Inkjet inks suitable for printing on non-porous substrates
Inkjet inks with terpene resin, methyl ethyl ketone, and polyether-modified silicone address solvent loss and adhesion issues, ensuring extended decap times and rapid drying with high image clarity on non-porous substrates.
Patent Information
- Application Number
- JP2023524326
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-21
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-10-21
AI Technical Summary
Thermal inkjet printing faces challenges with poor reliability due to solvent loss leading to printhead clogging, short decap times, and poor adhesion and image clarity on non-porous substrates like polypropylene, PET, nylon, and aluminum, requiring a balance between extended decap times and rapid drying times.
Inkjet inks comprising terpene resin, methyl ethyl ketone, and polyether-modified silicone with a hydrophilic-lipophilic balance (HLB) of 1 to 12, optionally with acetone and glycol ether, providing a solvent system that maintains extended decap times, rapid drying, and high image clarity on non-porous substrates.
The inkjet inks achieve extended decap times of up to 60 minutes, rapid drying within 30 seconds, and high image clarity on non-porous substrates without spreading, overcoming the limitations of traditional thermal inkjet inks.
Smart Images

Figure 0007579445000011 
Figure 0007579445000012 
Figure 0007579445000013
Abstract
Description
[Technical field]
[0001] The present invention relates to an inkjet ink, specifically to an inkjet ink comprising (A) a terpene resin, (B) a solvent system comprising (B1) methyl ethyl ketone, and (C) a polyether-modified silicone having a hydrophilic-lipophilic balance (HLB) value of 1 to 12. [Background technology]
[0002] The "Background" discussion provided herein is intended to generally present the context of the present disclosure. The inventors' work to the extent described in this Background section, and aspects of the description that may not be considered prior art at the time of filing, are not admitted explicitly or implicitly as prior art to the present invention.
[0003] Thermal inkjet (TIJ) printing is a desirable technology for printing, coding, and marking because it offers higher print resolution at a lower cost than competing technologies in the field, such as continuous inkjet methods. In the thermal inkjet printing process, the print cartridge contains a series of small chambers, each containing a heater, which generate ink droplets from the thermal evaporation of the ink solvent. In the jetting process, a resistor is rapidly heated to generate a vapor bubble (hence the term "bubble jet"), which subsequently expels a droplet from an orifice. The process is extremely efficient and repeatable, and the latest TIJ printheads for industrial graphics applications are capable of producing uniform droplets of 4 pL or less in volume at frequencies of 36 kHz or greater.
[0004] However, thermal inkjet printing can suffer from unreliability over time. For example, some inkjet inks suffer from short decap times, where solvent loss due to prolonged exposure to air in an uncapped printhead leads to clogging / plugging of the printhead nozzles, thus resulting in unreliable ink jetting and erosion of image quality over time. On the other hand, using special solvent systems with high boiling point components to prevent such premature solvent loss in an uncapped printhead situation requires extended drying times after the ink is applied, thus resulting in an overall inefficient printing process. As such, it is often difficult to balance the need for long decap times (the need for slow solvent loss rates) with the need for short drying times (the need for fast solvent loss rates).
[0005] Furthermore, as printing systems are increasingly integrated into more diverse production environments, there is a growing demand for greater versatility in thermal inkjet inks. For example, thermal inkjet printers typically print very well on porous / absorbent substrates, but adhesion to more "difficult" non-porous substrates such as those common to labels, plastic bottles, metal cans, food packaging, and blister packaging (e.g., varnished paper, biaxially oriented polypropylene (BOPP), polyethylene terephthalate (PET), nylon, and aluminum) is problematic. In an attempt to improve adhesion, several inkjet ink systems have been reported that utilize binder resins. For example, U.S. Patent No. 6,233,633 (incorporated herein in its entirety by reference) reports the use of binder resins such as cellulose ester resins, sulfonamide modified epoxy resins, rosin ester resins, terpene phenolic resins, polyurethanes, and acrylic resins to improve adhesion, and U.S. Patent No. 6,233,633 and U.S. Patent No. 6,233,633 (each of which is incorporated herein in its entirety by reference) report the use of terpene phenolic resins.
[0006] Even if adhesion to "difficult" substrates can be addressed, such non-porous substrates pose a challenge for thermal inkjet applications because the volatile solvents in thermal inkjet inks give the inks low surface energy, so that applied inkjet ink droplets tend to blend or bleed into each other on non-porous surfaces, resulting in poor image definition. Particularly for coding and marking applications, which involve printing of essential information such as personal information, production lots, and expiration dates, poor image definition is unacceptable for these applications. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] US Patent Application Publication No. 2018 / 0251650 [Patent Document 2] US Patent Application Publication No. 2017 / 0037269 [Patent Document 3] US Patent Application Publication No. 2015 / 0291816 Summary of the Invention [Problem to be solved by the invention]
[0008] In view of the foregoing, there is a need for an inkjet ink that has an extended decap time, dries quickly once applied, and produces images with desirable clarity.
[0009] Therefore, one object of the present invention is to provide novel ink-jet inks that meet these criteria.
[0010] Another object of the present disclosure is to provide novel printed articles that include the dried form of the ink-jet ink.
[0011] It is another object of the present disclosure to provide a novel method for forming a printed image on a substrate by applying and drying an inkjet ink onto the substrate. [Means for solving the problem]
[0012] These and other objects, as will become apparent from the detailed description below, have been achieved by the inventors' discovery that a combination of a terpene resin, methyl ethyl ketone (MEK) and a polyether modified silicone having an HLB value of 1-12 unexpectedly provides an inkjet ink that is characterized by extended decap times, short dry times, and high image sharpness even when printed on "difficult" non-porous substrates.
[0013] Thus, the present invention provides the following: (1) An inkjet ink comprising: (A) a terpene resin; (B) a solvent system comprising (B1) methyl ethyl ketone; and (C) a polyether modified silicone having a hydrophilic-lipophilic balance (HLB) value of 1-12. (2) The ink-jet ink according to (1), wherein the terpene resin (A) is a homopolymer produced from α-pinene. (3) The ink-jet ink according to (1) or (2), wherein the terpene resin (A) is present in an amount of 0.1 to 10% by weight based on the total weight of the ink-jet ink. (4) The ink-jet ink according to any one of (1) to (3), wherein the weight ratio of the methyl ethyl ketone (B1) to the terpene resin (A) ((B1):(A)) is 10:1 to 100:1. (5) The ink-jet ink according to any one of (1) to (4), wherein the solvent system (B) further contains (B2) acetone. (6) The ink-jet ink according to (5), wherein the weight ratio of the methyl ethyl ketone (B1) to the acetone (B2) ((B1):(B2)) is 1:1 to 5:1. (7) The ink-jet ink according to any one of (1) to (6), having a total ketone content of at least 50% by weight, based on the total weight of the ink-jet ink. (8) The ink-jet ink according to any one of (1) to (7), wherein the solvent system (B) further comprises (B3) a glycol ether. (9) The ink-jet ink according to any one of (1) to (8), which is substantially free of a solvent having a boiling point higher than 175° C. (10) The ink-jet ink according to any one of (1) to (9), wherein the polyether-modified silicone (C) is a block copolymer having a pendant graft structure. (11) The ink-jet ink according to any one of (1) to (10), wherein the polyether-modified silicone (C) has an HLB value of 3 to 10. (12) The ink-jet ink according to any one of (1) to (11), wherein the polyether-modified silicone (C) is present in an amount of 0.001 to 4% by weight based on the total weight of the ink-jet ink. (13) The ink-jet ink according to any one of (1) to (12), further comprising (D) a rosin resin. (14) The ink-jet ink according to (13), wherein the rosin resin (D) is a hydrogenated acidic rosin. (15) The ink-jet ink according to (13) or (14), wherein the rosin resin (D) is present in an amount of up to 10% by weight, based on the total weight of the ink-jet ink. (16) The ink-jet ink according to any one of (1) to (15), further comprising (E) a colorant. (17) A printed matter comprising a substrate and the ink-jet ink according to any one of (1) to (16) in a dried form disposed on the substrate. (18) A method for forming a printed image on a substrate, the method comprising: applying the inkjet ink according to any one of (1) to (16) onto the substrate using a thermal inkjet printhead; and drying the inkjet ink. (19) The method according to (18), wherein the ink-jet ink is dried by leaving it exposed to air for 30 seconds or less. (20) The method according to (18) or (19), wherein a heater is not used to dry the ink-jet ink.
[0014] The preceding paragraphs have been provided by way of a general introduction and are not intended to limit the scope of the following claims. The described embodiments, together with further advantages, will be best understood by reference to the following detailed description when considered in conjunction with the accompanying drawings, in which: [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 shows a test comparison of decap and dry times between (top) a typical ink containing a low boiling point component that dries quickly but suffers from poor decap behavior, (middle) a typical ink containing a high boiling point component that has good decap behavior but dries slowly, and (bottom) an ink according to the present invention that combines good decap behavior and fast drying properties. [Diagram 2] FIG. 13 illustrates the decap time evaluation criteria for a “good” rating (no missing / unclear lines in the thin line image), an “acceptable” rating (one or two missing / unclear lines in the thin line image), and a “poor” rating (more than two missing / unclear lines in the thin line image). [Diagram 3] FIG. 1 shows the evaluation criteria for image clarity for both fine line images and number strings printed on aluminum foil, with a "G" rating (clear image, good separation), an "A" rating (a little spread out, but the lines can be recognized, moderate separation), and an "NG" rating (too spread out, the lines cannot be recognized, insufficient separation). [Figure 4]FIG. 1 shows image clarity evaluation criteria for number row images printed on plain (uncoated) paper, varnished paper, biaxially oriented polypropylene, nylon, and aluminum foil, and a comparison of a typical ink that received an image clarity rating of "poor," Ink-A that received an image clarity rating of "acceptable," and Ink-B that received an image clarity rating of "good." DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In the following description, it is to be understood that other embodiments may be utilized and structural and operational changes may be made without departing from the scope of the present embodiments disclosed herein.
[0017] The phrase "substantially free," unless otherwise specified, means that the amount of a particular component in the inkjet ink is less than 1 wt. %, preferably less than 0.5 wt. %, more preferably less than 0.1 wt. %, even more preferably less than 0.05 wt. %, and even more preferably 0 wt. %, based on the total weight of the inkjet ink.
[0018] As used herein, the term "optional" or "optionally" means that the subsequently described event(s) may or may not occur, or that the subsequently described ingredient(s) may or may not be present (e.g., 0 wt %).
