Method and apparatus for etching a lithographic mask

The method addresses the inefficiencies in lithographic mask defect repair by using a controlled particle beam and gas atmosphere for precise etching, improving the quality and efficiency of microstructured component production.

JP7579426B2Active Publication Date: 2024-11-07CARL ZEISS SMT GMBH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023507771
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-07
Filing Date
2021-08-06
Publication Date
2024-11-07
Estimated Expiration
2041-08-06

AI Technical Summary

Technical Problem

Existing lithographic masks are complex and expensive to produce, and defects in these masks can lead to undesired structures during microstructured component manufacturing, necessitating costly and inefficient defect detection and repair processes.

Method used

A method for particle beam-induced etching of lithographic masks using a focused particle beam and a controlled atmosphere with specific gas components, including a first gas component that forms volatile compounds and a second gas component that prevents unwanted deposition, allowing for precise and controlled material removal.

Benefits of technology

The method enables targeted and efficient etching of defects with high resolution, reducing damage to the mask and improving the quality of microstructured components by minimizing unwanted side effects and enhancing process control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579426000001
    Figure 0007579426000001
  • Figure 0007579426000002
    Figure 0007579426000002
  • Figure 0007579426000003
    Figure 0007579426000003
Patent Text Reader

Abstract

A method for particle beam induced etching of a lithography mask (100), more particularly a non-transparent EUV lithography mask, comprising the steps of: a) providing (S1) the lithography mask (100) in a process atmosphere (ATM); b) emitting (S2) a focused particle beam (110) onto a target location (ZP) on the lithography mask (100); and c) supplying (S3) at least one first gas component (GK1) to the target location (ZP) in the process atmosphere (ATM), wherein the first gas component (G d) supplying (S4) at least one second gas component (GK2) to a target location (ZP) in a process atmosphere (ATM), wherein under predetermined process conditions involving exposure to a particle beam (110), the second gas component (GK2) forms a deposit comprising compounds of silicon and oxygen, nitrogen and / or carbon.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and apparatus for etching a lithographic mask.

[0002] The entire content of priority application number DE 10 2020 120 884.7 is incorporated herein by reference. [Background technology]

[0003] Microlithography is used to manufacture finely structured components, e.g. integrated circuits. Microlithographic processes are carried out using a lithographic apparatus having an illumination system and a projection system. To transfer the mask structure into a photosensitive coating of the substrate, the image of a mask (reticle), illuminated by the illumination system, is projected by the projection system onto a substrate, e.g. a silicon wafer, which in this case is coated with a photosensitive layer (photoresist) and positioned in the image plane of the projection system.

[0004] In order to achieve small structure sizes and thus increase the integration density of the components of the microstructure, light with very short wavelengths, for example called deep ultraviolet (DUV) or extreme ultraviolet (EUV), is increasingly used. DUV has a wavelength of, for example, 193 nm, and EUV has a wavelength of, for example, 13.5 nm. The lithography masks, in these cases, have themselves structure sizes that are in the range of 5 to 100 nm. The production of these types of lithography masks is very complex and therefore expensive, and there is otherwise no guarantee that the structures produced with the lithography mask have the desired functionality, especially since the lithography mask must be free of defects. For this reason, the lithography masks undergo verification, which means for example that the absence of defects in the lithography mask is tested. In this procedure, the defects are detected and localized, allowing a targeted repair of the defects. A typical defect is the absence of the intended structure, for example due to an unsuccessful implementation of an etching procedure, or the presence of an unintended structure, for example due to an overly rapid etching procedure or an etching procedure performed in the wrong place. These defects can be eliminated by targeted etching of excess material or targeted deposition of additional material at the relevant locations; such operations are made possible in a very targeted manner, for example, by focused electron beam induced processing (FEBIP).

[0005] DE 10 2017 208 114 A1 discloses a method for particle beam induced etching of a photolithography mask, the method comprising the steps of providing an activated particle beam to a location to be etched and providing an etching gas to the location to be etched, where the etching gas comprises a first gas component and water vapor as a second gas component, where the first gas component comprises nitrogen, oxygen and chlorine in one compound.

[0006] DE 10 2013 203 995 A1 discloses a method and an apparatus for protecting a substrate while it is acted upon with at least one particle beam, which comprises the steps of applying a locally confined protective layer on the substrate, etching the substrate and / or a layer deposited on the substrate by means of a particle beam and at least one gas and / or depositing material on the substrate by means of a particle beam and at least one precursor gas, and removing the locally confined protective layer from the substrate. Summary of the Invention

[0007] Against this background, it is an object of the present invention to improve the operation of lithographic masks.

[0008] According to a first aspect, a method is proposed for particle beam induced etching of a lithography mask, more specifically a non-transparent EUV lithography mask. In a first step a), a lithography mask is provided in a process atmosphere. In a second step b), a focused particle beam is emitted onto a target location on the lithography mask. In a third step c), at least one first gas component is supplied to the target location in the process atmosphere, where the first gas component can be converted into a reactive form by activation, where the reactive form reacts with a material of the lithography mask to form a volatile compound. In a fourth step d), at least one second gas component is supplied to the target location in the process atmosphere, where the second gas component comprises a compound of silicon with oxygen, nitrogen and / or carbon.

[0009] This method has the advantage that the etching process that takes place can be controlled more efficiently and therefore carried out in a more targeted and specific manner, which means that it is possible to increase the process resolution of the etching process overall, and thus to act in a targeted manner on lithographic masks with smaller structures and / or to act on defects with smaller sizes.

[0010] The specified sequence of the individual method steps, in particular steps b) to d), does not necessarily have to be performed in the order specified; instead, the steps can be performed simultaneously, alternating and / or in different combinations or temporal sequences.

[0011] Steps c) and d) are in particular carried out in time prior to and / or simultaneously with step b).

[0012] The etching process starts when the appropriate composition of the process atmosphere for etching the lithography mask is present and the particle beam is emitted with the appropriate energy onto the target location. By supplying the two gas components before the particle beam is actually emitted, it is possible to ensure that extraneous gases (e.g. still present in the process atmosphere from the preceding process step) are removed and thus the process atmosphere has the desired composition from the start of the etching process. The continuous supply of the gas components while the particle beam is emitted makes it possible to ensure that the composition of the process atmosphere is constant and / or remains within a defined range.

[0013] Steps c) and d) can be performed simultaneously or at different times, for example, the first and second gas components can be supplied intermittently or alternately. The first and second gas components are more specifically supplied so that the composition of the process atmosphere at the target location is within a predetermined range. In an embodiment, the first and second gas components can be mixed before being supplied to the target location, and a mixture with a desired composition can be supplied to the target location.

[0014] Particle beam induced etching is advantageously carried out substantially at the location where the particle beam impinges on the surface of the lithographic mask to be acted upon. The spatial limit or resolution of the etching process depends, for example, on the nature of the particle beam. The particle beam may, for example, comprise photons, ions, protons, neutrons or otherwise electrons. The use of an electron beam is particularly advantageous, since it can be focused on a very small impact area, while at the same time the electrons do not cause substantial damage to the surface receiving the beam. The resolution achievable with an electron beam is therefore particularly high.

[0015] In principle, the etching process at the molecular level consists in the impact of a particle beam on the surface to be acted upon, where it triggers, for example, secondary electrons which emanate from the surface, for example in the region of the impact area. The energy of these secondary electrons can be sufficient to bring about the dissociation of molecules. If such secondary electrons impact, for example, on previously inactive etching gas molecules adsorbed on the surface, the molecules undergo dissociation and thus enter reactive forms. The reactive forms react with atoms or molecules at the surface of the material, forming, for example, volatile compounds. Thus, in this way, the surface is eroded. The exact physicochemical processes taking place here are very diverse and complex, and are the subject of ongoing research.

[0016] Important parameters that substantially affect the etching process and are therefore used to control it are, for example, temperature, the composition of the process atmosphere, the local gas pressure at the target location, the partial pressures of the components, and the intensity and energy of the particle beam. This list is not exhaustive.

