Steel plate
A steel plate with refined austenite and controlled Mn segregation addresses the weakness of high-strength TRIP steel sheets in welded joints, achieving 1470 MPa tensile strength and strong welds by optimizing composition and structure.
Patent Information
- Application Number
- JP2023508801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-25
- Filing Date
- 2022-02-18
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2042-02-18
AI Technical Summary
Existing high-strength TRIP steel sheets with a tensile strength of 1470 MPa or more face challenges in achieving sufficient welded joint strength due to the presence of coarse residual austenite or fresh martensite in the weld heat-affected zone, which act as crack initiation points.
The steel plate composition includes specific elements within defined ranges to refine retained austenite, suppress Mn segregation, and maintain a metal structure with 70% martensite and 10% retained austenite, ensuring a maximum grain size of retained austenite is less than 5.0 μm, and controlled Mn concentration variations to enhance weld joint strength.
The solution results in a steel plate with excellent formability, a tensile strength of 1470 MPa or more, and sufficient welded joint strength, suitable for automotive applications.
Smart Images

Figure 0007578892000011 
Figure 0007578892000001 
Figure 0007578892000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel sheet. This application claims priority based on Japanese Patent Application No. 2021-051257, filed on March 25, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, there has been a demand for improved fuel efficiency in automobiles in light of restrictions on greenhouse gas emissions as part of measures to combat global warming, and the use of high-strength steel sheets is becoming more and more widespread in order to reduce the weight of vehicle bodies and ensure collision safety.
[0003] High-strength steel sheets for automotive parts are required to have not only strength but also properties necessary for part forming, such as press formability. Although strength and press formability are generally in a trade-off relationship, TRIP (Transformation Induced Plasticity) steel sheets, which utilize the transformation induced plasticity of retained austenite, are known as steel sheets that excel in both strength and press formability.
[0004] For example, Patent Documents 1 and 2 disclose techniques relating to high-strength TRIP steel sheets in which the volume fraction of the structure is controlled within a predetermined range to improve the elongation and hole expansion ratio. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2013 / 051238 [Patent Document 2] Japanese Patent No. 4445365 Summary of the Invention [Problem to be solved by the invention]
[0006] In the automotive industry, there has been a growing need for high-strength steel sheets with excellent formability and a tensile strength of 1470 MPa or more, particularly in recent years. However, TRIP steels with a tensile strength of 1470 MPa or more have an issue in that the strength of welded joints can be low when welded. Regarding these issues, although Patent Documents 1 and 2 relate to high-strength TRIP steel plate, they do not disclose that a tensile strength of 1,470 MPa or more can be obtained, and give no consideration to the joint strength in TRIP steel plate with a tensile strength of 1,470 MPa or more. As such, no technology had previously been proposed for improving the strength of welded joints in TRIP steel with a tensile strength of 1,470 MPa or more.
[0007] An object of the present invention is to provide a steel plate having excellent formability, a tensile strength of 1470 MPa or more, and capable of obtaining sufficient welded joint strength. [Means for solving the problem]
[0008] The present inventors have investigated the reason why sufficient weld joint strength cannot be obtained in TRIP steel sheets having a tensile strength of 1470 MPa or more. As a result, it was found that if coarse retained austenite or fresh martensite is present in the heat-affected zone of welding, cracks easily occur from these as starting points. As a result of further investigation, the inventors of the present invention found that refining the retained austenite is effective in suppressing such cracks, and that suppressing Mn segregation is effective for this purpose.
[0009] The present invention has been made in view of the above problems. [1] A steel sheet according to one embodiment of the present invention has the following composition: C: 0.20% or more, 0.45% or less, Si: 0.50% or more, 2.50% or less, Mn: 1.50% or more, 3.50% or less, Al: 0.005% or more, 1.500% or less, P: 0% or more, 0.040% or less, S: 0% or more, 0.010% or less, N: 0% or more, 0.0100% or less, O: 0% or more, 0.0060% or less, Cr: 0% or more, 0.50% or less, Ni: 0% or more, 1.00% or less, Cu: 0% or more, 1.00% or less, Mo: 0% or more, 0.50% or less, Ti: 0% or more, 0.200% or less, Nb: 0% or more, 0.200% or less, V: 0% or more, 0.500% or less, B: 0% or more, 0.0100% or less, W: 0% or more. Above, 0.1000% or less, Ta: 0% or more, 0.1000% or less, Sn: 0% or more, 0.0500% or less, Co: 0% or more, 0.5000% or less, Sb: 0% or more, 0.0500% or less, As: 0% or more, 0.0500% Mg: 0% or more, 0.0500% or less, Ca: 0% or more, 0.0400% or less, Y: 0% or more, 0.0500% or less, La: 0% or more, 0.0500% or less, Ce: 0% or more, 0.0500% or less, Zr: 0% or more, 0.0500% or less, and the balance: Fe and impurities, and where t is the thickness of the plate, the metal structure at the t / 4 position, which is a position t / 4 from the surface in the cross section in the plate thickness direction, is, in terms of volume fraction, martensite: 70% or more , retained austenite: 10% or more, wherein the maximum grain size of the retained austenite is less than 5.0 μm, and when the Mn concentration is measured at a plurality of measurement points at 1 μm intervals in a square region of the sheet thickness direction cross section, centered at the t / 4 position and with one side having a length of t / 4, the proportion of measurement points where the Mn concentration is 1.1 times or more the average value of the Mn concentrations of all the plurality of measurement points is less than 10.0%, and the tensile strength is 1470 MPa or more. [2] The steel sheet according to the above item [1], wherein the chemical composition is, in mass%, Cr: 0.01% or more, 0.50% or less, Ni: 0.01% or more, 1.00% or less, Cu: 0.01% or more, 1.00% or less, Mo: 0.01% or more, 0.50% or less, Ti: 0.001% or more, 0.200% or less, Nb: 0.001% or more, 0.200% or less, V: 0.001% or more, 0.500% or less, B: 0.0001% or more, 0.0100% or less, W: 0.0005% or more, 0.1000% or less, Ta: 0.0005% or more, 0.1000% or less, Sn: 0.0010% or less or less, Co: 0.0010% or more and 0.5000% or less, Sb: 0.0010% or more and 0.0500% or less, As: 0.0010% or more and 0.0500% or less, Mg: 0.0001% or more and 0.0500% or less, Ca: 0.0001% or more and 0.0400% or less, Y: 0.0001% or more and 0.0500% or less, La: 0.0001% or more and 0.0500% or less, Ce: 0.0001% or more and 0.0500% or less, and Zr: 0.0001% or more and 0.0500% or less. [3] The steel sheet according to the above [1] or [2] may have a hot-dip galvanized layer on the surface. [4] In the steel sheet according to the above item [3], the hot-dip galvanized layer may be a galvannealed layer. Effect of the Invention