[0019] The term "alkyl," as used herein, unless otherwise specified, refers to a straight-chain, branched or cyclic aliphatic fragment having at least 1, preferably at least 2, preferably at least 3, preferably at least 4 carbon atoms, and up to 22, preferably up to 20, preferably up to 18, preferably up to 12, preferably up to 8 carbon atoms. Examples of alkyl groups include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, t-butyl, pentyl, isopentyl, neopentyl, hexyl, isohexyl, 3-methylpentyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, lauryl, myristyl, cetyl, stearyl, and the like, including, but not limited to, Guerbet-type alkyl groups (e.g., 2-methylpentyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, 2-pentylnonyl, 2-hexyldecyl, 2-heptylundecyl, 2-octyldodecyl, 2-nonyltridecyl, 2-decyltetradecyl, and 2-undecylpentadecyl). Cycloalkyl is a type of cyclized alkyl group. Exemplary cycloalkyl groups include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, norbornyl, and adamantyl.
[0020] As used herein, the term "fatty" refers to compounds that have a long-chain (straight-chain) hydrophobic moiety composed of hydrogen and generally from 8 to 22 carbon atoms, and may be fully saturated or partially unsaturated.
[0021] As used herein, the term "aryl" refers to aromatic groups containing only carbon in the aromatic ring(s), for example, phenyl, biphenyl, naphthyl, anthracenyl, and the like.
[0022] The term "arylalkyl," as used herein, refers to a straight-chained, branched, or cyclic alkyl moiety (as defined above) substituted by an aryl group (as defined above), which itself may be optionally substituted by an alkyl group, examples of which include, but are not limited to, benzyl, phenethyl, 3-phenylpropyl, 2-phenylpropyl, 1-phenylpropyl, 4-phenylbutyl, 3-phenylbutyl, 2-phenylbutyl, 2-methylbenzyl, 3-methylbenzyl, 4-methylbenzyl, 2,4-dimethylbenzyl, 2-(4-ethylphenyl)ethyl, 3-(3-propylphenyl)propyl, and the like.
[0023] The term "(meth)acrylate" is used herein to refer to both acrylate and methacrylate groups. In other words, the term should be read with the "meth" being optional. Furthermore, the term "(meth)acrylate" is used generally to refer to both acrylic acid-based compounds and acrylic ester-based compounds.
[0024] The term "decap behavior" herein refers to the ability of an inkjet ink to easily eject from a printhead when exposed to air for an extended period of time. The "decap time" of an inkjet ink is measured as the amount of time an inkjet printhead can be left uncapped before the printer's nozzles fail to fire properly, potentially due to clogging or plugging upon restarting printing. In general, a nozzle(s) can become clogged (i.e., impeded, slowed down) or clogged (i.e., blocked, substantially or completely closed) by viscous plugs that form in the nozzle(s) as a result of solvent loss, ink scabbing, and / or kogation of various ink components in and / or around the nozzle. When a nozzle is clogged, ink droplets ejected through the nozzle orifice can be misdirected, adversely affecting print quality. When an orifice is clogged, it is substantially or completely blocked. As a result of a clogged nozzle, ink droplets may not be able to pass through the affected nozzle. Thus, the criterion for measuring failure to fire by a nozzle is whether the ink through the nozzle orifice is misdirected in any way, or is completely clogged, which can be measured by visually inspecting the printed image.
[0025] Inkjet ink The present disclosure is directed to inkjet inks that have suitable physical and chemical stability at both ambient and printhead operating temperatures, jet reliably, provide high image clarity, and have extended decap times while still drying quickly after application onto a substrate (e.g., drying times of 30 seconds or less).The combination of components disclosed herein has also been surprisingly found to provide a balance between fast drying times and extended decap times while providing sharp images on non-porous substrates (e.g., films and foils).
[0026] Ink-jet inks of the present disclosure generally include the following components: (A) a terpene resin, (B) a solvent system including (B1) methyl ethyl ketone, and (C) a polyether modified silicone having an HLB value of 1 to 12. Ink-jet inks of the present disclosure may also optionally include one or more of (B2) acetone as part of the solvent system (B), (B3) a glycol ether as part of the solvent system (B), (D) a rosin resin, (E) a colorant, and (F) additives.
[0027] (A) Terpene resin The terpene resin (A) of the present disclosure refers to an oligomer or polymer having at least 95% by weight, preferably at least 96% by weight, more preferably at least 97% by weight, more preferably at least 98% by weight, more preferably at least 99% by weight, even more preferably at least 99.5% by weight, and even more preferably 100% by weight of constitutional units derived from a polymerizable terpene(s) based on all constitutional units (100% by weight) of the terpene resin (A). A terpene is an oligomer or polymer having a basic skeleton (C 5 H 8 ) p where p is a positive integer indicating the number of consecutive head-to-tail linked isoprene units. For example, hemiterpenes (p=1) have the formula: 5 H 8 The monoterpene (p=2) has a C 10 H 16 The sesquiterpene (p=3) has a C 15 H 24 For example, it has a skeleton.
[0028] In some embodiments, the terpene resin (A) is based on monoterpene monomer units. The monoterpene may be a linear monoterpene (e.g., myrcene, ocimene, etc.), a monocyclic monoterpene (e.g., limonene, γ-terpinene, α-phellandrene, β-phellandrene, terpinolene, etc.), or a bicyclic monoterpene (e.g., 3-carene, α-pinene, β-pinene, α-fenchene, camphene, etc.) (including their various stereoisomers), and mixtures thereof. In some embodiments, the monoterpene is a monocyclic monoterpene, with limonene being particularly preferred. In a preferred embodiment, the monoterpene is a bicyclic monoterpene, with 3-carene, α-pinene, β-pinene, and camphene being particularly preferred, with α-pinene and / or β-pinene being more preferred, and even more preferred, with α-pinene.
[0029] A preferred inkjet ink is formulated with a terpene resin (A) produced from the polymerization or oligomerization of α-pinene. As known to those skilled in the art, such terpene resins can be easily obtained, for example, by catalytic polymerization / oligomerization (in solution) of α-pinene monomers, which are typically derived from fractional distillation of gum and sulfated turpentine oil obtained from pines such as Pistacia terebinthus, Pinus pinaster, Pinus halepensis, Pinus massoniana, Pinus merkusii, Pinus palustris, Pinus taeda, and Pinus ponderosa.
[0030] In a preferred embodiment, the terpene resin (A) is a homopolymer made from α-pinene, having an α-pinene content (units derived from α-pinene) of at least 95% by weight, preferably at least 96% by weight, more preferably at least 97% by weight, more preferably at least 98% by weight, more preferably at least 99% by weight, even more preferably at least 99.5% by weight, and even more preferably 100% by weight, based on the total unit (100% by weight) of the terpene resin (A). The terpene resin (A) of the present disclosure may contain a small amount of other units than the units derived from α-terpene monomers, but the amount of other (e.g., non-terpene) units is preferably less than 5% by weight, more preferably less than 3% by weight, more preferably less than 1% by weight, even more preferably less than 0.5% by weight, and even more preferably 0% by weight, based on the total unit (100% by weight) of the terpene resin (A).
[0031] In a preferred embodiment, the terpene resin (A) is a homopolymer made from β-pinene, having a β-pinene content (units derived from β-pinene) of at least 95% by weight, preferably at least 96% by weight, more preferably at least 97% by weight, more preferably at least 98% by weight, more preferably at least 99% by weight, even more preferably at least 99.5% by weight, and even more preferably 100% by weight, based on the total unit (100% by weight) of the terpene resin (A). The terpene resin (A) of the present disclosure may contain a small amount of other units than the units derived from β-terpene monomers, but the amount of other (e.g., non-terpene) units is preferably less than 5% by weight, more preferably less than 3% by weight, more preferably less than 1% by weight, even more preferably less than 0.5% by weight, and even more preferably 0% by weight, based on the total unit (100% by weight) of the terpene resin (A).
[0032] Both polymeric and oligomeric forms of the terpene resin (A) may be used herein, including combinations thereof.Typically, the number average molecular weight (M) is at least 330 g / mol, preferably at least 340 g / mol, preferably at least 400 g / mol, preferably at least 450 g / mol, preferably at least 500 g / mol, preferably at least 550 g / mol, more preferably at least 600 g / mol, more preferably at least 650 g / mol, even more preferably at least 700 g / mol, even more preferably at least 750 g / mol, and up to 1500 g / mol, preferably up to 1300 g / mol, more preferably up to 1100 g / mol, more preferably up to 1000 g / mol, more preferably up to 900 g / mol, even more preferably up to 800 g / mol, even more preferably up to 790 g / mol. n ) is used herein.
[0033] Terpene resin (A) can be in the form of solid or liquid at room temperature. When the terpene resin (A) utilized in the present invention is in the form of solid, it can be classified based on its softening point (SP), for example, according to the ring and ball softening point method. The ring and ball softening point is defined as the temperature at which the disk of sample held in a horizontal ring is pressed down by a distance of 1 inch (25.4 mm) under the weight of a steel ball while the sample is heated at a predetermined rate in a glycerol bath (for example, according to JIS B7410, which is incorporated herein by reference in its entirety). In some embodiments, the terpene resin (A) has a softening point of at least 20°C, preferably at least 40°C, preferably at least 60°C, preferably at least 80°C, more preferably at least 100°C, more preferably at least 110°C, more preferably at least 115°C, more preferably at least 120°C, even more preferably at least 125°C, even more preferably at least 130°C, and up to 160°C, preferably up to 155°C, preferably up to 150°C, preferably up to 145°C, preferably up to 140°C, preferably up to 138°C, preferably up to 135°C.
[0034] Bromine number is the amount of bromine in grams absorbed by 100 grams of sample (Br 2 ), which is an indication of the degree of unsaturation of the sample. In some embodiments, the terpene resin (A) used in the inkjet ink has a Bromine Number of at least 12, preferably at least 15, preferably at least 19, preferably at least 22, preferably at least 25, preferably at least 26, more preferably at least 27, and up to 35, preferably up to 34, more preferably up to 33, more preferably up to 32, even more preferably up to 31, and even more preferably up to 30, although terpene resins (A) having Bromine Numbers above or below these values (e.g., hydrogenated terpene resins (A)) can also be used in the disclosed inkjet inks.
[0035] The terpene resin (A) may be present in the inkjet ink in an amount of at least 0.1 wt.-%, preferably at least 0.5 wt.-%, more preferably at least 1 wt.-%, more preferably at least 1.5 wt.-%, more preferably at least 2 wt.-%, even more preferably at least 2.5 wt.-%, even more preferably at least 3 wt.-%, and up to 10 wt.-%, preferably up to 9 wt.-%, preferably up to 8 wt.-%, preferably up to 7 wt.-%, more preferably up to 6 wt.-%, even more preferably up to 5 wt.-%, even more preferably up to 4 wt.-%, based on the total weight of the inkjet ink.
