Optical glass and optical element made of optical glass

The optical glass composition with controlled oxide ratios addresses thermal stability and glass transition issues, ensuring high refractive index and improved thermal stability for precision press molding.

JP7579222B2Active Publication Date: 2024-11-07HOYA CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021138721
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-09
Filing Date
2021-08-27
Publication Date
2024-11-07
Estimated Expiration
2041-08-27

AI Technical Summary

Technical Problem

Existing high refractive index, low dispersion glasses face issues with decreased thermal stability and increased glass transition temperature, leading to devitrification and surface quality deterioration during press molding, especially for large products.

Method used

An optical glass composition comprising specific oxides such as B2O3, La2O3, Gd2O3, Ta2O5, Li2O, and ZnO, with controlled ratios and contents, maintains high refractive index and improves thermal stability, ensuring glass transition temperature remains below 600°C.

Benefits of technology

The solution provides optical glass with enhanced thermal stability and glass transition temperature characteristics, preventing devitrification and maintaining surface quality, suitable for precision press molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579222000001
    Figure 0007579222000001
  • Figure 0007579222000002
    Figure 0007579222000002
  • Figure 0007579222000003
    Figure 0007579222000003
Patent Text Reader

Abstract

To provide an optical glass that achieves improvement in thermal stability and glass transition temperature while maintaining a high refractive index, and an optical element composed of the glass.SOLUTION: An optical glass contains, as essential components, B2O3, La2O3, Gd2O3, Ta2O5, Li2O and ZnO; and also contains, in mass%, SiO2 2.5-12%, Li2O 0.70% or more, ZnO 6% or more, La2O3 25% or more, Gd2O3 17.5% or less, and Ta2O5 6% or more. The total content of Li2O and ZnO is 10% or more, and the total content of Nb2O5 and WO3 is 1.0% or more. The mass ratio (La2O3+Gd2O3) / B2O3 is 2.2 or more and the mass ratio (Li2O / SiO2) is 0.200 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical glass and an optical element made of optical glass. [Background technology]

[0002] A lens made of high refractive index, low dispersion glass can be combined with a lens made of extra-low dispersion glass to form a cemented lens, thereby making it possible to make the optical system compact while correcting chromatic aberration. For this reason, high refractive index, low dispersion glass occupies a very important position as an optical element that constitutes an imaging optical system or a projection optical system such as a projector.

[0003] Another method for producing optical elements is known to be a method in which a press-molding glass material is prepared from molten glass, and this press-molding glass material is precision-press-molded in a mold to obtain an optical element (known as precision press molding). In precision press molding, the shape of the molding surface of the mold is transferred, making it possible to form the optically functional surface of the optical element without mechanical processing such as polishing or grinding. [Prior art documents] [Patent documents]

[0004] Patent Documents 1 and 2 disclose optical glasses that are suitable for precision press molding and have a high refractive index and low dispersion. [Patent Document 1] JP 2006-137662 A [Patent Document 2] JP 2003-267748 A Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, as can be seen in high refractive index, low dispersion glass, when an attempt is made to increase the refractive index of the glass, there are cases in which the thermal stability of the glass tends to decrease and the glass transition temperature tends to increase. When the thermal stability is reduced, the glass is more likely to devitrify when it is molded. In addition, in the case of glass with a high glass transition temperature, the glass must be heated to a high temperature when it is press molded, and the glass reacts with the molding surface of the mold, causing the glass to foam, etc., which tends to deteriorate the surface quality of the molded glass product. In particular, the deterioration of surface quality tends to be noticeable when producing large molded products. The glasses described in Patent Documents 1 and 2 are both excellent optical glasses, but there is room for improvement in terms of further improving thermal stability while maintaining high refractive index characteristics, and achieving both a high refractive index and a low glass transition temperature.

