Manufacturing method for antibacterial ceramic tiles
The use of oolan tea crystals and alkaline earth metal oxides in a protective glaze for ceramic tiles addresses durability and UV issues, ensuring high antibacterial efficacy and surface quality, overcoming previous methods' limitations.
Patent Information
- Application Number
- JP2023554073
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-01
- Filing Date
- 2021-12-03
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-12-03
AI Technical Summary
Existing antibacterial ceramic tiles face issues with durability and UV harm, as antibacterial agents like silver or nano-zinc oxide degrade in high-temperature environments, and methods using nano titanium dioxide require UV excitation, posing health risks. Additionally, uniform application of bactericidal agents is challenging, leading to reduced efficacy from scratches and wear.
A manufacturing method involving an antibacterial protective glaze with 35-45% oolan tea crystals and high alkaline earth metal oxides, which excites metal ions to generate negative oxygen ions and free radicals for rapid bactericidal action, ensuring uniform distribution and high-temperature stability without relying on photocatalysis.
The method achieves over 90% antibacterial efficacy against Escherichia coli and Staphylococcus aureus, maintains antibacterial performance under wear, and avoids UV-related health hazards, with improved glaze surface quality and durability.
Smart Images

Figure 0007578845000001 
Figure 0007578845000002 
Figure 0007578845000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an antibacterial ceramic tile and a manufacturing method thereof, which belongs to the technical field of ceramic tile manufacturing. [Background technology]
[0002] Purifying the home environment and clean indoor air are very important to people's daily life. Ceramic tiles are used as home decoration materials and are often contacted in daily life, so some major ceramic brands in the industry are focusing on developing ceramics with antibacterial functions. At present, some ceramic manufacturers have launched ceramic tiles with antibacterial functions by adding negative ion powder for sterilization, but since the negative ion powder is mainly excited by radioactive elements, the ceramic products have a certain degree of radioactivity. For example, sterilization by photocatalysis is mainly by applying nano-titanium dioxide to the surface of the product, and since it is excited by ultraviolet light, a low-temperature treatment of 300°C is required to maintain activity. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] China Patent Application Publication No. 112062470 [Patent Document 2] China Patent Application Publication No. 107043249 [Patent Document 3] China Patent Application Publication No. 112194476 [Patent Document 4] China Patent Publication No. 112194478 Summary of the Invention [Problem to be solved by the invention]
[0004] As such, the ceramic products need to be improved in durability, and ultraviolet rays are harmful to the human body. For example, if antibacterial agents such as silver or nano zinc oxide are added to the glaze and directly fired, the silver or nano zinc oxide will undergo an oxidation reaction in a high-temperature environment, reducing the antibacterial activity. [Means for solving the problem]
[0005] In a first aspect, the present invention discloses a method for producing an antibacterial ceramic tile. The method includes applying an antibacterial protective glaze containing uranium tea crystal to the surface of a tile base material, and firing the tile to obtain an antibacterial ceramic tile. The antibacterial protective glaze contains uranium tea crystal in a mass percentage of 35-45%, and contains an alkaline earth metal oxide in the antibacterial protective glaze in a mass percentage of 10% or more. By controlling the mass percentage of uranium tea crystal in the antibacterial protective glaze within the above range, not only can excellent antibacterial performance be obtained, but also the ceramic glaze surface can be prevented from having an excessively high gloss, rough texture, and poor flatness.
[0006] In the existing antibacterial ceramic tile manufacturing method, some technical solutions use nano zinc oxide and single rare earth ions as bactericides, and need to form a specific microporous structure in the glaze layer by firing to achieve a good bactericidal effect, but it is difficult to control the microporous structure. There is also a technical solution that combines rare earth ions with titanium dioxide, controls the crystal grain size of titanium dioxide by rare earth ions, and uses the photocatalytic action of nano titanium dioxide to sterilize. The present invention utilizes the composite bactericidal effect of multiple rare earth ions, and does not need to form a microporous structure or rely on the photocatalytic action of nano titanium dioxide. In the above manufacturing method, the olan tea crystallite contains various rare earth elements, and the rare earth metals themselves are inorganic antibacterial materials, so that when they come into contact with bacteria, the rare earths can enter the inside of the cells through the transport channel by the membrane penetration action, and the highly reactive rare earth ions can react with the organic polymers in the cells and affect the proliferation of bacteria. Ceramic glazes contain a high content of alkaline earth metal oxides (such as magnesium oxide, calcium oxide, barium oxide, and some trace oxides with relatively large atomic weights), and these oxides have high surface energy under the excitation of rare earth elements, and under the action of light, the metal ions are excited and undergo electron transfer, generating a large amount of highly chemically active negative oxygen ions and free radicals -OH groups with the water adsorbed on the surface of the glaze layer and O2 in the air. When these negative oxygen ions and free radicals come into contact with microorganisms, they oxidize and decompose the organic matter in the microorganisms into CO2 and H2O, exerting a bactericidal effect in a short time.