[0017] The process atmosphere may be, for example, of controlled composition and, for example, 10 -2 ~10 -8 The process atmosphere is an atmosphere with a controlled pressure in the mBar range. The process atmosphere is provided, for example, by a vacuum housing. Nevertheless, the process atmosphere is subject to spatial and temperature variations. In particular, the process atmosphere in the action area has substantial variations in its composition, since this composition depends on the supply of process gases and also on chemical reactions. In addition, the pressure of the process atmosphere when subjected to the action of a lithography mask may be several orders of magnitude higher compared to when no action is occurring. Also, the pressure may differ by several orders of magnitude in the action area compared to the pressure elsewhere in the vacuum housing.

[0018] The lithography mask is more specifically an EUV lithography mask. EUV stands for "extreme ultraviolet" and denotes an active light wavelength in the range of 0.1-30 nm, more specifically 13.5 nm. At these wavelengths, it is necessary to use reflective optical elements, which also applies to lithography masks. The lithography mask therefore has a layer that is reflective for EUV radiation, more specifically embodied as a Bragg mirror, and also has a structured absorbing layer on the reflective surface. Such a mask is also called a binary lithography mask. The effect of the structured absorbing layer is to achieve a spatial modulation of the intensity of the reflected radiation, ultimately resulting in a controlled local variation in the exposure on the sample.

[0019] Thus, a lithographic mask, for example, has areas that reflect as much of the incident radiation as possible, and other areas that absorb certain parts of the radiation. The radiation does not have to be completely absorbed in these areas. The level of residual intensity that is still acceptable depends on the particular lithographic process. Preferably, less than 10% of the incident intensity is reflected.

[0020] Any defects or disturbances in the structure of the structured layer lead to undesired exposure in the lithography process, and it is therefore particularly important that the lithography mask has as few defects as possible. Any defects present are checked using defined test methods and then, if possible, undergo targeted repair. The method proposed here is particularly suitable for removing material remaining in positions where no material should be present. These are also called opaque defects, because the material absorbs EUV radiation and therefore the intensity of the reflected radiation is excessively low. These defects can be removed by targeted etching of the excess material.

[0021] In a third step c), at least one first gas component is supplied to the target location in the process atmosphere. In this case, the first gas component forms an etching gas. This gas is characterized by a relatively highly reactive constituent in a compound having a relatively low reactivity. The reactive constituents include in particular halogens such as fluorine or chlorine. The etching gas can be decomposed or otherwise converted into a reactive form by activation.

[0022] The etching gas is delivered as close as possible to the target location in the process atmosphere. The etching gas itself is, for example, 10 -3 ~10 -4The etching gas has a pressure in the range of mBar. Individual molecules of the etching gas adsorb to the surface of the lithography mask. In the adsorbed state, these molecules are bound to the surface at short distances, but may also diffuse over the surface. In this way, for example, an adsorbed monolayer of molecules can be formed on the surface of the lithography mask, preferably in the region of the target location. As a result of the physical proximity of the adsorbed molecules to the surface atoms of the lithography mask, the probability of the dissociated reactive molecules reacting with the atoms of the surface is greatly increased.

[0023] The etching gas is indirectly activated via the particle beam. As already explained, activation is triggered, for example, by secondary electrons induced from the surface of the particle beam. Activation can also be performed directly by the particles of the particle beam, but the effective cross section of such a reaction is very small and therefore its contribution is only minor. The effective cross section depends, for example, on the beam energy that can be used to influence it.

[0024] Advantageously, reactions of active species in the etching gas with surface atoms form volatile compounds, which can be pumped off from the target site through the process atmosphere.

[0025] Although the particle beam induced etching process described above already results in high process resolution, there may also be undesirable side effects such as spontaneous reactions not induced by the particle beam or etching reactions at locations other than the target location. Therefore, in order to have better control over the etching process, it is proposed that a second gas component is supplied to the target location in the process atmosphere. The second gas component comprises a compound of silicon with oxygen, nitrogen and / or carbon. The second gas component may more specifically comprise a compound which, upon exposure to the particle beam, under predefined process conditions, can form a deposit comprising a compound of silicon with oxygen, nitrogen and / or carbon. These predefined process conditions include in particular the pressure, and also the partial pressure of the second gas component at the target location, and also further compositions of the process atmosphere at the target location. It is also possible to say that the second gas component comprises a deposition gas.

[0026] This is unusual since the purpose of action is to ablate material, not to build it up. However, in experiments, applicants have shown that by supplying such a deposition gas, the etching process can be performed with improved control, particularly over the etch rate, and with significantly reduced damage to the lithography mask, not only at the target location, but also at other locations.

[0027] Corresponding to the first gas component, the second gas component is delivered in as targeted a manner as possible at the target location. The molecules of the second gas component can likewise adsorb to the surface of the lithography mask. In this case, the two gas components compete for free sites on the surface. In the equilibrium state, for example, a distribution occurs depending on factors including the partial pressures of the two components in the gas phase, their tendency to adsorb on the respective surfaces, and the individual mobility of some of the molecules.

[0028] When the molecules of the second gas component adsorbed on the surface are activated, as can occur for example by secondary electrons, the molecules can decompose, in which case silicon- and oxygen-containing molecules such as SiO or SiO2 are attached to the surface. During the proposed etching method, the process conditions are preferably set so that no deposits are formed or so that deposits are formed only to a very small extent. This means, for example, that the ratio of etching material to deposition material is at least 5:1, preferably 10:1, more preferably 20:1, even more preferably 50:1, and even more preferably 100:1.

[0029] It is also possible to state that a slower etching process is performed by a parallel deposition process proceeding significantly slower, and that the etching process can be controlled more effectively as a result. However, this is not the only effect, given the advantageously deactivating effect of the second gas component or its reactive form (following activation by the particle beam or secondary effects explained above); instead, the etching process can also be more effectively spatially limited, avoiding cases of damage in locations of the lithographic mask not subjected to the particle beam.

[0030] In order to obtain a targeted control over the etching process, the individual gas flows of the first and second gas components are preferably controlled. The gas flow of the first gas component is, for example, in the range of 0.1 sccm to 10 sccm (sccm = standard cubic centimeters). The gas flow of the second gas component is preferably set based on the gas flow of the first component. For example, a ratio of the first gas component to the second gas component of 100:1 to 10000:1 is set. The ratio of the gas flows of the first and second components is particularly relevant since it determines the stoichiometric ratio of the components in the region of the target location.

[0031] In embodiments, the process conditions of the etching process are more specifically set to avoid layering or deposition of material. Such layering can be obtained, for example, as a result of the presence of a second gas component in the process atmosphere. "Layering" in this context is more specifically set to avoid layering or deposition of material, for example, as a result of the presence of a second gas component in the process atmosphere. 2 This means that more than just a few atoms, such as individual atoms over an area of ​​100 nm, precipitate on or react with the surface. Layer formation is avoided, for example, when no coherent layer is formed. The process conditions include, among others, the pressure of the process atmosphere, the partial pressures of the first and second gas components at the target location, the further composition of the process atmosphere at the target location, the temperature, and the energy and intensity of the particle beam.

[0032] In one embodiment, the second gas component comprises a silicate, a silane, a siloxane, a silazane, and / or a silicon isocyanate.

[0033] Silicates are salts and esters of orthosilicic acid, Si(OH4). Silanes have a silicon backbone saturated with hydrogen. Siloxanes and silazanes are compounds derived from silanes, with siloxanes having the general empirical formula: R3Si-[O-SiR2] n -O-SiR3, where R is a group which can be a hydrogen atom or an alkyl group, and silazanes have the general empirical formula R3Si-[NH-SiR2] n -NH-SiR3.

[0034] An example of a silicate is tetraethylorthosilicate Si(OC2H5)4, and an example of a silane is cyclopentasilane H 10 Si5, and an example of a siloxane is pentamethyldisiloxane CH 15An example of a silazane is 1,1,3,3-tetramethyldisilazane (CH3)2(SiH)2O, and an example of a silicon isocyanate is tetraisocyanatosilane C4N4O4Si. The specific composition of any deposit formed will depend on factors including, among others, further additional gases provided in the working process. For example, when silane is used in combination with ammonia NH3, a deposit containing silicon nitride may be formed.

[0035] According to another embodiment, under certain process conditions involving exposure to a particle beam, the second gas component forms a deposit comprising compounds of silicon and oxygen, nitrogen and / or carbon.

