Ozone generation electrodes
A titanium-based electrode with a catalyst layer of tin, antimony, and nickel oxides addresses the challenge of stable ozone generation in neutral solutions, enhancing efficiency and durability through a specific coating and heat treatment process.
Patent Information
- Application Number
- JP2024530730
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-06-27
- Filing Date
- 2023-06-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-21
AI Technical Summary
Existing methods for generating ozone in neutral aqueous solutions, such as city water, face challenges in achieving stable and efficient ozone generation and durability due to the use of acidic electrolytes.
A titanium-based electrode coated with a catalyst layer composed of 79.0 mol% to 90.0 mol% tin oxide, 7.0 mol% to 17.0 mol% antimony oxide, and 0.1 mol% to 6.0 mol% nickel oxide, formed by mixing solutions of these oxides in lower alcohols and applying them to a titanium substrate, followed by heat treatment, to enhance ozone generation efficiency and durability.
The electrode achieves high ozone generation efficiency and excellent durability in neutral aqueous solutions, with an electric double layer capacitance of 2 to 40 mC/cm², improving catalyst utilization and reducing load per unit area.
Smart Images

Figure 0007579556000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an ozone generating electrode used for generating ozone water. [Background technology]
[0002] Hypochlorous acid sterilizing water, which uses chlorine generated by electrolysis of water, is used in many fields. However, in some areas, there is a problem that chlorine is not contained in city water, and salt must be added before electrolysis. As a result, ozone water, which uses ozone as a substance with stronger sterilizing power than hypochlorous acid, has attracted attention. There are currently two main methods for generating ozone water. One method is to generate ozone by discharging ozone such as silent discharge, and then dissolve it in water to obtain ozone water. The other method is to electrolyze water, where the ozone generated by the reaction at the anode is dissolved in the water, which is the electrolyte, and ozone water is obtained.
[0003] In the former case, there is a problem that ozone in the gas phase does not easily dissolve in water, making it difficult to adjust the concentration, whereas in the latter case, ozone water can be generated directly by electrolysis, making it easy to adjust the concentration by changing the electrolysis conditions.
[0004] Concerning a method for electrolyzing water, Non-Patent Document 1 discloses that ozone is generated by electrolysis in an acidic aqueous sulfuric acid solution using a platinum wire electrode as the anode. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Electrochemistry and Industrial Physical Chemistry, 54(10), p890-895, 1986 Summary of the Invention [Problem to be solved by the invention]
[0006] The method of Non-Patent Document 1 uses an acidic aqueous sulfuric acid solution as an electrolyte. Therefore, there is a strong demand for an electrode that can stably generate ozone in a neutral aqueous solution such as city water, which is easier to handle than sulfuric acid.
[0007] An object of the present invention is to provide an electrode for ozone generation which has excellent ozone generation efficiency even in a neutral aqueous solution such as city water, and which has excellent durability. [Means for solving the problem]
[0008] The inventors discovered that by providing a catalyst layer consisting of 79.0 mol % to 90.0 mol % tin oxide, 7.0 mol % to 17.0 mol % antimony oxide, and 0.1 mol % to 6.0 mol % nickel oxide, calculated as metals, on a substrate made of titanium or a titanium alloy, an electrode with high ozone generation efficiency in city water and excellent durability can be obtained, and thus completed the present invention.
[0009] That is, the above objective is to provide an electrode for electrolysis. An electrode substrate made of titanium or a titanium alloy; A catalyst layer is provided on the electrode substrate and is composed of, in terms of metal, 79.0 mol % to 90.0 mol % of tin oxide, 7.0 mol % to 17.0 mol % of antimony oxide, and 0.1 mol % to 6.0 mol % of nickel oxide. This is achieved by an ozone generating electrode characterized by the above.
[0010] The above-mentioned ozone generating electrodes have an electric double layer capacitance of 2 to 40 (mC / cm 2 ).
