Tempered glass and its manufacturing method

The described manufacturing process for tempered glass, involving slow cooling and heat treatment, addresses warpage issues by regenerating heterogeneous layers, ensuring uniform stress distribution and high compressive stress on both surfaces, thereby improving mechanical performance.

JP7578911B2Active Publication Date: 2024-11-07NIPPON ELECTRIC GLASS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021039209
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-11
Publication Date
2024-11-07
Estimated Expiration
2041-03-11

AI Technical Summary

Technical Problem

Tempered glass manufactured by chemically strengthening after mechanical polishing of one main surface experiences significant warpage due to stress differences between main surfaces caused by heterogeneous layers promoting uneven ion exchange.

Method used

A manufacturing process involving slow cooling, heat treatment at a holding temperature of -15°C or higher for 3 minutes or more, and chemical strengthening to regenerate heterogeneous layers on both main surfaces, ensuring uniform compressive stress and minimizing warpage.

Benefits of technology

The process results in tempered glass with high compressive stress on both main surfaces and reduced warpage, achieving superior mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578911000002
    Figure 0007578911000002
  • Figure 0007578911000003
    Figure 0007578911000003
  • Figure 0007578911000004
    Figure 0007578911000004
Patent Text Reader

Abstract

To provide strengthened glass with less warp, while having high compressive stress on both a first principal surface and a second principal surface .SOLUTION: A method for manufacturing strengthened glass includes: a preparation step S1 of preparing glass for strengthening having a first principal surface and a second principal surface, and a heterogeneous layer at a surface layer part of the second principal surface; a heat treatment step S2 of holding the glass for strengthening at a holding temperature of a strain point -15°C or higher for 3 minutes or longer to apply a heat treatment; and a chemical strengthening step S3 of chemically strengthening the glass for strengthening through an ion exchange treatment to obtain strengthened glass.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to tempered glass and a method for producing the same. [Background technology]

[0002] In recent years, tempered glass has been widely used as cover glass for various devices such as mobile phones (especially smartphones), digital cameras, PDAs (personal digital assistants), touch panel displays, etc. Such tempered glass is generally produced by chemically tempering tempered glass through ion exchange treatment (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2013 / 088856 Summary of the Invention [Problem to be solved by the invention]

[0004] In the manufacturing process of tempered glass, before chemically tempering the glass to be tempered, one main surface of the glass to be tempered (hereinafter referred to as the first main surface) may be removed by mechanical polishing, etc. Such removal of the surface layer portion of the first main surface is performed, for example, as part of processing the end face shape of the glass to be tempered into a special shape.

[0005] However, as a result of intensive research by the present inventors, it has been found that when the surface layer portion of the first main surface of the glass to be strengthened is removed by polishing or the like in this manner, the strengthened glass obtained by chemical strengthening suffers from significant warping that does not satisfy product standards.

[0006] The cause of this warpage has not been clearly elucidated, but is currently believed to be as follows. That is, a heterogeneous layer formed during the molding process of the glass to be strengthened exists in the surface layer portion of each of the first main surface and the second main surface located on the opposite side. This heterogeneous layer has the property of promoting ion exchange. Therefore, if the heterogeneous layer is removed by mechanical polishing or the like of the surface layer portion of the first main surface, the progress of ion exchange differs between the first main surface and the second main surface during chemical strengthening, resulting in a stress difference between the two main surfaces, and this stress difference causes a large warpage in the strengthened glass.

[0007] Furthermore, the first main surface from which the heterogeneous layer promoting ion exchange has been removed tends to have a lower compressive stress during chemical strengthening, which may result in a decrease in the strength of the strengthened glass.

[0008] Even if the heterogeneous layer on the first main surface side is not completely removed, it is believed that a similar phenomenon will occur if the thickness of the heterogeneous layer on the first main surface side and the thickness of the heterogeneous layer on the second main surface side are significantly different.

[0009] An object of the present invention is to provide a tempered glass that has high compressive stress on both of its first and second main surfaces and is small in warpage. [Means for solving the problem]

[0010] (1) The present invention has been invented to solve the above-mentioned problems, and comprises, in this order, a molding step of molding glass to be tempered, the glass having a first main surface and a second main surface opposite the first main surface; an annealing step of annealing the glass to be tempered at a cooling rate of 0.5°C / s or more immediately after forming; a removal step of removing a surface layer portion of the first main surface of the glass to be tempered; a heat treatment step of heat treating the glass to be tempered by holding it at a temperature of -15°C or more at its strain point for 3 minutes or more; and a chemical strengthening step of chemically strengthening the glass to be tempered by ion exchange treatment to obtain tempered glass.

[0011] In the tempered glass that has been subjected to the above-mentioned slow cooling step (cooling rate: 0.5°C / s or more), a heterogeneous layer is formed on the surface layer portion of each of the first main surface and the second main surface, but when the surface layer portion of the first main surface is removed in the removal step, a part or all of the heterogeneous layer on the first main surface side is also removed. Therefore, if chemical strengthening is performed in this state, the tempered glass may be significantly warped. Therefore, in the present invention, after the removal step and before the chemical strengthening step, a heat treatment step is performed in which the tempered glass is held at a holding temperature of the strain point -15°C or more for 3 minutes or more for heat treatment. By such heat treatment, a heterogeneous layer can be reproduced (or formed) on the surface layer portion of the first main surface of the tempered glass. Therefore, even if the tempered glass is subsequently chemically strengthened, the tempered glass can be prevented from being significantly warped. In addition, since the glass is chemically strengthened in a state in which a heterogeneous layer is formed on the surface layer portion of each of the first main surface and the second main surface, high compressive stress can be realized on both main surfaces.

[0012] (2) In the above configuration (1), it is preferable that, in the removing step, only the surface layer portion of the first main surface is removed out of the first main surface and the second main surface.

[0013] In this manner, only the heterogeneous layer on the first main surface side of the glass to be strengthened is removed, so that if chemical strengthening is performed in this state, the strengthened glass is likely to warp. In other words, the regeneration effect of the heterogeneous layer by the heat treatment step of the present invention is particularly useful.

[0014] (3) The present invention has been invented to solve the above-mentioned problems, and includes the steps of: a preparation step of preparing glass to be tempered, the glass having a first main surface and a second main surface opposite the first main surface, and a heterogeneous layer at a surface layer portion of the second main surface; a heat treatment step of heat treating the glass to be tempered by holding it at a temperature of not less than the strain point -15°C for not less than 3 minutes; and a chemical strengthening step of chemically strengthening the glass to be tempered by ion exchange treatment to obtain tempered glass, in this order.

[0015] In this way, after the preparation step and before the chemical strengthening step, a heat treatment step is performed in which the tempered glass is held at a holding temperature of -15°C or higher, which is equal to or higher than the strain point, for 3 minutes or more. This heat treatment allows a heterogeneous layer to be formed (regenerated) in the surface layer portion of the first main surface of the tempered glass. Therefore, even if the tempered glass is subsequently chemically strengthened, the tempered glass can be prevented from being significantly warped. In addition, since the glass is chemically strengthened in a state in which a heterogeneous layer is formed in the surface layer portions of the first and second main surfaces, high compressive stress can be achieved in both main surfaces.