[0006] In view of the above, an object of the present invention is to provide an optical glass which maintains a high refractive index while improving thermal stability and glass transition temperature characteristics, and an optical element made of said glass. [Means for solving the problem]

[0007] The present inventors have conducted extensive research and found that a glass having the following configuration can solve the above problems, and have completed the present invention. [1] The essential components are B2O3, La2O3, Gd2O3, Ta2O5, Li2O and ZnO. In mass %, SiO2 2.5-12%, Li2O 0.70% or more, ZnO 6% or more, La2O325% or more, Gd2O3 17.5% or less, Ta2O56% or more, Including, The total content of Li2O and ZnO is 10% or more, The total content of Nb2O5 and WO3 is 1.0% or more, Mass ratio (La2O3+Gd2O3) / B2O3 is 2.2 or more, Mass ratio (Li2O / SiO2) is 0.200 or more, Optical glass. [2] The optical glass according to [1], wherein the refractive index nd and the glass transition temperature Tg [°C] satisfy formula (1). Tg<1700×nd-2555 (1) [3] The optical glass according to [1], which has a refractive index nd of 1.80 or more and a glass transition temperature Tg of 600° C. or less. [4] An optical element made of the optical glass according to any one of [1] to [3]. Effect of the Invention

[0008] According to the present invention, it is possible to provide an optical glass which maintains a high refractive index while improving thermal stability and glass transition temperature characteristics, and an optical element made of said glass. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In the present invention and this specification, the glass composition of optical glass is expressed on an oxide basis unless otherwise specified. Here, "glass composition on an oxide basis" refers to a glass composition obtained by converting the glass raw materials into oxides that exist in the optical glass after all of them are decomposed during melting, and each glass component is conventionally expressed as SiO2, B2O3, etc. The content and total content of glass components are on a mass basis unless otherwise specified, and "%" means "mass%".

[0010] The content of the glass component can be quantified by known methods, such as inductively coupled plasma atomic emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), etc. In this specification and the present invention, the content of a component being 0% means that the component is substantially not contained, and it is acceptable for the component to be contained at an unavoidable impurity level.

[0011] The Abbe number νd is used as a value representing the properties related to dispersion, and is expressed by the following formula: Here, nF is the refractive index at the F line (wavelength 486.13 nm) of blue hydrogen, and nC is the refractive index at the C line (656.27 nm) of red hydrogen. νd=(nd-1) / nF-nC

[0012] The optical glass of this embodiment contains, as essential components, B2O3, La2O3, Gd2O3, Ta2O5, Li2O, and ZnO, In mass %, SiO2 2.5-12%, Li2O 0.70% or more, ZnO 6% or more, Gd2O3 17.5% or less, Ta2O56% or more, The optical glass comprises: a total content of Li2O and ZnO of 10% or more; a total content of Nb2O5 and WO3 of 1.0% or more; a mass ratio (La2O3+Gd2O3) / B2O3 of 2.2 or more; and a mass ratio (Li2O / SiO2) of 0.200 or more.

[0013] [Glass composition] B2O3 and SiO2 are network-forming components of glass. The content of SiO2 is 2.5% or more from the viewpoint of maintaining the thermal stability of the glass, and is 12% or less from the viewpoint of maintaining the refractive index and keeping the glass transition temperature low. The lower limit of the SiO2 content is preferably 2.55% or more, 2.60% or more, 2.65%, 2.70%, and 2.75% or more, in that order. The upper limit of the SiO2 content is preferably 11.0% or less, 10.75% or less, 10.50% or less, 10.25% or less, and 10.0% or less, in that order.

[0014] The content of B2O3 is preferably 10% or more from the viewpoint of maintaining the thermal stability and meltability of the glass, and is preferably 20% or less from the viewpoint of maintaining the refractive index. The lower limit of the B2O3 content is more preferably 7.92% or more, 8.50% or more, 9.0% or more, 9.50% or more, 10.0% or more, 10.5% or more, 11.0% or more, 11.46% or more, 12.0% or more, 12.47% or more, 13.0% or more, and 13.5% or more. The upper limit of the B2O3 content is more preferably 20.0% or less, 19.5% or less, 19% or less, 18.5% or less, 18% or less, 17.5% or less, and 17.0% or less.

[0015] Li2O is a component that lowers the glass transition temperature while suppressing the decrease in the refractive index, and in order to obtain this effect, the Li2O content is 0.70% or more. The lower limit of the Li2O content is more preferably 0.70% or more, 0.72% or more, 0.74% or more, 0.76% or more, 0.78% or more, and 0.80% or more, in that order. The upper limit of the LiO content is not particularly limited, but from the viewpoint of maintaining the thermal stability and high refractive index characteristics of the glass, the upper limit of the LiO content is more preferably 2.16% or less, 1.99% or less, 1.90% or less, 1.80% or less, 1.78% or less, 1.76% or less, 1.74% or less, 1.72% or less, and 1.70% or less, in that order.