[0010] According to the above aspect of the present invention, it is possible to provide a steel plate having excellent formability and a tensile strength of 1470 MPa or more, which allows sufficient weld joint strength to be obtained. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a diagram illustrating the observation area of the structure and the measurement area of the Mn concentration in a cross section in the sheet thickness direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] A steel sheet according to one embodiment of the present invention (steel sheet according to this embodiment) (a) has a predetermined chemical composition, (b) when the sheet thickness is t, a metal structure at a t / 4 position, which is a position t / 4 from the surface, in a cross section in the sheet thickness direction contains, in volume fractions, 70% or more of martensite and 10% or more of retained austenite, (c) the maximum grain size of the retained austenite is less than 5.0 μm, (d) when the Mn concentration is measured at a plurality of measurement points at 1 μm intervals in a square region of the cross section in the sheet thickness direction, the region being centered at the t / 4 position and having a side length of t / 4, the proportion of measurement points where the Mn concentration is 1.1 times or more the average value of the Mn concentrations of all the plurality of measurement points is less than 10.0%, and (e) the tensile strength is 1470 MPa or more. Each of these will be explained below.
[0013] <Chemical composition> The chemical composition of the steel sheet according to this embodiment will be described below. The percentage of the content of each element is mass % unless otherwise specified.
[0014] C: 0.20% or more, 0.45% or less C (carbon) is an essential element for ensuring the strength of a steel sheet. By setting the C content to 0.20% or more, a desired high strength can be obtained. The C content may be 0.21% or more or 0.22% or more. On the other hand, in order to ensure workability and weldability, the C content is set to 0.45% or less. The C content may be 0.42% or less, 0.40% or less, or 0.38% or less.
[0015] Si: 0.50% or more, 2.50% or less Silicon (Si) is a useful element for industrially manufacturing TRIP steel sheets. By including silicon, the formation of iron carbides in austenite with an increased C concentration is suppressed, and it becomes possible to obtain stable retained austenite even at room temperature. To obtain this effect, the Si content is set to 0.50% or more. On the other hand, in order to ensure the weldability of the steel plate, the Si content is set to 2.50% or less. The Si content may be 2.40% or less, 2.20% or less, or 2.00% or less.
[0016] Mn: 1.50% or more, 3.50% or less Mn (manganese) is a strong austenite stabilizing element and is an effective element for increasing the strength of steel plate. In order to obtain these effects, the Mn content is set to 1.50% or more. The Mn content may be set to 1.60% or more or 1.70% or more. In order to ensure weldability and low-temperature toughness, the Mn content is set to 3.50% or less. The Mn content may be set to 3.40% or less, 3.20% or less, or 3.00% or less.
[0017] Al: 0.005% or more, 1.500% or less Al (aluminum) is an element used for deoxidizing steel, and like Si, it is an effective element for suppressing the formation of iron carbides and retaining retained austenite. Therefore, the Al content is set to 0.005% or more. On the other hand, if Al is contained excessively, the effect becomes saturated and the cost increases unnecessarily, and the transformation temperature of the steel increases, increasing the load during hot rolling. Therefore, the Al content is set to 1.500% or less. The Al content is preferably 1.200% or less, 1.000% or less, or 0.800% or less.
[0018] P: 0% or more, 0.040% or less P (phosphorus) is a solid solution strengthening element and is effective in increasing the strength of steel plate, but excessive content deteriorates weldability and toughness. Therefore, the P content is set to 0.040% or less. The P content is preferably 0.035% or less, 0.030% or less, or 0.020% or less. The P content may be 0%, but reducing the P content to an extreme degree increases the dephosphorization cost. Therefore, from the viewpoint of economic efficiency, the P content may be set to 0.001% or more.
[0019] S: 0% or more, 0.010% or less S (sulfur) is an element contained as an impurity, and forms MnS in steel, which deteriorates toughness and hole expandability. Therefore, the S content is set to 0.010% or less as a range in which the deterioration of toughness and hole expandability is not significant. The S content is preferably 0.005% or less, 0.004% or less, or 0.003% or less. The S content may be 0%, but if the S content is reduced excessively, the desulfurization cost will be high. Therefore, from the viewpoint of economic efficiency, the S content may be set to 0.0001% or more, or 0.001% or more.
[0020] N: 0% or more, 0.0100% or less N (nitrogen) is an element contained as an impurity, and when its content exceeds 0.0100%, it forms coarse nitrides in the steel, deteriorating its bendability and hole expandability. Therefore, the N content is set to 0.0100% or less. The N content is preferably 0.0080% or less, 0.0060% or less, or 0.0050% or less. The N content may be 0%, but if the N content is reduced too much, the cost of denitrification will be high. Therefore, from the viewpoint of economy, the N content may be set to 0.0001% or more.