[0011] In addition, the above objectives are: A solution of tin oxide particles and antimony oxide particles dispersed in lower alcohol was mixed with a solution of nickel compound dissolved in lower alcohol, The mixture is applied to a titanium substrate, dried, and then heat-treated at 300°C to 700°C in air to obtain an electrode for ozone generation.
[0012] According to the present invention, it is possible to provide an ozone generating electrode that has excellent ozone generating efficiency even in a neutral aqueous solution such as city water and has excellent durability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention provides An electrode substrate made of titanium or a titanium alloy; The electrode for ozone generation is characterized by comprising a catalyst layer provided on the electrode substrate and containing, in terms of metals, 79.0 mol % to 90.0 mol % tin oxide, 7.0 mol % to 17.0 mol % antimony oxide, and 0.1 mol % to 6.0 mol % nickel oxide.
[0014] In addition, the manufacturing method of the ozone generating electrode of the present invention is characterized in that a solution in which tin oxide particles and antimony oxide particles are dispersed in a lower alcohol is mixed with a solution in which a nickel compound is dissolved in a lower alcohol, the mixture is then coated and dried on a titanium substrate, and the coated and dried titanium substrate is then heat-treated in air at 300°C to 700°C.
[0015] In the above, a mixed liquid may be prepared by mixing a solution in which tin oxide particles are dispersed in a lower alcohol, a solution in which antimony oxide particles are dispersed in a lower alcohol, and a solution in which a nickel compound is dissolved in a lower alcohol.
[0016] Alternatively, the mixture may be applied to a titanium substrate that has been degreased and roughened with an acid, dried, and the coated and dried titanium substrate may then be heat-treated at 300°C to 700°C in air.
[0017] The ozone generating electrode and the method for producing the same of the present invention will be described below.
[0018] <Electrode base> Examples of the material of the electrode substrate used in the present invention include titanium and titanium-based alloys. As the titanium-based alloy, a corrosion-resistant conductive alloy mainly made of titanium is used, and examples thereof include Ti-based alloys that are usually used as electrode materials and are made of combinations of Ti-Ta-Nb, Ti-Zr, Ti-Al, etc. These electrode materials can be processed into desired shapes such as plate, perforated plate, rod, mesh plate, etc. and used as electrode substrates.
[0019] <Pretreatment of electrode substrate> It is desirable to pretreat the electrode substrate as described above in advance, as is usually done. Specific examples of suitable pretreatments include the following. First, the surface of the electrode substrate (hereinafter sometimes referred to as "titanium substrate") made of titanium or a titanium-based alloy as described above is washed with, for example, alcohol, acetone, etc. and / or degreased by electrolysis in an alkaline solution according to a conventional method, and then treated with hydrofluoric acid having a hydrogen fluoride concentration of 1 to 20% by weight or a mixed acid of hydrofluoric acid and other acids such as nitric acid or sulfuric acid, thereby removing the oxide film on the titanium substrate surface and roughening the titanium grain boundary unit. The acid treatment can be carried out at room temperature to about 40°C for several minutes to 10-odd minutes depending on the surface condition of the titanium substrate. Note that blasting treatment may be used in combination to achieve sufficient roughening.
[0020] <Hydrogenated Titanium Treatment> The surface of the titanium substrate thus treated with acid is brought into contact with concentrated sulfuric acid, so that the inner surface of the titanium grain boundaries is roughened finely in the form of protrusions, and a thin layer of titanium hydride is formed on the surface of the titanium substrate. The concentrated sulfuric acid used is generally at a concentration of 40 to 80% by weight, preferably 50 to 60% by weight, and a small amount of sodium sulfate or other sulfates may be added to this concentrated sulfuric acid, if necessary, for the purpose of stabilizing the treatment. The contact with the concentrated sulfuric acid is generally carried out by immersing the titanium substrate in a bath of concentrated sulfuric acid, and the bath temperature is generally within a range of about 100 to about 150°C, preferably about 110 to about 130°C, and the immersion time is generally about 0.5 to about 10 minutes, preferably about 1 to about 3 minutes, which is sufficient. This sulfuric acid treatment makes it possible to roughen the inner surface of the titanium grain boundaries finely in the form of protrusions, and to form a very thin coating of titanium hydride on the surface of the titanium substrate. The titanium substrate treated with sulfuric acid is removed from the sulfuric acid bath and is then rapidly cooled, preferably in an inert gas atmosphere such as nitrogen or argon, to reduce the surface temperature of the titanium substrate to below about 60° C. For this rapid cooling, it is appropriate to use a large amount of cold water, which also serves as washing water.