[0016] (4) In the above configuration (3), the heterogeneous layer in the preparation step may be formed by slowly cooling the glass to be tempered at a cooling rate of 0.5° C. / s or more during the forming process.

[0017] (5) In any one of the above configurations (1) to (4), the glass to be tempered is preferably formed by an overflow downdraw method or a slot downdraw method.

[0018] (6) In any one of the above configurations (1) to (5), the heat treatment step is preferably performed with a holding temperature of not more than the strain point plus 50° C. and a holding time at the holding temperature of not less than 10 minutes.

[0019] In this way, the heat treatment is carried out at a relatively low temperature for a long period of time, so that unintended deformation of the glass to be strengthened can be suppressed.

[0020] (7) In any one of the above configurations (1) to (5), the heat treatment step is preferably performed at a holding temperature of the strain point plus 85° C. or higher.

[0021] In this way, the formation (regeneration) of the heterogeneous layer can be carried out efficiently.

[0022] (8) In any one of the above configurations (1) to (7), in the heat treatment step, the holding time at the holding temperature is preferably 60 minutes or less.

[0023] In the heat treatment process, it is believed that the longer the holding time at the holding temperature, the more effective the formation (regeneration) of the heterogeneous layer, but a holding time of 60 minutes or less can form (regenerate) the heterogeneous layer to a level that does not cause practical problems. Therefore, when considering production efficiency, it is preferable that the holding time at the holding temperature is 60 minutes or less.

[0024] (9) In any of the above configurations (1) to (8), the tempered glass obtained by the chemical tempering step preferably has an absolute value of a difference (CS1-CS2) between a compressive stress CS1 at the first main surface and a compressive stress CS2 at the second main surface of 40 MPa or less.

[0025] By carrying out the above-mentioned heat treatment process in advance, it is possible to easily and reliably produce tempered glass having an absolute value of CS1-CS2 of 40 MPa or less in the chemical tempering process. Furthermore, tempered glass having a small absolute value of CS1-CS2 can reliably suppress the occurrence of large warpage.

[0026] (10) In any one of the above configurations (1) to (9), the glass to be tempered may be a plate glass having a thickness of 0.3 mm or less.

[0027] In other words, the present invention is an effective technique for producing such very thin plate glass.

[0028] (11) In any of the above configurations (1) to (10), the glass to be tempered preferably contains, as a glass composition, by mol %, 50 to 80% of SiO2, 5 to 25% of Al2O3, 0 to 15% of B2O3, 0 to 20% of Li2O, 1 to 20% of Na2O, and 0 to 10% of K2O.

[0029] Glass to be strengthened having such a glass composition is prone to warping problems associated with the heterogeneous layer during chemical strengthening, and the effects of the present invention are particularly useful.

[0030] (12) The present invention has been invented to solve the above problems, and provides tempered glass having a first compressive stress layer in a surface layer portion of a first main surface, and a second compressive stress layer in a surface layer portion of a second main surface opposite the first main surface, wherein an absolute value of a difference (Ra1-Ra2) between a surface roughness Ra1 of the first main surface and a surface roughness Ra2 of the second main surface is 0.1 nm or more, each of a compressive stress CS1 of the first main surface and a compressive stress CS2 of the second main surface is 820 MPa or more, and an absolute value of a difference (CS1-CS2) between the compressive stress CS1 of the first main surface and the compressive stress CS2 of the second main surface is 40 MPa or less.

[0031] In this way, even when the absolute value of the difference between the surface roughness Ra1 of the first main surface and the surface roughness Ra2 of the second main surface is large, such as when the first main surface is a polished surface and the second main surface is an unpolished surface, it is possible to provide tempered glass that has high compressive stress on both main surfaces and is small in warpage. Effect of the Invention

[0032] According to the present invention, it is possible to provide a tempered glass having high compressive stress at both the first main surface and the second main surface and having small warpage. [Brief description of the drawings]

[0033] [Figure 1] FIG. 1 is a flow diagram showing a method for producing tempered glass according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a glass to be tempered in a preparation step according to the first embodiment. [Diagram 3] 4 is a graph illustrating heat treatment conditions in the heat treatment step of the first embodiment. [Figure 4] FIG. 2 is a cross-sectional view showing the glass to be tempered according to the first embodiment after a heat treatment step and before a tempering step. [Diagram 5] FIG. 4 is a flow diagram showing a method for producing tempered glass according to a second embodiment of the present invention. [Figure 6] FIG. 11 is a cross-sectional view showing a manufacturing apparatus used in a second embodiment. [Figure 7] FIG. 11 is a cross-sectional view showing a glass to be strengthened in a cutting step of a second embodiment. [Figure 8] FIG. 11 is a cross-sectional view showing a glass to be strengthened in a removing step of a second embodiment. [Figure 9] FIG. 6 is a cross-sectional view showing a glass to be tempered in a heat treatment step according to a second embodiment. [Figure 10] FIG. 4 is a cross-sectional view showing a strengthened glass according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] Hereinafter, the strengthened glass according to the embodiment of the present invention and the manufacturing method thereof will be described with reference to the drawings. In each embodiment, the same reference numerals are given to corresponding components, and duplicated descriptions may be omitted. When only a part of the configuration is described in each embodiment, the configuration of the other embodiment described above can be applied to the other parts of the configuration. In addition to the combination of the configurations clearly stated in the description of each embodiment, the configurations of multiple embodiments can be partially combined together even if not clearly stated, as long as there is no particular problem with the combination.

[0035] First embodiment As shown in FIG. 1, in the first embodiment of the present invention, a method for producing tempered glass is illustrated.

[0036] As shown in the figure, the method for manufacturing tempered glass according to this embodiment includes, in this order, a preparation step S1, a heat treatment step S2, and a chemical strengthening step S3. That is, the heat treatment step S2 is carried out after the preparation step S1, and the chemical strengthening step S3 is carried out after the heat treatment step S2.

[0037] The preparation step S1 is a step of preparing a glass to be tempered 1 shown in Fig. 2. The glass to be tempered 1 is an untempered plate glass, and has a first main surface 2 and a second main surface 3 located opposite the first main surface 2. In other words, the first main surface 2 and the second main surface 3 face each other in the thickness direction.

[0038] The tempered glass 1 is a plate-like glass having a thickness of 2 mm or less. The thickness of the tempered glass 1 is preferably 300 μm or less, 150 μm or less, 20 μm or more to 150 μm or less, 20 μm or more to 120 μm or less, or 25 μm or more to 120 μm or less. If the tempered glass obtained from the tempered glass 1 is very thin and has a thickness of 300 μm or less, it can be suitably used as a cover glass for a so-called foldable type device that allows the display surface of the display to be folded. On the other hand, for example, when the tempered glass obtained from the tempered glass 1 is used as a cover glass for a non-bending type (straight type) device, the thickness of the tempered glass 1 is preferably more than 0.3 mm and 2 mm or less, 0.45 mm or more to 2 mm or less, or 0.5 mm or more to 0.85 mm or less. The tempered glass obtained from the tempered glass 1 also has substantially the same thickness as the tempered glass 1. When the surface layer portion 2a of the first main surface 2 and / or the surface layer portion 3a of the second main surface 3 of the glass to be tempered 1 is removed during the manufacturing process of the tempered glass, the thickness of the glass to be tempered 1 described above refers to the thickness after the removal (see symbol D1 in Figure 8).