[0036] It may be noted that in the context of the proposed etching process, the formation of such deposits is preferably avoided by appropriate setting of the process conditions.

[0037] As already mentioned above, the exact chemical composition of any deposit formed also depends on the further additional gases supplied in the working process. For example, when silane is combined with ammonia NH3, a deposit containing silicon nitride can be formed.

[0038] According to another embodiment, the deposits formed during the etching process with the second gas component are removed in a step of wet chemical cleaning of the lithography mask.

[0039] This has the advantage that deposits which have a protective effect during particle beam induced etching processes are removed without residue and therefore have no effect on lithographic processes using the affected lithographic mask.

[0040] According to another embodiment, the first gas component comprises one of xenon difluoride XeF2, sulfur hexafluoride SF6, sulfur tetrafluoride SF4, nitrogen trifluoride NF3, phosphorus trifluoride PF3, tungsten hexafluoride WF6, tungsten hexachloride WCl6, molybdenum hexafluoride MoF6, hydrogen fluoride HF, nitrogen oxygen fluoride NOF, and / or phosphorus hexafluoride P3N3F6.

[0041] According to another embodiment, the second gas component is supplied temporally before and / or after projecting the particle beam to the target location.

[0042] The second gas component is passed to the target location, for example, via a line system. In this case, a valve or similar control device can be provided for the purpose of setting the amount or mass flow rate of the second gas component in the line system in order to have a strict control over the supply of the second gas component. For example, before the target location receives the emitted beam, the second gas component is supplied by opening the corresponding valve. The valve is then closed and the particle beam is emitted. Depending on the length of the line from the valve to the nozzle at the target location, even with the valve closed, there is still a reduced gas flow in the process atmosphere. Furthermore, the gas molecules adsorbed on the surface still remain adsorbed on the surface for a certain time, so that a positive effect is achieved, even though the second gas component is no longer supplied during the emission of the beam. It can also be stated that even after the valve is closed, the partial pressure or stoichiometric proportion of the second gas component in the process atmosphere in the area of ​​the target location is still high enough for a certain period of time to achieve a positive effect.

[0043] According to another embodiment, the second gas component is supplied during projection of the particle beam to the target location.

[0044] According to another embodiment, a third gas component comprising an oxidizing agent and / or a reducing agent is further provided.

[0045] The third gas component may occur in time before, during, and / or after delivery of the particle beam to the target location. The third gas component may be supplied in time before, during, and / or after delivery of the first and / or second gas components, and / or intermittently with respect to the first and / or second gas components. Intermittently in this context means that the respective components are supplied in an alternating manner.

[0046] Examples of oxidizing agents are hydrogen peroxide H2O2, nitrous oxide NO2O. Examples of reducing agents are nitric oxide NO, nitrogen dioxide NO2, nitric acid HNO3, hydrogen H2, ammonia NH3 and / or methane CH4. It can be pointed out that oxidizing agents can also function as reducing agents and reducing agents can also function as oxidizing agents, depending on the strength of the oxidizing or reducing ability of the respective other components being oxidized or reduced.

[0047] A third gas component can add even more effective control to the etching process by creating additional reaction pathways and / or by favorably influencing the chemical balance of equilibrium reactions.

[0048] In an embodiment, it is further possible to supply a chemically inert buffer gas, which can particularly contribute to the stabilization of the etching process, such as a substantially uniform etching rate in space and time. A suitable buffer gas is preferably a noble gas, such as argon.

[0049] According to a further embodiment, supplying the first, second and / or third gas component comprises providing a solid or liquid phase of each component; setting a temperature of the solid or liquid phase of each component such that a required vapor pressure of the respective component is reached across the solid or liquid phase; supplying each gas component into the process atmosphere via a respective supply line; Includes.

[0050] This embodiment is particularly advantageous with regard to the control of the individual gas flows of each component. For example, for each component to be fed, a separate container or tank is provided in which the respective solid or liquid phase is stored. Each tank has its own thermal regulation means which can be used to set the temperature of the tank contents. Thermal regulation means include, for example, electric heating elements such as Peltier elements which can be used for cooling or heating. It is also possible that a cooling circuit is provided to achieve temperatures well below 0°C.

[0051] The vapor pressure of the solid or liquid phase of each component can be very precisely controlled via temperature. Due to the low pressure of the process atmosphere, a pressure gradient exists from each tank into the process atmosphere, which causes each gas component to flow from the tank through the supply line into the process atmosphere.

[0052] Separate gas streams of two or more gas components are mixed together, for example in a common mixing chamber, at the end of the respective supply lines from which further supply lines lead into the process atmosphere, so that a homogenous mixture is formed.

[0053] According to another embodiment, the mass flow rate and / or the volume flow rate of the respective gas component is controlled by setting the line cross-section of the respective supply line and / or by controlling the duty cycle of the closing valves.

[0054] In this way, it is possible to control the gas flow rates with greater control and achieve fast variations in the gas flow. For example, a first gas flow ratio of the first and second gas components is selected before the particle beam is emitted, while a second gas flow ratio is selected during the emission of the beam and a third gas flow ratio is selected after the emission of the beam, where the duration of each is in the range of minutes. The temperature of the solid or liquid phase of each component cannot change fast, because the heat transfer process itself operates on a time scale in the range of minutes.

[0055] For example, in each supply line there is a respective supply valve for controlling the mass flow rate and / or the volume flow rate of the respective gas component, the respective supply valve being configured to set a required line cross-section.

[0056] Alternatively or additionally, the valve can be switched between closed and open positions according to a mandated duty cycle or duty factor of 0 to 100, where the duty cycle indicates the ratio of the supply valve's closed time to its operating time, where 0 = always open, and 100 = always closed. For example, choosing 1 second as the base interval, which means that the shortest possible open or closed time is 1 second, a duty cycle of 10 means that the supply valve opens for 1 second and then closes for 10 seconds. This method, also called "chopping", results in only negligible fluctuations in the partial pressure of the respective gas component in the process atmosphere, especially due to the fact that the volume of the supply line maintains the gas flow in the manner of a buffer even when the valve is closed.

[0057] According to another embodiment, the particle beam consists of charged particles, more specifically electrons.

[0058] One advantage of electrons is that they cause very little or no damage to the surface under the beam, since they do not penetrate deeply into the material but can simply flow as an electric current. Furthermore, electron beams can be focused to a very small incident area, with a diameter in the region of 10 nm, resulting in a particularly high resolution of the etching process.

[0059] According to another embodiment, a lithography mask is embodied for use in EUV lithography.

[0060] EUV lithography masks have a fundamentally different structure than lithography masks that can be used transparently, such as lithography masks for DUV lithography (DUV: deep ultraviolet, e.g. 193 nm working light wavelength). DUV lithography masks are characterized, for example, by a transparent quartz substrate and a structured layer that is also transparent but has phase-influencing qualities, such as silicon nitride. The chemical properties of EUV lithography masks are fundamentally different from this, since the optical properties of the materials are fundamentally different at EUV wavelengths.

[0061] For example, EUV lithography masks feature a layered structure, the base of which is formed by a carrier or substrate, which can be made of, for example, fused silica or silicon. On the side that receives the beam of active light in a later operation, a Bragg mirror or multilayer mirror is arranged. The Bragg mirror or multilayer mirror is embodied specifically for the respective wavelength of active light. In this configuration, layers with high and low refractive indices based on the wavelength of active light and with a layer thickness of about half the wavelength of active light are arranged alternately with each other. The active light has, for example, a wavelength of 13.5 nm. A suitable mirror is then a multilayer mirror, which includes, for example, a number of double lamellae made of molybdenum and silicon, each with a layer thickness of 6.75 nm (for normal incidence) in the form of a Bragg mirror. The multilayer mirror can be manufactured using known deposition processes, such as chemical vapor deposition (CVD). An etch stop layer is arranged on top of the multilayer mirror. Firstly, the etch stop layer has the function of the etch stop process utilized when structuring the structured lamellae, so that the multilayer mirror is not attacked. Secondly, the etching stop layer is itself part of the multilayer mirror. Therefore, the etching stop layer has a layer thickness that is adapted to the actinic radiation. The etching stop layer is, for example, made of ruthenium or another noble metal. The structured layer on the etching stop layer is a layer that absorbs EUV radiation and thus leads to a modulation in the spatial illumination intensity of the radiation.