[0021] The titanium substrate thus formed with a very thin titanium hydride coating layer on its surface is immersed in dilute hydrofluoric acid or a dilute fluoride aqueous solution (e.g., an aqueous solution of sodium fluoride, potassium fluoride, etc.) to grow the titanium hydride coating and to make the coating uniform and stable. The concentration of hydrogen fluoride in the dilute hydrofluoric acid or dilute fluoride aqueous solution that can be used here can be generally within the range of 0.05 to 3% by weight, preferably 0.3 to 1% by weight, and the temperature during the immersion treatment with these solutions can be generally within the range of 10 to 40°C, preferably 20 to 30°C. The treatment can be carried out until a uniform titanium hydride coating having a thickness of generally 0.5 to 10 microns, preferably 1 to 3 microns, is formed on the surface of the titanium substrate. This titanium hydride (TiHy, where y is a number between 1.5 and 2) exhibits a gray-brown to blackish brown color depending on the degree of hydrogenation, so the production of a titanium hydride coating having a thickness within the above range can be empirically controlled by comparing the change in color tone of the substrate surface with its brightness in comparison with a standard color source.
[0022] <Formation of catalyst layer> Next, a mixture of a solution in which tin oxide particles and antimony oxide particles are dispersed in a lower alcohol and a solution in which a nickel compound is dissolved in a lower alcohol is applied to the pretreated titanium substrate, dried, and heat-treated (fired) to form a catalyst layer consisting of tin oxide, antimony oxide, and nickel oxide.
[0023] In the above, a mixed liquid may be prepared by mixing a solution in which tin oxide particles are dispersed in a lower alcohol, a solution in which antimony oxide particles are dispersed in a lower alcohol, and a solution in which a nickel compound is dissolved in a lower alcohol.
[0024] As the solvent for the above solution, a lower alcohol is suitable, and for example, methanol, ethanol, propanol, butanol, isobutanol, or a mixture thereof is advantageously used. In addition, when fine tin oxide particles and fine antimony oxide particles are contained, a dispersant may be added. As the dispersant, acetylacetone, alkyl ether carboxylic acid, etc. can be used.
[0025] The total metal concentration of the tin compound, antimony compound, and nickel compound in the lower alcohol solution can generally be within the range of 20 to 300 g / L, preferably 40 to 290 g / L. If the metal concentration is lower than 20 g / L, the catalyst loading efficiency will be poor, and if it exceeds 300 g / L, the catalyst will be prone to segregation, resulting in problems such as catalytic activity, adhesion strength, and non-uniform loading amount.
[0026] The titanium substrate with the solution applied to its surface is dried at a temperature within the range of about 20 to about 150°C as necessary, and then heat-treated in an oxygen-containing gas atmosphere, for example, in air. The heat treatment can be carried out in an appropriate heating furnace, such as an electric furnace, gas furnace, or infrared furnace, by heating to a temperature of 300°C or higher at which each metal compound is generally decomposed and each metal forms a stable oxide, but at a temperature (700°C or lower) at which the oxidation of the titanium substrate does not grow too thick. The heating time can be about 3 to 30 minutes, depending on the size of the substrate to be heat-treated. This heat treatment allows metal oxides consisting of tin oxide, antimony oxide, and nickel oxide to be formed and supported on the titanium surface.
[0027] Furthermore, if a sufficient amount of metal oxide consisting of tin oxide, antimony oxide, and nickel oxide cannot be formed and supported in a single support operation, the above-mentioned process of applying the solution, drying, and heat treating can be repeated as many times as desired.