[0036] Ink-jet inks of the present disclosure may be formulated using one type of terpene resin (A) or a combination of two or more types of terpene resins (A). Examples of terpene resins (A) that may be used alone or in combination in the ink-jet inks herein include PICCOLYTE A115 (global ball SP=112-118° C., bromine number=31.5), PICCOLYTE A125 (global ball SP=122-128° C., bromine number=31.5), PICCOLYTE A135 (global ball SP=132-138° C., bromine number=27), PICCOLYTE A135 PLUS (global ball SP=132-138° C.), PICCOLYTE AO PLUS (oligomer, liquid), and PINOVA RESIN 2495 (global ball SP=132-138° C., bromine number=27), all available from Pinova, each of which is manufactured from high purity α-pinene, and PICCOLYTE A135 PLUS (global ball SP=132-138° C., bromine number=27), all of which are .... Examples of suitable β-pinene include, but are not limited to, S25 (produced from high-purity β-pinene, ring-ball SP=22 to 28° C., bromine number 19).
[0037] It has been unexpectedly discovered that inkjet inks formulated with terpene resin (A) have superior dry times and decap times (see, for example, Tables 1 and 6, Examples 3 to 11) compared to inkjet inks in which the terpene resin (A) has been replaced with other binder resins / tackifiers / adhesive materials (e.g., terpene phenolic resins such as DERTOPHENE T, rosin resins, e.g., hydrogenated acidic rosins such as FORAL AX, each available from Pinova, Inc.) that tend to suffer from poor (i.e., short) decap times with nozzle non-firing occurring within 30 seconds after decap (see, for example, Tables 2 and 7, Examples 13 and 14).
[0038] (B) Solvent system In many printing processes utilizing solvent-based inks, especially in thermal inkjet printing, the selection of an appropriate solvent system can affect the reliability of the printing process, the properties / appearance of the printed ink product, and the overall printing process efficiency. For example, in thermal inkjet printing, the selection of the solvent system can 1) aid in bubble formation during the jetting process, resulting in reliable ink jetting, 2) affect the stability / volatility of the inkjet ink by changing the interaction dynamics between the solvent(s) and various inkjet ink components, thus affecting the decap behavior, kogation, and / or droplet trajectory, 3) affect the adhesion, rub and scratch resistance, and optical density properties of the printed image, even when the solvent(s) are no longer present or present in lesser amounts after drying, due to interaction forces between the solvent system and other inkjet ink components, and / or 4) affect the drying time after application or the equipment required to dry the applied ink.
[0039] In light of the above, particularly preferred herein are inkjet inks comprising a solvent system (B) comprising (B1) methyl ethyl ketone (MEK). The inclusion of methyl ethyl ketone (B1) may aid in solvation of the inkjet ink components and provide the inkjet ink with acceptable volatility for drying time purposes. It is preferred that methyl ethyl ketone (B1) constitutes the majority of the solvent system used in the inkjet inks herein, i.e., MEK (B1) constitutes at least 50% by weight, preferably at least 55% by weight, preferably at least 60% by weight, more preferably at least 65% by weight, even more preferably at least 70% by weight, even more preferably at least 75% by weight, and up to 100% by weight, preferably up to 95% by weight, more preferably up to 90% by weight, even more preferably up to 85% by weight, even more preferably up to 80% by weight, based on the total weight of the solvent system (B). In some embodiments, methyl ethyl ketone (B1) is present in the inkjet ink in an amount of at least 40 wt.-%, preferably at least 45 wt.-%, more preferably at least 50 wt.-%, more preferably at least 55 wt.-%, even more preferably at least 60 wt.-%, even more preferably at least 65 wt.-%, and up to 90 wt.-%, preferably up to 88 wt.-%, preferably up to 85 wt.-%, more preferably up to 80 wt.-%, more preferably up to 75 wt.-%, even more preferably up to 70 wt.-%, and even more preferably up to 67 wt.-%, based on the total weight of the inkjet ink.
[0040] In some embodiments, the weight ratio of methyl ethyl ketone (B1) to terpene resin (A) ((B1):(A)) is at least 10:1, preferably at least 14:1, preferably at least 16:1, preferably at least 18:1, preferably at least 20:1, more preferably at least 22:1, even more preferably at least 24:1, even more preferably at least 26:1, and up to 100:1, preferably up to 80:1, preferably up to 60:1, preferably up to 50:1, preferably up to 40:1, more preferably up to 35:1, even more preferably up to 34:1, even more preferably up to 32:1.
[0041] Besides methyl ethyl ketone (B1), additional ketone solvents, such as those containing 3 to 6 carbon atoms, may be optionally included in the solvent system (B) herein. Examples of (non-MEK) ketone solvents include, but are not limited to, acetone, 3-pentanone, methyl n-propyl ketone, methyl isopropyl ketone, methyl n-butyl ketone, methyl isobutyl ketone, and cyclohexanone. Preferably, the inkjet ink has a total ketone content of at least 50% by weight, preferably at least 55% by weight, more preferably at least 60% by weight, more preferably at least 62% by weight, even more preferably at least 64% by weight, even more preferably at least 66% by weight, and up to 95% by weight, preferably up to 92% by weight, more preferably up to 90% by weight, more preferably up to 88% by weight, even more preferably up to 86% by weight, even more preferably up to 84% by weight, based on the total weight of the inkjet ink. The "total ketone content" above refers to the total amount of ketone-based solvents used in the inkjet ink, expressed as a percentage based on the total weight of the inkjet ink. Thus, when MEK(B1) is used alone without any additional ketone solvent, the total ketone content represents the amount of MEK(B1) present in the inkjet ink, and when MEK(B1) is used in combination with one or more additional ketones (e.g., acetone), the total ketone content represents the combined total of MEK(B1) plus the additional ketone solvent(s).
[0042] In particular, when the solvent system (B) further comprises (B2) acetone, extremely fast drying times and advantageous decap times can be achieved. For example, when formulated to include acetone (B2), the inkjet ink may have an acetone (B2) content of at least 1 wt.-%, preferably at least 5 wt.-%, more preferably at least 10 wt.-%, even more preferably at least 15 wt.-%, even more preferably at least 20 wt.-%, and up to 40 wt.-%, preferably up to 35 wt.-%, more preferably up to 30 wt.-%, and even more preferably up to 25 wt.-%, based on the total weight of the inkjet ink.
[0043] When acetone (B2) is present, the weight ratio of methyl ethyl ketone (B1) to acetone (B2) can be adjusted for the desired drying and decap times, but typically the weight ratio of methyl ethyl ketone (B1) to acetone (B2) ((B1):(B2)) is at least 1:1, preferably at least 2:1, preferably at least 3:1, preferably at least 3.2:1, and ranges up to 5:1, preferably up to 4:1, preferably up to 3.5:1.
[0044] The solvent system (B) may also optionally contain a glycol ether (B3) to further improve decap performance without substantially compromising the drying time of the ink. The glycol ether (B3) may be a monoalkyl ether, a dialkyl ether, a monoalkyl monoester ether, or a combination thereof. In a preferred embodiment, the glycol ether (B3) is a monoalkyl ether, i.e., contains one free hydroxyl group. The glycol ether (B3) preferably contains at least 3 carbon atoms, more preferably at least 4 carbon atoms, and may contain up to 12 carbon atoms, preferably up to 10 carbon atoms, more preferably up to 8 carbon atoms. Acceptable examples of glycol ethers (B3) that may be optionally included in the disclosed ink-jet inks include, but are not limited to, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-t-butyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-t-butyl ether, propylene glycol mono-n-propyl ether, propylene glycol monoisopropyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, propylene glycol methyl ether acetate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol mono-n-propyl ether, and mixtures thereof.
[0045] If used, the glycol ether (B3) may be present in the inkjet ink in an amount of at least 1 wt.-%, preferably at least 5 wt.-%, more preferably at least 10 wt.-%, even more preferably at least 15 wt.-%, even more preferably at least 20 wt.-%, and up to 40 wt.-%, preferably up to 35 wt.-%, more preferably up to 30 wt.-%, even more preferably up to 25 wt.-%, based on the total weight of the inkjet ink.
[0046] With a view to improving the decap performance of the inkjet ink without significantly extending the drying time, preferred glycol ethers (B3) are those having a boiling point (at standard pressure) of less than 214°C, preferably less than 200°C, preferably less than 190°C, preferably less than 180°C, more preferably less than 175°C, more preferably less than 170°C, more preferably less than 165°C, more preferably less than 160°C, even more preferably less than 155°C, and even more preferably less than 150°C.
[0047] In view of the above, glycol ethers (B3) selected from the group consisting of ethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol mono-n-propyl ether and dipropylene glycol mono-n-propyl ether (including mixtures thereof) are preferred, with propylene glycol mono-n-propyl ether being particularly preferred.
[0048] In addition to methyl ethyl ketone (B1), and optionally additional ketone solvents (e.g., acetone (B2)) and / or glycol ethers (B3), other organic solvents that may optionally be utilized as part of the solvent system (B) herein include, but are not limited to, the following: - lower alcohols containing 1 to 8 carbon atoms, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, etc.; - ethers (non-glycol ethers), for example ethers containing 4 to 8 carbon atoms, such as diethyl ether, dipropyl ether, methyl tert-butyl ether, dibutyl ether, dioxane, and tetrahydrofuran; - esters, including those having 3 to 8 carbon atoms, for example, methyl acetate, ethyl acetate, n-butyl acetate, methyl lactate, ethyl lactate; - and equivalents, as well as mixtures of two or more of these.
[0049] If present, the additional organic solvent may be included in an amount of up to 20 wt.-%, preferably up to 15 wt.-%, preferably up to 10 wt.-%, preferably up to 5 wt.-%, more preferably up to 4 wt.-%, even more preferably up to 2 wt.-%, and even more preferably up to 1 wt.-%, based on the total weight of the inkjet ink.
[0050] Generally, preferred inkjet inks are substantially free of solvents having a boiling point above 175°C, preferably above 170°C, preferably above 165°C, more preferably above 160°C, even more preferably above 155°C.
[0051] In some embodiments, the inkjet ink is substantially free of lower alcohol solvents (having 1-8 carbon atoms). In some embodiments, the inkjet ink is substantially free of ether solvents (other than glycol ethers (B3)). In some embodiments, the inkjet ink is substantially free of glycol ethers (B3). In some embodiments, the inkjet ink is substantially free of ketone solvents (other than MEK), in particular acetone (B2). In some embodiments, the inkjet ink is substantially free of ester solvents. In some embodiments, the inkjet ink is substantially free of additional organic solvents, i.e., methyl ethyl ketone (B1), additional ketone solvents (e.g., acetone (B2)), and organic solvents other than glycol ethers (B3). In a preferred embodiment, the solvent system (B) consists of methyl ethyl ketone (B1) and one of acetone (B2) or glycol ethers (B3).