[0007] In the manufacturing process of existing antibacterial ceramic tiles, some technical solutions mix a zinc-containing salt solution with a rare earth ion-containing salt solution to form an antibacterial salt solution, which is then sprayed onto the surface of a transparent glaze to form an antibacterial layer. In this method, it is difficult to uniformly spray the antibacterial agent onto the tile surface due to the existing manufacturing equipment, and if the amount sprayed is too large, problems such as the swelling of the glaze layer and the explosion of the tiles in the kiln may occur, so this method is suitable for laboratory sample preparation but not suitable for mass production. In addition, in the ceramic obtained by this method, the antibacterial agent is distributed on the tile surface, so scratches and wear on the tile surface will greatly affect the antibacterial effect. The present invention introduces rare earth ions by olan tea crystal, so that the rare earth ions are uniformly distributed on the glaze layer, that is, rare earth ions are present throughout the entire glaze layer, making it easy to apply the glaze, and scratches and wear on the tile surface will not greatly affect the antibacterial effect.
[0008] Preferably, the mineral composition of the antibacterial protective glaze includes, by mass percentage, 35-45% olan tea shard, 15-25% clay, 30-42% calcium magnesium barium zinc fluxing mineral, and 5-8% aluminum oxide. Among them, the calcium magnesium barium zinc fluxing mineral is a fluxing mineral containing calcium oxide, magnesium oxide, barium oxide, and zinc oxide in high content, and is used to adjust the high temperature viscosity, gloss, and glaze surface flatness of the glaze. The clay is an aluminum silicate salt with adhesiveness and plasticity. For example, the mineral composition of the antibacterial protective glaze includes, by mass percentage, 35-45% olan tea shard, 3-5% zinc oxide, 15-20% barium carbonate, 7-9% calcined talc, 15-25% kaolin, 5-8% aluminum oxide, and 5-8% dolomite.
[0009] Unlike the glaze with silk-like surface effect, which uses the fluidity of the slurry containing olan tea crystal to improve the thixotropy problem of the glaze slurry caused by the introduction of barium sulfate, improves the bonding between the base and the glaze, makes the glaze smooth, and creates a glaze with silk-like surface effect, the present invention uses the low aluminum oxide content of olan tea crystal, and introduces a large amount of calcium, magnesium, barium, and zinc fluxing minerals to avoid the ceramic glaze surface having too high gloss, rough touch, and poor flatness. In addition, the mass percentage content of olan tea crystal in the glaze with silk-like surface effect is low, and it is necessary to introduce albite to reduce the high-temperature viscosity of the glaze, reduce the crystallization of the glaze surface, and increase the fluidity of the glaze. However, the antibacterial protective glaze of the present invention uses a large amount of calcium, magnesium, barium, and zinc fluxing minerals to ensure both antibacterial performance and high glaze surface quality at the same time.
[0010] Preferably, the chemical composition of the antibacterial protective glaze includes, by mass percentage, SiO2: 40%-50%, Al2O3: 16%-20%, alkali metal oxides: 3%-6%, alkaline earth metal oxides: 15%-23%, zinc oxide: 3-5%, and rare earth oxides: 17 ppm-45 ppm.
[0011] Preferably, the chemical composition of the antibacterial protective glaze is, in mass percentage, SiO2: 40% to 50%, Al2O3: 16% to 20%, Fe2O3: 0.21 to 0.31%, TiO2: 0.21 to 0.31%, CaO: 1.5 to 3.0%, MgO: 3.0 to 5.0%, BaO: 11 to 15%, ZnO: 3 to 5%, K2O: 2.0 to 3.0%, Na2O: 1.3 to 2.3%, La2O3: 4 to 9 ppm, CeO2: 9 to 20 ppm, Nd2O3: 2 to 6 ppm. pm, Sm2O3: 0.03-1.5ppm, Eu2O3: 0.09-0.35ppm, Gd2O3: 0.3-1.5ppm, Tb4O7: 0.03-0.15ppm, Ho2O3: 0.06-0.15ppm, Er2O3: 0.12-0.35ppm, Tm2O3: 0.01-0.05ppm, Yb2O3: 0.12-0.35ppm, Lu2O3: 0-0.15ppm, Y2O3: 1.8-4.5ppm, Ignition loss: 8-10%.