[0028] The ratio of each component in the catalyst layer made of tin oxide, antimony oxide, and nickel oxide is 79.0 mol% to 90.0 mol% for tin oxide, 7.0 mol% to 17.0 mol% for antimony oxide, and 0.1 mol% to 6.0 mol% for nickel oxide, calculated as metal. The ratio of each component is 100% in total.
[0029] Here, in another embodiment, the proportion of the tin oxide can be more than 79.0 mol % and less than 90.0 mol % in terms of metal. In still another embodiment, the proportion of the tin oxide can be 80.0 mol % to 89.7 mol % in terms of metal. In still another embodiment, the proportion of the tin oxide can be 81.0 mol % to 89.5 mol % in terms of metal. In still another embodiment, the proportion of the tin oxide can be 82.0 mol % to 89.0 mol % in terms of metal. If the proportion of the tin oxide is less than 79.0 mol % or exceeds 90.0 mol %, the durability of the catalyst layer becomes insufficient.
[0030] In another embodiment, the proportion of the antimony oxide can be 7.6 mol% to 16.0 mol% in terms of metal. In another embodiment, the proportion of the antimony oxide can be 8.0 mol% to 15.0 mol% in terms of metal. If the proportion of the antimony oxide is less than 7.0 mol% or exceeds 17.0 mol%, the durability of the catalyst layer becomes insufficient.
[0031] In another embodiment, the proportion of the nickel oxide may be 0.2 mol % to 5.5 mol % in terms of metal. In another embodiment, the proportion of the nickel oxide may be 0.4 mol % to 2 mol % in terms of metal. If the proportion of the nickel oxide is less than 0.1 mol % or exceeds 6.0 mol %, the durability of the catalyst layer becomes insufficient.
[0032] In the manufacturing method of the present invention, a solution in which fine tin oxide particles and fine antimony oxide particles are dispersed, or a solution in which fine tin oxide particles are dispersed in a lower alcohol and a solution in which fine antimony oxide particles are dispersed in a lower alcohol, are used, and the catalyst layer is obtained by coating, drying, and then heat treatment. The average particle size of the tin oxide particles and antimony oxide particles used here is 10 to 300 nm, preferably 40 to 150 nm.
[0033] The ozone generating electrode of the present invention has an electric double layer capacitance of 2 to 40 (mC / cm 2 ).
[0034] The method for producing an ozone generating electrode of the present invention involves mixing a solution in which tin oxide particles and antimony oxide particles are dispersed in a lower alcohol (or a solution in which tin oxide particles are dispersed in a lower alcohol and a solution in which antimony oxide particles are dispersed in a lower alcohol) with a solution in which a nickel compound is dissolved in a lower alcohol, applying the mixture onto a titanium substrate and drying it, and then heat-treating the coated and dried titanium substrate in air at 300°C to 700°C. Increasing the number of steps of applying, drying and heat-treating the solution to thicken the catalyst layer also increases the electric double layer capacity. By setting the number of steps of applying, drying and heat-treating to a number ranging from a few layers to around 20 layers, the electric double layer capacity can be increased to a value of 2 to 40 (mC / cm 2 ) can be used. In order to further stabilize the catalyst layer, a post-treatment step may be added in the atmosphere at 500°C to 700°C for 2 to 20 hours. The treatment time may be 4 to 18 hours. For example, the post-treatment may be performed in the atmosphere at 550°C for 16 hours.
[0035] The ozone generating electrode of the present invention has an electric double layer capacitance of 3 to 30 (mC / cm 2 ) is preferred.
[0036] The electrode produced by the manufacturing method of the present invention is characterized by an extremely large electric double layer capacity. (1) The electric double layer capacity is positively correlated with the surface area of the electrode. It is considered that the larger the electric double layer capacity of an electrode is, the larger the surface area of the catalyst layer is. (2) When the electric double layer capacity is large, i.e., the surface area of the catalyst layer is large, the catalyst utilization rate is high. It is presumed that a high catalyst utilization rate leads to improved activity because many catalytic active sites are involved in the reaction, and also leads to improved durability because the load per unit area is reduced. EXAMPLES
[0037] The present invention will be specifically described with reference to examples, but the present invention is not limited to these examples.