[0062] For EUV lithography masks, the surface uniformity requirements are particularly stringent: in particular any roughness of the reflective surface in the sub-nanometer range must be controlled, since otherwise scattering losses will be present and the lithography process will be impaired accordingly.

[0063] According to another embodiment, a lithography mask has an etch stop layer, the facing side of which carries a structured thin plate made of a material that absorbs radiation used in the lithography process, whereby the etching rate of the activated first gas component on the etch stop layer is at least 2 times, preferably 5 times, more preferably 10 times lower than the etching rate on the structured thin plate.

[0064] In particular, the structured thin plate comprises a compound of tantalum, such as, for example, tantalum nitride TaN, tantalum oxide TaO, tantalum oxynitride TaNO, tantalum boron nitride TaBN, etc. However, other materials that absorb the radiation used for exposure in the lithographic process are possible here as well. The etching stop layer comprises, in particular, a noble metal, such as, for example, ruthenium. The etching process can be controlled more effectively through the etching selectivity.

[0065] According to another embodiment, the lithographic mask has a mirror layer embodied as a multilayer mirror composed of a plurality of bilayers, where each bilayer comprises a first layer composed of a first chemical composition and a second layer composed of a second chemical composition, and where each of the first and second layers has a layer thickness in the range of 3 to 50 nm, preferably 3 to 20 nm, more preferably 5 to 10 nm, very preferably 5 to 8 nm, even more preferably 6 to 7 nm.

[0066] The chemical properties, particularly the refractive index, of the first and second chemical compositions are different with respect to the radiation used in the lithographic process.

[0067] The multilayer mirror comprises, for example, 50 to 100 bilayers, i.e. 100 to 200 individual layers. The multilayer mirror may additionally have further intermediate layers, which have the effect, for example, of reducing the diffusion of atoms from one layer into the adjacent layer in the multilayer stack. Such intermediate layers preferably have a layer thickness that is practically imperceptible from an optical point of view, for example a thickness of a few atomic layers.

[0068] Each combination of the first and second chemical compositions is preferably selected based on the refractive index contrast in part of the two chemical compositions. The thickness of each layer is preferably selected so that the optically active thickness of the layer corresponds to about half a wavelength, taking into account the angle of incidence. There may be slight deviations from this, for example to compensate for intermediate layers.

[0069] According to another embodiment, the particle beam has an energy between 1 eV and 100 keV, preferably between 3 eV and 30 keV, more preferably between 10 eV and 10 keV, very preferably between 30 eV and 3 keV, even more preferably between 100 eV and 1 keV.

[0070] The beam energy is preferably selected so that as many incident particles as possible in the beam lead to the activation of the molecules of the first gas component. For this purpose, a very reduced beam energy is advantageous. On the other hand, the charging effect of the lithography mask, which may occur as a result of the charge carriers being supplied via the particle beam, may lead to the dispersion of the particle beam and thus to a reduction in the resolution. To minimize this effect, a higher beam energy is advantageous.

[0071] For example, the particle beam consists of electrons, the electron beam having a current in the range of 1-1000 pA, preferably in the range of 1-100 pA, more preferably in the range of 10-70 pA, very preferably in the range of 20-40 pA. A higher current may lead to a higher reaction rate and thus an acceleration of the etching process, but a higher current may also lead to a higher charging of the surface.

[0072] According to a second aspect, there is proposed a lithography mask, more particularly a non-transmissive EUV lithography mask, manufactured by the method according to the first aspect.

[0073] According to a third aspect, an apparatus for particle beam induced etching of a lithography mask, more particularly a non-transparent EUV lithography mask, is proposed. The apparatus comprises a housing for providing a process atmosphere and means for focusing and emitting a particle beam at a target location on the lithography mask. Means are further provided for providing a first gas component at the target location in the process atmosphere, where the first gas component can be converted by activation into a reactive form, where the reactive form reacts with a material of the lithography mask to form a volatile compound. Means are further provided for providing a second gas component at the target location in the process atmosphere, where the second gas component comprises a compound of silicon with oxygen, nitrogen and / or carbon.

[0074] The apparatus comprises a control device configured in particular to activate the means for focusing and emitting a particle beam at the target location, to activate the means for providing a first gas component at the target location, and to activate the means for providing a second gas component at the target location, such that the first gas component and the second gas component are provided temporally before and / or simultaneously with focusing and emitting the particle beam at the target location.

[0075] The apparatus preferably operates according to the method according to the first aspect. The apparatus has the same advantages as the method described above.

[0076] The embodiments and features described for the proposed method are correspondingly valid for the proposed device and vice versa.

[0077] For example, the apparatus may include an electron column disposed within a vacuum housing configured to focus and emit an electron beam onto a sample disposed on a sample holder. The apparatus may be, for example, a modified electron microscope. The vacuum housing advantageously provides a process atmosphere, and the pressure provided may be, for example, 10 -5 ~10 -8 The pressure in the process atmosphere may be in the range of mBar. The pressure in the process atmosphere may be subject to spatial and temporal variations. The respective means for providing the first and second gaseous components in particular comprise a container or tank in which a large amount of the respective component is kept. If the respective component is stored in gas form, the means is preferably a high-pressure container which keeps the gas under a pressure of several hundred bar. Advantageously, in the container, a liquid or solid phase of the respective component is provided, the vapor pressure of the component being controlled via the temperature. In this case, the individual gas molecules evaporate or sublime from the liquid or solid phase directly into the gas phase. The respective means further comprise a supply line which terminates in a nozzle as close as possible to the target position. In this way, the respective gaseous component is supplied in a targeted manner very close to the target position on the lithographic mask. This supply line may comprise a valve and / or other process engineering devices.

[0078] The control device is configured to control the time course of a process carried out with the apparatus, such as an etching process, among others. For example, the control device controls an electron microscope and controls valves in supply lines for the first and second gas components. The control device can be technically implemented as hardware and / or software. If implemented as hardware, the control device can be embodied, for example, as a computer or microprocessor. If implemented as software, the control device can be embodied as a computer program product, as a function, as a routine, as an algorithm, as a part of a program code or as an executable object.

[0079] "A" in this instance should not be understood as necessarily being limited to exactly one element. Rather, a plurality of elements can be provided, for example, two, three or more. Any other numbers used herein should not be understood as implying that there is a strict limitation to the stated number of elements. Rather, there can be upward and downward numerical deviations unless specifically stated.

[0080] Further possible implementations of the present invention also include combinations not expressly mentioned of the features or embodiments described above or below with respect to the exemplary embodiments, in which case the skilled person will also add individual aspects as improvements or supplements to the respective basic forms of the invention.

[0081] Further advantageous configurations and aspects of the invention are the subject of the dependent claims and also of the exemplary embodiments of the invention described below. In the following text, the invention is explained in more detail on the basis of preferred embodiments with reference to the attached drawings. [Brief description of the drawings]

[0082] [Figure 1] 1A-1C show schematic cross-sections through a lithographic mask undergoing a particle beam induced processing operation; [Diagram 2] 1 is a schematic block diagram of an apparatus for particle beam induced etching of a lithography mask; [Figure 3a] Electron microscope images of a lithography mask before and after a particle beam induced etching process. [Figure 3b] Electron microscope images of a lithography mask before and after a particle beam induced etching process. [Figure 4a] FIG. 1 illustrates a known particle beam induced etching process for a lithography mask. [Figure 4b] FIG. 1 illustrates a known particle beam induced etching process for a lithography mask. [Figure 4c]FIG. 1 illustrates a known particle beam induced etching process for a lithography mask. [Figure 5a] 1A-1D show a sequence of electron microscope images of a lithography mask before and after etching by a known etching process. [Figure 5b] 1A-1D show a sequence of electron microscope images of a lithography mask before and after etching by a known etching process. [Figure 5c] 1A-1D show a sequence of electron microscope images of a lithography mask before and after etching by a known etching process. [Figure 6a] 1 illustrates damage to a substrate caused by known etching processes; [Figure 6b] 1 illustrates damage to a substrate caused by known etching processes; [Figure 6c] 1 illustrates damage to a substrate caused by known etching processes; [Figure 7a] FIG. 2 illustrates the particle beam induced etching process of the present invention for a lithography mask. [Figure 7b] FIG. 2 illustrates the particle beam induced etching process of the present invention for a lithography mask. [Figure 7c] FIG. 2 illustrates the particle beam induced etching process of the present invention for a lithography mask. [Figure 8a] FIG. 1 illustrates a lithographic mask subjected to the etching process of the present invention. [Figure 8b] FIG. 1 illustrates a lithographic mask subjected to the etching process of the present invention. [Figure 8c] FIG. 1 illustrates a lithographic mask subjected to the etching process of the present invention. [Figure 9] 1 is a schematic block diagram of a method for operating on a lithographic mask using a particle beam induced etching process. [Figure 10]2 is a schematic block diagram of another apparatus for particle beam induced etching of a lithography mask; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0083] In the drawings, identical elements or elements having identical functions are designated by the same reference numerals unless otherwise noted, and it should be understood that the figures in the drawings are not necessarily drawn to scale.