[0012] Preferably, the antibacterial protective glaze is applied by spraying, and the specific gravity of the glaze is 1.35 to 1.40 g / cm 3 , weight 250~300 g / m 2 It is.
[0013] Preferably, the maximum firing temperature may be 1200 to 1220° C. and the firing period may be 60 to 70 minutes.
[0014] Preferably, before applying the antibacterial protective glaze containing oolan tea crystal to the surface of the tile base, the manufacturing method further comprises applying a top glaze to the surface of the tile base.
[0015] Preferably, the chemical composition of the top glaze contains, by mass percentage, SiO2: 60% to 68%, Al2O3: 20% to 24%, alkali metal oxides: 4 to 7%, and ZrO2: 3.2 to 9.6%.
[0016] Preferably, the method of applying the top glaze is spray application, and the specific gravity is 1.40 to 1.50 g / cm 3 , weight 500~600 g / m 2 It is.
[0017] In a second aspect, the present invention provides an antibacterial ceramic tile obtained by any one of the above-mentioned manufacturing methods, wherein the antibacterial rate of the antibacterial ceramic tile against Escherichia coli and Staphylococcus aureus are both 90% or more.
[0018] In a third aspect, the present invention discloses the use of oolan tea stone in antibacterial ceramic tiles. [Brief description of the drawings]
[0019] [Figure 1] 1 is a manufacturing flowchart of an antibacterial ceramic tile according to Example 1 of the present invention. [Diagram 2] FIG. 2 is a diagram showing the effect of the antibacterial ceramic tile surface according to Example 1 of the present invention. [Diagram 3] FIG. 13 is a graph showing the effect of an antibacterial ceramic tile surface according to Comparative Example 3 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be further described in connection with the following embodiments. The following embodiments are for the purpose of explaining the present invention, but are not intended to limit the present invention. In the following, each "%" means "mass %" unless otherwise specified. Hereinafter, the manufacturing method of the antibacterial ceramic tile of the present invention will be described by way of example.
[0021] The tile base is manufactured. The powdered base material is dry-pressed to form the tile base. The composition of the powdered base material is not limited, and the powdered base material of ceramic tiles commonly used in this field may be used. For example, the chemical composition of the powdered base material includes, in mass percentage, SiO2: 63.5-65%, Al2O3: 19-22%, Fe2O3: 0.4-0.7%, TiO2: 0.25-0.35%, CaO: 0.25-0.35%, MgO: 0.5-0.80%, K2O: 2.0-2.4%, Na2O: 2.6-3.0%, and loss on ignition: 4.5-5.5%.
[0022] The tile base is dried. The moisture content of the tile base after drying is controlled to 0.3 to 0.5 wt %. The drying time may be 50 to 60 minutes.
[0023] A top glaze is produced. The chemical composition of the top glaze may include, by mass percentage, SiO2: 60% to 68%, Al2O3: 20% to 24%, alkali metal oxide: 4 to 7%, and ZrO2: 3.2 to 9.6%.
[0024] The mineral composition of the top glaze may include, by mass percentage, 30% to 40% potassium feldspar, 15% to 25% albite, 5% to 15% kaolin, 10% to 20% quartz sand, 5% to 15% zirconium silicate, 5% to 10% calcined kaolin, and 5% to 10% aluminum oxide.
[0025] According to the above raw material ratio, the glaze is mixed, pulverized in a ball mill, and sieved to obtain a glaze slurry of the glaze. When pulverizing in a ball mill, auxiliary materials and water are added to the mixed raw materials. In some embodiments, the blending ratio of the glaze slurry of the glaze is, in mass percentage, 70.4% to 72.4% of the dry raw materials of the glaze (i.e., "total mass of the glaze raw materials"), 0.11 to 0.16% of sodium tripolyphosphate, 0.14 to 0.21% of sodium carboxymethylcellulose, and 28.5 to 29.5% of water. The 325 mesh sieve residue of the glaze is ≦0.6wt%.