[0038] [Example 1] A coating solution was prepared by adding 0.012 g of an ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) to 1 g of an isobutanol solution (Sn concentration = 197 g / kg, Sb concentration = 32 g / kg) in which tin dioxide particles and antimony pentoxide particles were dispersed, and irradiating the solution with 31 kHz ultrasound for 10 minutes. The average particle size of the tin dioxide particles and antimony pentoxide particles in the butanol solution used here was measured with a laser diffraction / scattering type particle size distribution measuring device and was found to be 146 nm. Next, a titanium plate (t0.5mm x 100mm x 50mm) equivalent to JIS Class 1 was immersed in acetone and ultrasonically cleaned for 10 minutes to degrease it, then treated in 8% by weight hydrofluoric acid at 20°C for 1 minute, and then treated in a 60% by weight aqueous sulfuric acid solution at 120°C for 1 minute. The titanium substrate was then treated in 0.3% by weight hydrofluoric acid at 20°C for 45 seconds. 0.13 mL of the coating solution was applied onto the surface-treated titanium substrate, which was then dried at room temperature for 5 minutes and then treated in air at 550° C. for 5 minutes. The above process was repeated six times to prepare an electrode of Example 1 in which metal oxides consisting of 86.0 mol % tin oxide, 13.5 mol % antimony oxide, and 0.5 mol % nickel oxide were supported on the titanium substrate in terms of metal.
[0039] [Example 2] An electrode of Example 2 was prepared in the same manner as in Example 1, except that the amount of ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) added was changed to 0.023 g. In this embodiment, a metal oxide consisting of 85.6 mol % tin oxide, 13.5 mol % antimony oxide, and 0.9 mol % nickel oxide was supported on a titanium substrate.
[0040] [Example 3] An electrode of Example 3 was prepared in the same manner as in Example 1, except that the amount of ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) added was changed to 0.047 g. In this embodiment, a metal oxide consisting of 84.7 mol % tin oxide, 13.4 mol % antimony oxide, and 1.9 mol % nickel oxide was supported on a titanium substrate.
[0041] [Example 4] An electrode of Example 4 was prepared in the same manner as in Example 1, except that the amount of ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) added was changed to 0.071 g. In this embodiment, a metal oxide consisting of 83.9 mol % tin oxide, 13.3 mol % antimony oxide, and 2.8 mol % nickel oxide was supported on a titanium substrate.
[0042] [Example 5] An electrode of Example 5 was prepared in the same manner as in Example 1, except that the amount of ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) added was changed to 0.096 g. In this embodiment, a metal oxide consisting of 83.0 mol % tin oxide, 13.2 mol % antimony oxide, and 3.8 mol % nickel oxide was supported on a titanium substrate.
[0043] [Example 6] A coating solution was prepared by adding 0.062 g of an ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) to 1 g of an isobutanol solution (Sn concentration = 256 g / kg, Sb concentration = 27 g / kg) in which tin dioxide particles and antimony pentoxide particles were dispersed, and irradiating the solution with 31 kHz ultrasound for 10 minutes. The average particle size of the tin dioxide particles and antimony pentoxide particles in the butanol solution used here was measured with a laser diffraction / scattering type particle size distribution measuring device and was found to be 146 nm. Next, a titanium plate (t0.5mm x 100mm x 50mm) equivalent to JIS Class 1 was immersed in acetone and ultrasonically cleaned for 10 minutes to degrease it, then treated in 8% by weight hydrofluoric acid at 20°C for 1 minute, and then treated in a 60% by weight aqueous sulfuric acid solution at 120°C for 1 minute. The titanium substrate was then treated in 0.3% by weight hydrofluoric acid at 20°C for 45 seconds. 0.13 mL of the coating solution was applied onto the surface-treated titanium substrate, which was then dried at room temperature for 5 minutes and then treated in air at 550° C. for 5 minutes. The above steps were repeated six times, and finally, as a post-treatment step, treatment was performed in air at 550°C for 16 hours to produce an electrode of Example 6 in which a metal oxide consisting of 88.9 mol % tin oxide, 9.1 mol % antimony oxide, and 2.0 mol % nickel oxide was supported on the titanium substrate.