[0016] ZnO is also a component that reduces the glass transition temperature and improves meltability while suppressing the decrease in the refractive index, and in order to obtain this effect, the ZnO content is 6% or more. The lower limit of the ZnO content is more preferably 6.0% or more, 7.0% or more, 8.0% or more, 9.0% or more, 10.0% or more, and 11.0% or more, in that order. The upper limit of ZnO is not particularly limited, but from the viewpoint of maintaining the chemical durability and thermal stability of the glass, the upper limit of the ZnO content is more preferably 22.0% or less, 21.0% or less, 20.0% or less, 19.0% or less, 18.0% or less, 17.0% or less, and 16.0% or less, in that order.

[0017] From the viewpoint of achieving both a high refractive index and a low glass transition temperature, the total content of Li2O and ZnO (Li2O+ZnO content) is 10% or more. The lower limit of the Li2O+ZnO content is more preferably 10.0% or more, 10.5% or more, 11.0% or more, 11.5% or more, 12.0% or more, and 12.5% ​​or more in that order. The upper limit of the Li2O+ZnO content is not particularly limited, but is more preferably 23.0% or less, 22.0% or less, 21.0% or less, 20.0% or less, 19.0% or less, 18.0% or less, and 17.0% or less in that order.

[0018] La2O3 and Gd2O3 are components that increase the refractive index while maintaining low dispersion. From the viewpoint of maintaining the thermal stability of the glass, the Gd2O3 content is set to 17.5% or less. The upper limit of the Gd2O3 content is preferably 17.25% or less, 17.0% or less, 16.75% or less, 16.50% or less, 16.25% or less, and 16.0% or less, in that order. The lower limit of the Gd2O3 content is not particularly limited, but from the viewpoint of obtaining high refractive index and low dispersion characteristics with excellent thermal stability, the lower limit of the Gd2O3 content is preferably 3.0% or more, 3.5% or more, 4.0% or more, 4.5% or more, and 5.0% or more, in that order. In order to further improve the thermal stability of the glass, the Gd2O3 content is preferably less than 13.0%, more preferably 12.5% ​​or less, even more preferably 12.0% or less, and even more preferably less than 11.5%. When these preferred examples are expressed in mol%, the Gd2O3 content is preferably less than 6.7 mol%, more preferably 5.5 mol% or less, more preferably 4.9 mol% or less, even more preferably 4.8 mol% or less, and even more preferably less than 4.5 mol%.

[0019] La2O3 is a component that increases the refractive index and improves the chemical durability without decreasing the thermal stability of the glass or increasing the dispersion, and its content is 25% or more. The lower limit of the La2O3 content is preferably 25.5% or more, 26.0% or more, 26.5% or more, 27.0% or more, 27.5% or more, 28.0% or more, and 28.5% or more, in that order. In addition, the upper limit of the La2O3 content is not particularly limited, but since excessive introduction may tend to decrease thermal stability, the upper limit is preferably 41.0% or less, 40.5% or less, 40.0% or less, 39.5% or less, 39.0% or less, 38.5% or less, and 38.0% or less, in that order.

[0020] The lower limit of the total content of La2O3 and Gd2O3 (La2O3+Gd2O3 content) is preferably 37.0% or more, 37.5% or more, 38.0% or more, 38.5% or more, 39.0% or more, 39.5% or more, and 40.0% or more, in that order. Moreover, the upper limit of the total content of La2O3 and Gd2O3 (the content of La2O3 + Gd2O3) is preferably 50.0% or less, 49.5% or less, 49.0% or less, 48.5% or less, 48.0% or less, and 47.5% or less, in that order.