[0084] 1 shows a schematic cross section through a lithographic mask 100 undergoing a particle beam induced processing operation. This operation is more specifically a locally induced etching process in which material is ablated from the lithographic mask 100. The etching process can also be applied to foreign objects such as, for example, dust particles that have settled on the surface of the lithographic mask 100 (not shown).

[0085] In the shown example of lithography mask 100, the mask is for example a mask suitable for EUV lithography, operating on the basis of reflectivity. This means that the actinic light impinges on the lithography mask 100 and is reflected back into the same half space. Here, EUV stands for "extreme ultraviolet" and denotes an actinic light wavelength between 0.1 and 30 nm.

[0086] In this example, the lithography mask 100 has a layered structure, where the base is formed by a carrier or substrate 102, which can be made of, for example, fused quartz. On the side that is subsequently illuminated in operation with the action light, a multilayer mirror 104 is arranged. The multilayer mirror is embodied as a Bragg mirror, dedicated to the respective wavelength of the action light. In this configuration, layers are arranged alternately with each other, with high and low refractive indices depending on the wavelength of the action light, and with a layer thickness of about half the wavelength of the action light multiplied by the sine value of the angle of incidence of the action light on the lithography mask 100. The action light has, for example, a wavelength of 13.5 nm. A multilayer mirror suitable for an angle of incidence of 90° is then a mirror 104, which includes a number of double laminae of molybdenum and silicon, each with a layer thickness of 6.75 nm, as a Bragg mirror. If the light incidence has an inclination, the selected layer thickness must be smaller. The multilayer mirror 104 includes, for example, up to 100 such double laminae. The multilayer mirror 104 can be manufactured by known deposition processes, such as chemical vapor deposition (CVD). An etch stop layer 106 is arranged on top of the multilayer mirror 104. The first function of this etch stop layer 106 is to stop the etching process used in the structuring of the structured sheet 108, so that the multilayer mirror 104 or the substrate 102 are not attacked. Furthermore, the etch stop layer 106 is itself part of the multilayer mirror 104 and thus forms a first layer of the multilayer mirror 104. The etch stop layer 106 therefore has a layer thickness that is in particular adapted accordingly to the actinic light. The etch stop layer 106 consists, for example, of ruthenium or another noble metal.

[0087] This type of layer structure achieves, for example, a reflectivity of about 70% of the radiation intensity for EUV radiation. To achieve the local modulation of the illumination intensity required for lithography, a structured layer 108 is arranged on the etching stop layer 106. The structured layer 108 comprises, for example, tantalum boron nitride TaBN, tantalum nitride TaN, tantalum boron oxide TaBO and / or tantalum oxide TaO. To produce the structured layer 108, for example, a layer of TaBN is first applied over the entire area and then selectively etched. In the areas where the TaBN layer remains, the incident action light is significantly attenuated. The reflected beam bundle passes twice through the TaBN layer, so that less than about 10% of the incident intensity is reflected in the area of ​​the TaBN layer.

[0088] During the manufacture of the lithography mask 100, defects may occur (see, for example, FIG. 3). In the case of intensity-modulated lithography masks, in particular, a distinction is made between transparent and opaque defects. The result of a transparent defect is an excessively high intensity upon exposure at locations with only low or no intensity. The result of an opaque defect is the opposite, in other words, at the respective location, the intensity is absent or is excessively low compared to the desired intensity.

[0089] In this example, possible error sources are in particular errors in the structure of the multilayer mirror 104, including the etching stop layer 106, and also errors during the structuring of the structured layer 108. The latter can be repaired in a very targeted manner, since these defects are on the surface and therefore directly accessible. One suitable technique for this purpose is particle beam induced processes, since they allow targeted local action. Particles contemplated in this context include ions, electrons and photons (lasers, etc.). Particularly advantageous are electron beams, since on the one hand they can be focused on a very small target point and, on the other hand, they cause only relatively very small damage, such as structural changes to the surface receiving the beam, or no damage at all. The reasons for this include, in particular, that electrons have a relatively low penetration depth. In contrast, ions penetrate in particular deeper into the material, where they can possibly cause doping and thus structural changes of the material, with possible harmful consequences. A laser beam has the disadvantage, in comparison with an electron beam, that it cannot be focused onto a very small area and therefore has a lower spatial selectivity and therefore a lower resolution of the action process. The radiation in this example is an electron beam 110.

[0090] In this example, there is an opaque defect 112 in the form of an unremoved portion of the TaBN layer of the structured layer 108. The defect 112 is to be removed by means of a locally induced etching process. What is needed for this purpose is, firstly, an activating electron beam 110 (collectively, particle beam 110) and, secondly, a first gas component GK1 that can be converted into a reactive form by activation.

[0091] The focused electron beam 110 is scanned in particular over a target position ZP. The target position ZP has a spread, for example, in the range of 5 nm to 2 μm. At the impact point, the focused particle beam 110 preferably has a substantially Gaussian beam profile (based on intensity) with a full width at half maximum in the range of 1 to 50 nm. The focusing can advantageously be adjusted. The electron beam 110 is deflected to irradiate a point having the size of the impact point, for a mandatory dwell time in each case. Here, it is also possible to use the term "pixel". The target position ZP is divided, for example, into pixels that are successively irradiated by the electron beam 110. The dwell time lies, for example, in the range of a few hundred picoseconds to microseconds. Depending on the target position ZP and the size of the pixel, there is a defined cycle time for a complete pass. 10 6 For pixels and a dwell time of 1000 ps, ​​the cycle time is, for example, 1 ms. In the etching process, for example, millions of cycles are applied to the standard position ZP, which means that the electron beam 110 scans over the target position ZP millions of times.

[0092] The first gas component GK1, for example XeF2, is preferably supplied to the target location ZP in a targeted manner. In this case, individual XeF2 molecules can be adsorbed on the surface of the lithography mask 100. In the adsorbed state, the interaction between the adsorbed molecules and the surface atoms is relatively strong. As a result of the activation electron beam 110 and / or as a result of secondary processes triggered by the electron beam 110 at the target point ZP, in particular by secondary electrons from near-surface atoms, the molecules of the first gas component GK1 are activated. In the example of XeF2, this molecule is for example dissociated and the resulting fluorine atoms or fluorine groups react with the surface atoms of the TaBN layer and form volatile gas compounds that volatilize via the process atmosphere ATM. In this way, the material is locally ablated.

[0093] Since XeF2 is a relatively reactive substance, even without activation by the particle beam 110, there is to some extent a spontaneous reaction with the surface atoms, which can lead to uncontrolled etching. This depends largely on the combination utilized between the first gas component GK1 (etching gas) and the chemistry of the free surface. To obtain a more efficient control over the etching process, it is possible to supply various additional gases that fulfill a buffer or passivation function. Known in this context is the use of water, which has a passivation effect, in the etching process. However, a problem with water is that it may attack the etch stop layer 106, which consists, for example, of ruthenium or another noble metal. An alternative to water, which is supplied as the second gas component GK2 in this example, is tetraethylorthosilicate (Si(OC2H5)4, tetraethoxysilane, hereinafter also called TEOS for short). TEOS is a known deposition gas in particle beam induced processes, used, for example, for the local generation of a layer of silicon oxide. Firstly, TEOS has a passivating effect, whereby the spontaneous etching process does not occur substantially or not at all, and secondly, the etch stop layer 106 is not attacked. Under exposure to the electron beam 110, TEOS may result in a deposit containing silicon oxide, silicon nitride and silicon carbide, and also mixed phases of these compounds. This can contribute to the selectivity or control of the etching process. Furthermore, silicon oxide, silicon nitride and silicon carbide only cause a small attenuation of the EUV radiation, so that the thin layers that may be formed by silicon oxide, silicon nitride and silicon carbide in this case can be neglected.