[0052] In a preferred embodiment, the inkjet ink of the present disclosure is substantially non-aqueous, meaning that no water is added to the inkjet ink other than what may be incidental amounts of moisture from ambient conditions. In such a case, the inkjet ink may have less than 1 wt. %, preferably less than 0.5 wt. %, preferably less than 0.1 wt. %, preferably less than 0.05 wt. %, preferably less than 0.01 wt. %, and more preferably 0 wt. % water, based on the total weight of the inkjet ink.
[0053] Polyether modified silicone (C) The inkjet ink of the present disclosure is formulated with a specific surfactant, namely, polyether-modified silicone (C). In particular, when a polyether-modified silicone (C) having a Griffin hydrophilic-lipophilic balance (HLB) value of at least 1, preferably at least 2, preferably at least 3, more preferably at least 4, even more preferably at least 4.5, even more preferably at least 5, and up to 12, preferably up to 11, preferably up to 10, preferably up to 9, more preferably up to 8, even more preferably up to 7, even more preferably up to 6 is used, suitable image clarity can be achieved.
[0054] The polyether modified silicone (C) utilized in the disclosed inkjet ink is preferably a block copolymer with a pendant graft structure, comprising or consisting of (i) a silicone backbone (main chain), (ii) one or more polyether side chains attached to the silicone backbone, and optionally (iii) one or more fatty alkyl side chains attached to the silicone backbone. Thus, as long as at least one polyether side chain is attached to the silicone backbone, the material meets the definition of "polyether modified silicone (C)", regardless of whether additional side chain types (e.g., fatty alkyl side chains) are also attached to the silicone backbone. Preferably, in the polyether modified silicone (C), there are no other side chains other than the polyether side chain(s) and, optionally, the fatty alkyl side chain(s). As referred to herein, the "side chains" are attached to the silicone backbone (main chain) as pendant grafts, rather than as a continuation of the silicone backbone (as is the case for linear block copolymers with an ABA structure), thereby forming branch points on the silicone backbone with side chains extending from the silicone backbone via covalent bonds. Preferred polyether-modified silicones (C) are non-hydrolyzable, i.e., those in which the side chains are attached to the silicone backbone via Si-C bonds.
[0055] <(i) Silicone backbone> Silicone backbone can be formed from polymerization and / or polycondensation of appropriately functionalized silanes, and can be based on any organosilicon polymer or oligomer (polyorganosiloxane) of various molecular weights, linear or branched, having a polysiloxane backbone structure (silicon atoms are connected via oxygen atoms; -Si-O-Si-) with alkyl, aryl, and / or arylalkyl groups directly bonded to (tetravalent) silicon atoms.For example, polyorganosiloxane backbone can be linear, including but not limited to polydimethylsiloxane (dimethicone) backbone (each silicon atom in this backbone is directly bonded to two methyl groups), poly(dimethylsiloxane-co-methylphenylsiloxane) backbone, poly(dimethylsiloxane-co-diphenylsiloxane) backbone, and poly(dimethylsiloxane-co-methylalkylsiloxane) backbone, or branched, of which polydimethylsiloxyethyl dimethicone is specifically mentioned.
[0056] <(ii) Polyether Side Chain> The polyether-modified silicone (C) comprises at least one polyether side chain based on a polyalkylene glycol oligomer or polymer, such as one formed from the ring-opening polymerization of one or more alkylene oxides, most preferably ethylene oxide (EO), propylene oxide (PO), and / or butylene oxide (BO), including copolymers such as block copolymers thereof. Preferably, the polyether side chain is a polyethylene glycol or polyethylene glycol-polypropylene glycol copolymer extending from the silicone backbone, more preferably the polyether side chain is a polyethylene glycol side chain (formed only from ethylene oxide (EO)).
[0057] As long as the HLB value of the polyether modified silicone (C) remains within the range indicated above, polyether side chain(s) of various lengths can be utilized.Typically, the mole number of alkylene oxide units per side chain is at least 2 mol, preferably at least 3 mol, more preferably at least 4 mol, even more preferably at least 5 mol, even more preferably at least 6 mol, and ranges up to 50 mol, preferably up to 40 mol, preferably up to 30 mol, preferably up to 20 mol, preferably up to 15 mol, more preferably up to 12 mol, even more preferably up to 10 mol, even more preferably up to 9 mol, where 3 mol to 10 mol, preferably 4 mol to 9 mol of ethylene oxide (EO) units per side chain is particularly preferred.
[0058] Additionally, any polyether side chains present may be uncapped (whereby the end of the polyether side chain opposite the silicone backbone terminates with -H, forming a terminal hydroxyl functionality) or may be capped with alkyl groups having 1, 2, 3, or 4 carbon atoms (forming a terminal alkyl ether group), specifically including methyl, ethyl, propyl, and butyl. In a preferred embodiment, the polyether modified silicone (C) contains only uncapped polyether side chains, i.e., each polyether side chain contains a terminal hydroxyl group.
[0059] <(iii) Fatty Alkyl Side Chain> The polyether modified silicone (C) may be optionally modified with one or more fatty alkyl side chains, such as those containing at least 8 carbon atoms, preferably at least 10 carbon atoms, more preferably at least 12 carbon atoms, and up to 22 carbon atoms, preferably up to 20 carbon atoms, more preferably up to 18 carbon atoms, even more preferably up to 16 carbon atoms, and even more preferably up to 14 carbon atoms. Exemplary fatty alkyl side chain groups include, but are not limited to, capryl, nonyl, decyl, undecyl, lauryl, tridecyl, myristyl, pentadecyl, cetyl, palmitoleic, heptadecyl, stearyl, oleyl, arachidyl, and behenyl, specifically lauryl, myristyl, cetyl, and stearyl, preferably lauryl.
[0060] In some embodiments, the polyether-modified silicone (C) has a viscosity of at least 120 mm 2 / s, preferably at least 130 mm 2 / s, more preferably at least 140 mm 2 / s, and even more preferably at least 150 mm 2 / s, even more preferably at least 160 mm 2 / s and 1000 mm 2 / s, preferably up to 950mm 2 / s, preferably up to 900mm 2 / s, preferably up to 850mm 2 / s, preferably up to 800 mm 2 / s, and even more preferably 750 mm 2 / s, and even more preferably up to 700 mm 2 It has a kinematic viscosity at 25°C of up to 1 / s.
[0061] The polyether modified silicone (C) can provide the desired image sharpness effect without sacrificing decap time when used in the inkjet ink in an amount of at least 0.001 wt%, preferably at least 0.005 wt%, preferably at least 0.01 wt%, preferably at least 0.02 wt%, more preferably at least 0.03 wt%, even more preferably at least 0.04 wt%, even more preferably at least 0.05 wt%, and up to 4 wt%, preferably up to 3.5 wt%, preferably up to 3 wt%, preferably up to 2.5 wt%, preferably up to 2 wt%, preferably up to 1.5 wt%, preferably up to 1 wt%, preferably up to 0.8 wt%, preferably up to 0.5 wt%, more preferably up to 0.3 wt%, even more preferably up to 0.2 wt%, even more preferably up to 0.1 wt%, based on the total net amount of the inkjet.
[0062] In some embodiments, the polyether-modified silicone (C) is a block copolymer having pendant graft structures formed from a linear polydimethylsiloxane backbone containing one or more polyether side chains, for example represented by formula (IA): [ka] In formula (IA), o is 0 or a positive integer, for example at least 1, preferably at least 2, more preferably at least 3, even more preferably at least 4, even more preferably at least 5, and up to 500, preferably up to 400, preferably up to 300, more preferably up to 200, even more preferably up to 100, even more preferably up to 50; p represents the number of constitutional units comprising the polyether side chains and is a positive integer, for example at least 1, preferably at least 2, more preferably at least 3, even more preferably at least 4, even more preferably at least 5, and up to 100, preferably up to 80, preferably up to 60, more preferably up to 40, even more preferably up to 20, even more preferably up to 10; and A is a polyether-containing group represented by formula (II), [ka] In formula (II), w is at least 2, preferably at least 3, and up to 6, preferably up to 5, more preferably up to 4, even more preferably w is 3; n is 0 or at least 1, preferably at least 2, more preferably at least 3, even more preferably at least 4, and is an integer up to 30, preferably up to 20, more preferably up to 10, even more preferably up to 9, even more preferably n is from 3 to 10; m is an integer of 0 or up to 30, preferably up to 10, preferably up to 9, preferably up to 5, more preferably up to 2, even more preferably up to 1, even more preferably m is 0, and Z is H or an alkyl group having 1 to 4 carbon atoms, preferably H (unblocked).
[0063] Suitable examples of this type of polyether modified silicone (C) that can be used in the disclosed ink-jet inks include, but are not limited to, KF-6013 (PEG-9 dimethicone, unblocked, HLB=10.0), KF-6015 (PEG-3 dimethicone, unblocked, HLB=4.5), and KF-6017 (PEG-10 dimethicone, unblocked, HLB=4.5), each available from Shin-Etsu Chemical Co.
[0064] In some embodiments, the polyether-modified silicone (C) is a block copolymer having pendant graft structures formed from a branched polydimethylsiloxane backbone containing one or more polyether side chains and one or more fatty alkyl side chains, such as represented by formula (IB): [ka] In formula (IB), o, p, and A are as defined above; B is a fatty alkyl group, preferably having at least 10 carbon atoms, preferably at least 12 carbon atoms, and up to 18 carbon atoms, preferably at least 16 carbon atoms, preferably at least 14 carbon atoms, including, in particular, lauryl, myristyl, cetyl, and stearyl; q represents the number of constitutional units comprising a fatty alkyl side chain and is a positive integer, for example, at least 1, preferably at least 2, more preferably at least 3, even more preferably at least 4, even more preferably at least 5, and up to 50, preferably up to 40, preferably up to 30, more preferably up to 20, even more preferably up to 10, even more preferably up to 5; r represents the branching in the polydimethylsiloxane backbone and is a positive integer, for example up to 50, preferably up to 40, preferably up to 30, preferably up to 20, preferably up to 10, preferably up to 5, more preferably up to 3, even more preferably up to 2, and even more preferably up to 1; x is a positive integer, for example at least 1, preferably at least 2, more preferably at least 3, even more preferably at least 4, even more preferably at least 5, and up to 200, preferably up to 150, preferably up to 100, more preferably up to 75, even more preferably up to 50, more preferably up to 30, even more preferably up to 20, even more preferably up to 10, and y is at least 2 and up to 6, preferably 2.