[0021] O: 0% or more, 0.0060% or less O (oxygen) is an element contained as an impurity, and when its content exceeds 0.0060%, it forms coarse oxides in the steel, deteriorating the bendability and hole expandability. Therefore, the O content is set to 0.0060% or less. The O content is preferably 0.0050% or less or 0.0040% or less. The O content may be 0%, but from the viewpoint of manufacturing costs, the O content may be set to 0.0001% or more.
[0022] The basic chemical composition of the steel sheet according to this embodiment contains the above elements (basic elements), with the balance being Fe and impurities. Here, the term "impurities" refers to components that are mixed in due to various factors in raw materials such as ores and scraps and manufacturing processes during industrial production of steel sheets, and are permissible within a range that does not adversely affect the present invention. However, the steel sheet may contain the following elements (optional elements) instead of part of Fe, if necessary. These elements do not necessarily have to be contained, so the lower limit is 0%. In addition, the following elements may be mixed in from raw material scrap, etc., but may be contained as impurities as long as the content is equal to or less than the upper limit described below.
[0023] Cr: 0% or more, 0.50% or less Ni: 0% or more, 1.00% or less Cu: 0% or more, 1.00% or less Cr (chromium), Ni (nickel) and Cu (copper) are all elements that contribute to improving strength. Therefore, one or more selected from these elements may be contained as necessary. To obtain the above effects, the content of one or more selected from Cr, Ni and Cu is preferably 0.01% or more, more preferably 0.10% or more. On the other hand, a Cr content of more than 0.50%, a Ni content of more than 1.00%, or a Cu content of more than 1.00% may deteriorate the pickling property, weldability, and hot workability. Therefore, the Cr content is 0.50% or less, the Ni content is 1.00% or less, and the Cu content is 1.00% or less. The Cr content may be 0.40% or less, 0.30% or less, or 0.10% or less. The Ni content may be 0.80% or less, 0.60% or less, or 0.20% or less. The Cu content may be 0.80% or less, 0.60% or less, or 0.20% or less.
[0024] Mo: 0% or more, 0.50% or less Mo (molybdenum), like Mn, is an element that improves the hardenability of steel and contributes to improving strength. Therefore, Mo may be contained as necessary. To obtain the above effects, the Mo content is preferably 0.01% or more, and more preferably 0.10% or more. On the other hand, if the Mo content exceeds 0.50%, the hot workability may deteriorate, and the productivity may decrease. Therefore, the Mo content is set to 0.50% or less. The Mo content is preferably 0.40% or less, 0.30% or less, or 0.10% or less.
[0025] Ti: 0% or more, 0.200% or less Nb: 0% or more, 0.200% or less V: 0% or more, 0.500% or less Ti (titanium), Nb (niobium) and V (vanadium) are all elements that contribute to improving the strength of steel sheets by precipitation strengthening, fine grain strengthening by inhibiting the growth of crystal grains, and dislocation strengthening through inhibiting recrystallization. Therefore, one or more elements selected from these elements may be contained as necessary. To obtain the above effects, it is preferable to contain one or more elements selected from 0.001% or more of Ti, 0.0001% or more of Nb, and 0.001% or more of V in the steel sheet. On the other hand, if the content of Ti exceeds 0.200%, if the content of Nb exceeds 0.200%, or if the content of V exceeds 0.500%, coarse carbonitrides may be precipitated, which may deteriorate the formability. Therefore, the Ti content is set to 0.200% or less, the Nb content is set to 0.200% or less, and the V content is set to 0.500% or less. The Ti content may be set to 0.180% or less, 0.150% or less, or 0.100% or less. The Nb content may be set to 0.180% or less, 0.150% or less, or 0.100% or less. The V content may be set to 0.400% or less, 0.300% or less, or 0.100% or less.
[0026] B: 0% or more, 0.0100% or less B (boron) is an element that segregates to the austenite grain boundary during welding to strengthen the grain boundary and contribute to improving the resistance to molten metal embrittlement cracking. Therefore, B may be contained as necessary. To obtain the above effects, the B content is preferably 0.0001% or more, more preferably 0.0005% or more or 0.0008% or more. On the other hand, if the B content exceeds 0.0100%, carbides and nitrides are generated, the above effects are saturated, and the hot workability is deteriorated. Therefore, the B content is set to 0.0100% or less. The B content is preferably 0.0080% or less, 0.0050% or less, or 0.0030% or less.
[0027] W: 0% or more, 0.1000% or less Ta: 0% or more, 0.1000% or less Sn: 0% or more, 0.0500% or less Co: 0% or more, 0.5000% or less As: 0% or more, 0.0500% or less W (tungsten), Ta (tantalum), Sn (tin), Co (cobalt), and As (arsenic) are elements that contribute to improving the strength of the steel sheet by suppressing precipitation strengthening and coarsening of crystal grains. Therefore, these elements may be contained. When the effect is obtained, the W content may be 0.0005% or more, 0.0010% or more, 0.0050% or more, or 0.0100% or more. The Ta content may be 0.0005% or more, 0.0010% or more, 0.0050% or more, or 0.0100% or more. The Sn content may be 0.0010% or more, 0.0020% or more, or 0.0050% or more. The Co content may be 0.0010% or more, 0.0100% or more, or 0.0300% or more. The As content may be 0.0010% or more, 0.0020% or more, or 0.0050% or more. On the other hand, if these elements are present in large amounts, the various properties of the steel sheet may be impaired. Therefore, the W content is set to 0.1000% or less, the Ta content is set to 0.1000% or less, the Sn content is set to 0.0500% or less, the Co content is set to 0.5000% or less, and the As content is set to 0.0500% or less. The W content may be set to 0.0800% or less, 0.0500% or less, or 0.0300% or less. The Ta content may be set to 0.0800% or less, 0.0500% or less, or 0.0300% or less. The Sn content may be set to 0.0400% or less, 0.0300% or less, or 0.0100% or less. The Co content may be set to 0.4000% or less, 0.3000% or less, or 0.1000% or less. The As content may be 0.0400% or less, 0.0300% or less, or 0.0100% or less.