[0094] In the etching process of the present invention, the first and second gas components GK1, GK2 are preferably supplied to the target location ZP in time before and / or during the emission of the electron beam 110 to the target location ZP. Thus, the composition of the process atmosphere ATM can be controlled while the electron beam 110 is being emitted to the target location ZP, thereby achieving the advantageous effects described above and below through the use of the second gas component GK2 in the etching process.

[0095] 2 shows a schematic block diagram of an apparatus 200 for particle beam induced etching of the lithography mask 100, e.g., the EUV lithography mask 100, from FIG. 1. The apparatus 200 comprises a housing 210, which is evacuated to a temperature of 100° C. by a vacuum pump 250 to generate a process atmosphere ATM within the housing 210. -2 ~10 -8 The apparatus 200 comprises a housing 210 which is evacuated to a pressure in the range of mBar. The apparatus 200 comprises means 220 arranged in the vacuum housing 210 for providing a focused particle beam 110. The means 220 comprises a beam preparation unit 222 and also one or more beam steering and / or beam shaping means 224, 225 for directing the particle beam 110 in a desired manner to a target point ZP. The device in question here is for example an electron column 220 configured to provide a focused electron beam 110. The beam steering and beam shaping elements 224, 225 are in this case embodied in particular as multipoles. Advantageously, a detector 226 is further provided which is configured to detect backscattered and / or secondary electrons and thus capture an electron microscope image of the lithography mask 100. In this way, it is possible to follow the operations acting on the lithography mask 100 in situ.

[0096] The apparatus 200 comprises a sample stage 202 for holding and positioning the lithographic mask 100 to be acted upon, which sample stage can preferably be moved in two, more preferably three, directions in space. Furthermore, the sample stage 202 can be tiltably and rotatably mounted (not shown) in order to align the lithographic mask 100 with the greatest possible precision relative to the means 220, and more particularly relative to the particle beam 110. The sample stage 202 is advantageously mounted in a vibration damped manner and is mechanically isolated from the rest of the structure (not shown).

[0097] Outside the housing 210, means 230 for providing a first gas component GK1 and means 240 for providing a second gas component GK2 are arranged. The embodiment of the respective means 230, 240 is preferably adapted to control the temperature of the solid or liquid phase of the respective gas component GK1, GK2 in order to set the vapor pressure of the respective gas component GK1, GK2. In this way, it is advantageously possible to achieve a gas flow of the respective gas component GK1, GK2 optimized for the respective process without the use of valves or the like. However, this does not exclude the additional provision of valves or the like, since the valves advantageously allow a very fast change of the gas flow. Each of the means 230, 240 has a supply line 232, 242 into the housing 210 opening into a respective nozzle. The nozzle is advantageously directed towards a target point ZP, whereby the gas GK1, GK2 supplied comes into contact in a targeted manner with the surface of the lithographic mask 100. This increases the process control and the efficiency of the etching process. The means 230, 240 may be further provided with further means (not shown) embodied in a similar manner for supplying further gas components, such as a buffer gas, an oxidizing or reducing gas, into the process atmosphere ATM.

[0098] Also shown is a suction recovery unit 260 configured to draw off excess gas, and also in particular volatile reaction products, under suction from the region of the target point ZP, for example by means of a further vacuum pump 250. This allows the composition of the process atmosphere ATM to be controlled more effectively, in particular to prevent precipitation of reactive products elsewhere on the lithographic mask 100 or other unknown processes caused by the excess gas.

[0099] 3a and 3b show electron microscope images of a lithography mask 100 before and after a particle beam induced etching process. The example shown here has a parallel structure, but this is merely an example and should not be construed as limiting in any way. Other lithography masks can have a variety of other geometric shapes. The lithography mask 100 shown is in particular an EUV lithography mask having a layer structure as shown in FIG. 1, for example.

[0100] Fig. 3a shows a lithography mask 100 with a defect in the form of an absorbing area, which is not intended in this respect. The box with the white dashed line serves to highlight the defective area. The EUV lithography mask 100 is subjected to, for example, the proposed particle beam induced etching process using the apparatus 200 of Fig. 2, and the designated target positions ZP (see Fig. 1) are areas of the lithography mask 100 from which material is to be removed.

[0101] 3b shows the EUV lithography mask 100 after an etching process has been performed. It is clear that the defects have been successfully removed and the lines on the lithography mask 100 are now all separate from each other. The white boxes serve to highlight the repaired sites. The lithography mask 100 now has the intended structure and can be used, for example, in an EUV lithography process.

[0102] 4a-4c show a schematic representation of a known particle beam induced etching process for a lithography mask 100. With the known process, there are undesirable side effects, as will be elucidated below. FIG. 4a shows an initial situation in which the lithography mask 100 is arranged in a process atmosphere ATM1. A structured layer 108, which is essentially made of a first material 108a, for example tantalum nitride TaN, is being etched. The surface of the layer 108 is made of a different material 108b, which for example comprises tantalum oxide TaO and / or tantalum oxynitride TaON. A near-surface layer 108b of this kind can form spontaneously by itself, in which case the layer 108b has a thickness of a few nanometers, or a near-surface layer 108b of this kind can be deposited in a targeted manner, in which case for example the layer thickness can be set arbitrarily. The lithography mask 100 can have further layers as shown in FIG. 1, which are not shown here for the sake of clarity. The etching process is carried out, for example, by the apparatus 200 of FIG. 2.

[0103] The process in Figures 4a-4c is carried out using a process atmosphere ATM1, which comprises, for example, XeF2 as etching gas and H2O as passivation gas. The intention is to remove a defect 112, for example as shown in Figure 3a, where the defect 112 is bounded by a dashed line. The target position ZP is accordingly located within the area of ​​the defect 112.

[0104] As shown in Fig. 4b, the etching process is performed in a targeted manner by the particle beam 110, and the layer 108 at the target location ZP is removed down to the substrate 101. The target location ZP is for example divided into pixels, one pixel corresponding to the area of ​​impact of the focused particle beam 110 on the layer 108, and the particle beam 110 scans pixel by pixel over the target location. In each cycle, several layers of atoms of the layer 108 are ablated, where first the outer layer 108b and then the inner layer 108a are exposed in the cross section.

[0105] During the etching process, there may be undesirable cases of damage DMG1, DMG2. For example, the substrate 101 of the lithography mask 100 may be damaged as represented by the rough surface DMG1. Since the etching procedure does not always take place at exactly the same speed in all pixels of the target position ZP, situations arise where the substrate 101 is already exposed in certain pixels, while elsewhere there remains material to be ablated. The etching process is therefore continued, which may result in cases of damage DMG1 in areas where the substrate 101 is already open, as a result of the particle beam 110, and also by aggressive etching gases in a particularly activated form and / or by water present as a passivating gas in the process atmosphere ATM1.

[0106] Furthermore, there may be further instances of damage DMG2 at the edges of the target location ZP where the sidewalls of layer 108 become exposed as the etching procedure progresses. An example of this is an etching process that attacks the exposed sidewalls of layer 108, potentially resulting in degradation of the sidewalls.

[0107] After the end of this etching process at the indicated target location ZP, an etching process is performed, for example, at another location of the lithography mask 100 (not shown). During this procedure, the gas in the process atmosphere ATM1 remains in direct contact with the exposed layer 108a. In this scenario, there may be spontaneous reactions in which the exposed material 108a is attacked. As a result, an undesirable etching process may occur, which may lead to further damage DMG3 in the form of under-etching of the superficial layer 108b, as shown in FIG. 4c. This process, proceeding without control, may therefore be an obstacle to a targeted etching process. Damage DMG3 occurs, for example, when the material 108a is heavily attacked, while the near-surface layer 108b is not attacked or is only slightly attacked by the first gas component GK1.