[0026] In some embodiments, the chemical composition of the top glaze includes, by mass percentage, SiO2: 60%-68%, Al2O3: 20%-24%, Fe2O3: 0.3-0.6%, TiO2: 0.20-0.30%, CaO: 0.3-0.6%, MgO: 0.1-0.3%, K2O: 1.5-2.5%, Na2O: 3.0-4.0%, ZrO2: 3.2-9.6%, and loss on ignition: 1.3-1.7%.
[0027] The linear expansion coefficient of the upper glaze at 40℃ to 400℃ is 8.1716×10 -6 / K~8.3916×10 -6 The linear expansion coefficient of the overglaze is preferably as close as possible to or larger than the linear expansion coefficient of the base material, in order to facilitate adjustment of the tile shape during firing.
[0028] After drying, the surface of the tile body is coated with a top glaze. The top glaze may be coated using a spray glazing method. For example, the process parameters for the spray glazing are: specific gravity of 1.40 to 1.50 g / cm 3 , weight 500~600 g / m 2 It is.
[0029] A pattern is printed on the surface of the tile base with a top glaze applied. The color and design of the inkjet printed pattern change according to the effect of the layout design.
[0030] A protective glaze (also referred to as "antibacterial protective glaze") is manufactured. The chemical composition of the antibacterial protective glaze may include, by mass percentage, SiO2: 40% to 50%, Al2O3: 16% to 20%, alkali metal oxides: 3% to 6%, alkaline earth metal oxides: 15% to 23%, zinc oxide: 3% to 5%, and rare earth oxides: 17 ppm to 45 ppm.
[0031] The mass percentage content of olan tea crystal in the above antibacterial protective glaze is 35-45%. The mechanism by which olan tea crystal exerts the far-infrared function is to provide lanthanide rare earth ions doped into the lattice of MgO-SiO2-Al2O3 of the glaze, forming a highly asymmetric magnesium aluminum silicate compound, so that the glaze has a high far-infrared radiation function. The present invention realizes the antibacterial function by olan tea crystal. Olan tea crystal contains various rare earth elements, and the rare earth metals themselves are inorganic antibacterial materials. Upon contact with bacteria, the rare earth elements can enter the inside of the cells through the transport channel by the membrane penetration action, and the highly reactive rare earth ions can react with the organic polymers in the cells and affect the proliferation of bacteria. Ceramic glazes contain a high content of alkaline earth metal oxides (such as magnesium oxide, calcium oxide, barium oxide, and some trace oxides with relatively large atomic weights). When excited by rare earth elements, these oxides have high surface energy. Under the action of light, the metal ions are excited and undergo electron transfer, which generates a large amount of highly chemically active negative oxygen ions and free radicals -OH groups together with the water adsorbed on the surface of the glaze layer and O2 in the air. When these negative oxygen ions and free radicals come into contact with microorganisms, they oxidize and decompose the organic matter in the microorganisms into CO2 and H2O, exerting a sterilizing effect in a short time.
[0032] The chemical composition of ulan tea quartz is, by mass percentage, SiO2: 70-80%, Al2O3: 10-15%, Fe2O3: 0.05-0.15%, P2O5: 0.25-0.35%, CaO: 0.5-1.0%, MgO: 0.1-0.3%, K2O: 4.0-6.0%, Na2O: 3.0-5.0%, La2O3: 14-17ppm, CeO2: 35-40ppm, Nd2O3: 9-12ppm, Sm 2O3: 1-3ppm, Eu2O3: 0.3-0.7ppm, Gd2O3: 1-3ppm, Tb4O7: 0.1-0.3ppm, Ho2O3: 0.2-0.3ppm, Er2O3: 0.4-0.7ppm, Tm2O3: 0.05-0.1ppm, Yb2O3: 0.4-0.7ppm, Lu2O3: 0-0.3ppm, Y2O3: 6-9ppm, loss on ignition: 0.5-1.0%. Olan tea crystal contains various rare earth metal elements in small amounts, does not contain antibacterial agents such as silver and zinc oxide, has low radioactivity, is resistant to high temperatures, has a long-lasting effect, has excellent antibacterial function, and is non-toxic and harmless to the human body and the environment. By adding oolan tea crystal powder to the glaze, ceramic tiles can be given antibacterial properties.
