode including a negative electrode thin film layer is shown in Fig. 3.
[0072] 3.1.4.Evaluation of Drag Increase Rate The laminate after the initial charging evaluation was released from the restraint and then clamped again with a restraining pressure of 10 MPa to fix the distance between the two restraining plates. Next, the laminate was charged at a constant current of 1 / 10 C up to 3.0 V, and then charged at a constant voltage of 3.0 V up to a final current of 1 / 100 C to adjust the state of charge. The laminate with the adjusted state of charge had a capacity of 8.2 mAh / cm 2A current of 10 ...
[0073] The laminate whose initial resistance value had been measured was subjected to a durability test in which charging and discharging were repeated 300 times under the following conditions. Charging conditions: 1C, constant current charging up to 4.2V Discharge conditions: 1C, constant current discharge to 2.5V
[0074] The laminate after the durability test was charged at a constant current of 1 / 10C to 3.0V, and then charged at a constant voltage of 3.0V to a cut-off current of 1 / 100C, thereby adjusting the state of charge. The laminate with the adjusted state of charge had a capacity of 8.2mAh / cm 2 A current of 10 ...
[0075] Based on the obtained initial resistance value and resistance value after durability test, the resistance increase rate was calculated from the following formula. Here, in the test of the laminate using the negative electrode layer including the negative electrode composite layer, the resistance increase rate of test B1 was set as the reference (100%) to calculate the relative resistance increase rate. In the test of the laminate using the negative electrode layer including the negative electrode thin film layer, the resistance increase rate of test B5 was set as the reference (100%) to calculate the relative resistance increase rate. A small relative resistance increase rate indicates that deterioration of the battery laminate due to durability is suppressed. The results are shown in Tables 2 to 5. Resistance increase rate (%) = Resistance after durability (Ω) / Initial resistance (Ω) x 100
[0076] [Table 2]
[0077] [Table 3]
[0078] [Table 4]
[0079] [Table 5]
[0080] 3.1.5.Results Tables 2 to 4 show the results of test examples of laminates provided with a negative electrode layer including a negative electrode mixture layer. Table 2 shows a test example in which the particle size of the negative electrode active material and the capacity ratio of the laminate were fixed, while the binding pressure at the start of charging and the binding pressure at the end of charging were changed. Based on the results of Table 2, FIG. 4 shows the relationship between the binding pressure at the end of the first charge and the relative resistance increase rate. From Table 2 and FIG. 4, it was confirmed that the vertical crack rate increased and the relative resistance increase rate decreased in Tests A1 to A3, which were performed under conditions of a binding pressure of 30 MPa or more at the start of charging and a binding pressure of 40 MPa or more at the end of charging, compared to Tests B1 and B2, which were performed under a binding pressure of 10 MPa to 20 MPa, which is generally applied in the first charge. From these results, it can be seen that the deterioration of the laminate due to the durability test is suppressed in Tests A1 to A3 compared to Tests B1 and B2.
[0081] Table 3 shows the results of changing the capacity ratio of the laminate while fixing the particle size of the negative electrode active material, the binding pressure at the start of charging, and the binding pressure at the end of charging. From Table 3, it can be seen that the relative resistance increase rate is reduced in the range of the capacity ratio of 5 or less, that is, the deterioration of the laminate due to the durability test is suppressed. The softness of Si used in the alloy-based negative electrode active material changes by absorbing Li. Therefore, the reason why the relative resistance increase rate is reduced in the range of the capacity ratio of 5 or less is thought to be because the capacity ratio of 5 or less allows LiSi to reach a softness that easily causes binding during charging.
[0082] Table 4 shows the results when the particle size of the negative active material was changed while the capacity ratio of the laminate, the confining pressure at the start of charging, and the confining pressure at the end of charging were fixed. From Table 4, it can be seen that the relative resistance increase rate is reduced when the particle size of the negative active material is 1 μm or less, that is, the deterioration of the battery laminate due to durability is suppressed. This is because the smaller the particle size of the negative active material, the more the interface between the negative active material and the negative active material in the negative electrode increases, and it shows that when an active material with a particle size of 1 μm or less is used, the effect of reducing the inactive interface due to fusion between active materials is large.
[0083] Table 5 shows the results of a test example of a laminate using a negative electrode layer including a negative electrode thin film layer. From Table 5, even when such a laminate was used and the initial charge was performed under conditions of a confining pressure of 30 MPa at the start of charge and a confining pressure of 50 MPa at the end of charge, an increase in the longitudinal crack rate and a decrease in the relative resistance increase rate were confirmed, and it can be seen that the deterioration of the battery laminate due to the durability test was suppressed. In particular, it can be seen that the longitudinal crack rate was 100% in test A7.
[0084] 3.2. Surface roughness test of negative electrode current collector layer 3.2.1.Laminate preparation Laminates for evaluation in Tests A11 to A16 and Tests B11 to B14 were prepared as follows.
[0085] 3.2.1a. Preparation of the positive electrode layer The positive electrode layer was prepared in the same manner as in Tests A1 to A7 and Tests B1 to B5.