[0065] Suitable examples of this type of polyether-modified silicone (C) that can be used in the disclosed inkjet inks include, but are not limited to, KF-6038 (Lauryl PEG-9 Polydimethylsiloxyethyl Dimethicone, Unblocked, HLB=3.0) available from Shin-Etsu Chemical Co., Ltd.
[0066] As will become apparent, it has been unexpectedly discovered that a particular class of surfactants (polyether modified silicones (C) having a pendant graft structure with HLB values between 1 and 12 and preferably with unblocked polyether side chains) allows for the production of desired image definition even when printing on "difficult" non-porous substrates such as varnish-coated paper, biaxially oriented polypropylene (BOPP), polyethylene terephthalate (PET), nylon, aluminum, etc. (see, for example, Tables 1, 2, 6, and 7, Examples 3-11, 15, and 17-19). Without being bound by theory, it is believed that the polyether side chain(s) of the polyether modified silicones (C) adsorb onto / orient towards the substrate surface, while the silicone backbone orients away from the substrate surface, thereby rendering the substrate surface more hydrophobic with respect to the solvent(s) and any other inkjet ink components, thus preventing the inkjet ink from spreading excessively upon application. It is believed that this interaction between the polyether modified silicone (C) and the substrate surface allows for the production of high image definition, with the HLB value providing a balance between vehicle solubility and substrate adsorption.
[0067] On the other hand, other types of surfactants, including polyether modified silicones having HLB values outside the range of 1-12, as well as silicone acrylate copolymers and other surfactants common to inkjet inks (e.g., U.S. Patent No. 5,399,433, U.S. Patent No. 5,399,462, U.S. Patent No. 5,399,493, and U.S. Patent No. 5,399,462, each of which is incorporated herein by reference in its entirety), have been found to be unable to provide acceptable image sharpness when used in place of polyether modified silicones having HLB values of 1-12 (see, e.g., Tables 1 and 6, Examples 2 and 12). Examples of these other surfactant types include, but are not limited to, the following: - polysiloxanes, including organo-modified silicones (e.g., alkyl, aryl, and / or arylalkyl modified silicones), such as SILTECH C-32 available from Siltech Corporation, COATOSIL 1211C and 3573, respectively, available from Momentive, KF-410 (arylalkyl modified polydimethylsiloxane) available from Shin-Etsu Chemical Co., Ltd., and BYK-322 and BYK-323 (arylalkyl modified poly(dimethylsiloxane-co-methylalkylsiloxane)), respectively, available from BYK Additives & Instruments; - silicone acrylate copolymers such as KP-541, KP-543, KP-545, KP-550, and KP-575 (acrylic polymers grafted with polydimethylsiloxane side chains, available from Shin-Etsu Chemical Co., Ltd.), and BYK-3550 (available from BYK Japan KK); - photocrosslinkable silicone acrylates or silicone polyether acrylates such as TEGO RAD 2100, TEGO RAD 2200, TEGO RAD 2250, TEGO RAD 2300 (silicone polyether acrylates), respectively, available from Evonik Industries, and BYK-UV 3500 and 3530, available from BYK; - polyacrylates, including polyacrylate copolymers and crosspolymers, such as BYK-381 and BYK-361N (polyacrylate copolymers), respectively, available from BYK, and PEMULEN EZ-4U (Acrylates / C10-C30 Alkyl Acrylate Crosspolymer) and PEMULEN TR-2 (Acrylic Acid / C10-C30 Alkyl Acrylate Crosspolymer), respectively, available from Lubrizol; - Fluoropolymers such as FC-4430 and FC-4432 available from 3M Corporation; - Acetylene diol and acetylene glycol based gemini surfactants such as SURFYNOL SEF and DYNOL surfactants available from Evonik Industries; - Polysiloxane-based gemini surfactants such as TEGO TWIN 4100 available from Evonik Industries; - non-ionic polyethers as substrate wetting surfactants, for example TEGO WET 510 (hydrophilic polyether substrate wetting surfactant) available from Evonik Industries; - amides or monoalkanolamides of fatty acids, including alkoxylated monoalkanolamides of fatty acids, such as coconut fatty acid monoethanolamide and coconut fatty acid monoethanolamide reacted with 2 to 20 moles of ethylene oxide; - Alkoxylated C including alkoxylated fatty alcohols such as BIO-SOFT N-600 (C12-C13 alcohol ethoxylate), MAKON DA-4 (ethoxylated isodecyl alcohol), MERPOL SE (alcohol ethoxylate), and POLYSTEP TD-6 (ethoxylated tridecyl alcohol), ethylene oxide / propylene oxide copolymers, alkoxylated alkylphenols, each available from Stepan Corporation. 1 ~C 22ethers such as alcohols and alkyl polyglycosides (APGs), such as those made from the reaction of fatty alcohols with glucose; - fatty esters such as ethoxylated and / or propoxylated fatty acids (e.g. castor oil containing 2 to 40 moles of ethylene oxide), alkoxylated glycerides (e.g. PEG-24 glyceryl monostearate), glycol esters and derivatives, monoglycerides, polyglyceryl esters, esters of polyalcohols, and polysorbates, including sorbitan / sorbitol esters such as sorbitan monolaurate (e.g. EMASOL L-10V available from Kao Corporation), and mono-, di-, or tri- fatty acid esterified polysorbates such as TOXIMUL SEE-340 (sorbitan trioleate ethoxylate (20)) available from Stepan Corporation; and - Glycosides of fatty alcohols such as PLANTASENS NATURAL EMULSIFIER HE20 (cetearyl glucoside, sorbitan-olivate) available from Clariant.
[0068] Other types of surfactants are not necessarily excluded from use in the disclosed inkjet inks, but their optional use should be accompanied by the polyether modified silicone (C) for acceptable image sharpness. However, the preferred inkjet inks are those in which the polyether modified silicone (C) is the only surfactant present.
[0069] Rosin Resin (D) The inkjet ink may be optionally formulated with a rosin resin (D). Any rosin resin (D) compatible with the terpene resin (A), methyl ethyl ketone (B1), and polyether modified silicone (C) may be utilized herein, including rosin resins (D) derived from gum rosin, wood rosin, and tall oil rosin (whose main components are resin acids such as abietic acid, palustric acid, neoabietic acid, pimaric acid, isopimaric acid, and / or dehydroabietic acid), preferably wood rosin. If used, the rosin resin (D) may be used in an amount of up to 10 wt%, for example at least 0.5 wt%, preferably at least 1 wt%, more preferably at least 1.5 wt%, more preferably at least 2 wt%, even more preferably at least 2.5 wt%, even more preferably at least 3 wt%, and up to 10 wt%, preferably up to 8 wt%, more preferably up to 6 wt%, even more preferably up to 5 wt%, even more preferably up to 4 wt%, based on the total weight of the inkjet ink. If the inkjet ink is formulated with rosin resin (D), it is preferred that the amount (in terms of weight %) of rosin resin (D) is less than or equal to the amount of terpene resin (A).
[0070] Rosin resins (D) may be formed by modifying the aforementioned rosins by esterification, hydrogenation (including partial hydrogenation), dimerization, and / or other modifications / functionalizations, such as Diels-Alder reaction with unsaturated diacids (e.g., maleic or fumaric acids / anhydrides), carboxylic acid reduction to the respective aldehydes / alcohols, double bond isomerization, dehydrogenation, oxidation, disproportionation, etc. Exemplary rosin resins (D) include, but are not limited to, the following: - rosin ester resins, such as esters of rosin composed mainly of abietic or pimaric acid type resin acids reacted with alcohol(s), such as glycerin, pentaerythritol, ethylene glycol, diethylene glycol, triethylene glycol, methanol, optionally hydrogenated or partially hydrogenated, such as HARIESTER products available from Harima Chemicals, Inc., STAYBELITE ESTER 10-E and PERMALYN 6110, respectively, available from Eastman, SUPER ESTER A-125, SUPER ESTER A-75, PENSEL D-125, PINECRYSTAL KE-359 available from Arakawa Chemical Industries, Ltd., and FORAL 85, FORAL 105, HERCOLYN products, PEXALYN products and PENTALYN products available from Pinova; - Hydrogenated acid rosins such as FORAL AX and FORAL DX, respectively, available from Pinova; - partially hydrogenated acidic rosins, such as STAYBELITE RESIN-E available from Eastman Co., and STAYBELITE and STAYBELITE A, respectively, available from Pinova Co.; - dimerized rosin, such as POLY-PALE partially dimerized rosin available from Eastman Co.; and - functionalized rosin resins, such as esters of rosin modified with maleic anhydride (e.g., glycerol esters), or rosin subjected to carboxylic acid reducing conditions, specifically LEWISOL 28-M and Abitol-E hydroabietyl alcohol, each available from Eastman Co.; - and mixtures thereof.
[0071] In some embodiments, the rosin resin (D) has a softening point (Ring and Ball SP) of at least 50° C., preferably at least 55° C., more preferably at least 60° C., even more preferably at least 65° C., and up to 80° C., preferably up to 75° C., more preferably up to 70° C., and even more preferably up to 68° C. In some embodiments, the rosin resin (D) is an acidic rosin (non-esterified) and has an acid number (mg KOH / g) of at least 100, preferably at least 110, more preferably at least 120, more preferably at least 130, even more preferably at least 140, still even more preferably at least 150, and up to 170, preferably up to 165, more preferably up to 160, and even more preferably up to 158.
[0072] In a preferred embodiment, the rosin resin (D) is a hydrogenated acidic rosin, preferably a hydrogenated acidic wood rosin, such as FORAL AX and FORAL DX, each available from Pinova. In some embodiments, the inkjet ink is substantially free of rosin resin (D). In some embodiments, the inkjet ink is substantially free of rosin ester resins, partially hydrogenated acidic rosin, dimerized rosin, and other functionalized / modified rosin resins. In some embodiments, the hydrogenated acidic rosin is the only rosin resin (D) present in the inkjet ink.