[0039] A heterogeneous layer 4 is formed on the surface layer portion 2a of the second main surface 3 of the glass 1 to be strengthened. In this embodiment, the heterogeneous layer 4 is formed only on the surface layer portion 3a of the second main surface 3 of the first main surface 2 and the second main surface 3 of the glass 1 to be strengthened. The heterogeneous layer 4 is a layer having a thickness of, for example, 5 to 10 μm. The heterogeneous layer 4 is a layer having properties different from those of the internal layer 5 of the glass 1 to be strengthened, and has a property of promoting ion exchange in the chemical strengthening step S3. In this embodiment, since no heterogeneous layer is formed on the surface layer portion 2a of the first main surface 2, the surface layer portion 2a of the first main surface 2 has the same properties as the internal layer 5. Note that a heterogeneous layer thinner than the heterogeneous layer 4 on the second main surface 3 side may be formed on the surface layer portion 2a of the first main surface 2.

[0040] Although the detailed structure of the heterogeneous layer 4 has not been elucidated at present, it is presumed to be composed of (1) a layer whose structure is more relaxed than that of the inner layer 5, (2) a layer whose moisture content is different from that of the inner layer 5, and (3) a layer whose composition is different from that of the inner layer 5. However, it has been found that the heterogeneous layer 4 is formed during annealing (annealing conditions: cooling rate of 0.5°C / s or more) performed immediately after forming the plate-shaped tempered glass 1 (strictly speaking, glass ribbon) from molten glass. Examples of forming methods of tempered glass 1 that satisfy such annealing conditions include downdraw methods such as overflow downdraw and slot downdraw (for example, cooling conditions of 3 to 10°C / s) and float methods (for example, cooling conditions of 0.5 to 2°C / s). In order to obtain a smooth surface, it is preferable to use the overflow downdraw method as a forming method. The tempered glass 1 formed by the overflow downdraw method has a forming junction surface inside.

[0041] The tempered glass 1 is, for example, an alkali aluminosilicate glass, and contains, for example, in mole percent, SiO2 50-80%, Al2O3 5-25%, B2O3 0-35%, Li2O 0-20%, Na2O 1-20%, Li2O+Na2O 1-20%, and K2O 0-10% as a glass composition. A representative glass that satisfies such a glass composition is T2X-1 manufactured by Nippon Electric Glass Co., Ltd. The tempered glass 1 may have a glass composition that does not substantially contain Li2O. The phrase "substantially does not contain Li2O" means that Li2O is not actively added as a glass component, but is allowed to be mixed at an impurity level, and specifically means that the content of Li2O is less than 500 ppm. The tempered glass obtained by chemically tempering the tempered glass 1 and the molten glass for forming the tempered glass 1 also have substantially the same glass composition as the tempered glass 1.

[0042] The above glass composition is preferable for the following reasons: In the explanation of the content range of each component, % indicates mol % unless otherwise specified.

[0043] SiO2 is a component that forms a glass network. If the content of SiO2 is too low, vitrification becomes difficult, and the thermal expansion coefficient becomes too high, so that the thermal shock resistance is easily reduced. Therefore, the preferred lower limit range of SiO2 is 50% or more, 55% or more, 57% or more, 59% or more, and particularly 61% or more. On the other hand, if the content of SiO2 is too high, the melting property and moldability are easily reduced, and the thermal expansion coefficient becomes too low, so that it is difficult to match the thermal expansion coefficient of the surrounding material. Therefore, the preferred upper limit range of SiO2 is 80% or less, 70% or less, 68% or less, 66% or less, 65% or less, and particularly 64.5% or less.

[0044] Al2O3 is a component that enhances ion exchange performance, and also enhances strain point, Young's modulus, fracture toughness, and Vickers hardness. Therefore, the preferred lower limit range of Al2O3 is 5% or more, 8% or more, 10% or more, 11% or more, or 11.2% or more. On the other hand, if the content of Al2O3 is too high, the high-temperature viscosity increases, and melting property and formability tend to decrease. In addition, if the content of Al2O3 is too high, devitrification crystals tend to precipitate in the glass, making it difficult to form into a plate shape by the overflow downdraw method or the like. In particular, when an alumina-based refractory is used as the molded body refractory and a glass plate is formed by the overflow downdraw method, devitrification crystals of spinel tend to precipitate at the interface with the alumina-based refractory. Furthermore, if the content of Al2O3 is too high, acid resistance also decreases, making it difficult to apply to an acid treatment process. Therefore, the upper limit range of Al2O3 is preferably 25% or less, 21% or less, 20.5% or less, 20% or less, 19.9% ​​or less, 19.5% or less, 19.0% or less, particularly preferably 18.9% or less.

[0045] B2O3 is a component that reduces high-temperature viscosity and density, stabilizes glass, makes crystals less likely to precipitate, and lowers the liquidus temperature. In addition, B2O3 is a component that suppresses Young's modulus and increases bending strength and crack resistance. However, if the content of B2O3 is too high, ion exchange treatment tends to cause surface coloring called fading, reduce water resistance, and reduce the compressive stress of the compressive stress layer. Therefore, the preferred lower limit range of B2O3 is 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, or 0.3% or more, and the preferred upper limit range is 35% or less, 30% or less, 25% or less, 22% or less, 20% or less, and particularly 15% or less. In terms of prioritizing increasing CS, the content of B2O3 can be more preferably 0.2 to 5%, or 0.3 to 1%. On the other hand, from the viewpoint of prioritizing suppression of the Young's modulus, the content of B2O3 can be more preferably set to 10 to 25%, 15 to 23%, or 18 to 22%.

[0046] Li2O is an ion-exchange component, and in particular, Li ions contained in glass and K ions in molten salt are ion-exchanged to obtain high surface compressive stress. Li2O is also a component that reduces high-temperature viscosity and improves meltability and formability. Therefore, the preferred lower limit range of Li2O is 0% or more, 3% or more, 4% or more, 4.2% or more, 5% or more, 5.5% or more, 6.5% or more, 7% or more, 7.3% or more, 7.5% or more, 7.8% or more, particularly 8% or more. The preferred upper limit range of Li2O is 20% or less, 15% or less, 13% or less, 12% or less, 11.5% or less, 11% or less, 10.5% or less, less than 10%, 9.9% or less, 9% or less, particularly 8.9% or less.

[0047] Na2O is an ion exchange component, and is a component that reduces high-temperature viscosity and improves melting and moldability. Na2O is also a component that improves devitrification resistance and reaction devitrification with a shaped refractory, especially an alumina refractory. If the content of Na2O is too small, the melting property decreases, the thermal expansion coefficient decreases too much, and the ion exchange rate tends to decrease. Therefore, the preferable lower limit range of Na2O is 1% or more, 5% or more, 7% or more, 8% or more, 8.5% or more, 9% or more, 9.5% or more, 10% or more, 11% or more, 12% or more, and particularly 12.5% ​​or more. On the other hand, if the content of Na2O is too high, the phase separation generation viscosity tends to decrease. Also, if the content of Na2O is too high, the acid resistance decreases, the glass composition loses its component balance, and the devitrification resistance may decrease. Therefore, a suitable upper limit range of Na2O is 20% or less, 19.5% or less, 19% or less, 18% or less, 17% or less, 16.5% or less, 16% or less, 15.5% or less, particularly 15% or less.