[0086] 3.2.1b. Preparation of the negative electrode layer (negative electrode layer having a negative electrode mixture layer) A negative electrode slurry was prepared by stirring the powdered Si particles, sulfide-based solid electrolyte (Li2S-P2S5), vapor-grown carbon fiber, PVdF-based binder, and butyl butyrate-containing negative electrode mixture as raw materials with an ultrasonic dispersing device. Here, the weight ratio of powdered Si particles: sulfide-based solid electrolyte: vapor-grown carbon fiber: PVdF-based binder in the negative electrode slurry was adjusted to 46.8: 44.4: 7.0: 1.4. This negative electrode slurry was applied by the blade method onto a metal foil having Rz shown in Tables 6 and 7 as a negative electrode current collector, and this was dried at 100 ° C. on a hot plate for 30 minutes to obtain a negative electrode layer having a negative electrode mixture layer.
[0087] 3.2.1c. Preparation of the negative electrode layer (negative electrode layer having a thin negative electrode layer) The negative electrode current collector was a Ni foil having the Rz shown in Table 8. A RF sputtering device was used to form a thin Si film on the surface of the negative electrode current collector to obtain a negative electrode layer. The conditions for forming the thin Si film were the same as those in Table 1 above.
[0088] 3.2.1d. Preparation of solid electrolyte layer The solid electrolyte layers were prepared in the same manner as in Tests A1 to A7 and Tests B1 to B5.
[0089] 3.2.1e. Preparation of the laminate The laminates were also prepared in the same manner as in Tests A1 to A7 and Tests B1 to B5.
[0090] 3.2.2. First charge evaluation The battery stack obtained as described above was sandwiched between two restraining plates, and these two restraining plates were fastened with a fastener to the restraining pressure at the start of charging shown in Tables 6 to 8, to fix the distance between these two restraining plates. Next, the restrained stack was charged at a constant current of 1 / 10C to 4.05V, and then charged at a constant voltage of 4.05V to a cut-off current of 1 / 100C. The restraining pressure at the end of charging was recorded. Furthermore, a constant current discharge was performed at 1 / 10C to 2.5V, and then a constant voltage discharge was performed at 2.5V to a cut-off current of 1 / 100C.
[0091] 3.2.3.Evaluation of Drag Increase Rate The laminate after the initial charging evaluation was released from the restraint and then clamped again with a restraining pressure of 10 MPa to fix the distance between the two restraining plates. Next, the laminate was charged at a constant current of 1 / 10 C up to 3.0 V, and then charged at a constant voltage of 3.0 V up to a final current of 1 / 100 C to adjust the state of charge. The laminate with the adjusted state of charge had a capacity of 8.2 mAh / cm 2 A current of 10 ...
[0092] The laminate whose initial resistance value had been measured was subjected to a durability test in which charging and discharging were repeated 300 times under the following conditions. Durable charging: 1C, constant current charging up to 4.05V Durability discharge: 1C, constant current discharge up to 2.5V
[0093] The laminate after the durability test was charged at a constant current of 1 / 10C to 3.0V, and then charged at a constant voltage of 3.0V to a cut-off current of 1 / 100C, thereby adjusting the state of charge. The laminate with the adjusted state of charge had a capacity of 8.2mAh / cm 2 A current of 10 ...
[0094] Based on the obtained initial resistance value and resistance value after durability test, the resistance increase rate was calculated from the following formula. Here, in the test of the laminate using the negative electrode layer including the negative electrode composite layer, the resistance increase rate of test A11 was set as the reference (100%) to calculate the relative resistance increase rate. In the test of the laminate using the negative electrode layer including the negative electrode thin film layer, the resistance increase rate of test A16 was set as the reference (100%) to calculate the relative resistance increase rate. A small relative resistance increase rate indicates that deterioration of the battery laminate due to durability is suppressed. The results are shown in Tables 6 to 8. Resistance increase rate (%) = Resistance after durability (Ω) / Initial resistance (Ω) x 100
[0095] [Table 6]
[0096] [Table 7]
[0097] [Table 8]
[0098] 3.2.4.Results 3.2.4a. Relationship between surface roughness of negative electrode current collector and relative resistance increase rate FIG. 5 shows a graph of Rz on the horizontal axis and the relative resistance increase rate on the vertical axis for Tests A11 to A13, B11, and B12 in Table 6. From Tests A11 to A13, B11, and B12 in Table 6, it can be seen that when the surface roughness Rz of the negative electrode current collector is 0.8 μm or more and 4.0 μm or less, and the initial charge is performed under the conditions of a confining pressure of 30 MPa at the start of charge and a confining pressure of 40 MPa at the end of charge, the relative resistance increase rate is reduced, that is, the deterioration of the battery stack due to durability is suppressed. This is thought to be because the adhesion between the negative electrode current collector and the negative electrode mixture is increased, and the expansion of the negative electrode active material in the planar direction is suppressed by the strength of the negative electrode current collector, which promotes fusion of the active material in the thickness direction, and the cracks in the electrode due to the contraction of the active material can be controlled in the vertical direction. When Rz is less than 0.8 μm, the adhesion between the negative electrode composite and the negative electrode current collector is low, peeling occurs at the interface between the negative electrode composite and the negative electrode current collector, and expansion of the negative electrode composite in the planar direction cannot be suppressed, making it impossible to control cracking, which is thought to result in an increase in the resistance increase rate. In addition, when Rz is larger than 4.0 μm, the difference in thickness between the valleys and peaks in the roughened portion of the negative electrode current collector is large, and the local counter capacity ratio in the valleys and the local counter capacity ratio in the peaks are shifted, which is considered to cause reaction unevenness and increase the resistance increase rate. In addition, it is not preferable to make the surface roughness Rz of the negative electrode current collector larger than 4.0 μm from the viewpoint of the strength of the negative electrode current collector and the volume density because the thickness of the negative electrode current collector must be increased. Moreover, from the results of Test A12 and Test B13 in Table 6, it can be seen that even if the surface roughness Rz of the negative electrode current collector is 0.8 μm or more and 4.0 μm or less, the relative resistance increase rate does not decrease unless the confining pressure at the start of charge is 30 MPa or more and the confining pressure at the end of charge is 40 MPa or more.