[0033] The mineral composition of the antibacterial protective glaze may include, by mass percentage, 35-45% olan spar, 15-25% clay, 30-42% calcium magnesium barium zinc fluxing minerals, and 5-8% aluminum oxide. The antibacterial protective glaze formulation avoids introducing a large amount of lithium carbonate, a powerful flux, to prevent the strong flux property of lithium carbonate from significantly affecting the antibacterial activity of rare earth elements.
[0034] The oolan tea crystal used in the present invention contains a variety of rare earth ions, and different rare earth ions work together to exert their antibacterial effects, thereby further expanding the antibacterial range of the antibacterial ceramic tile and improving its antibacterial stability. In addition, the rare earth ions are uniformly present in the glaze layer, so that the antibacterial ceramic tile still has a strong antibacterial effect even after it has been worn to a certain extent.
[0035] In some embodiments, the mineral composition of the antimicrobial protective glaze may include, by weight percentage, 35-45% olancite, 3-5% zinc oxide, 15-20% barium carbonate, 7-9% calcined talc, 15-25% kaolin, 5-8% aluminum oxide, and 5-8% dolomite.
[0036] Even if porcelain tile is used as the base material, the antibacterial property of the ceramic tile surface will be reduced when the base material is covered with glaze, so the ceramic tile surface needs to be glazed with antibacterial glaze to impart antibacterial property, which will undoubtedly increase the process complexity and production cost. Moreover, as can be seen from the experiment, porcelain tile does not react violently in the ceramic base material and does not reduce the antibacterial effect of rare earth elements, but porcelain tile reacts violently in the protective glaze and reduces the antibacterial effect of rare earth elements. In response to this, the present invention proposes to combine a certain content of porcelain tile with calcium, magnesium, barium and zinc flux minerals with a high content of alkali metal oxides to improve the antibacterial effect and glaze surface quality.
[0037] According to the above raw material ratio, the antibacterial protective glaze is mixed, pulverized by a ball mill, and sieved to obtain a glaze slurry of the protective glaze. When pulverizing by the ball mill, auxiliary materials and water are added to the mixed raw materials. In some embodiments, the blending ratio of the glaze slurry of the protective glaze is, in mass percentage, 71.5% to 73.5% of the dry raw materials of the protective glaze (i.e., "total mass of the protective glaze raw materials"), 0.14 to 0.21% of sodium tripolyphosphate, 0.10 to 0.12% of sodium carboxymethylcellulose, and 27 to 29% of water. The sieve residue of the protective glaze on a 325 mesh screen is ≦0.3 wt%.
[0038] In some embodiments, the chemical composition of the antibacterial protective glaze is, by mass percentage, SiO2: 40%-50%, Al2O3: 16%-20%, Fe2O3: 0.21-0.31%, TiO2: 0.21-0.31%, CaO: 1.5-3.0%, MgO: 3.0-5.0%, BaO: 11-15%, ZnO: 3-5%, K2O: 2.0-3.0%, Na2O: 1.3-2.3%, La2O3: 4-9 ppm, CeO2: 9-20 ppm, Nd2O3: 2.0-2.0 ppm, and SiO2: 2.0-2.0 ppm. ~6ppm, Sm2O3: 0.03~1.5ppm, Eu2O3: 0.09~0.35ppm, Gd2O3: 0.3~1.5ppm, Tb4O7: 0.03~0.15ppm, Ho2O3: 0.06~0.15ppm, Er2O3: 0.12~0.35ppm, Tm2O3: 0.01~0.05ppm, Yb2O3: 0.12~0.35ppm, Lu2O3: 0~0.15ppm, Y2O3: 1.8~4.5ppm, Ignition loss: 8~10%.
[0039] The linear expansion coefficient of the antibacterial protective glaze at 40℃ to 400℃ is 6.0416×10 -6 / K~6.3516×10 -6 By controlling the linear expansion coefficient of the antibacterial protective glaze within this range, it is possible to avoid the influence on the shape of the ceramic tile caused by the low linear expansion coefficient of the antibacterial protective glaze, and to ensure the antibacterial performance and high glaze surface quality of the antibacterial protective glaze by adapting it to the formulation of the antibacterial protective glaze.
[0040] An antibacterial protective glaze is applied to the surface of the tile substrate on which the pattern is inkjet printed. The protective glaze may be applied using a spray glaze method. In some embodiments, the process parameters of the spray glaze are: specific gravity of 1.35 to 1.40 g / cm 3 , weight 250~300 g / m 2 It is.