[0048] K2O is a component that reduces high-temperature viscosity and improves melting and moldability. Furthermore, K2O is also a component that improves devitrification resistance and increases Vickers hardness. However, if the content of K2O is too high, the phase separation viscosity is likely to decrease. In addition, if the content of K2O is too high, the acid resistance decreases, the glass composition loses its component balance, and the devitrification resistance tends to decrease. Therefore, the preferred lower limit range of K2O is 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, particularly 3.5% or more, and the preferred upper limit range of K2O is 10% or less, 5.5% or less, 5% or less, particularly less than 4.5%.

[0049] Both Li2O and Na2O are components that exchange with K ions in the molten salt to obtain high surface compressive stress. Therefore, the preferred lower limit range of Li2O+Na2O is 1% or more, 3% or more, 4% or more, 5% or more, 6% or more, 7% or more, 8% or more, 9% or more, 10% or more, 11% or more, 12% or more, 13% or more, 14% or more, 15% or more, 16% or more, 17% or more, 18% or more, and particularly 18.5% or more. On the other hand, if the content of Li2O+Na2O is too high, the thermal expansion coefficient becomes too high, and the thermal shock resistance is likely to decrease. In addition, if the content of Li2O+Na2O is too high, the component balance of the glass composition may be lost, and the devitrification resistance may decrease. Therefore, the preferred upper limit range of Li2O+Na2O is 20% or less, and particularly 19% or less. Here, "Li2O+Na2O" refers to the combined amount of Li2O and Na2O.

[0050] In addition to the above components, the glass to be tempered 1 may contain, for example, the following components as a glass composition.

[0051] MgO is a component that reduces high-temperature viscosity, improves meltability and formability, and increases strain point and Young's modulus. Among alkaline earth metal oxides, MgO is a component that has a large effect of improving ion exchange performance. However, if the content of MgO is too high, the density and thermal expansion coefficient tend to increase, and the glass tends to devitrify. Therefore, the preferred upper limit range of MgO is 12% or less, 10% or less, 8% or less, 6% or less, and particularly 5% or less. When MgO is introduced into the glass composition, the preferred lower limit range of MgO is 0.1% or more, 0.5% or more, 1% or more, and particularly 2% or more.

[0052] Compared with other components, CaO has a large effect of lowering high-temperature viscosity, improving meltability and moldability, and increasing strain point and Young's modulus without decreasing devitrification resistance. The CaO content is preferably 0 to 10%. However, if the CaO content is too high, the density and thermal expansion coefficient increase, and the glass composition loses its component balance, making the glass more susceptible to devitrification and the ion exchange performance more susceptible to deterioration. Therefore, the preferred CaO content is 0 to 5%, 0.01 to 4%, 0.1 to 3%, and particularly 1 to 2.5%.

[0053] SrO is a component that reduces high-temperature viscosity, improves meltability and formability, and increases strain point and Young's modulus without decreasing devitrification resistance. However, if the SrO content is too high, the density and thermal expansion coefficient increase, the ion exchange performance decreases, and the glass composition loses its component balance, making the glass more susceptible to devitrification. The preferred content range of SrO is 0 to 5%, 0 to 3%, 0 to 1%, and particularly 0 to less than 0.1%.

[0054] BaO is a component that reduces high-temperature viscosity, improves meltability and moldability, and increases strain point and Young's modulus without decreasing devitrification resistance. However, if the BaO content is too high, the density and thermal expansion coefficient increase, the ion exchange performance decreases, and the glass composition loses its component balance, making the glass more susceptible to devitrification. The preferred content range of BaO is 0 to 5%, 0 to 3%, 0 to 1%, and particularly 0 to less than 0.1%.

[0055] ZnO is a component that enhances ion exchange performance, and is particularly effective in increasing compressive stress. ZnO is also a component that reduces high-temperature viscosity without reducing low-temperature viscosity. However, if the ZnO content is too high, the glass tends to undergo phase separation, the devitrification resistance to decrease, the density to increase, and the stress depth of the compressive stress layer to decrease. Therefore, the ZnO content is preferably 0 to 6%, 0 to 5%, 0 to 1%, 0 to 0.5%, and particularly preferably less than 0 to 0.1%.

[0056] ZrO2 is a component that significantly increases ion exchange performance and also increases the viscosity near the liquidus viscosity and the strain point, but if the content is too high, there is a risk of significantly decreasing the devitrification resistance and of the density becoming too high. Therefore, the preferred upper limit range of ZrO2 is 10% or less, 8% or less, 6% or less, and particularly 5% or less. In addition, when it is desired to increase the ion exchange performance, it is preferable to introduce ZrO2 into the glass composition, and in this case, the preferred lower limit range of ZrO2 is 0.001% or more, 0.01% or more, 0.5% or more, and particularly 1% or more.

[0057] P2O5 is a component that enhances ion exchange performance, particularly increasing the stress depth of the compressive stress layer. P2O5 is also a component that suppresses the Young's modulus. However, if the P2O5 content is too high, the glass is prone to phase separation. Therefore, the preferred upper limit range of P2O5 is 10% or less, 8% or less, 6% or less, 4% or less, 2% or less, 1% or less, and particularly less than 0.1%.

[0058] As a fining agent, one or more selected from the group of As2O3, Sb2O3, SnO2, F, Cl, and SO3 (preferably the group of SnO2, Cl, and SO3) may be introduced at 0 to 30,000 ppm (3%). From the viewpoint of accurately enjoying the fining effect, the content of SnO2+SO3+Cl is preferably 0 to 10,000 ppm, 50 to 5,000 ppm, 80 to 4,000 ppm, 100 to 3,000 ppm, and particularly 300 to 3,000 ppm. Here, "SnO2+SO3+Cl" refers to the total amount of SnO2, SO3, and Cl.

[0059] The preferred range of SnO2 is 0 to 10,000 ppm, 0 to 7,000 ppm, and particularly 50 to 6,000 ppm. The preferred range of SO3 is 0 to 1,000 ppm, 0 to 800 ppm, and particularly 10 to 500 ppm. The preferred range of Cl is 0 to 1,500 ppm, 0 to 1,200 ppm, 0 to 800 ppm, 0 to 500 ppm, and particularly 50 to 300 ppm.

[0060] Rare earth oxides such as Nd2O3 and La2O3 are components that increase the Young's modulus, and when a complementary color is added, the color is eliminated, and the color of the glass can be controlled. However, the cost of the raw material itself of rare earth oxides is high, and when a large amount is introduced, the devitrification resistance is easily reduced. Therefore, the content of rare earth oxides is preferably 4% or less, 3% or less, 2% or less, 1% or less, and particularly 0.5% or less.