[0021] Nb2O5 is a component that improves the thermal stability of glass and increases the refractive index. WO3 is a component that improves the thermal stability and meltability of glass and increases the refractive index. Therefore, in the present invention, the lower limit of the total content of Nb2O5 and WO3 (Nb2O5+WO3) is 1.0% or more from the viewpoint of obtaining a high refractive index glass, and although the upper limit is not particularly limited, it is preferable that it is as low as possible from the viewpoint of maintaining good precision press moldability. In consideration of the above, the lower limit of the Nb2O5+WO3 content is preferably 1.00% or more, 1.25% or more, 1.50% or more, 1.75% or more, 2.00% or more, 2.25% or more, and 2.50% or more, in that order. Moreover, the upper limit of the Nb2O5+WO3 content is more preferably 10.0% or less, 9.5% or less, 9.0% or less, 8.5% or less, 8.0% or less, 7.5% or less, 7.0% or less, 6.5% or less, and 6.0% or less, in that order.

[0022] The content of Nb2O5 is not particularly limited as long as the content of Nb2O5+WO3 is satisfied. Although the lower limit of the Nb2O5 content is 0%, when Nb2O5 is contained, the content is preferably 0.8% or more, 0.9% or more, 1.0% or more, 1.1% or more, 1.2% or more, and 1.3% or more in that order. The upper limit of the Nb2O5 content is preferably 9.0% or less, 8.5% or less, 8.0% or less, 7.5% or less, 7.0% or less, 6.5% or less, and 6.0% or less, in that order, since an excessive amount of Nb2O5 introduced can cause large dispersion.

[0023] The content of WO3 is not particularly limited as long as the content of Nb2O5+WO3 is satisfied. Although the lower limit of the content of WO3 is 0%, when WO3 is contained, it is preferably 0.05% or more, 0.1% or more, 0.15% or more, 0.20% or more, and 0.25% or more in that order. The upper limit of the WO3 content is preferably 9.0% or less, 8.5% or less, 8.0% or less, 7.5% or less, 7.0% or less, and 6.5% or less, in that order, since an excessive amount of WO3 introduced can cause large dispersion.

[0024] In order to obtain a high refractive index, low dispersion glass, the ratio of the total content of La2O3 and Gd2O3 to the content of B2O3 (mass ratio (La2O3+Gd2O3) / B2O3) is 2.2 or more. The lower limit of the mass ratio (La2O3+Gd2O3) / B2O3) is more preferably 2.25% or more, 2.30% or more, 2.35% or more, 2.38% or more, 2.49% or more, 2.54% or more, 2.58% or more, and 2.60% or more, in that order. The upper limit of the mass ratio (La2O3+Gd2O3) / B2O3) is not particularly limited, but from the viewpoint of maintaining the thermal stability of the glass, it is preferable that the upper limit be 5.1% or less, 4.9% or less, 4.7% or less, 4.5% or less, 4.2% or less, 4.1% or less, 4.0% or less, 3.9% or less, 3.8% or less, and 3.7% or less, in that order.

[0025] In order to suppress an increase in the glass transition temperature, the mass ratio (La2O3+Gd2O3) / (Li2O+ZnO) is more preferably 4.00 or less, 3.90 or less, 3.80 or less, 3.70 or less, 3.60 or less, and 3.50 or less, in that order; and in order to maintain the high refractive index and low dispersion characteristics, it is more preferably 2.00 or more, 2.10 or more, 2.20 or more, 2.30 or more, 2.40 or more, and 2.50 or more.

[0026] Ta2O5 is a component that maintains high refractive index, low dispersion characteristics, and thermal stability. In order to obtain the above effects, the Ta2O5 content is 6.0% or more. The lower limit of Ta2O5 is preferably 6.0% or more, 7.0% or more, 8.0% or more, 9.0% or more, and 10.0% or more, in that order. The upper limit of the Ta2O5 content is not particularly limited, but from the viewpoint of maintaining the thermal stability of the glass, it is preferable that the upper limit be 20.0% or less, 19.5% or less, 19.0% or less, 18.5% or less, 18.0% or less, and 17.5% or less, in that order.

[0027] Furthermore, in order to maintain the thermal stability of the glass, the mass ratio (ZrO2+Ta2O5+Nb2O5+WO3) / (SiO2+B2O3) is more preferably 1.60 or less, 1.55 or less, 1.50 or less, 1.45 or less, 1.40 or less, and 1.35 or less, in that order; and in order to maintain high refractive index characteristics, it is more preferably 0.75 or more, 0.80 or more, 0.85 or more, 0.90 or more, 0.95 or more, and 1.00 or more.