[0041] According to the present invention, the antibacterial protective glaze can provide the ceramic tile with excellent antibacterial performance, the antibacterial rate of the ceramic tile against Escherichia coli is ≧90%, and the antibacterial rate of the ceramic tile against Staphylococcus aureus is ≧90%.
[0042] Finally, the tile body coated with the antibacterial protective glaze is fired. For example, the maximum firing temperature is 1220°C and the firing period is 70 min.
[0043] In the conventional technology, the layered clay is used to adsorb strontium ions and single rare earth ions between the clay crystal layers, thereby realizing the antibacterial effect activated by the rare earth ions and improving the heat resistance of the antibacterial particles. However, in the technology using this clay aqueous solution, many open pores are generated on the tile surface, the tile is poorly sintered, and the wear resistance of the glaze layer is reduced. The present invention utilizes the composite bactericidal function of multiple rare earth ions, does not need to use layered clay, and the wear resistance of the ceramic tile is relatively good.
[0044] The present invention will be described in more detail below with reference to examples. The following examples are merely for further explanation of the present invention and do not limit the scope of protection of the present invention. Non-essential improvements and modifications made by those skilled in the art based on the above content of the present invention are also within the scope of protection of the present invention. The specific process parameters in the following examples are merely examples within the applicable range, that is, those skilled in the art can select within an appropriate range based on the description of the present invention, and are not limited to the specific numerical values in the following examples.
[0045] The linear expansion coefficient of the top glaze and antibacterial protective glaze is tested according to "Part 8 of the test method for ceramic tiles: Measurement of linear thermal expansion" (GB / T 3810.8-2016). The antibacterial test method for ceramic tiles is tested according to the "Antibacterial performance of antibacterial ceramic products" (JC / T897-2014) standard. The abrasion resistance test method for ceramics is tested according to the abrasion resistance of glazed tile surface GB / T3810.7-2016 standard.
[0046] Example 1 In step 1, the powdered base material is molded in a press to obtain a tile base.
[0047] In step 2, the tile substrate is dried.
[0048] In step 3, the top glaze is sprayed onto the surface of the dried tile base. The mineral composition of the top glaze is, by mass percentage, 35% potassium feldspar, 20% albite, 10% kaolin, 10% quartz sand, 10% zirconium silicate, 10% calcined kaolin, and 5% aluminum oxide. The chemical composition of the top glaze is, by mass percentage, 64.65% SiO2, 21.13% Al2O3, 0.32% Fe2O3, 0.23% TiO2, 0.44% CaO, 0.15% MgO, 2.14% K2O, 3.37% Na2O, 6.37% ZrO2, and 1.5% loss on ignition. The linear expansion coefficient of the top glaze at 40°C to 400°C is 8.1716×10 -6 / K~8.3916×10 -6 / K.
[0049] In step 4, a pattern is inkjet printed onto the surface of the tile base that has been sprayed with a top glaze.
[0050] In step 5, the surface of the tile substrate on which the pattern is inkjet printed is sprayed with an antibacterial protective glaze. The mineral composition of the antibacterial protective glaze is, by mass percentage, 41% olan spar, 4% zinc oxide, 15% barium carbonate, 7% calcined talc, 20% kaolin, 5% aluminum oxide, and 8% dolomite. The chemical composition of the antibacterial protective glaze is, by mass percentage, 46.16% SiO2, 17.37% Al2O3, 0.25% Fe2O3, 0.24% TiO2, 2.92% CaO, 4.09% MgO, 11.63% BaO, 3.97% ZnO, 2.60% K2O, 1.74% Na2O, 7ppm La2O3, 15ppm CeO2, 8ppm Nd2O, 1.2ppm Na2O, 1.2ppm La2O3, 1.2ppm Na2O ... O3: 4ppm, Sm2O3: 1ppm, Eu2O3: 0.18ppm, Gd2O3: 0.77ppm, Tb4O7: 0.07ppm, Ho2O3: 0.09ppm, Er2O3: 0.22ppm, Tm2O3: 0.02ppm, Yb2O3: 0.25ppm, Lu2O3: 0.07ppm, Y2O3: 2.9ppm, Ignition loss: 9.48%. The linear expansion coefficient of the antibacterial protective glaze at 40℃ to 400℃ is 6.0416×10 -6 / K~6.3516×10 -6 / K.