[0028] Mg: 0% or more, 0.0500% or less Ca: 0% or more, 0.0400% or less Y: 0% or more, 0.0500% or less La: 0% or more, 0.0500% or less Ce: 0% or more, 0.0500% or less Zr: 0% or more, 0.0500% or less Sb: 0% or more, 0.0500% or less Ca (calcium), Mg (magnesium), Y (yttrium), La (lanthanum), Ce (cerium), Zr (zirconium), and Sb (antimony) are all elements that contribute to improving formability. Therefore, one or more selected from these elements may be contained as necessary. In order to obtain the above effects, the content of one or more selected from Mg, Ca, Y, La, Ce, Zr, and Sb is preferably 0.0001% or more, or 0.0010% or more. The Sb content is more preferably 0.0020% or more, or 0.0050% or more. On the other hand, Mg, Y, La, Ce, Zr, Sb with a content exceeding 0.0500%, or Ca with a content exceeding 0.0400%, may deteriorate pickling property, weldability, and hot workability. Therefore, the contents of Mg, Y, La, Ce, Zr, and Sb are all set to 0.0500% or less, and the Ca content is set to 0.0400% or less. The contents of Mg, Ca, Y, La, Ce, Zr, and Sb are each preferably set to 0.0350% or less, 0.0300% or less, or 0.0100% or less.
[0029] As described above, the chemical composition of the steel sheet according to this embodiment includes basic elements with the balance being Fe and impurities, or includes basic elements and further includes one or more optional elements with the balance being Fe and impurities.
[0030] <When the plate thickness is t, the metal structure at the t / 4 position, which is the position t / 4 from the surface in the plate thickness direction cross section> [Martensite: 70% by volume or more] In the steel plate according to the present embodiment, the volume fraction of martensite is set to 70% or more in order to ensure a tensile strength of 1470 MPa or more. If the volume fraction of martensite is less than 70%, sufficient tensile strength cannot be ensured. If the volume fraction of martensite is more than 90%, a sufficient volume fraction of retained austenite cannot be ensured, so the volume fraction of martensite is 90% or less. In the steel sheet according to the present embodiment, martensite includes so-called fresh martensite and tempered martensite.
[0031] [Retained austenite: 10% or more by volume] Retained austenite is a structure that improves the elongation of steel sheets by the TRIP effect, which transforms into martensite through stress-induced transformation during deformation of the steel sheet. Therefore, the volume fraction of retained austenite is set to 10% or more. The higher the volume fraction of retained austenite, the higher the elongation of the steel sheet, but to obtain a large amount of retained austenite, it is necessary to contain a large amount of alloying elements such as C. Therefore, the volume fraction of retained austenite is set to 30% or less.
[0032] [Remainder: one or more selected from ferrite, pearlite, and bainite] The remainder other than martensite and retained austenite may include one or more selected from ferrite, pearlite, and bainite. The volume fraction of the remainder is, for example, 10% or less, or 5% or less. The volume fraction of the remainder may be 0%.
[0033] The volume fraction of martensite at the t / 4 position is determined by the following procedure. The observation surface of the sample is etched with a Lepera solution, and a 100 μm×100 μm area within 1 / 8 to 3 / 8 of the plate thickness from the surface, centered at 1 / 4 of the plate thickness from the surface of the plate thickness direction cross section as shown in FIG. 1A, is observed at a magnification of 3000 times using a FE-SEM. In Lepera corrosion, martensite and retained austenite are not corroded, so the area ratio of the uncorroded area is the total area ratio of martensite and retained austenite. In this embodiment, the total area ratio of martensite and retained austenite is considered to be the total volume ratio of these. The volume ratio of martensite is calculated by subtracting the volume ratio of retained austenite measured by a method described later from the area ratio (i.e., volume ratio) of the uncorroded area.
[0034] The volume fraction of retained austenite can be calculated by measurements using an X-ray diffractometer. In measurements using an X-ray diffractometer, first, the area from the plate surface (rolled surface) of the sample to a surface at a depth of 1 / 4 of the plate thickness is removed by mechanical and chemical polishing. Next, on the surface at a depth of 1 / 4 of the plate thickness t, MoKα rays are used as characteristic X-rays to determine the integrated intensity ratio of the diffraction peaks of (200), (211) of the bcc phase and (200), (220), and (311) of the fcc phase, and the volume fraction of retained austenite is calculated based on these integrated intensity ratios.
[0035] The volume fractions of ferrite, bainite, and pearlite at the t / 4 position are determined by the following procedure: The observation surface of the sample is etched with a repeller solution, and an area of 100 μm × 100 μm within a range of 1 / 8 to 3 / 8 of the plate thickness from the surface, centered at a position 1 / 4 of the plate thickness from the surface of the plate thickness direction cross section as shown in A of Figure 1, is observed at a magnification of 3000 times using an FE-SEM. Regions that do not contain cementite in the crystal are judged as ferrite, regions that contain cementite in the crystal and where the cementite is arranged in a lamellar shape are judged as pearlite, and regions that contain cementite in the crystal and where the cementite has multiple variants are judged as bainite, and the area ratio is calculated using the point counting method (in accordance with ASTM E562). The area ratio and volume ratio are considered to be equivalent, and the obtained area ratio of each structure is taken as the volume ratio.
[0036] [Maximum grain size of retained austenite in the metal structure at the t / 4 position: less than 5.0 μm] If coarse retained austenite or fresh martensite is present in the heat-affected zone of welding, cracks can easily initiate from these. In order to suppress cracks originating from retained austenite (γ) or fresh martensite in the heat-affected zone in order to increase the strength of welded joints, it is sufficient for the maximum grain size of retained γ to be less than 5.0 μm at the t / 4 position of the final product (steel plate). Although there is no lower limit for the maximum particle size, it is not easy to make it less than 0.1 μm, so the practical lower limit is 0.1 μm.