[0061] In the present invention, it is preferable that the glass does not substantially contain As2O3, F, PbO, and Bi2O3 from the viewpoint of environmental consideration. Here, "substantially does not contain As2O3" means that As2O3 is not actively added as a glass component, but is allowed to be mixed at the impurity level, specifically, the content of As2O3 is less than 500 ppm. "Substantially does not contain F" means that F is not actively added as a glass component, but is allowed to be mixed at the impurity level, specifically, the content of F is less than 500 ppm. "Substantially does not contain PbO" means that PbO is not actively added as a glass component, but is allowed to be mixed at the impurity level, specifically, the content of PbO is less than 500 ppm. "Substantially does not contain Bi2O3" means that Bi2O3 is not actively added as a glass component, but is allowed to be mixed at the impurity level, specifically, the content of Bi2O3 is less than 500 ppm.

[0062] The composition of the glass to be strengthened 1 is an example, and glass of any composition can be used as long as it contains an ion-exchangeable component. Note that the glass to be strengthened in the present invention includes glass articles in a broad sense, including glassy materials, such as glass ceramics (or called crystallized glass) that include both crystalline and glassy materials.

[0063] The strain point of glass 1 to be tempered varies depending on the glass composition and is not particularly limited, but is, for example, 500 to 650° C. Here, the strain point of glass 1 to be tempered is a value measured in accordance with ASTM C336.

[0064] The heat treatment step S2 is a step of regenerating a heterogeneous layer by subjecting the tempering glass 1 to a heat treatment. As shown in Fig. 3, the heat treatment step S2 includes a temperature increasing step S21 of increasing the temperature of the tempering glass 1 from near room temperature to a holding temperature P, a holding step S22 of holding the tempering glass 1 at the holding temperature P for a predetermined holding time Q, and a temperature decreasing step S23 of decreasing the temperature of the tempering glass 1 from the holding temperature to near room temperature, in this order. The heat treatment step S2 can be performed using a batch-type or continuous-type heating furnace.

[0065] The temperature increase rate in the temperature increase step S21 is, for example, 10 to 1000° C. / min. The temperature decrease rate in the temperature decrease step S23 is, for example, 10 to 1000° C. / min. The temperature increase rate in the temperature increase step S21 and the temperature decrease rate in the temperature decrease step S23 are not particularly limited as long as the heat treatment conditions in the holding step S22 are satisfied.

[0066] The holding temperature P in the holding step S22 is equal to or higher than the strain point of the glass to be strengthened by −15° C., and the holding time Q in the holding step S22 is equal to or longer than 3 minutes. According to the heat treatment step S2 including the holding step S22, a heterogeneous layer 6 is reproduced on the first main surface 2 of the glass to be strengthened 1, as shown in Fig. 4. That is, the heterogeneous layers 4, 6 having approximately the same thickness can be formed again on the surface layer portions 2a, 3a of the first main surface 2 and the second main surface 3 of the glass to be strengthened 1, respectively.

[0067] In the holding step S22, from the viewpoint of suppressing unintended deformation of the glass 1 to be tempered, it is preferable that the holding temperature P is equal to or lower than the strain point +50°C, and the holding time Q is equal to or longer than 10 minutes. In this case, it is more preferable that the holding time Q is equal to or longer than 30 minutes. Of course, even in this case, it is sufficient that the holding time Q is equal to or longer than 3 minutes.

[0068] In the holding step S22, from the viewpoint of efficiently regenerating the heterogeneous layer 6, the holding temperature P is preferably equal to or higher than the strain point +85° C. In this case, the holding time Q is preferably 3 minutes or more, 10 minutes or more, particularly preferably 30 minutes or more.

[0069] In the holding step S22, from the viewpoint of improving production efficiency, the holding time Q is preferably 60 minutes or less.

[0070] The chemical strengthening step S3 is a step of obtaining strengthened glass by chemically strengthening the glass to be strengthened 1 by ion exchange treatment. The glass to be strengthened 1 is treated by, for example, immersing it in a molten salt for the ion exchange treatment.

[0071] The molten salt is a salt containing a component that is ion-exchangeable with the components in the tempered glass 1, and is typically an alkali nitrate. Examples of the alkali nitrate include NaNO3, KNO3, LiNO3, etc., which can be used alone (100 mass%) or in combination of two or more kinds. When two or more kinds of alkali nitrates are mixed, the mixing ratio may be determined arbitrarily, but may be, for example, 5-95% NaNO3, 5-95% KNO3, preferably 30-80% NaNO3, 20-70% KNO3, and more preferably 50-70% NaNO3, 30-50% KNO3, in mass%.

[0072] The conditions such as the temperature of the molten salt and the immersion time may be set according to the glass composition and the like within a range in which the desired stress characteristics can be obtained, and the temperature of the molten salt is, for example, 350° C. to 500° C., preferably 355° C. to 470° C., 360° C. to 450° C., 365° C. to 430° C., particularly 370° C. to 410° C. The immersion time is, for example, 3 to 300 minutes, preferably 5 to 120 minutes, more preferably 7 to 100 minutes.

[0073] The chemical strengthening step S3 may include a preheating step of preheating the glass 1 to be strengthened in order to prevent breakage of the glass 1 to be strengthened due to thermal shock during strengthening. In this case, the heat treatment step S2 may be performed as part of the preheating step. If changing the existing steps would rather reduce production efficiency, it is preferable to perform the preheating step and the heat treatment step S2 independently as described above. In this case, after the heat treatment step S2 and before the preheating step, the glass 1 to be strengthened may be cooled once to room temperature (0 to 50°C).

[0074] After the chemical strengthening step S3, the tempered glass is preferably washed and dried. In addition, the tempered glass is preferably protected by attaching a protective film to the surface. As the protective film, a self-adhesive film or a slightly adhesive film is preferably used.

[0075] In the manufacturing method of tempered glass as described above, the heat treatment in the heat treatment step S2 regenerates the heterogeneous layer 6 also in the surface layer portion 2a of the first main surface 2 of the glass to be tempered 1. In other words, heterogeneous layers 4, 6 of approximately the same thickness are formed on the surface layer portions 2a, 3a of the first main surface 2 and the second main surface 3 of the glass to be tempered 1. Therefore, by chemically tempering the glass to be tempered 1 in the subsequent chemical tempering step S3, it is possible to obtain tempered glass that has high compressive stress on both main surfaces and has little warping.

[0076] Second Embodiment As shown in FIG. 5, in the second embodiment of the present invention, a method for producing tempered glass is illustrated.

[0077] As shown in the figure, the manufacturing method of tempered glass according to this embodiment includes, in this order, a forming step T1, an annealing step T2, a cooling step T3, a cutting step T4, a removal step T5, a heat treatment step T6, and a chemical strengthening step T7. The forming step T1, the annealing step T2, the cooling step T3, the cutting step T4, and the removal step T5 correspond to the preparation step S1 of the first embodiment. Note that the preparation step S1 of the first embodiment is not limited to these steps T1 to T5. The preparation step S1 may be, for example, a step in which only a part of these steps (for example, the removal step T5) is performed.

[0078] In this embodiment, the forming step T1 is a step of forming a glass 1 to be strengthened (strictly speaking, a glass ribbon) by using an overflow downdraw method. Note that the forming method of the glass 1 to be strengthened is not limited thereto, and may be any other known forming method such as a slot downdraw method or a float method.

[0079] The annealing step T2 is a step of annealing the glass to be tempered 1 at a cooling rate of 0.5° C. / s or more immediately after forming. Here, "immediately after forming" means a high-temperature state of the formed glass to be tempered 1 before it is cooled to about room temperature. In other words, the annealing step T2 is different from a heat treatment of reheating the glass to be tempered 1 that has been once cooled to about room temperature.