[0028] TiO2 is a component that increases the refractive index and dispersion, and the content of TiO2 is not particularly limited in the present invention, but excessive introduction tends to deteriorate the surface quality of the glass by reacting with the molding surface of the mold during press molding, and may also intensify the coloring of the glass. Therefore, the upper limit of the content of TiO2 is preferably 3% or less, 2% or less, 1% or less, 0.5% or less, 0.1% or less, and 0% (not contained), in that order.

[0029] Y2O3 is a high refractive index, low dispersion component, and is not particularly limited in the present invention. 、 Compared to Gd2O3, which is also a rare earth oxide, it has a smaller effect of increasing the refractive index. If the total content of rare earth oxides is excessive, the thermal stability of the glass tends to decrease. Therefore, in order to maintain thermal stability and high refractive index properties, it is preferable to incorporate La2O3 and Gd2O3 rather than Y2O3. From the above viewpoint, the upper limit of the Y2O3 content is 3% or less, 2% or less, 1% or less. belowThe preferred range is 0.5% or less, 0.1% or less, and 0% is also acceptable.

[0030] Yb2O3 is an optional component used as a component with a high refractive index and low dispersion. Excessive introduction reduces the thermal stability of the glass and increases the glass transition temperature. Also, the absorption of the glass in the infrared region tends to increase. The preferred upper limit of the Yb2O3 content is 3%, 2%, 1%, 0.5%, and 0.1%, in that order. 0% is also acceptable.

[0031] Although ZrO2 is an optional component in the present invention, it is preferable to incorporate it because it has the effect of improving the thermal stability of the glass without decreasing the refractive index of the glass. The lower limit of the ZrO2 content is more preferably 2.50% or more, 2.55% or more, 2.60% or more, 2.65% or more, 2.70% or more, and 2.75% or more, in that order. The upper limit of the ZrO2 content is preferably 10.0% or less, 9.5% or less, 9.0% or less, 8.5% or less, 8.0% or less, 7.5% or less, 7.0% or less, and 6.5% or less, in that order. Note that as the content increases, the liquidus temperature (thermal stability deteriorates) increases rapidly.

[0032] Sb2O3 functions as a fining agent. If too much Sb2O3 is added, the molding surface of the press mold may be damaged during precision press molding, and the glass may tend to become more strongly colored. The lower limit of the Sb2O3 content is preferably 0% or more, 0.01% or more, and 0.02% or more, in that order, and the upper limit of the Sb2O3 content is preferably 1.0% or less, 0.9% or less, 0.8% or less, 0.7% or less, 0.6% or less, and 0.5% or less, in that order. Note that the Sb2O3 content is an exclusive ratio (the proportion of Sb2O3 when the total mass of glass components other than Sb2O3 is taken as 100).

[0033] From the viewpoint of lowering the glass transition temperature, the mass ratio of the Li2O content to the SiO2 content (Li2O / SiO2) is 0.200 or more. The lower limit of the mass ratio (Li2O / SiO2) is preferably 0.200 or more, 0.210 or more, and 0.220 or more, in that order. Moreover, in order to suppress an increase in the glass transition temperature and maintain thermal stability, the upper limit of the mass ratio (Li2O / SiO2) is preferably 0.300 or less, 0.290 or less, 0.280 or less, and 0.270 or less, in that order.

[0034] Furthermore, in order to solve the problems of the invention, the total content of the above components and clarifier is preferably 90% or more, and more preferably 93% or more, 95% or more, 96% or more, 98% or more, 99% or more, 99.5% or more, and 99.9% or more in that order. In order to solve the problems of the invention, the total content of Bi2O3, Ga2O3, Al2O3, BaO, SrO, CaO, MgO, Lu2O3, P2O5, and GeO2 is preferably 8% or less, and more preferably 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, and 0.1% or less in that order.

[0035] Due to problems such as volatilization during glass melting, the F content is preferably 0.1% or less, and more preferably contains no F. In order to reduce the burden on the environment, it is preferable that the material is substantially free of Pb, Cd, Te, Tl, U, Th, Se, and As. In order to prevent coloration of the glass, it is preferable that the glass is substantially free of Fe, Cr, V, Co, Ni, Nd, Er, Eu, Cu, Tb, and Ho.