[0099] 3.2.4b. Relationship between type of negative electrode current collector and relative resistance increase rate Tests A14 and A15 in Table 7 show that when the surface roughness Rz of the negative electrode current collector is 0.8 μm or more and 4.0 μm or less, the confining pressure at the start of charge is 30 MPa, and the confining pressure at the end of charge is 40 MPa, the same effect of suppressing deterioration of the battery stack due to durability can be achieved, regardless of the type of metal used for the negative electrode current collector.
[0100] 3.2.4c. Anode layer with thin anode layer From Test A16 and Test B14 in Table 8, it can be seen that even when the negative electrode layer is a thin film, similarly to the above-mentioned composite, when the surface roughness Rz of the negative electrode current collector is 0.8 μm or more and 4.0 μm or less, and the initial charge is performed with a confining pressure of 30 MPa or more at the start of charge and a confining pressure of 40 MPa or more at the end of charge, the relative resistance increase rate decreases, that is, deterioration of the battery stack due to durability is suppressed.
Claims
1. A solid-state battery having a laminate including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer including an alloy-based negative electrode active material, the voids in the stacking direction of the negative electrode layer account for 55% by volume or more and 100% by volume or less of the total voids of the negative electrode layer, The negative electrode layer further includes a negative electrode current collector, The negative electrode current collector has a surface roughness, which is a maximum height Rz according to JIS B 0601:2013, of 0.8 μm or more and 4.0 μm or less. solid state battery.
2. The solid-state battery according to claim 1 , wherein the alloy-based negative electrode active material comprises silicon.
3. 3. The solid-state battery of claim 2, wherein the silicon is in particulate form.
4. The solid-state battery according to claim 3 , wherein the particle size D50 of the silicon particles is 1 μm or less.
5. 3. The solid-state battery of claim 2, wherein the silicon is a thin film.
6. The solid-state battery according to any one of claims 1 to 5, wherein the solid electrolyte layer contains a sulfide solid electrolyte.
7. A preparation step of preparing a laminate including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer; and an initial charging step of constraining the stack in a stacking direction and performing an initial constant-current constant-voltage charging of the stack, In the initial charging step, the confining pressure of the laminate at the start of charging is 30 MPa or more and 70 MPa or less, and the confining pressure of the laminate at the end of charging is 40 MPa or more and 80 MPa or less, The negative electrode layer further includes a negative electrode current collector, The negative electrode current collector has a surface roughness, which is a maximum height Rz according to JIS B 0601:2013, of 0.8 μm or more and 4.0 μm or less. How solid-state batteries are manufactured.
8. The method for producing a solid-state battery according to claim 7 , wherein after the initial charging step, the laminate is constrained at a confining pressure of 10 MPa or less.
9. the negative electrode layer contains an alloy-based negative electrode active material, The method for producing a solid-state battery according to claim 7 or 8, wherein the alloy-based negative electrode active material contains silicon.
10. The method for producing a solid-state battery according to claim 9 , wherein the silicon is in the form of particles.
11. The method for producing a solid-state battery according to claim 10, wherein the particle diameter D50 of the silicon particles is 1 μm or less.
12. The method for producing a solid-state battery according to claim 9 , wherein the silicon is a thin film.
13. The method for producing a solid-state battery according to any one of claims 7 to 12, wherein the solid electrolyte layer contains a sulfide solid electrolyte.
Citation Information
Patent Citations
Typing device
JP1980057471A
Lithium secondary battery
JP2005285651A
Negative electrode and battery
JP2006155959A
Method of manufacturing all-solid secondary battery
JP2010272210A
Metho for manufacturing all-solid-state lithium secondary battery
JP2014107163A