[0073] Other binder resins In addition to the terpene resin (A) and the optional rosin resin (D), the inkjet ink may optionally contain other binder resins / tackifiers / adhesive substances in an amount of at least 0.1 wt.%, preferably at least 0.5 wt.%, preferably at least 1 wt.%, preferably at least 1.5 wt.%, preferably at least 2 wt.%, preferably at least 2.5 wt.%, and up to 10 wt.%, preferably up to 9 wt.%, preferably up to 8 wt.%, preferably up to 7 wt.%, preferably up to 6 wt.%, preferably up to 5 wt.%, preferably up to 4 wt.%, preferably up to 3 wt.%, based on the total weight of the inkjet ink. Such additional resins, binders, tackifiers, or adhesive substances include, but are not limited to: - terpene phenolic resins (TPRs), which are copolymer reaction products from the alkylation of (i) one or more monohydric or polyhydric phenolic compounds having at least two replaceable hydrogen atoms ortho and / or para to at least one hydroxyl group with (ii) one or more terpenes, such as (i) phenol, o-cresol, m-cresol, p-cresol, 2,5-xylenol, 2,3-xylenol, 3,4-xylenol, 3,5-xylenol, 2,3,5-trimethylphenol, isopropylphenol (e.g., 4-isopropylphenol), tert-butylphenol (e.g., 4-tert-butylphenol), amylphenol (e.g., 4-tert-amylphenol), heptylphenol (e.g., 4-heptylphenol), octylphenol (e.g., o-octylphenol, p-octylphenol, etc.), nonylphenol (e.g., 4-(2,4-dimethylheptane), etc.), and (ii) those formed from the copolymerization of one or more phenolic compounds, such as bisphenol A, phenylphenol (e.g., 3-phenylphenol), cumylphenol, mequinol, benzyloxyphenol, guaiacol, ethoxyphenol (e.g., 4-ethoxyphenol), resorcinol, pyrogallol, catechol, p-hydroquinone, 1-naphthol, and / or 2-naphthol, with one or more terpene monomers, including linear monoterpenes (e.g., myrcene, ocimene, etc.), monocyclic monoterpenes (e.g., limonene, γ-terpinene, α-phellandrene, β-phellandrene, terpinolene, etc.), and / or bicyclic monoterpenes (e.g., 3-carene, α-pinene, β-pinene, α-fenchene, camphene, etc.); Chemical Co. Ltd.) available from Polypropylene Co., Ltd.; and DERTOPHENE T (OHV=40 mg KOH / g), DERTOPHENE T160 (OHV=60 mg KOH / g) and DERTOPHENE T160 (OHV=60 mg KOH / g) available from Pinova Co., Ltd.; - phenolic resins (i.e. copolymers of phenolic compounds and formaldehyde), for example novolac resins such as PHENOLITE TD-2131 and PHENOLITE TD-2090 available from DIC Corp.; - polyamide resins, such as VERSAMID 725, 744, 756, 759 available from BASF Japan Ltd., TOHMIDE 90, 92, 394-N available from Sanho Chemical Co. Ltd., and SUNMIDE 550, 554, 615A, 638, 640 available from Evonik; - epoxy resins, including sulfonamide modified epoxy resins, such as AD-PRO MTS available from Rit-Chem; - (meth)acrylate and styrene / (meth)acrylate resins, such as JONCRYL 63, JONCRYL 67, JONCRYL 586, JONCRYL 611, JONCRYL 682, JONCRYL 693 available from BASF, PARALOID DM-55 and PARALOID B-66 available from Palmer Holland, PARALOID B-72 available from Dow Chemical (USA), and ELVACITE 2013 available from Lucite Inc.; - polyurethane resins, such as those formed from the reaction of (i) polyols, including but not limited to polyester polyols, carbonate polyols, such as ethylene glycol, propylene glycol, propanediol, butanediol, polyethylene glycol, polypropylene glycol, polytetrahydrofuran diol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, polyethylene glycol adipate diol, polyethylene glycol succinate diol, poly(3-methyl-1,5-pentanediol adipate) glycol, poly(3-methyl-1,5-pentanediol terephthalate) glycol, with (ii) diisocyanates, including but not limited to 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4-diphenylmethane diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate, e.g., PERMAX 200, PERMAX 202, and SANCURE available from Lubrizol Corporation; 20025F; - polyvinyl butyral resins, such as PIOLOFORM BN16 and MOWITAL B20H available from Kuraray America, Inc.; - polyhydroxystyrene resins, such as poly(p-hydroxystyrene) from DuPont; - vinyl resins such as UCAR VYHH, VMCH, VMCA, and VAGF available from The Dow Chemical Company, and VINNOL E15 / 45, H14 / 36, E15 / 45M, and E16 / 40A available from Wacker Chemie AG (Germany); - sulfonamide-modified formaldehyde resins, such as p-toluenesulfonamide formaldehyde resins; - cellulose ester resins such as cellulose acetate butyrate (CAB-551-0.01) available from Eastman; - as well as polyesters, sulfonated polyesters, cellulose ethers, cellulose nitrate resins, polymaleic anhydrides, acetal polymers, styrene / butadiene copolymers, melamine formaldehyde resins, sulfonamide-modified melamine formaldehyde resins, ketone-aldehyde resins, and polyketone resins; - and equivalents, including mixtures thereof.
[0074] In some embodiments, the inkjet ink is substantially free of additional binder resins / tackifiers / adhesive materials, such as those described above, other than the terpene resin (A) and optional rosin resin (D). In some embodiments, the inkjet ink is substantially free of polyurethane resins. In some embodiments, the terpene resin (A) is the only binder resin / tackifier / adhesive material present in the inkjet ink. In some embodiments, the inkjet ink comprises a combination of the terpene resin (A) and the rosin resin (D), and is preferably substantially free of additional resins, binders, tackifiers, or adhesive materials.
[0075] (E) Coloring agent It should be readily understood by those skilled in the art that the inkjet ink may optionally include one or more colorants (E) to provide colored inks that can be used for various printing purposes, and that the inkjet ink is not limited to any particular color. Any colorant (E) including dyes, pigments, mixtures thereof, and the like may be used in the inkjet ink to provide the desired color, provided that the colorant (E) can be dissolved or dispersed in the inkjet ink. Suitable colors include, for example, cyan, magenta, yellow, and key (black) ("CMYK"), white, orange, green, light cyan, light magenta, violet, and the like (including both spot and process colors). In general, the colorant (E) may be used in an amount of at least 0.1 wt%, preferably at least 0.5 wt%, preferably at least 1 wt%, preferably at least 2 wt%, preferably at least 3 wt%, and up to 20 wt%, preferably up to 15 wt%, preferably up to 10 wt%, preferably up to 8 wt%, preferably up to 7 wt%, based on the total weight of the inkjet ink.
[0076] Inkjet inks can be formulated with a variety of dyes, with organic dyes, such as OIL BLACK 860 available from Orient Chemical Industries, and metal complex dyes being particularly preferred.
[0077] Ink-jet inks can be formulated with a variety of inorganic and / or organic pigments. In addition to imparting color to the ink-jet ink, such pigments may be able to improve the lightfastness, weatherability, etc. of the printed image.
[0078] (F) Additive(s) In addition to the components already mentioned, the inkjet ink may also be optionally formulated with various additives (F) to improve various ink properties and performance. For example, the inkjet ink may optionally include one or more of anti-kogation agents, stabilizers, humectants, and security taggants at art appropriate levels known to those skilled in the art.
[0079] Manufacturing method Embodiments of the ink-jet inks described herein can be prepared by any suitable technique known to one of ordinary skill in the art, for example, by combining components (A) terpene resin, (C) polyether modified silicone, and any desired optional ingredients (e.g., (D) rosin resin, (E) colorant, and / or additives (F)) in any order with a suitable solvent system (B) comprising or consisting of one or more of (B1) methyl ethyl ketone and optionally (B2) acetone and (B3) glycol ether, and stirring, agitating, and / or homogenizing at a temperature between 20° C. and 100° C. for a suitable amount of time to form a homogenous solution.
[0080] In one example, the inkjet ink can be prepared by first combining the terpene resin (A) and the polyether modified silicone (C) with the methyl ethyl ketone (B1) and any optional resin (e.g., (D) rosin resin) or other optional additive(s) (F) in a container, followed by stirring for at least 10 minutes, preferably at least 15 minutes, preferably at least 20 minutes, preferably at least 25 minutes, preferably at least 30 minutes, preferably at least 35 minutes, preferably at least 40 minutes, preferably at least 45 minutes. If acetone (B2) and / or glycol ether (B3) are used, they can be added to the resulting mixture, followed by stirring for at least 10 minutes, preferably at least 15 minutes, preferably at least 20 minutes, preferably at least 25 minutes. The colorant (E) is then added as the final component with continuous mixing, and the solution is then mixed for at least 10 minutes, preferably at least 15 minutes, preferably at least 20 minutes, preferably at least 25 minutes, preferably at least 30 minutes, preferably at least 35 minutes, preferably at least 40 minutes, preferably at least 45 minutes to obtain the inkjet ink. The resulting inkjet ink can then be loaded into a print cartridge, such as a FUNAI TIJ cartridge manufactured by Funai Co., or other printhead suitable for MEK-based inks.
[0081] characteristics Among other advantages, the inkjet inks disclosed herein have an excellent combination of extended decap times and fast drying times after application, resulting in image quality definition even on non-porous substrates that tend to promote ink spreading. The inkjet inks disclosed herein can also be tailored to provide a desired gloss.
[0082] Drying time can be measured by applying the inkjet ink on a substrate in the form of a solid block image (e.g., 1 cm x 10 cm), waiting for the inkjet ink to dry under ambient conditions (room temperature, in air at about 23°C, without heat) for a certain time, e.g., 5 seconds, 10 seconds, 20 seconds, or 30 seconds, and then performing a finger rub test to test whether color transfers from the printed image to the finger at the tested time interval (see, e.g., Figure 1). If color transfer occurs, the tested drying time is not sufficient to achieve complete drying (a rating of "fail"). If color transfer does not occur, the tested drying time is sufficient to achieve complete drying (a rating of "pass"). Any inkjet ink requiring more than 30 seconds of drying time to achieve a "pass" rating is considered unacceptable / slow drying ("bad"), those achieving a "pass" rating with drying times of more than 20 to 30 seconds are considered "acceptable", those achieving a "pass" rating with drying times of more than 10 to 20 seconds are considered "fast", and those achieving a "pass" rating with drying times of 10 seconds or less are considered "very fast". In a preferred embodiment, the inkjet inks of the present disclosure have an "acceptable", "fast", or "very fast" drying time rating, preferably a "fast" or "very fast" drying time rating, and more preferably a "very fast" drying time rating, because they dry within 30 seconds after application, preferably within 25 seconds, more preferably within 20 seconds, even more preferably within 15 seconds, and even more preferably within 10 seconds.