[0036] [Glass characteristics] In the optical glass of this embodiment, it is preferable that the refractive index nd and the glass transition temperature Tg [° C.] satisfy the formula (1). Tg<1700×nd-2555 (1) By satisfying the formula (1), it is possible to achieve both high refractive index properties and press moldability. The optical glass of this embodiment preferably has a refractive index nd of 1.80 or more and a glass transition temperature Tg of 600° C. or less. The lower limit of the refractive index nd is more preferably 1.805, 1.810, 1.815, 1.820, 1.825, 1.830, 1.835, 1.840, and 1.845, in that order. The upper limit of the refractive index is more preferably 1.880 or less, 1.875 or less, 1.870 or less, 1.865 or less, and 1.860 or less, in that order. More preferable lower limits of the Abbe number vd are 39.0 or more, 39.1 or more, 39.2 or more, 39.3 or more, 39.4 or more, and 39.5 or more, in that order. More preferable upper limit of the Abbe number vd: 41.0 or less, 40.9 or less, 40.8 or less, 40.7 or less, and 40.6 or less are more preferable in this order. Increasing the refractive index of glass corresponds to expanding the degree of freedom of glass when considering glass as a material for optical elements. Increasing the refractive index is preferable from the viewpoint of expanding the degree of freedom, but if the refractive index is increased while maintaining dispersion, there is a tendency for the stability of the glass to decrease, so the above range is preferable.

[0037] The lower limit of the glass transition temperature Tg is more preferably 530° C. or more, 535° C. or more, 540° C. or more, 545° C. or more, and 550° C. or more, in that order. The upper limit of the glass transition temperature Tg is more preferably 600° C. or less, 595° C. or less, 590° C. or less, and 585° C. or less, in that order.

[0038] A low glass transition temperature (Tg) is preferable to prevent wear on the press mold and damage to the release film, but lowering the Tg too much reduces the refractive index and the thermal stability of the glass. Regarding glass stability, the difference (Tx-Tg) between the crystallization temperature Tx and the glass transition temperature Tg can be used as an index of resistance to devitrification when a solidified glass is reheated. It can be considered that the greater the difference (Tx-Tg) between the crystallization temperature Tx and the glass transition temperature Tg, the better the resistance to devitrification.

[0039] The glass transition temperature Tg and the crystallization peak temperature Tx can be determined as follows. In differential scanning calorimetry, when a glass sample is heated, endothermic behavior associated with a change in specific heat, that is, an endothermic peak appears, and when the temperature is further increased, an exothermic peak appears. In differential scanning calorimetry, a differential scanning calorimetry curve (DSC curve) is obtained, with the horizontal axis representing temperature and the vertical axis representing the amount corresponding to the heat generation and endothermic heat of the sample. In this curve, the intersection point of the tangent at the point where the slope is maximum when the endothermic peak appears from the baseline and the baseline is the glass transition temperature Tg, and the intersection point of the tangent at the point where the slope is maximum when the exothermic peak appears and the baseline is the crystallization peak temperature Tx. The glass transition temperature Tg and the crystallization peak temperature Tx can be measured by using a sample obtained by thoroughly crushing glass in a mortar, for example, using a high-temperature differential scanning calorimeter "DSC3300SA" manufactured by Bruker Corporation. In the reheat press molding method, in which glass material is heated and softened to form it into the required shape, it is necessary to heat the glass material to a temperature higher than the glass transition temperature. When the temperature of the glass during molding reaches the crystallization temperature range, crystals precipitate, so glass with a small (Tx - Tg) is disadvantageous in terms of molding while preventing devitrification. Conversely, glass with a large (Tx - Tg) is advantageous in terms of reheating, softening, and forming without devitrification.

[0040] From the above viewpoints, the lower limit of Tx-Tg is more preferably 130.0°C or more, 135.0°C or more, 140.0°C or more, 145.0°C or more, 150.0°C or more, and 155.0°C or more, in that order. Tx-Tg can be, for example, 300.0° C. or less, 280.0° C. or less, 260.0° C. or less, 240.0° C. or less, or 220.0° C. or less, but can also be greater than the values ​​exemplified herein.

[0041] From the viewpoint of maintaining resistance to devitrification (thermal stability at high temperatures) when melting the glass or forming the molten glass, the upper limit of the liquidus temperature is preferably 1210°C, 1200°C, 1190°C, and 1180°C, in that order. From the viewpoint of maintaining a high refractive index and a low glass transition temperature, the lower limit of the liquidus temperature is preferably 1080°C, 1090°C, 1100°C, and 1110°C, in that order.