[0051] In step 6, the piece is placed in a kiln and fired. The maximum firing temperature is 1200-1220℃, and the firing cycle is 60-70 minutes.
[0052] According to tests, the ceramic tile according to this embodiment has an antibacterial rate of 93.3% against Escherichia coli and 91.8% against Staphylococcus aureus, and its wear resistance is level 4 at 2100 rpm.
[0053] Comparative Example 1 The embodiment is basically the same as the embodiment 1, except that the mineral composition of the antibacterial protective glaze is, by mass percentage, 20% olan tea crystal, 21% potassium feldspar powder, 4% zinc oxide, 15% barium carbonate, 7% calcined talc, 20% kaolin, 5% aluminum oxide, and 8% dolomite, and the chemical composition of the antibacterial protective glaze is, by mass percentage, SiO2: 44.57%, Al2O3: 17.72%, Fe2O3: 0.23%, TiO2: 0.22%, CaO: 2.77%, MgO: 4.20%, BaO: 11.67%, ZnO: The only difference is that it contains 3.97%, K2O:4.18%, Na2O:1.36%, La2O3:3.5pm, CeO2:7.5ppm, Nd2O3:2ppm, Sm2O3:0.5ppm, Eu2O3:0.09ppm, Gd2O3:0.38ppm, Tb4O7:0.03ppm, Ho2O3:0.05ppm, Er2O3:0.11ppm, Tm2O3:0.01ppm, Yb2O3:0.13ppm, Lu2O3:0.04ppm, Y2O3:1.5ppm, and loss on ignition:9.29%.
[0054] According to the test, the antibacterial rate of the ceramic tile against Escherichia coli is 40.7%, and the antibacterial rate against Staphylococcus aureus is 68.5%, because the dosage of olan tea crystal is low, the antibacterial effect is significantly reduced.
[0055] Comparative Example 2 The embodiment is basically the same as the embodiment 1, except that the mineral composition of the antibacterial protective glaze is, by mass percentage, 41% olan spar, 24% albite powder, 5% barium carbonate, 2% calcined talc, 20% kaolin, 5% aluminum oxide, and 3% dolomite, and the chemical composition of the antibacterial protective glaze is, by mass percentage, SiO2: 59.96%, Al2O3: 20.37%, Fe2O3: 0.24%, TiO2: 0.23%, CaO: 1.36%, MgO: 1.79%, BaO: 3.89%, K2O: 3.93%, Na2O: 3.47%, La2O3: 7pm, CeO2: 15ppm, Nd2O3: 4ppm, Sm2O3: 1ppm, E The only differences are that it contains U2O3: 0.18 ppm, Gd2O3: 0.77 ppm, Tb4O7: 0.07 ppm, Ho2O3: 0.09 ppm, Er2O3: 0.22 ppm, Tm2O3: 0.02 ppm, Yb2O3: 0.25 ppm, Lu2O3: 0.07 ppm, Y2O3: 2.9 ppm, and loss on ignition: 4.91%.
[0056] According to the test, the antibacterial rate of the ceramic tile against Escherichia coli is 66.3%, and the antibacterial rate against Staphylococcus aureus is 77.5%. In this comparative example, the amount of olan tea crystal is sufficient, but the glaze contains less magnesium oxide, zinc oxide, titanium oxide, calcium oxide, zirconia and some trace oxides with relatively large atomic weight, especially the content of alkaline earth metal oxide is less than 10%, so the antibacterial glaze generates less negative oxygen ions and free radicals -OH groups, and the antibacterial effect is also reduced.
[0057] Comparative Example 3 The embodiment is basically the same as the embodiment 1, but the difference is that the mineral composition of the antibacterial protective glaze is, by mass percentage, 42% olan tea crystal, 20% albite powder, 5% calcined talc, 18% kaolin, 10% aluminum oxide, 3% dolomite, and 2% zinc oxide, and the chemical composition of the antibacterial protective glaze is, by mass percentage, 58.71% SiO2, 24.11% Al2O3, 0.22% Fe2O3, 0.21% TiO2, 1.35% CaO, 2.76% MgO, and 3.96% K2O. %, Na2O:3.13%, La2O3:7pm, CeO2:15ppm, Nd2O3:4ppm, Sm2O3:1ppm, Eu2O3:0.18ppm, Gd2O3:0.77ppm, Tb4O7:0.07ppm, Ho2O3:0.09ppm, Er2O3:0.22ppm, Tm2O3:0.02ppm, Yb2O3:0.25ppm, Lu2O3:0.07ppm, Y2O3:2.9ppm, loss on ignition:3.62%.