[0083] The inkjet inks disclosed herein also have an extended decap time, as measured, for example, by printing a fine line image (e.g., a barcode) (1 mm x 1 cm, fine lines, monochrome bitmap), exposing the inkjet ink to air (decap the ink cartridge) for a specific time (e.g., 30 seconds, 1 minute, 60 minutes, etc.), reprinting the same fine line image, and comparing the reprinted image after decap to the original image to determine whether any missing lines / loss of line clarity occurred in the fine line image (see, for example, FIG. 2). If no missing lines / loss of line clarity occurs in the time interval tested, the inkjet ink is given a decap rating of "good" for that time interval. If one to two lines are missing / lost clarity in the time interval tested, but not enough to significantly affect the clarity or readability of the fine line image, the inkjet ink is given a decap rating of "acceptable." If more than two lines are missing / lost clarity in the time interval tested, the inkjet ink is classified as "bad" for that time interval. Suitable inkjet inks are those that can be decapped over time intervals of 30 seconds, 1 minute, and 60 minutes, and that can achieve a decap classification of "good" or "acceptable" when decapped (i.e. exposed to air) over one or more of the time intervals tested, preferably over two or more of the time intervals tested, and more preferably at each tested time interval. Preferred inkjet inks are those that maintain a "good" or "acceptable" decap rating when decapped for 30 seconds or more, preferably 1 minute or more, more preferably 10 minutes or more, even more preferably 30 minutes or more, and even more preferably 60 minutes or more.
[0084] To test inkjet inks for image clarity, fine line images and number strings can be printed on a porous control substrate (plain uncoated paper) and a series of non-porous substrates (e.g., varnished paper, biaxially oriented polypropylene, nylon, and aluminum foil). The printed images can then be visually evaluated for spreading on each substrate. Inkjet inks that produce fine line images with no spreading / number strings where all individual lines can be recognized and where each number is distinct and separate from adjacent numbers are given a "G" (Good) rating. Inkjet inks that produce fine line images where some spreading occurs but where individual lines can still be recognized and number strings where each number is distinct but where some numbers are not separated from adjacent numbers are given an "A" (Acceptable) rating. Inkjet inks that produce fine line images where substantial spreading occurs to the extent that individual lines cannot be recognized and number strings where the numbers are not distinct (excessive spreading) and are generally not separated from adjacent numbers are given a "NG" (Poor) rating (see, e.g., Figures 3 and 4). The evaluations for each substrate are then compiled and the inkjet ink is scored for image distinctness according to the following criteria: "Good" if only a "G" rating is obtained, "Acceptable" if both "G" and "A" ratings are obtained without any "NG" ratings, and "Poor" if a "NG" rating is obtained for at least one substrate.
[0085] Another advantage of the disclosed inkjet inks is that they can be easily adjusted for gloss to provide printed images with high, medium, or low gloss, as desired for a particular application. Gloss can be assessed by simple visual inspection methods and classified as "high" gloss, "medium" gloss, or "low" gloss. Alternatively, a gloss meter (e.g., a BYK-Gardner Haze-Gloss Reflectometer from BYK-Gardner, Goeretsort, Germany) can be used to measure the gloss intensity of the printed image at a 60° measurement angle (specular reflection) and gloss is recorded in gloss units (GU), with "high" gloss being a 60° value of more than 70 GU, "medium" gloss being a 60° value of 10-70 GU, and "low" gloss being a 60° value of less than 10 GU.
[0086] printed matter Inkjet inks can be printed on a variety of substrates, including three-dimensional parts and flat sheets or webs supplied in roll form, for the production of a wide variety of printed products. In addition, the substrates can have a variety of surface types, such as flat surfaces, structured surfaces such as grained surfaces, and three-dimensional surfaces such as curved and / or complex surfaces, which are well known to be challenging substrates due to the long distances that the ink must travel to reach all parts of the curved and / or complex surfaces. Such printed products may be suitable in the graphic arts, textile, packaging (e.g., food packaging, pharmaceutical packaging, etc.), lottery tickets, direct mail, business forms, and publishing industries, examples of which include tags or labels, lottery tickets, publications, packaging (e.g., food packaging, pharmaceutical packaging, blister packaging, various other flexible packaging, etc.), folding cartons, rigid containers (e.g., plastic cups or pails, glass containers, metal cans, bottles such as PET bottles, jars, and tubes), envelopes, corrugates, point-of-sale displays, and the like.
[0087] Inkjet inks can be printed on porous (i.e., permeable) substrates, examples of which include, but are not limited to, uncoated paper, wood, membrane, corrugated (cardboard / fiberboard), and fabrics (such as, but not limited to, woven, nonwoven, and foil-laminated fabrics).
[0088] Inkjet inks can also be printed on non-porous (i.e. non-permeable) substrates such as various plastics, glass, metals (e.g., steel, aluminum, etc.), and / or non-permeable papers (e.g., coated papers such as varnished papers), including, but not limited to, molded plastic or metal parts and flat sheets or rolls of plastic or metal films. Examples include substrates including polyesters such as polyethylene terephthalate (PET), polyolefins such as biaxially oriented polystyrene (OPS), polyethylene (PE), polypropylene (PP), oriented polypropylene (OPP), and biaxially oriented polypropylene (BOPP), polylactic acid (PLA), nylon and oriented nylon, polyvinyl chloride (PVC), cellulose triacetate (TAC), polycarbonate, acrylonitrile butadiene styrene (ABS), polyacetal, polyvinyl alcohol (PVA), coated papers such as varnished papers, and metals such as steel and aluminum. In particular, the inkjet inks of the present disclosure are formulated for use on such non-porous substrates without undue spreading, allowing for the formation of sharp images even on the most difficult substrates, such as aluminum foil.
[0089] Method for forming a print image In inkjet printing, a desired printed image is formed when precise patterns of dots are ejected from a drop-generating device known as a printhead onto a print medium. The printhead has an array of precisely formed nozzles located on a nozzle plate and attached to an inkjet printhead substrate. The inkjet printhead substrate houses an array of firing chambers that receive inkjet ink through fluid communication with one or more ink reservoirs. Each firing chamber has a resistive element, known as a firing resistor, that is located opposite the nozzle so that inkjet ink collects between the firing resistor and the nozzle. Each resistive element is typically a pad of resistive material, measuring, for example, about 35 μm by 35 μm. The printhead is held and protected by an enclosure called a print cartridge or inkjet pen. When a particular resistive element is energized, a droplet of inkjet ink is ejected through the nozzle toward the print medium. The firing of the ink droplets is typically under the control of a microprocessor, whose signals are conveyed by electrical traces to the resistive elements to form alphanumeric and other image patterns on the print medium. Because the nozzles are small, typically 10 μm to 40 μm in diameter, inks that minimize clogging are desirable. In particular, because thermal inkjet (TIJ) is an open atmosphere printhead design (the nozzle orifice is open to the atmosphere and there is no valve seal at the orifice to allow ink pressurization), TIJ printing has historically suffered from poor performance during intermittent printing, where decap times (print idle time) cause premature drying of the ink in and around the nozzle.
[0090] The present disclosure, in one or more embodiments, provides a method of forming a printed image by applying an inkjet ink onto a surface of a substrate by a thermal inkjet printhead and drying the inkjet ink. Using the inkjet inks described herein, high quality prints are still produced even on "difficult" non-porous substrates while overcoming the conflicting problems of short decap times (solvent loss is too fast) and slow dry times (solvent loss is too slow) commonly associated with thermal inkjet processes.
[0091] The printing unit of the present method can be any drop-on-demand printhead known to those skilled in the art of inkjet printing, including continuous, thermal, electrostatic, and acoustic printheads, but preferably a thermal printhead (with a heat transducer) is used. Typical parameters such as print resolution, print speed, printhead pulse warming temperature, drive voltage, and pulse length can be adjusted according to the specifications of the printhead. Printheads generally suitable for use in the methods herein have a drop size in the range of 2-80 pL and a drop frequency in the range of 10-100 kHz, and high quality prints can be obtained, for example, by setting the drive voltage at 8.0-9.5 volts, the print speed up to 300 feet / minute, the pulse warming temperature at 25-45°C, and the pulse length at 0.7-2.5 microseconds, although values above or below these values can also be used and still obtain satisfactory prints. One non-limiting example of a printhead suitable for use in the disclosed method is the FUNAI TIJ cartridge manufactured by Funai Electric Co., Ltd.
[0092] After application, the inkjet ink is dried. In a preferred embodiment, drying is achieved by drying the applied inkjet ink under ambient conditions (in air, at about 23° C.) for 30 seconds or less, preferably 25 seconds or less, more preferably 20 seconds or less, even more preferably 15 seconds or less, and even more preferably 10 seconds or less.
[0093] Although external heat may be applied to dry the applied inkjet ink, in a preferred embodiment, external heat is not applied to accelerate drying or increase the drying rate. For example, it is preferred not to use a heater to dry the inkjet ink after application. Furthermore, the method of the present disclosure does not require energy curing (e.g., UV or electron beam curing). Once the applied ink is considered dry, further coatings of inkjet ink may be applied or any processing steps known to those skilled in the art may be performed as necessary.
[0094] It should also be appreciated that in the methods herein, substrate surface treatments such as corona treatments, atmospheric plasma treatments, and flame treatments may be optionally used prior to application of the inkjet ink to improve print properties, such as ink adhesion. The parameters of such substrate surface treatments may vary widely depending on the substrate material being printed, the particular inkjet ink being utilized, the printing method being applied, and the desired properties and use of the print.
[0095] The following examples are intended to further illustrate the ink-jet inks, but are not intended to limit the scope of the claims. EXAMPLES
[0096] Inkjet ink Some examples of inkjet inks are shown below in Tables 1 and 2. The amount of each component is expressed as a weight percentage relative to the total weight (100%) of the inkjet ink. * indicates that the example is a comparative example.
[0097] Materials used Glycol ether PnP is propylene glycol mono-n-propyl ether (boiling point 150°C). Glycol ether DPnP is dipropylene glycol mono-n-propyl ether (boiling point 212°C). PICCOLYTE A135 is a terpene resin made from alpha-pinene (Ring Ball SP = 132-138°C, Bromine Number = 27) available from Pinova. PICCOLYTE S25 is a terpene resin made from beta-pinene (Ring Ball SP = 22-28°C, Bromine Number = 19) available from Pinova. DERTOPHENE T is a terpene phenolic resin (OHV = 40 mg KOH / g) available from Pinova. FORAL AX is a rosin resin (hydrogenated acidic wood rosin) available from Pinova. KF-6011 (PEG-11 Dimethicone, methyl ether blocked, HLB=14.5), KF-6013 (PEG-9 Dimethicone, unblocked, HLB=10.0), KF-6015 (PEG-3 Dimethicone, unblocked, HLB=4.5), KF-6017 (PEG-10 Dimethicone, unblocked, HLB=4.5), and KF-6038 (Lauryl PEG-9 Polydimethylsiloxyethyl Dimethicone, unblocked, HLB=3.0) are polyether modified silicones available from Shin-Etsu Chemical Co., Ltd. BYK-3550 is a silicone acrylate copolymer available from BYK Japan Co., Ltd. OIL BLACK 860 is an organic dye available from Orient Chemical Industries Co., Ltd.