[0037] The maximum grain size of retained austenite is determined by the following method: A scanning electron microscope (SEM) and backscattered electron beam diffraction (EBSD) are used to observe the structure. First, the observation surface of the sample is wet polished with emery paper, and then buffed with diamond abrasive grains with an average diameter of 1 μm to give a mirror finish. Next, in order to remove the distortion introduced to the polished surface by the mechanical polishing described above, colloidal silica polishing is performed using a suspension with alcohol as a solvent. In colloidal silica polishing, if the load increases during polishing, further distortion may be introduced, so it is important to keep the load low during polishing. For this reason, automatic polishing with BUEHLER Vibromet 2 may be performed for 1 hour at 40% power setting for colloidal silica polishing. Observe the sample prepared by the above procedure within a range of 1 / 8 to 3 / 8 of the plate thickness from the surface centered at the t / 4 position using SEM-EBSD. The magnification for observation is selected from 1000 to 9000 times, at which the number of retained austenite grains in the microstructure is 10 or more, for example, 3000 times. Measure the crystal orientation data of FCC-iron using SEM-EBSD. The measurement interval (STEP) is 0.01 to 0.10 μm, and 0.05 μm may be selected. In the crystal orientation MAP data of FCC-iron obtained under these measurement conditions, the boundary where the crystal orientation difference is 15 degrees or more is regarded as the crystal grain boundary, and the maximum grain size of the retained austenite is obtained.
[0038] <When the Mn concentration is measured at multiple measurement points at 1 μm intervals in a square region with a side length of t / 4 centered at the t / 4 position on a cross section in the sheet thickness direction, the percentage of measurement points where the Mn concentration is 1.1 times or more the average value of the Mn concentrations at multiple measurement points (all measurement points): less than 10.0%> As described above, if coarse retained austenite or fresh martensite is present in the heat-affected zone of a welded joint, these will act as the starting points for cracks, and cracks will easily occur. In order to suppress such cracks, it is effective to refine the retained austenite in the steel sheet before welding. Since coarse retained austenite is generated in the Mn segregated area, suppressing Mn segregation is effective in refining the retained austenite. Specifically, when the Mn concentration is measured at multiple measurement points at 1 μm intervals using an EPMA (Electron Probe Micro Analyzer) in a square region with a side length of t / 4 centered at the t / 4 position in a cross section in the sheet thickness direction as shown in B in Figure 1, the proportion (number proportion) of measurement points where the Mn concentration is 1.1 times or more (1.1 or more when the average value is 1.0) relative to the average Mn concentration of the multiple measurement points (all measurement points) must be less than 10.0%. In other words, when the segregation degree is defined as "concentration at each measurement point / average concentration of all measurement points in the measurement region," the proportion where this segregation degree is 1.1 or more must be less than 10.0%.
[0039] <Mechanical properties> [Tensile strength: 1470MPa or more] The steel plate according to this embodiment has a tensile strength of 1470 MPa or more, taking into consideration its contribution to weight reduction of automobile bodies. In addition, in the steel sheet according to this embodiment, the tensile strength x total elongation (TS x tEl) is preferably 18000 MPa·% or more. The tensile strength (TS) and total elongation (tEl) are determined by taking a JIS No. 5 tensile test piece from the steel plate in the direction perpendicular to the rolling direction and conducting a tensile test in accordance with JIS Z 2241:2011.
[0040] [Plating layer] The steel sheet according to the present embodiment described above may have a hot-dip galvanized layer on the surface. The presence of the hot-dip galvanized layer on the surface improves corrosion resistance. For example, when a steel sheet is used in a corrosive environment, there are concerns about holes, etc., so even if the steel sheet is made stronger, it may not be possible to make the sheet thinner than a certain thickness. One of the purposes of increasing the strength of steel sheets is to reduce the weight by making them thinner, so even if a high-strength steel sheet is developed, if the corrosion resistance is low, the application sites are limited. For this reason, it is possible to apply a highly corrosion-resistant coating such as hot-dip galvanizing to the steel sheet. The coating layer is, for example, a zinc coating layer such as a hot-dip galvanizing layer or an electrolytic zinc coating layer. The zinc coating layer may also be a coating containing Si, Al and / or Mg in addition to Zn. The hot-dip galvanized layer may be an alloyed hot-dip galvanized layer, in which Fe is incorporated into the hot-dip galvanized layer by alloying treatment, and thus excellent weldability and paintability can be obtained. In addition, an upper layer of plating may be applied on the galvanized layer for the purpose of improving paintability and weldability. In addition, in the cold-rolled steel sheet according to the present embodiment, various treatments, such as chromate treatment, phosphate treatment, lubricity improvement treatment, weldability improvement treatment, etc., may be applied on the hot-dip galvanized layer.
[0041] [Joint strength] In the steel plate according to this embodiment, in consideration of weldability in the assembly of an automobile body, it is preferable that the joint strength when joined exceeds 6.0 kN. The joint strength is determined by taking test pieces as specified in JIS Z 3137 (1999) from the steel plate in a direction perpendicular to the rolling direction, welding them using a servo motor pressure type single-phase AC spot welding machine (power frequency 50 Hz), and then conducting a cross tensile test in accordance with JIS Z 3137 (1999).