[0080] The cooling step T3 is a step of cooling the glass to be tempered 1 to about room temperature.

[0081] In this embodiment, the forming step T1, the annealing step T2, and the cooling step T3 use a manufacturing apparatus 11 shown in Fig. 6. The manufacturing apparatus 11 includes a forming zone 14 for continuously forming a glass ribbon 13 from the molten glass 12, an annealing zone 15 for annealing the glass ribbon 13, a cooling zone 16 for cooling the glass ribbon 13 to approximately room temperature, and roller pairs 17 provided in multiple stages above and below in each of the forming zone 14, the annealing zone 15, and the cooling zone 16. The forming step T1 is performed in the forming zone 14, the annealing step T2 is performed in the annealing zone 15, and the cooling step T3 is performed in the cooling zone 16.

[0082] The forming zone 14 and the annealing zone 15 are constituted by furnaces in which the transport path of the glass ribbon 13 is surrounded by walls, and heating devices such as heaters for adjusting the temperature of the glass ribbon 13 are arranged at appropriate positions in the furnaces. On the other hand, the cooling zone 16 is open to the outside atmosphere at room temperature without the transport path of the glass ribbon 13 being surrounded by walls, and no heating device such as a heater is arranged therein. By passing through the annealing zone 15 and the cooling zone 16, the glass ribbon 13 is given a desired thermal history.

[0083] In the internal space of the forming zone 14, a forming body 18 is disposed which forms a glass ribbon 13 from the molten glass 12 by an overflow downdraw method. In the forming step T1, in the internal space of the forming zone 14, the molten glass 12 supplied to the forming body 18 overflows from a groove (not shown) formed in a top 18a of the forming body 18, and the overflowing molten glass 12 flows along both side surfaces 18b having a wedge-shaped cross section of the forming body 18 and joins at a lower end 18c, thereby continuously forming a plate-shaped glass ribbon 13. The formed glass ribbon 13 is transported downward while maintaining the vertical position.

[0084] The internal space of the annealing zone 15 has a predetermined temperature gradient downward. In the annealing step T2, the glass ribbon 13 in the vertical position moves downward in the internal space of the annealing zone 15, so that the glass ribbon 13 is annealed at a cooling rate of 0.5°C / s or more. The cooling rate during annealing is preferably 1°C / s or more, 2°C / s or more, 3.5°C / s or more, 4°C / s or more, particularly 5°C / s or more. The cooling rate during annealing is preferably 20°C / s or less, 15°C / s or less, particularly 12°C / s or less. By such annealing step T2, internal distortion of the glass ribbon 13 is suppressed, and heterogeneous layers are formed on both main surfaces of the glass ribbon 13. The temperature gradient of the internal space of the annealing zone 15 can be adjusted, for example, by a heating device provided on the inner wall surface of the annealing zone 15.

[0085] The multiple roller pairs 17 clamp both widthwise ends of the glass ribbon 13 in a vertical position from both the front and back sides. The uppermost roller pair 17 arranged in the forming zone 14 is a cooling roller, and may also be called an edge roller. Note that, in the internal space of the annealing zone 15, the multiple roller pairs 17 may include ones that do not clamp both widthwise ends of the glass ribbon 13. In other words, the opposing distance between the roller pairs 17 may be made larger than the thickness of both widthwise ends of the glass ribbon 13, and the glass ribbon 13 may pass between the roller pairs 17.

[0086] In this embodiment, both widthwise ends of the glass ribbon 13 obtained by the manufacturing apparatus 11 include portions (hereinafter also referred to as "ear portions") that are thicker than the widthwise central portion due to the influence of shrinkage during the molding process.

[0087] The cutting step T4 is a step of cutting the glass ribbon 13 that has been subjected to the above-mentioned shaping step T1, annealing step T2, and cooling step T3, to obtain the glass to be strengthened 21 shown in Fig. 7. In detail, the cutting step T4 may be performed, for example, in the following cases: (1) the glass ribbon 13 is cut to obtain a large sheet of mother glass, and then the mother glass is cut to obtain the glass to be strengthened 21; or (2) the glass ribbon 13 is wound into a roll to obtain a glass roll, and then the glass ribbon 13 unwound from the glass roll is cut to obtain the glass to be strengthened 21.

[0088] As shown in FIG. 7, heterogeneous layers 24, 25 resulting from the annealing process T2 are formed on surface layer portions 22a, 23a of the first main surface 22 and the second main surface 23 of the tempered glass 21 obtained through the cutting process T4.

[0089] As shown in FIG. 8, the removal step T5 is a step of removing only the surface layer portion 23a of the first main surface 22 of the glass to be strengthened 21 from the first main surface 22 and the second main surface 23. That is, the thickness D1 of the glass to be strengthened 21 after the removal step T5 is thinner than the thickness D0 of the glass to be strengthened 21 before the removal step T5 (cutting step T4) by a removal thickness ΔD. ΔD is preferably 1 to 50 μm, 2 to 40 μm, and particularly 3 to 30 μm. Note that, if the removal thickness of the second main surface 23 is smaller than the removal thickness of the first main surface 22, the surface layer portions 22a and 23a of the first main surface 22 and the second main surface 23 may be removed. By such a removal step T5, a part or all of the heterogeneous layer 24 on the first main surface 22 side is removed, and the thickness of the heterogeneous layer 25 on the second main surface 23 side becomes larger than the thickness (including zero) of the heterogeneous layer 24 on the first main surface 22 side. The removing step T5 is performed as part of processing the end face of the glass 21 to be strengthened into a special shape such as a so-called 2.5D shape, in which the end face is inclined obliquely.

[0090] The method for removing the surface layer portion of the glass to be strengthened 21 is not particularly limited, but examples thereof include chemical polishing such as etching, mechanical polishing such as abrasive polishing, chemical mechanical polishing (CMP), etc. In the present embodiment, etching is used as the method for removing the surface layer portion of the glass to be strengthened 21.

[0091] When mechanical polishing is used, for example, it is performed by sliding a waterproof abrasive paper with #1000 alumina abrasive grains attached thereto while adding water against the first main surface 22 of the glass to be strengthened 21. Then, chemical mechanical polishing may be performed using cerium oxide powder.

[0092] When etching is used, for example, with a protective film formed on the second main surface 23 of the glass to be strengthened 21, the glass to be strengthened 21 is entirely immersed in a liquid etching solution to wet-etch the glass to be strengthened 21. As the protective film, in addition to an etching prevention film that completely prevents the second main surface 23 from being removed by etching, an etching suppression film that makes the etching rate of the second main surface 23 slower than the etching rate of the first main surface 22 can be used. The protective film is peeled off from the glass to be strengthened 21 after etching is completed.

[0093] The etching solution may be an acidic or alkaline aqueous solution capable of etching glass.

[0094] As the acidic etching solution, for example, an acidic aqueous solution containing HF can be used. When an aqueous solution containing HF is used, the etching rate for glass is high, and the productivity is improved.