[0098] [Table 1]
[0099] [Table 2]
[0100] Preparation method To prepare the example inks, the resin(s) and any surfactants were first combined with methyl ethyl ketone (MEK) and mixed by a mechanical stirrer for at least 30 minutes. Acetone or glycol ether was then added to the mixture and mixed for at least 15 minutes. The dye was then added to the mixture and mixed for at least 30 minutes to obtain the inkjet inks. The example inkjet inks were then evaluated with a FUNAI TIJ cartridge manufactured by Funai Electric Co., Ltd.
[0101] Resin softening point (SP) value An example of a method for determining the softening point of a resin is as follows: 2.1 g of a molten sample is poured into a given ring, and then the sample is cooled to room temperature, after which the SP value is measured under the following conditions specified in JIS B7410. Measuring device: automatic ring and ball softening point Testing machine: ASP-MGK2 (manufactured by MEITECH Company Ltd.) Heating rate: 5℃ / min Start heating temperature: 40℃ Measurement solvent: glycerol.
[0102] Inkjet ink evaluation method Print sample creation The inks were evaluated using thermal printing technology associated with Funai Electric Co., Ltd. (software and hardware from XiJet, carrier stage from Kirk Rudy).
[0103] Drying time evaluation The printing conditions utilized to evaluate the dry times were as follows: - Printing substrate: varnished paper - Print resolution: 600dpi x 300dpi (vertical x horizontal) - Print speed: 100 feet per minute - Prefire 260nsec - Dead time 1200nsec - Main fire 500nsec - Voltage 9.0V - Temperature 30℃ - Printing image: 100% duty (1cm x 10cm, monochrome bitmap, solid block image) (see Figure 1 for example).
[0104] The rub test was performed with a finger after a specific time (10 seconds, 20 seconds, and 30 seconds). A colored finger indicates that not enough time has passed for complete drying ("fail"), whereas a non-colored finger indicates that enough time has passed for complete drying ("pass"). The inkjet inks were then scored according to the drying time required to achieve a "pass" rating according to Table 3 below.
[0105] [Table 3]
[0106] Decap Time Evaluation The printing conditions used to evaluate the decap time were as follows: - Printing substrate: Plain (uncoated) paper - Print resolution: 300dpi x 300dpi (vertical x horizontal) - Print speed: 100 feet per minute - Prefire 260nsec - Dead time 1200nsec - Main fire 500nsec - Voltage 9.0V - Temperature 30℃ - Print image: 100% duty (1mm x 1cm, monochrome bitmap, fine line image) (see Figure 2 for an example).
[0107] Fine line images were printed to verify that the printed image contained no missing or unclear lines (a precursor to clogged or missing nozzles). After verification, the printhead was left decapped for a specified time (30 seconds, 1 minute, or 60 minutes) and then reprinted using the same fine line image. The reprinted fine line image (after the specified time) was checked to see if any missing lines / loss of line clarity had occurred. If no missing lines / loss of line clarity occurred in the time interval tested, the inkjet ink was given a decap score of "Good" for that time interval. If 1-2 lines were missing / lost clarity in the time interval tested, but not enough to significantly affect the clarity or readability of the fine line image, the inkjet ink was given a decap score of "Acceptable" for the time interval tested. If more than 2 lines were missing / lost clarity in the time interval tested, the inkjet ink was classified as "Poor" for that time interval. A suitable / desirable inkjet ink is one that achieves a decap classification of "good" or "acceptable" when decapped (i.e., exposed to air) over one or more of the time intervals tested.
[0108] Image clarity assessment The printing conditions used to evaluate image clarity were as follows: - The printing substrates used to determine image clarity were plain (uncoated) paper, varnished paper, biaxially oriented polypropylene, nylon, and aluminum foil. - Print resolution: 300dpi x 300dpi (vertical x horizontal) - Print speed: 100 feet per minute - Prefire 260nsec - Dead time 1200nsec - Main fire 500nsec - Voltage 9.0V - Temperature 30℃ - Print image: 100% duty (see Figure 3 and Figure 4 for example) 1mm x 12.7mm, monochrome bitmap, thin line image, A string of numbers that reads "123456789".
[0109] Fine line images and number strings were printed on a porous control substrate (plain uncoated paper) and on a series of non-porous substrates: varnish-coated paper, biaxially oriented polypropylene, nylon, and aluminum foil. The resulting printed images were visually evaluated for spreading on each substrate according to the evaluation criteria in Table 4 below.
[0110] [Table 4]
[0111] The results from the above evaluations for each substrate were then compiled, and the inkjet inks were then given an image clarity rating of "good," "acceptable," or "poor" according to the rating system in Table 5 below.
[0112] [Table 5]
[0113] Gloss rating After complete drying, the printed image samples from the dry time measurements were visually inspected for gloss and classified as "high" gloss, "medium" gloss, or "low" gloss.
[0114] Inkjet ink performance As shown in Tables 6 and 7 below, inkjet inks formulated with polyether modified silicones and methyl ethyl ketones having HLB values of 1 to 12 were found to have image clarity ratings of "acceptable" or "good" (Examples 3 to 11, 13 to 15, 17 to 19). In contrast, an inkjet ink without surfactant (Example 1), an inkjet ink containing polyether modified silicones with too high HLB values (Example 2, using a polyether modified silicone surfactant with an HLB value of 14.5), an inkjet ink containing silicone acrylate copolymers (Example 12, using BYK-3550 as the surfactant), or an inkjet ink replacing MEK with another low boiling point solvent (Example 16, using ethanol), were found to result in unacceptable images in terms of image clarity, respectively (see Tables 6 and 7).
[0115] [Table 6]
[0116] [Table 7]
[0117] With regard to the amount of polyether modified silicone with HLB value of 1-12, even very low loadings were found to be sufficient to obtain acceptable image clarity (Example 5, 0.001 wt% loading of polyether modified silicone). Higher loadings of polyether modified silicone, such as 1 wt% in Example 9 and 3 wt% in Example 10, also provided desired image clarity, but 3 wt% loading of polyether modified silicone began to affect early decap time (Table 6, Example 10). Nevertheless, 3 wt% loading of polyether modified silicone in Example 10 performed satisfactorily at the longest decap time tested, 60 minutes.
[0118] As seen in Tables 6 and 7, when polyether modified silicones having HLB values of 1 to 12 were used in combination with terpene resins and methyl ethyl ketone, significant effects were achieved in terms of image clarity, drying time, and decap time (Examples 3 to 11, 15, and 17 to 19).
[0119] On the other hand, inkjet inks in which the terpene resin was replaced with a terpene phenolic resin (Example 13), or inkjet inks using only rosin resin (Example 14), suffered unacceptable decap times at all decap times tested (Table 7).
[0120] In addition to solvent systems based on mixtures of MEK and acetone (Examples 3-11, and 15), the use of MEK alone (Example 19) or MEK in combination with glycol ethers (Examples 17 and 18) can produce inkjet inks with desirable decap times, although the inks prepared using the combination of MEK and glycol ethers resulted in slightly longer drying times.
[0121] Where numerical limits or ranges are stated herein, the endpoints are included, and all values and subranges within the numerical limit or range are specifically included, as if expressly written.
[0122] As used herein, the words "a" and "an" and the like mean "one or more."
[0123] The present disclosure also contemplates other embodiments that "comprising," "consisting of," and "consisting essentially of" the embodiments or elements presented herein, whether or not explicitly stated.
[0124] Obviously, numerous modifications and variations of the present invention are possible in light of the above teachings, and it is therefore to be understood that, within the scope of the appended claims, the invention may be practiced otherwise than as specifically described herein.
[0125] All patents and other references cited above are incorporated herein by reference in their entirety as if fully set forth herein.
Claims
1. (A) a terpene resin; (B) (B1) a solvent system comprising methyl ethyl ketone; (C) a polyether-modified silicone having a hydrophilic-lipophilic balance (HLB) value of 1 to 12; 1. An inkjet ink comprising:
2. The ink-jet ink of claim 1, wherein the terpene resin (A) is a homopolymer of α-pinene.
3. The ink-jet ink of claim 1 or 2, wherein the terpene resin (A) is present in an amount of 0.1 to 10 wt %, based on the total weight of the ink-jet ink.
4. 4. The ink-jet ink according to claim 1, wherein the weight ratio ((B1):(A)) of the methyl ethyl ketone (B1) to the terpene resin (A) is 10:1 to 100:
1.
5. The ink-jet ink according to any one of claims 1 to 4, wherein the solvent system (B) further comprises (B2) acetone.
6. 6. The ink-jet ink according to claim 5, wherein the weight ratio of the methyl ethyl ketone (B1) to the acetone (B2) ((B1):(B2)) is from 1:1 to 5:
1.
7. The ink-jet ink of any of the preceding claims having a total ketone content of at least 50% by weight, based on the total weight of the ink-jet ink.
8. The ink-jet ink according to any one of claims 1 to 7, wherein the solvent system (B) further comprises (B3) a glycol ether.
9. 9. The ink-jet ink of claim 1, which is substantially free of a solvent having a boiling point higher than 175°C.
10. The ink-jet ink according to any one of claims 1 to 9, wherein the polyether-modified silicone (C) is a block copolymer having a pendant graft structure.
11. The ink-jet ink of any of the preceding claims, wherein the polyether modified silicone (C) is present in an amount of 0.001 to 4 wt %, based on the total weight of the ink-jet ink.
12. The ink-jet ink according to any one of claims 1 to 11, further comprising (D) a rosin resin.
13. The ink-jet ink of claim 12, wherein the rosin resin (D) is present in an amount of up to 10 wt%, based on the total weight of the ink-jet ink.
14. The ink-jet ink according to any one of claims 1 to 13, further comprising (E) a colorant.
15. 1. A method for forming a printed image on a substrate, comprising: applying an inkjet ink according to any one of claims 1 to 14 onto the substrate using a thermal inkjet printhead; drying the inkjet ink; and A method comprising:
Citation Information
Patent Citations
Marking ink for jet printer
JP1993163448A
Marking ink for jet printer
JP1993163449A
Ink for jet printer
JP1994057188A
Ink for jet printer
JP1997176531A
Ink for jet printer
JP1998140060A