[0042] <Manufacturing method> The steel plate according to this embodiment can be manufactured by a manufacturing method including the following steps. (I) a first Mn segregation reduction step in which a slab obtained by continuous casting or the like is held at 1,300°C or higher for 5.0 hours or more and then cooled to 200°C or lower at an average cooling rate of 20°C / hour or more and 80°C / hour or less; (II) a second Mn segregation reduction step of heating the slab and holding it at 1200°C or higher for 1.0 hour or more; (III) a hot rolling step of hot rolling the slab after the second Mn segregation reducing step to obtain a hot rolled steel sheet; (IV) a winding step of winding the hot-rolled steel sheet; (V) a cold rolling step of cold rolling the hot-rolled steel sheet after the coiling step to obtain a cold-rolled steel sheet; (VI) An annealing step of annealing the cold-rolled steel sheet. Each step will be described below.
[0043] [First Mn segregation reduction process] In the first Mn segregation reduction step, a slab obtained by continuous casting or the like is held at 1,300°C or higher for 5.0 hours or more before the hot rolling step, and then cooled to 200°C or lower at an average cooling rate of 20°C / hour or more and 80°C / hour or less. By holding the slab at a high temperature of 1300°C or higher for 5.0 hours or more, the diffusion rate of Mn is increased and Mn segregation is reduced. However, this holding alone is not sufficient to reduce Mn segregation. Furthermore, it is necessary to cool the slab to 200°C or lower at an average cooling rate of 20°C / hour or more. By cooling the slab to 200°C or lower at an average cooling rate of 20°C / hour or more, dislocations due to thermal contraction differences are introduced. These dislocations become a high-speed diffusion path for Mn during heating in the next step, the second Mn segregation step, so Mn can be diffused efficiently and the degree of Mn segregation is reduced. The faster the average cooling rate, the more dislocations are introduced. However, if the cooling rate is too fast, the thermal contraction difference becomes excessive, increasing the risk of slab cracking, so the average cooling rate is set to 80°C / hour or less. If the heating temperature is too high, the manufacturing cost increases, and if the heating time is too long, the productivity decreases. From these viewpoints, the heating temperature of the slab may be set to 1400°C or less, and the holding time at 1300°C or more may be set to 50.0 hours or less.
[0044] [Second Mn segregation reduction process] In the second Mn segregation reducing step, the slab after the first Mn segregation reducing step is heated to 1200° C. or higher in a heating furnace and held at that temperature range for 1.0 hour or more. By holding the slab at 1200°C or higher for 1.0 hour or more after the first Mn segregation step, Mn can be diffused by utilizing the dislocations introduced into the slab as a high-speed diffusion path, which further reduces Mn segregation. If the heating temperature is too high, the manufacturing cost increases, and if the heating time is too long, the productivity decreases. From these viewpoints, the heating temperature of the slab may be set to 1300°C or less, and the holding time at 1200°C or more may be set to 5.0 hours or less. This second Mn segregation reducing step may be performed in a hot rolling heating furnace as heating for hot rolling.
[0045] [Hot rolling process] In the hot rolling step, the slab that has been heated to 1200° C. or higher in a heating furnace in the second Mn segregation reducing step and held at that temperature range for 1.0 hour or more is hot rolled to obtain a hot-rolled steel sheet. The hot rolling conditions are not particularly limited. For example, the finish rolling may be completed at 800° C. or more and 980° C. or less, and then the steel sheet may be cooled to a coiling temperature of 600° C. or less at an average cooling rate of 2.5° C. / sec or more to a temperature of 600° C. or more and 750° C. or less.
[0046] [Winding process] [Cold rolling process] The hot-rolled steel sheet after the hot rolling process is coiled under known conditions to form a hot-rolled coil, and then cold-rolled under known conditions to form a cold-rolled steel sheet. For example, the total rolling reduction may be 20% or more and 85% or less.
[0047] [Annealing process] In the annealing process, the cold-rolled steel sheet is heated to a soaking temperature of Ac3°C or higher and lower than 900°C so that it has a structure containing 70 volume% or more of martensite and 10 volume% or more of retained austenite after the annealing process, held at this soaking temperature for 5 seconds or more, then cooled to a temperature range of (Ms point - 100)°C or higher and Bs point or lower at an average cooling rate of 10°C / sec or higher and 50°C / sec or lower, and further held in the temperature range of (Ms point - 100)°C or higher and Bs point or lower for 10 seconds or more and 600 seconds or less.
[0048] In order to sufficiently promote austenitization, the steel sheet is heated to at least the Ac3 point (°C) and soaked at that temperature (maximum heating temperature). However, if the heating temperature is excessively increased, not only will the austenite grain size increase, causing a deterioration in toughness, but it may also lead to damage to the annealing equipment. Therefore, the maximum heating temperature is set to 950°C or less, and preferably 900°C or less. If the soaking time is short, austenitization does not proceed sufficiently. Therefore, the soaking time is set to 5 seconds or more, preferably 30 seconds or more or 60 seconds or more. On the other hand, if the soaking time is too long, productivity is hindered. Therefore, the soaking time is preferably set to 600 seconds or less, more preferably 500 seconds or less. During soaking, it is not necessary to keep the steel sheet at a constant temperature, and the temperature may fluctuate within a range that satisfies the above conditions. The Ac3 point is determined in the following manner. Ac3(℃)=910-203×√[C]+44.7×[Si]-30×[Mn]+700×[P]-20×[Cu]-15.2×[Ni]-11×[Cr]+31.5×[Mo]+400×[Ti]+104×[V]+120×[Al] Here, [C], [Si], [Mn], [P], [Cu], [Ni], [Cr], [Mo], [Ti], [V] and [Al] are the contents (mass%) of each element contained in the slab.