[0042] The optical glass of the present invention is not particularly limited, but it is preferable that it satisfies the following physical properties. The lower limit of the coloring degree λ80 is naturally determined by the composition. The upper limit of the coloring degree λ80 is preferably 490 nm or less, 485 nm or less, 480 nm or less, and 475 nm or less, in that order. The lower limit of the coloring degree λ70 is naturally determined by the composition. The upper limit of the coloring degree λ70 is preferably 400 nm or less, 395 nm or less, 390 nm or less, and 385 nm or less, in that order. The lower limit of the coloring degree λ5 is naturally determined by the composition. The upper limit of the coloring degree λ5 is preferably 360 nm or less, 355 nm or less, 350 nm or less, and 345 nm or less, in that order. The lower limit of the partial dispersion ratio Pg,F is preferably 0.525 or more, 0.535 or more, 0.545 or more, and 0.555 or more, in that order. The upper limit of the partial dispersion ratio Pg,F is preferably 0.610 or less, 0.600 or less, 0.590 or less, and 0.580 or less, in that order.

[0043] [Optical glass manufacturing] The optical glass according to the embodiment of the present invention may be produced by mixing glass raw materials to obtain the above-mentioned predetermined composition, and by using the mixed glass raw materials according to a known glass manufacturing method. For example, a plurality of compounds are mixed and mixed sufficiently to obtain a batch raw material, and the batch raw material is put into a crucible such as a quartz crucible or a platinum crucible to be roughly melted (rough melt). The melt obtained by the rough melting is quenched and crushed to produce cullet. The cullet is further put into a platinum crucible, heated and remelted (remelt) to obtain a molten glass, which is then clarified and homogenized, molded, and slowly cooled to obtain an optical glass. A known method may be applied to the molding and slowly cooling of the molten glass. In addition, as long as a desired glass component can be introduced into the glass in a desired content, the compound used when preparing the batch raw materials is not particularly limited. Examples of such compounds include oxides, carbonates, nitrates, hydroxides, etc.

[0044] [Manufacturing of optical elements, etc.] To manufacture an optical element using the optical glass according to the embodiment of the present invention, a known method may be applied. For example, glass raw material is melted to form molten glass, and the molten glass is poured into a mold to form a plate shape and annealed to manufacture a glass material made of the optical glass according to the present invention. The obtained glass material is appropriately cut, ground, and polished to prepare a press-molded preliminary body (preform) having a size suitable for press molding. The preform is heated and softened, and precision press-molded by a known method, and centering and other processes are performed as necessary to manufacture an optical element such as an aspherical lens. The optically functional surface of the prepared optical element may be coated with an anti-reflection film, a total reflection film, or the like depending on the intended use. Examples of optical elements include various lenses such as aspherical lenses, prisms, and diffraction gratings. EXAMPLES

[0045] [Preparation of glass samples] Example 1 To obtain glass having each composition shown in Tables 1 to 3 (in terms of mass %) (Tables 4 to 6, in terms of mol %), compound raw materials corresponding to each component, i.e., raw materials such as boric acid, carbonates, and oxides, were weighed and thoroughly mixed to obtain a blended raw material. The blended raw materials were placed in a platinum crucible, heated to 1300 to 1400°C for 2 hours in an air atmosphere to melt, and homogenized and clarified by stirring to obtain a molten glass. The molten glass was cast into a mold to be shaped, and slowly cooled to obtain a block-shaped glass sample. Alternatively, the raw materials may be roughly melted to produce cullet, the cullet remelted, homogenized by stirring, and clarified to obtain molten glass, which may then be cast into a mold and molded, followed by slow cooling.