[0095] The aqueous solution containing HF is, for example, an aqueous solution containing only HF, or a combination of HF and HCl, HF and HNO3, HF and H2SO4, or HF and NH4F. The concentration of each of the compounds HF, HCL, HNO3, H2SO4, and NH4F is preferably 0.1 to 30 mol / L. In etching using an aqueous solution containing HF, fluorides containing glass components are generated as by-products, which can cause a decrease in etching rate and defects. However, as described above, by using a mixed acid with other acids such as HCL, HNO3, or H2SO4, the by-products can be decomposed to suppress a decrease in productivity. When etching is performed using an acidic aqueous solution, the temperature of the acidic aqueous solution is, for example, 10 to 30°C, and the time for immersing the tempered glass 1 is preferably, for example, 0.1 to 60 minutes.

[0096] As the alkaline etching medium, an alkaline aqueous solution containing NaOH or KOH can be used. The alkaline aqueous solution has a relatively small etching rate for glass compared to the above-mentioned etching medium containing HF, and therefore has the advantage that the amount of etching can be easily controlled precisely.

[0097] In the aqueous solution containing NaOH or KOH, the concentration of the alkaline component is preferably 1 to 20 mol / L. When etching is performed using an aqueous alkaline solution, the temperature of the aqueous alkaline solution is, for example, 10 to 130° C., and the time for immersing the glass to be tempered 1 is preferably, for example, 0.5 to 120 minutes. When increasing the etching rate to increase productivity, it is preferable to heat the aqueous alkaline solution to 80° C. or higher. Conversely, when it is desired to control the amount of etching with higher accuracy, it is preferable to limit the temperature of the aqueous alkaline solution to 70° C. or lower. When placing more importance on the etching rate, it is preferable to use an aqueous NaOH solution.

[0098] The etching may be performed by applying or spraying an etching solution onto the first main surface 22 of the glass 21 to be strengthened.

[0099] The heat treatment step T6 is a step of regenerating the heterogeneous layer by subjecting the glass to be strengthened 21 to a heat treatment. Specifically, the heat treatment step T6 is a step of holding the glass to be strengthened 21 at a holding temperature of −15° C. or higher, which is equal to or higher than the strain point, for 3 minutes or more, and is similar in detail to the heat treatment step S2 of the first embodiment. According to such a heat treatment step T6, as shown in FIG. 9, the heterogeneous layer 24 is regenerated on the first main surface 22 of the glass to be strengthened 21. That is, the heterogeneous layers 24 and 25 having approximately the same thickness can be formed again on the surface layer portions 22a and 23a of the first main surface 22 and the second main surface 23 of the glass to be strengthened 21, respectively.

[0100] The chemical strengthening step T7 is a step of chemically strengthening the tempering glass 21 by ion exchange treatment to obtain tempered glass, and the details are the same as those of the chemical strengthening step S3 in the first embodiment. If the chemical strengthening step T7 is performed after the heat treatment step T6, it is possible to obtain tempered glass that has high compressive stress on both main surfaces and has little warping.

[0101] Third embodiment As shown in FIG. 10, in the third embodiment of the present invention, a tempered glass manufactured by the method for manufacturing tempered glass described in the first or second embodiment is exemplified.

[0102] As shown in the figure, the tempered glass 31 has a first compressive stress layer 33 in a surface layer portion 32a of a first main surface 32, and a second compressive stress layer 35 in a surface layer portion 34a of a second main surface 34. The tempered glass 31 also has a tensile stress layer 37 in an internal layer 36 between the compressive stress layers 33 and 35. The tempered glass 31 may have a compressive stress layer in a surface layer portion of an end surface connecting the first main surface 32 and the second main surface 34.

[0103] The first main surface 32 is a polished surface, and the second main surface 34 is an unpolished surface. The second main surface 34 is a fire-polished surface as formed by the overflow downdraw method. That is, the surface roughness Ra1 of the first main surface 32, which is a polished surface, is larger than the surface roughness Ra2 of the second main surface 34, which is an unpolished surface. The surface roughness Ra1 of the first main surface 32 is 0.1 nm to 2.0 nm, preferably 0.1 nm to 1.0 nm, and particularly 0.1 nm to 0.5 nm. The surface roughness Ra2 of the second main surface 34 is 0.1 nm to 1.0 nm, preferably 0.1 nm to 0.5 nm, and particularly 0.1 nm to 0.2 nm. The absolute value of the difference between the surface roughness Ra1 of the first main surface 32 and the surface roughness Ra2 of the second main surface 34 is 0.1 nm or more, preferably 0.1 nm to 1.0 nm, and particularly 0.1 nm to 0.5 nm. Here, "surface roughness Ra (Ra1 and Ra2)" refers to a value measured by a method in accordance with JIS B0601: 2001. Both the first main surface 32 and the second main surface 34 may be polished surfaces.

[0104] The compressive stress CS1 of the first compressive stress layer 33 and the compressive stress CS2 of the second compressive stress layer 35 are each 820 MPa or more, preferably 830 MPa, 840 MPa, and particularly 850 MPa. However, the compressive stress CS1 of the first compressive stress layer 33 on the polished first main surface 32 side tends to be smaller than the compressive stress CS2 of the second compressive stress layer 35 on the unpolished second main surface 34 side. The absolute value of the difference (CS1-CS2) between the compressive stress CS1 of the first compressive stress layer 33 and the second compressive stress CS2 of the second compressive stress layer 35 is 40 MPa or less, preferably 30 MPa or less, 20 MPa or less, and particularly 10 MPa or less. CS1 / CS2 is preferably 95% or more and 105% or less. The stress depth DOL1 of the first compressive stress layer 33 and the stress depth DOL2 of the second compressive stress layer 35 are each 1 to 100 μm, preferably 10 to 90 μm, 20 to 80 μm, and particularly 30 to 70 μm. The absolute value of the difference (DOL1-DOL2) between the stress depth DOL1 of the first compressive stress layer 33 and the stress depth DOL2 of the second compressive stress layer 35 is 10 μm or less, preferably 5 μm or less, 3 μm or less, and particularly 1 μm or less. Here, the "compressive stresses CS (CS1 and CS2)" and the "stress depths DOL (DOL1 and DOL2)" are calculated by observing the number of interference fringes and their intervals using a surface stress meter (for example, FSM-6000 manufactured by Orihara Seisakusho Co., Ltd.).

[0105] The tempered glass 31 has a flat plate shape. The warp of the tempered glass 31 is preferably 250 μm or less, more preferably 200 μm or less, and particularly preferably 10 to 150 μm or less.

[0106] Although the tempered glass and the manufacturing method thereof according to the embodiment of the present invention have been described, the embodiment of the present invention is not limited thereto, and various modifications can be made without departing from the gist of the present invention.

[0107] In the above embodiment, the shape of the tempered glass is rectangular (rectangular or square) in a planar view. However, the shape of the tempered glass is not particularly limited and may be any shape, such as a circle or an ellipse, in a planar view.

[0108] In the above embodiment, the case where tempered glass is produced by one ion exchange treatment has been exemplified. However, tempered glass may be produced by two or more ion exchange treatments.