[0108] Figures 5a-5c show a sequence of electron microscope images of a lithography mask 100 before (Figure 5a) and after (Figures 5b and 5c) particle beam induced etching using the etching process described with reference to Figures 4a-4c. The lithography mask 100 has a structure such as that shown in Figure 1, for example.

[0109] The substrate 106 and the structured layer 108 are clearly visible in the electron microscope image. Figure 5a shows a target location ZP in the form of a dashed box. In this case, the target location ZP is located on the substrate 106. As explained with reference to Figure 1, a focused particle beam 110 is scanned over the target location ZP (see Figure 1 or Figure 2).

[0110] FIG. 5b shows the affected area after the etching process. The image was captured with an electron beam energy of 600 V. With this energy it is possible to capture in particular topological structures. In the areas subjected to the particle beam 110, a slight discoloration is perceptible, indicating that in this area the substrate surface has been damaged. The damaged area is highlighted by the dashed lines DMG1. Furthermore, a comparison of the edges of layer 108 with FIG. 5a shows that these edges also exhibit damage DMG2 and are no longer very sharply defined.

[0111] Fig. 5c shows a further image of the affected area, captured at a higher electron beam energy, making the material contrast particularly visible. The dark spots DMG1 indicate that the etch stop layer 106 has been completely etched away at these sites. Also, it is not possible to exclude deeper damage at these sites, e.g. to the multilayer mirror 104 (see Fig. 1).

[0112] The illustrated damage cases DMG1, DMG2 can lead, for example, to a reduction in the reflection of EUV radiation in the lithography process, resulting in errors in the production of microstructured components. At the worn edges, additional radiation is scattered, which can likewise impair the exposure process.

[0113] 6a-6c show further damage caused by a known etching process to an etch stop layer 106 on an EUV lithography mask 100 having the same structure as the lithography mask shown in Fig. 1, for example. In this case, for example, the etching process used involved the supply of XeF2 as the etching gas, H2O as the passivation gas, and NO2 as the buffer gas. The etching process was used to remove columns of tantalum boron nitride TaBN located in the region of the target location ZP.

[0114] FIG. 6a shows an electron microscope image of the acted area of ​​the lithography mask 100. A distinct illumination can be seen in the area of ​​the target position ZP, suggesting damage DMG1. Four position markers DC are also clearly visible. For clarity, only one is labeled with a reference number. The purpose of the position markers DC is to visualize and compensate for the relative shift between the lithography mask 100 and the means 220 (see FIG. 2) to provide a focused particle beam 110 (see FIG. 1 or FIG. 2) during the beam-emitting process. In this case, the position markers DC are periodically scanned during the etching process, and for this reason, illuminated and damaged areas can also be seen around them.

[0115] FIG. 6b shows an image of the lithographic mask 100 captured with actinic radiation. FIG. 6b shows, for example, a two-dimensional intensity distribution of reflected radiation occurring on a sample in a lithographic process using the lithographic mask 100. The difference in luminosity corresponds to the difference in intensity. The reflected intensity is about 70% in the area of ​​the etch stop layer 106 and less than 10% in the area of ​​the structured layer 108. The damaged area DMG1 can be considered to be brightened as well. A region of interest ROI is shown passing through the damaged area DMG1. In FIG. 6c, the intensity values ​​of the region of interest ROI are plotted as a function of position, with markers ("z" and "0") coinciding with FIG. 6b.

[0116] The drawing in Fig. 6c shows the reflected intensity R of EUV radiation in the region of interest ROI as a function of position. The positions "z" and "0" correspond to Fig. 6b. The vertical axis shows the intensity I, which is for example normalized to the maximum value. The measurements show that at position "z" there is a minimum of the reflected intensity. This indicates that damage to the etch stop layer 106 leads to a decrease in the reflectivity of EUV radiation and thus to a degradation of the lithographic process.

[0117] Figures 7a-7c show an etching process, similar to Figures 4a-4c, but now carried out in accordance with the present invention, as a result of which the undesirable or uncontrolled side effects elucidated with reference to Figures 4a-4c are substantially suppressed.

[0118] In the example of Fig. 7a-7c, the process atmosphere ATM contains, for example, XeF2 as etching gas and TEOS as additional gas. The etching process proceeds in a targeted manner as in the example of Fig. 4b and as shown in Fig. 7b. In contrast to Fig. 4b, however, the presence of TEOS in the process atmosphere ATM leads to the formation of a passivation layer 109, which essentially consists, for example, of silicon oxide or silicon dioxide. This passivation layer 109 can be generated, for example, by deposition of the second gas component GK2 from the process atmosphere ATM and / or by chemical reaction of molecules of the second gas component GK2 with the exposed material 108a. The passivation layer 109 has the advantageous effect that the exposed surfaces of the substrate 101 and also of the layer 108a are sealed or passivated, so that no or only little damage of the kind described with reference to Fig. 3b occurs. It can be noted that the layer 109 can also be ablated by the activated etching process. Advantageously, therefore, high layer thicknesses of the layer 109 are not formed. The process is controlled by the control of the gas supply, which determines in particular the composition of the process atmosphere ATM in the region of the target position ZP.

[0119] The passivation layer 109 therefore has the advantage that damage to the substrate 101 is reduced or completely prevented. Furthermore, spontaneous etching reactions, which may also limit the quality of the lithographic mask 100, are prevented. Thus, a very targeted and clean etch is possible.

[0120] In particular, it may be the case that no integrated layer 109 is formed, but instead only atoms of the second gas component GK2 are deposited on the surface ablated by the etching process from the process atmosphere ATM and / or react with atoms from the surface layer, thus avoiding the formation of a layer.

[0121] 8a-8c show a lithography mask 100 subjected to an etching process of the invention. The lithography mask 100 has the layer structure elucidated with reference to FIG. 1. On the upper side, a partially structured layer 108 and partially an etch stop layer 106 are visible. The lithography mask 100 was subjected to an etching process in which the first gas component GK1 (see FIG. 1 or FIG. 2) supplied was XeF2 and the second gas component (see FIG. 1 or FIG. 2) supplied was TEOS. No further additional gases were used. The gas flow was controlled via the temperature of the respective liquid or solid phase of the components, XeF2 being held in this example at a temperature of −20° C. and TEOS at a temperature of −33° C. To activate the first gas component GK1, a focused electron beam 110 (see FIG. 2) was used. The etching process was carried out on two adjacent rectangular target positions ZP on the exposed etch stop layer 106.

[0122] 8a shows an electron microscope image of an affected area of ​​the lithography mask 100 captured with an electron energy of 600V, which means that the surface structure is readily apparent. In the area of ​​the two target positions ZP, very little lightening is perceptible, suggesting little modification to the surface structure, e.g. surface roughness.

[0123] Figure 8b shows an electron microscope image of an affected area of ​​the lithography mask 100 that was captured using a higher electron energy, resulting in sharp contrast of the materials. In this image, it becomes clear if a deposit formed on the etch stop layer 106, or if the etch stop layer 106 was etched away, as seen in Figure 5c. Figure 8b shows that essentially no deposit formed, and also that the etch stop layer 106 was not substantially attacked during the etching process.

[0124] 8c shows an image of the lithographic mask 100 acquired with actinic radiation, showing the reflection intensity, which is about 70% in the area of ​​the etch stop layer 106 and less than 10% in the area of ​​the structured layer 108. In the area of ​​the target position ZP, only very slight deviations can be seen compared to the remaining unirradiated surface of the etch stop layer 106.

[0125] In this case, the etch stop layer 106 is not damaged, as compared to conventional processes which lead to damage (see Figures 5a-5c and 6a-6c).

[0126] Figure 9 shows a schematic block diagram of a method for operating on a lithography mask 100 (see Figures 1 to 8) using a particle beam induced etching process. In a first step S1, the lithography mask 100 is provided in a process atmosphere ATM (see Figures 1, 2 and 7). For example, the lithography mask 100 is placed on a sample stage 202 of an apparatus 200, and a housing 210 is placed at 10 -6 -10 -8The atmosphere is evacuated to a pressure of 10 ... Under certain process conditions, the second gas component GK2 forms a deposit comprising compounds of silicon with oxygen, nitrogen and / or carbon upon exposure to the particle beam 110. The process conditions in the etching process are preferably selected such that no or only very little deposit is formed.