[0049] The steel sheet is then cooled to a temperature range of (Ms point - 100)°C or more and Bs point (°C or less) at an average cooling rate of 10 to 50°C / sec, and the temperature of the steel sheet is further maintained in this temperature range. The holding time of the steel sheet in the temperature range of (Ms point - 100)°C or more and Bs point or less is 10 to 600 seconds. The Ms point is the temperature at which martensite begins to form during cooling after quenching. In the manufacturing method according to the present embodiment, the value calculated by the following formula is regarded as the Ms point (° C.). Ms(℃)=541-474×[C] / (1-Sα / 100)-15×[Si]-35×[Mn]-17×[Cr]-17×[Ni]+19×[Al] The Bs point is the temperature (° C.) at which bainite transformation starts during cooling after quenching. In the manufacturing method according to the present embodiment, the value calculated by the following formula is regarded as the Bs point. Bs(℃)=820-290×[C] / (1-Sα / 100)-37×[Si]-90×[Mn]-65×[Cr]-50×[Ni]+70×[Al] Here, the [element symbol] included in the Ms calculation formula and the Bs calculation formula indicates the content (mass%) of each element included in the steel sheet, and the symbol Sα included in the formula indicates the ferrite fraction (volume%) of the steel sheet at the time when heating for quenching is completed. It is difficult to determine the area ratio of ferrite in a steel plate during manufacturing. For this reason, a steel plate that has undergone the same temperature history as the actual manufacturing process of the steel plate is prepared in advance, the area ratio of ferrite in the center of the steel plate is determined, and the area ratio of ferrite is used to calculate Ms and Bs. The ferrite fraction of a steel plate is largely dependent on the heating temperature for quenching. For this reason, when considering the cooling conditions, the manufacturing conditions of the process before cooling are first determined, and a steel plate is manufactured under those manufacturing conditions, and the ferrite fraction of the steel plate is measured, so that Sα can be specified. In addition, when the cooling rate of quenching is fast (a cooling rate at which ferrite transformation does not occur), the ferrite fraction after quenching can also be regarded as the ferrite fraction at the time when the heating for quenching is completed. The average cooling rate is the difference between the surface temperature of the steel sheet at the start of cooling and the surface temperature of the steel sheet at the end of cooling (i.e., the cooling stop temperature), divided by the cooling time. For example, when annealing and temperature holding, which will be described later, are performed using a furnace, the time when cooling starts is the time when the steel sheet is removed from the annealing furnace, and the time when cooling ends is the time when the steel sheet is loaded into the temperature holding furnace. The holding time in the temperature range of (Ms point - 100) °C or more and Bs point (°C) or less means the time during which the surface temperature of the steel sheet is within this temperature range. The temperature of the steel sheet may fluctuate within this temperature range.
[0050] By setting the average cooling rate of the steel sheet from (Ms point - 100)°C to Bs point (°C) at 10 to 50°C / sec, a sufficient amount of martensite and / or bainite can be generated in the steel sheet. By setting the cooling stop temperature of the steel sheet within the temperature range of (Ms point - 100)°C to Bs point (°C), a sufficient amount of retained austenite can be generated in the subsequent temperature holding. Furthermore, by setting the holding time of the steel sheet in the temperature range of (Ms point - 100)°C to Bs point (°C) for 10 to 600 seconds, a sufficient amount of retained austenite can be generated and a decrease in the tensile strength of the steel sheet can be prevented.
[0051] [Hot-dip galvanizing process] [Alloying process] The cold-rolled steel sheet after annealing may be immersed in a hot-dip galvanizing bath to form a hot-dip galvanized steel sheet having a hot-dip galvanized layer on the surface. The hot-dip galvanized steel sheet may also be alloyed to form an alloyed hot-dip galvanized steel sheet. In this case, the temperature of the steel sheet can be maintained as described above by utilizing the heat applied to the steel sheet during hot-dip galvanizing and alloying. Known conditions can be applied to both processes. EXAMPLES
[0052] Slabs (steels Nos. A to Z) having the chemical compositions (units are mass %, the remainder being Fe and impurities) shown in Tables 1-1 and 1-2 were produced by continuous casting. These slabs were heated, held, and cooled to 200°C or lower as shown in Tables 2-1 and 2-2. The slab was then reheated and held as shown in Tables 2-1 and 2-2, and then hot rolled so that the finish rolling was completed at 800 to 980°C. The slab was then cooled to a coiling temperature of 600°C or less at an average cooling rate of 2.5°C / sec or more to a temperature of 600°C or more and 750°C or less, and coiled at 600°C or less to obtain a hot-rolled steel sheet of 2.0 to 4.0 mm. Furthermore, these hot rolled steel sheets were subjected to cold rolling at a rolling reduction of 20 to 85% to obtain cold rolled steel sheets having a thickness of 0.8 to 2.0 mm. These cold-rolled steel sheets were annealed under the conditions shown in Tables 3-1 and 3-2 (however, in the cases where the slabs were cracked, no processes subsequent to hot rolling were carried out). As shown in Tables 3-1 and 3-2, some of the cold-rolled steel sheets were subjected to hot-dip galvanizing, and some of the cold-rolled steel sheets were subjected to alloying treatment.
[0053] Samples were taken from the obtained cold-rolled steel sheets (including plated steel sheets) in the manner described above, and the microstructures were observed to determine the martensite, retained austenite, and other volume fractions, and the maximum grain size of retained austenite. Furthermore, the Mn concentration was measured using EPMA in the manner described above, and the ratio of measurement points where the measurement point concentration / average concentration of all measurement points in the measurement area (segregation degree) was 1.1 or more was determined. The results are shown in Tables 4-1 and 4-2.
[0054] In addition, JIS No. 5 tensile test pieces were taken from the annealed cold-rolled steel sheets in a direction perpendicular to the rolling direction, and tensile tests were performed according to JIS Z 2241:2011 to determine the tensile strength and total elongation. A material was judged to have high strength and excellent formability if its tensile strength (TS) was 1,470 MPa or more and its tensile strength × total elongation (TS × tEl) was 18,000 MPa·% or more. The results are shown in Tables 5-1 and 5-2.