[0058] In this comparative example, the amount of olan tea feldspar is sufficient, but the amount of calcium magnesium barium zinc fluxing minerals is small, and aluminum oxide is used to adjust the gloss of the glaze surface, so the glaze surface effect is rough and not delicate, as shown in Figure 3. In addition, due to the poor glaze surface effect, its antibacterial performance cannot be detected.
Claims
1. The surface of the tile base is coated with an antibacterial protective glaze containing olan tea crystal, the mineral composition of the antibacterial protective glaze is, by mass percentage, 35-45% olan tea crystal, 15-25% clay, 30-42% calcium, magnesium, barium and zinc fluxing minerals, and 5-8% aluminum oxide, the calcium, magnesium, barium and zinc fluxing minerals being fluxing minerals containing calcium oxide, magnesium oxide, barium oxide and zinc oxide, and used to adjust the high temperature viscosity, gloss and glaze surface flatness of the glaze, the clay being an aluminum silicate salt having adhesiveness and plasticity; The chemical composition of the antibacterial protective glaze is, by mass percentage, SiO 2 : 40%-50%, Al 2 O 3 : 16% to 20%, alkali metal oxide 3% to 6%, alkaline earth metal oxide 15% to 23%, zinc oxide 3 to 5%, rare earth oxide 17 ppm to 45 ppm, the alkali metal oxides being sodium oxide and potassium oxide, and the alkaline earth metal oxides being calcium oxide, magnesium oxide and barium oxide; By firing, an antibacterial ceramic tile having an antibacterial rate of 90% or more against Escherichia coli and Staphylococcus aureus is obtained. A method for producing an antibacterial ceramic tile, comprising:
2. The chemical composition of the antibacterial protective glaze is, by mass percentage, SiO 2 : 40%-50%, Al 2 O 3 : 16%-20%, Fe 2 O 3 : 0.21-0.31%, TiO 2 :0.21~0.31%, CaO: 1.5~3.0%, MgO: 3.0~5.0%, BaO: 11~15%, ZnO: 3~5%, K 2 O: 2.0-3.0%, Na 2 O: 1.3-2.3%, La 2 O 3 : 4 to 9 ppm, CeO 2 : 9-20 ppm, Nd 2 O 3: 2-6 ppm, Sm 2 O 3 : 0.03 to 1.5 ppm, Eu 2 O 3 : 0.09 to 0.35 ppm, Gd 2 O 3 : 0.3 to 1.5 ppm, Tb 4 O 7 : 0.03 to 0.15 ppm, Ho 2 O 3 : 0.06 to 0.15 ppm, Er 2 O 3 : 0.12-0.35 ppm, Tm 2 O 3 : 0.01 to 0.05 ppm, Yb 2 O 3 : 0.12 to 0.35 ppm, Lu 2 O 3 : 0 to 0.15 ppm, Y 2 O 3 2. The method according to claim 1, characterized in that the content of fluorine is 1.8 to 4.5 ppm, and the content of ignition loss is 8 to 10%.
3. The antibacterial protective glaze is applied by spraying, and has a specific gravity of 1.35-1.40 g / cm 3 , weight 250-300 g / m 2 The method according to claim 1, characterized in that
4. The manufacturing method according to claim 1, characterized in that the maximum firing temperature is 1200-1220°C and the firing period is 60-70min.
5. The method further includes applying a top glaze to the surface of the tile base before applying the antibacterial protective glaze containing olan tea crystal to the surface of the tile base; The chemical composition of the above-mentioned top glaze is, by mass percentage, SiO2: 60% to 68%, Al2O3: 20% to 24%, alkali metal oxides: 4 to 7%, ZrO2: 3.2 to 9.6%, The manufacturing method according to claim 1, characterized in that the method of applying the top glaze is spray glaze, the specific gravity of which is 1.40-1.50 g / cm 3 and the weight of which is 500-600 g / m 2 .
Citation Information
Patent Citations
Antibacterial ceramic tile capable of releasing negative oxygen ions and preparation method thereof
CN107043249A
Glaze with silk glaze effect, ceramic tile and preparation method
CN112062470A
Wulan yellow quartz being healthy and heat-resistant porcelain
CN112159217A