[0127] In the method, the third step S3 and the fourth step S4 are in particular carried out in time prior to and / or simultaneously with the second step S2.

[0128] Fig. 10 shows a schematic block diagram of another embodiment of an apparatus 200 for particle beam induced etching of a lithographic mask 100. The apparatus 200 of Fig. 10 has all the features of the apparatus 200 elucidated with reference to Fig. 2, and for this reason these features will not be elucidated again here. The apparatus 200 operates in particular according to the method elucidated with reference to Fig. 9.

[0129] In addition, the apparatus 200 in Fig. 10 has a control device 270. The control device 270 is embodied, for example, as a part of a control computer for controlling the apparatus 200. The control device 270 is configured to operate the means 220 for focusing and emitting the particle beam 110 at the target position ZP, to operate the means 230 for providing the first gas component GK1 at the target position ZP, and to operate the means 240 for providing the second gas component GK2 at the target position ZP. In this arrangement, the control device 270 operates the means 230 and the means 240 such that the first gas component GK1 and the second gas component GK2 are provided before and / or simultaneously with the focusing and emitting of the particle beam 110 at the target position ZP in time.

[0130] The notion of a control device 270 actuating the respective means is understood to mean, for example, that the control device 270 transmits control commands to the respective means, more specifically to the controller of the respective means, which control commands include the intended settings of the respective means at the respective point in time in the method. The control commands can be transmitted by wire or else wirelessly, for example via an optical transmission section.

[0131] Although the present invention has been described based on exemplary embodiments, it can be modified in various ways. [Explanation of symbols]

[0132] 100 Lithography Mask 101 Substrate 102 Substrate 104 Multilayer Mirror 106 Etch stop layer 108 Structured layer 108a layer 108b layer 109 layers 110 Particle Beam 112 Defects 200 equipment 202 Sample stage 210 Housing 220 means 222 Beam Preparation Unit 224 Beam Guidance Means 225 Beam Shaping Means 226 Detector 230 means 240 means 250 Vacuum Pump 260 Suction Recovery Unit 270 Control Device ATM process atmosphere ATM1 Process atmosphere DC Position Marker DMG1 damage DMG2 damage DMG3 damage GK1 Gas Components GK2 Gas Components I strength POS position R reflection intensity ROI Region of Interest S1 Method Steps S2 Method Steps S3 Method Steps S4 Method Steps z position ZP target point

Claims

1. A method for particle beam induced etching of a lithographic mask (100), comprising: a) providing (S1) said lithography mask (100) in a process atmosphere (ATM); b) emitting (S2) a focused particle beam (110) onto a target location (ZP) on said lithographic mask (100); c) supplying (S3) at least one first gas component (GK1) to said target location (ZP) in said process atmosphere (ATM), said first gas component (GK1) being convertible by activation into a reactive form, said reactive form reacting with a material of said lithography mask (100) to form a volatile compound; d) supplying (S4) at least one second gas component (GK2) to said target location (ZP) in said process atmosphere (ATM), wherein said second gas component (GK2) comprises a compound of silicon with oxygen, nitrogen and / or carbon; wherein steps c) and d) are carried out temporally prior to and / or simultaneously with step b).

2. 2. The method according to claim 1, wherein the second gas component (GK2) comprises a silicate, a silane, a siloxane, a silazane and / or a silicon isocyanate.

3. 3. The method according to claim 1 or 2, wherein under predetermined process conditions involving exposure to the particle beam (110), the second gas component (GK2) forms a deposit comprising compounds of silicon with oxygen, nitrogen and / or carbon.

4. 4. The method of claim 3, wherein deposits formed by the second gas component (GK2) during the etching process are removed in a step of wet chemical cleaning of the lithography mask (100).

5. The first gas component (GK1) is xenon difluoride XeF 2 , sulfur hexafluoride SF 6 , sulfur tetrafluoride SF 4 , nitrogen trifluoride NF 3 , phosphorus trifluoride PF 3 , tungsten hexafluoride WF 6 , tungsten hexachloride WCl 6 , Molybdenum hexafluoride (MoF 6 , Hydrogen fluoride HF, Nitrogen oxygen fluoride NOF, Triphosphorus hexafluoride Trinitrogen P 3 N 3 F 6 The method according to any one of claims 1 to 4, comprising one of the following:

6. The method according to any one of the preceding claims, wherein the supply of the second gas component (GK2) is performed in time prior to the emission of the particle beam (110) to the target position (ZP).

7. The method according to any one of the preceding claims, wherein the supply of the second gas component (GK2) is performed during projection of the particle beam (110) to the target position (ZP).

8. A method according to any one of claims 1 to 7, comprising supplying a third gas component comprising an oxidant and / or a reductant.

9. The supplying of the first gas component (GK1), the second gas component (GK2) and / or the third gas component comprises: Providing a solid or liquid phase of each of said components; setting the temperature of the solid or liquid phase of the respective component to achieve a required vapor pressure of the respective component across the solid or liquid phase; Feed each of said gas components (GK1, GK2) into said process atmosphere (ATM) via respective feed lines (232, 242); The method according to any one of claims 1 to 8, comprising:

10. 10. The method of claim 9, wherein the mass flow rate and / or the volume flow rate of each component is controlled by setting a line cross-sectional area of ​​each supply line (232, 242) and / or controlling a duty cycle of a closing valve.

11. The method according to any one of claims 1 to 10, wherein the particle beam (110) consists of charged particles.

12. The method of any one of claims 1 to 11, wherein the lithographic mask (100) is embodied for use in EUV lithography.

13. 13. The method according to claim 1, wherein the lithography mask (100) has an etching stop layer (106) whose front side carries a structured thin plate (108) made of a material that is an absorber of radiation used in the lithography process, and wherein the etching rate of the activated first gas component (GK1) on the etching stop layer (106) is at least 2 and / or 5 and / or 10 times lower than the etching rate on the structured thin plate (108).

14. 14. The method according to claim 12 or 13, wherein the lithographic mask (100) has a mirror layer embodied as a multilayer mirror (104) composed of a plurality of bilayers, each bilayer comprising a first layer composed of a first chemical composition and a second layer composed of a second chemical composition, and wherein a layer thickness of each of the first and second layers is in the range of 3 to 50 nm, and / or 3 to 20 nm, and / or 5 to 10 nm, and / or 5 to 8 nm.

15. The method according to any one of the preceding claims, wherein the particle beam (110) has an energy between 1 eV and 100 keV, and / or between 3 eV and 30 keV, and / or between 10 eV and 10 keV, and / or between 30 eV and 3 keV, and / or between 100 eV and 1 keV.

16. An apparatus (200) for particle beam induced etching of a lithography mask (100), comprising: a housing (210) for providing a process atmosphere (ATM); a means (220) for focusing and directing a particle beam (110) at a target location (ZP) on said lithographic mask (100); a means (230) for providing a first gas component (GK1) at the target location (ZP) in the process atmosphere (ATM), where the first gas component (GK1) can be converted by activation into a reactive form, where the reactive form reacts with a material of the lithography mask (100) to form a volatile compound; Means (240) for providing a second gas component (GK2) at said target location (ZP) in said process atmosphere (ATM), wherein said second gas component (GK2) comprises a compound of silicon with oxygen, nitrogen and / or carbon; a control device (270) configured to activate a means (220) for focusing and emitting a particle beam (110) at a target location (ZP), to activate a means (230) for providing a first gas component (GK1) at said target location (ZP), and to activate a means (240) for providing a second gas component (GK2) at said target location (ZP), such that said first gas component (GK1) and said second gas component (GK2) are provided temporally before and / or simultaneously with focusing and emitting the particle beam (110) at said target location (ZP); An apparatus having the above configuration.

Citation Information

Patent Citations

  • Method and apparatus for protecting substrate during processing using particle beam

    JP2014174552A

  • Method for manufacturing reflective type mask and reflective type mask

    JP2015125166A

  • Apparatus and method for repairing a photolithographic mask

    US20200249564A1