[0055] In addition, test pieces described in JIS Z 3137 (1999) were taken from the obtained cold-rolled steel sheets in a direction perpendicular to the rolling direction, and welding was performed using a servo motor pressure type single-phase AC spot welding machine (power frequency 50 Hz) with the electrode diameter set to 6 mm, welding pressure set to 4 kN, welding current set to 6.0 kA to 9.0 kA, current flow time set to 0.4 seconds, and holding time set to 0.1 seconds so that the nugget diameter was 5√t (t: plate thickness). Thereafter, a cross tensile test was performed according to JIS Z 3137 (1999) to determine the joint strength. If the joint strength was more than 6.0 kN, it was determined that the welded joint strength was excellent. The results are shown in Tables 5-1 and 5-2.
[0056] [Table 1-1]
[0057] [Table 1-2]
[0058] [Table 2-1]
[0059] [Table 2-2]
[0060] [Table 3-1]
[0061] [Table 3-2]
[0062] [Table 4-1]
[0063] [Table 4-2]
[0064] [Table 5-1]
[0065] [Table 5-2]
[0066] As can be seen from Tables 1-1 to 5-2, all of the inventive examples are steel plates with excellent formability and tensile strengths of 1470 MPa or more, and sufficient welded joint strength is obtained. On the other hand, for the comparative examples in which at least one of the chemical composition, the volume fraction of each phase in the microstructure, the maximum grain size of retained austenite, and the proportion of measurement points where the segregation degree is 1.1 or more does not satisfy the range of the present invention, at least one of the tensile strength, formability, and welded joint strength does not satisfy the target value. [Explanation of symbols]
[0067] A. Tissue observation area (100 μm × 100 μm area in the range of t / 8 to 3t / 8 centered at the t / 4 position) B. Measurement area of Mn concentration (square area with one side of length t / 4 centered at the t / 4 position) t Plate thickness [Industrial Applicability]
[0068] INDUSTRIAL APPLICABILITY According to the present invention, it is possible to provide a steel plate having excellent formability, a tensile strength of 1470 MPa or more, and capable of obtaining sufficient welded joint strength, and therefore has high industrial applicability.
Claims
1. In mass percent, C: 0.20% or more, 0.45% or less, Si: 0.50% or more, 2.50% or less, Mn: 1.50% or more, 3.50% or less, Al: 0.005% or more, 1.500% or less, P: 0% or more, 0.040% or less, S: 0% or more, 0.010% or less, N: 0% or more, 0.0100% or less, O: 0% or more, 0.0060% or less, Cr: 0% or more, 0.50% or less, Ni: 0% or more, 1.00% or less, Cu: 0% or more, 1.00% or less, Mo: 0% or more, 0.50% or less, Ti: 0% or more, 0.200% or less, Nb: 0% or more, 0.200% or less, V: 0% or more, 0.500% or less, B: 0% or more, 0.0100% or less, W: 0% or more, 0.1000% or less, Ta: 0% or more, 0.1000% or less, Sn: 0% or more, 0.0500% or less, Co: 0% or more, 0.5000% or less, Sb: 0% or more, 0.0500% or less, As: 0% or more, 0.0500% or less, Mg: 0% or more, 0.0500% or less, Ca: 0% or more, 0.0400% or less, Y: 0% or more, 0.0500% or less, La: 0% or more, 0.0500% or less, Ce: 0% or more, 0.0500% or less, Zr: 0% or more and 0.0500% or less, and The balance: Fe and impurities, having a chemical composition consisting of When the plate thickness is t, the metal structure at the t / 4 position, which is a position t / 4 from the surface in the plate thickness direction cross section, is expressed as the volume fraction: Martensite: 70% or more, Retained austenite: 10% or more, The maximum grain size of the retained austenite is less than 5.0 μm, When the Mn concentration is measured at a plurality of measurement points at 1 μm intervals in a square region of the sheet thickness direction cross section, the region being centered at the t / 4 position and having a side length of t / 4, the proportion of measurement points at which the Mn concentration is 1.1 times or more the average value of the Mn concentrations at all of the plurality of measurement points is less than 10.0%, Tensile strength is 1470 MPa or more steel plate.
2. The chemical composition, in mass%, Cr: 0.01% or more, 0.50% or less, Ni: 0.01% or more, 1.00% or less, Cu: 0.01% or more, 1.00% or less, Mo: 0.01% or more, 0.50% or less, Ti: 0.001% or more, 0.200% or less, Nb: 0.001% or more, 0.200% or less, V: 0.001% or more, 0.500% or less, B: 0.0001% or more, 0.0100% or less, W: 0.0005% or more, 0.1000% or less, Ta: 0.0005% or more, 0.1000% or less, Sn: 0.0010% or more, 0.0500% or less, Co: 0.0010% or more, 0.5000% or less, Sb: 0.0010% or more, 0.0500% or less, As: 0.0010% or more, 0.0500% or less, Mg: 0.0001% or more, 0.0500% or less, Ca: 0.0001% or more, 0.0400% or less, Y: 0.0001% or more, 0.0500% or less, La: 0.0001% or more, 0.0500% or less, Ce: 0.0001% or more and 0.0500% or less, and Zr: 0.0001% or more, 0.0500% or less, Contains one or more selected from the group consisting of The steel sheet according to claim 1.
3. The surface has a hot-dip galvanized layer. The steel sheet according to claim 1 or 2.
4. The hot-dip galvanized layer is a galvannealed layer. The steel sheet according to claim 3.
Citation Information
Patent Citations
Preparation of steel material with reduced microsegregation
JP1980128533A
High strength thin steel sheet having excellent elongation and hole expandability, and method for producing the same
JP2007070661A
Method for producing ultra-high-strength coated or uncoated steel sheet and resulting steel sheet
JP2017524818A
Cold-rolled high-strength steel with a tensile strength of 1500 MPa or more and excellent formability, and its manufacturing method
JP2019534941A
A method for manufacturing high-strength thin steel sheets with excellent elongation and hole-expanding properties.
JP4445365B2