[0046] [Glass sample evaluation] [1] Glass composition The contents of the glass components of the obtained glass samples were measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES). Note that the F content was 0% in all the glass samples shown in Tables 1 to 3 (Tables 4 to 6 are shown in mol %). [2] Refractive index nd, Abbe number νd and partial dispersion ratio Pg,F The refractive index of the glass sample annealed at a cooling rate of -30°C / hour was measured at a predetermined wavelength in accordance with the Japan Optical Glass Industry Association standard JOGIS-01. The Abbe number νd and partial dispersion ratio Pg,F were calculated from the refractive index measurement results. [3] Specific gravity Measurements were made based on the Japan Optical Glass Industry Association standard JOGIS-05. [4] λ80, λ70, λ5 A glass sample was processed to have a thickness of 10 mm and parallel optically polished flat surfaces, and the spectral transmittance was measured in the wavelength range from 280 nm to 700 nm. The intensity of the light beam perpendicularly incident on one of the optically polished flat surfaces was defined as intensity A, and the intensity of the light beam emerging from the other flat surface was defined as intensity B, and the spectral transmittance B / A was calculated. The wavelengths at which the spectral transmittance was 80%, 70%, and 5% were defined as λ80, λ70, and λ5, respectively. Note that the spectral transmittance also includes the reflection loss of the light beam on the sample surface. [5] Glass transition temperature Tg, crystallization peak temperature Tx The glass was thoroughly crushed in a mortar to prepare a sample, and the measurement was carried out using, for example, a high-temperature differential scanning calorimeter "DSC3300SA" manufactured by Bruker Corporation. No crystals were observed on the surface or inside of each glass sample. [6] Liquidus temperature 5-8cc of glass sample was placed in a furnace heated to 1300℃ and held for 20 minutes. After it was fully melted, it was transferred to a furnace heated to a specified temperature and held for 2 hours, after which it was cooled at room temperature. After cooling, the inside of the glass was observed with an optical microscope, and the liquidus temperature was determined from the presence or absence of crystals. The measured physical properties of the glass are shown in Tables 7 to 9.

[0047] [Table 1] [Table 2] [Table 3] [Table 4] [Table 5] [Table 6] [Table 7] [Table 8] [Table 9]

[0048] Example 2 Each glass sample obtained in Example 1 was cut and ground to prepare a preform. The preform was heated, precision press-molded, and precision annealed to prepare an aspheric lens. No foreign matter such as crystals or bubbles was found inside or on the surface of the fabricated aspheric lens, and an optical element with excellent internal and surface quality was obtained. The precision press molding conditions, molding mold, release film, and the like may be any known conditions, molding mold, and release film.

Claims

1. As an essential component, B 2 O 3 , La 2 O 3 , Gd 2 O 3 , Ta 2 O 5 , Li 2 O and ZnO, In mass %, Yes 2 2.5 to 12%, Li 2 0.70% or more, ZnO 6% or more, La 2 O 3 25% or more, Gd 2 O 3 17.5% or less, Ta 2 O 5 6% or more, TIO 2 Below 1%, Including, Li 2 The total content of O and ZnO is 10% or more, Nb 2 O 5 and W.O. 3 The total content is 1.0% or more and 9.0% or less, Mass ratio (La 2 O 3 +Gd 2 O 3 ) / B 2 O 3 is 2.2 or more, Mass ratio (Li 2 O / SiO 2 ) is 0.200 or more, And, An optical glass having a refractive index nd and a glass transition temperature Tg [°C] that satisfy formula (1). Tg<1700×nd-2555... (1)

2. The optical glass according to claim 1, having a refractive index nd of 1.80 or more and a glass transition temperature Tg of 600°C or less.

3. A mass ratio (ZrO2 + Ta2O5 + Nb2O5 + WO3) / (SiO2 + B2O3) is 0.85 or more and 1.45 or less, Y 2 O 3 1% or less, The optical glass of claim 1 .

4. Nb 2 O 5 1.1% or more, WO 3 8.0% or less, The optical glass of claim 1 .

5. The total content of Li 2 O and ZnO is 11.0% or more, The total content of Nb 2 O 5 and WO 3 is 2.50% or more; 2. The optical glass according to claim 1,

6. TiO 2 0.1% or less, Y 2 O 3 0.5% or less, The optical glass of claim 1 .

7. An optical element comprising an optical glass according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Optical glass for precision press molding, preform for precision press molding and its manufacturing method

    JP2003267748A

  • Optical glass, preform for precision press molding and its manufacturing method and optical element and its manufacturing method

    JP2006137662A

  • Optical glass, preform for precision press-molding, optical element, and methods for manufacturing the same

    JP2008201661A

  • Optical glass

    JP2011006318A

  • Optical glass

    JP2013256438A