[0109] The tempered glass according to the above embodiment can be laminated with any plate- or sheet-shaped resin material, or a transparent material such as a metal material or glass via an adhesive or the like to be used as a laminate. EXAMPLES

[0110] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0111] As the tempered glass, a glass plate (strain point: 564°C) containing, in mole percent, SiO2 66.4%, Al2O3 11.5%, B2O3 0.5%, K2O 1.4%, Na2O 15.2%, Li2O 0.02%, MgO 4.8%, CaO 0.1%, and SnO2 0.1% was prepared. The tempered glass in this example is a glass plate formed by the overflow downdraw method, and the cooling rate during annealing immediately after forming is 5°C / s. The size of the tempered glass is 50 mm in both length and width, and 0.7 mm in thickness.

[0112] Of the first and second main surfaces of this tempered glass, only the first main surface was removed by 50 μm by mechanical polishing and chemical mechanical polishing, and heat treatment was performed at different holding temperatures and holding times to prepare each sample (Examples 1 to 6, Comparative Examples 1 to 4). Note that the sample according to Comparative Example 4 was not subjected to heat treatment after polishing one side. The surface roughness Ra1 of the first main surface constituted by the polished surface is 0.40 nm, and the surface roughness Ra2 of the second main surface constituted by the unpolished surface is 0.17 nm. Here, "Ra1" and "Ra2" refer to values ​​measured by a method conforming to JIS B0601:2001.

[0113] Each sample was chemically strengthened (molten salt: KNO3, treatment temperature: 430°C, treatment time: 4 hours) to form a first compressive stress layer on the first main surface of each sample and a second compressive stress layer on the second main surface. Then, for each sample, the compressive stress CS1 and stress depth DOL1 of the first compressive stress layer were measured, and the compressive stress CS2 and stress depth DOL2 of the second compressive stress layer were measured. In addition, from these measured values, CS2-CS1 and CS1 / CS2 were calculated for each sample. The results are shown in Table 1. Here, "CS1", "CS2", "DOL1" and "DOL2" refer to values ​​measured using an FSM-6000 manufactured by Orihara Seisakusho Co., Ltd.

[0114] [Table 1]

[0115] In Comparative Examples 1 to 3, in which the holding temperature was less than strain point-15°C (450°C), and in Comparative Example 4, in which no heat treatment was performed, the CS1 of the first main surface, which was the polished surface, was less than 820 MPa, and tempered glass with high CS on both main surfaces could not be produced. This also confirms that in Comparative Examples 1 to 4, there was no heterogeneous layer on the first main surface of the glass to be tempered, or the glass was not sufficiently regenerated.

[0116] In contrast, in Examples 1 to 6, where the holding temperature was strain point -15°C or more (550°C) and the holding time was 3 minutes or more, the CS was 820MPa or more even on the first main surface, which was the polished surface, and tempered glass with high CS on both main surfaces could be produced. This also confirms that in Examples 1 to 6, a heterogeneous layer was sufficiently regenerated on the first main surface of the glass to be tempered. In particular, in Examples 1 to 3, where the holding temperature was strain point +85°C or more (650°C) and the holding time was 3 minutes or more, and in Examples 5 to 6, where the holding temperature was strain point +50°C or less (550°C) and the holding time was 10 minutes or more, good results were obtained in that tempered glass with a CS1 / CS2 (front and back CS ratio) of 96% or more and a particularly small CS2-CS1 (front and back CS difference) could be produced.

[0117] In Comparative Example 4, the warpage was about 100 μm before strengthening, but increased to about 300 μm after strengthening. In contrast, in all of Examples 1 to 6, the warpage after strengthening could be suppressed to 250 μm or less. Here, "warpage" refers to a value measured using a laser displacement meter-type warpage measuring device manufactured by Apollo Corporation. [Industrial Applicability]

[0118] The tempered glass of the present invention can be used, for example, for mobile phones (particularly smartphones), tablet computers, personal computers, digital cameras, touch panel displays, cover glasses for other display devices, in-vehicle display devices, in-vehicle panels, and the like. [Explanation of symbols]

[0119] 1. Tempered glass 2 First major surface 3 Second main surface 4, 6 Heterogeneous layers 21 Tempered Glass 22 First major surface 23 Second main surface 24, 25 Heterogeneous Layer 31 Tempered Glass 32 First major surface 33 First compressive stress layer 34 Second main surface 35 Second compressive stress layer 37 Tensile stress layer S1 Preparation process S2 Heat treatment process S3 Chemical strengthening process T1 Molding process T2 slow cooling process T3 cooling process T4 cutting process T5 removal process T6 heat treatment process T7 Chemical strengthening process

Claims

1. A forming step of forming a glass to be strengthened having a first main surface and a second main surface opposite to the first main surface; a slow cooling step of slowly cooling the glass to be tempered at a cooling rate of 0.5 ° C. / s or more immediately after forming; a removing step of removing only a surface layer portion of the first main surface out of the first main surface and the second main surface of the glass to be strengthened; a heat treatment step of heat-treating the tempered glass by holding the tempered glass at a holding temperature of −15° C. or higher for 3 minutes or more; and a chemical strengthening step of chemically strengthening the glass to be strengthened by an ion exchange treatment to obtain strengthened glass, in this order.

2. The method for producing tempered glass according to claim 1 , wherein the glass to be tempered is formed by an overflow downdraw method or a slot downdraw method.

3. 3 . The method for producing tempered glass according to claim 1 , wherein in the heat treatment, the holding temperature is equal to or lower than a strain point plus 50° C., and a holding time at the holding temperature is 10 minutes or longer. 4 .

4. The method for producing tempered glass according to any one of claims 1 to 3, wherein in the heat treatment step, the holding temperature is a strain point plus 85°C or higher.

5. The method for producing tempered glass according to any one of claims 1 to 4, wherein in the heat treatment step, a holding time at the holding temperature is 60 minutes or less.

6. The tempered glass obtained in the chemical strengthening step has an absolute value of a difference between the compressive stress CS1 at the first main surface and the compressive stress CS2 at the second main surface of 40 MPa or less. The method for producing tempered glass according to any one of claims 1 to 5.

7. The method for producing tempered glass according to any one of claims 1 to 6, wherein the glass to be tempered is a plate glass with a thickness of 0.3 mm or less.

8. The glass to be strengthened has a glass composition, in mol %, of SiO 2 50-80%, Al 2 O 3 5-25%, B 2 O 3 0-35%, Li 2 O 0-20%, Na 2 O 1-20%, Li 2 O+Na 2 O 1-20%, K 2 The method for producing tempered glass according to any one of claims 1 to 7, containing 0 to 10% of O.

9. A tempered glass having a first compressive stress layer in a surface layer portion of a first main surface and a second compressive stress layer in a surface layer portion of a second main surface located opposite to the first main surface, an absolute value of a difference between a surface roughness Ra1 of the first main surface and a surface roughness Ra2 of the second main surface is 0.1 nm or more; The compressive stress CS1 of the first compressive stress layer and the compressive stress CS2 of the second compressive stress layer are each 820 MPa or more, and the absolute value of the difference between the compressive stress CS1 of the first compressive stress layer and the compressive stress CS2 of the second compressive stress layer is 40 MPa or less.

Citation Information

Patent Citations

  • Process for manufactuing chemically strengthened glass

    WO2012077796A1

  • Display cover glass and display cover glass fabrication method

    WO2013088856A1

  • Glass plate for chemical tempering and method for producing chemically tempered glass plate

    WO2018124084A1