[0044] [Example 7] An electrode of Example 7 was prepared in the same manner as in Example 6, except that the amount of ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) added was changed to 0.159 g. In this embodiment, a metal oxide consisting of 86.2 mol % tin oxide, 8.8 mol % antimony oxide, and 5.0 mol % nickel oxide was supported on a titanium substrate.
[0045] [Example 8] The electrode of Example 9 was prepared in the same manner as in Example 6, except that the coating and baking process was performed 21 times. The electrode had a metal oxide supported on a titanium substrate, the metal oxide consisting of 88.9 mol % tin oxide, 9.1 mol % antimony oxide, and 2.0 mol % nickel oxide.
[0046] [Example 9] An electrode of Example 10 was prepared in the same manner as in Example 6, except that the temperature in the post-treatment process was 650°C, in which a metal oxide consisting of 88.9 mol % tin oxide, 9.1 mol % antimony oxide, and 2.0 mol % nickel oxide was supported on a titanium substrate.
[0047] [Comparative Example 1] A JIS Class 1 titanium plate (t 0.5 mm × 100 mm × 100 mm) was immersed in acetone and ultrasonically cleaned for 10 minutes to degrease it, then treated in 8 wt% hydrofluoric acid at 20°C for 2 minutes, and then treated in a 60 wt% aqueous sulfuric acid solution at 120°C for 3 minutes. The titanium substrate was then removed from the aqueous sulfuric acid solution and quenched by spraying cold water in a nitrogen atmosphere. It was then immersed in a 0.3 wt% aqueous hydrofluoric acid solution at 20°C for 2 minutes and then rinsed with water. After rinsing the titanium substrate with water, it was electroplated in a platinum plating bath adjusted to a platinum content of 5 g / L, pH ≒ 2, and 50°C by dissolving dinitrodiammine platinum in the sulfuric acid solution, and platinum was deposited at 6.5 mg / cm.2 An electrode of Comparative Example 1 was prepared in which the metal was supported.
[0048] [Comparative Example 2] A coating solution was prepared by adding 14.770 g of tin (IV) chloride pentahydrate, 0.620 g of antimony (III) oxide, and 0.107 g of nickel (II) chloride hexahydrate to 34.5 g of ethanol and stirring the mixture. Next, a titanium plate (t0.5mm x 100mm x 100mm) equivalent to JIS Class 1 was immersed in acetone and ultrasonically cleaned for 10 minutes to degrease it, after which it was treated for 1 minute in 8% by weight hydrofluoric acid at 20°C, and then for 1 minute in a 60% by weight aqueous sulfuric acid solution at 120°C. The titanium substrate was then treated for 45 seconds in 0.3% by weight hydrofluoric acid at 20°C. 0.24 mL of the coating solution was applied onto the surface-treated titanium substrate, which was then dried at room temperature for 10 minutes and then treated in air at 550° C. for 10 minutes. The above process was repeated 14 times to prepare an electrode of Comparative Example 2 in which metal oxides consisting of 93.0 mol % tin oxide, 6.0 mol % antimony oxide, and 1.0 mol % nickel oxide were supported on the titanium substrate in terms of metal.
[0049] [Comparative Example 3] A coating solution was prepared by adding 0.009 g of an ethanol solution of nickel (II) chloride hexahydrate (Ni concentration = 46 g / kg) to 1 g of an isobutanol solution (Sn concentration = 256 g / kg, Sb concentration = 27 g / kg) in which tin dioxide particles and antimony pentoxide particles were dispersed, and irradiating with 31 kHz ultrasound for 10 minutes. The average particle size of the tin dioxide particles and antimony pentoxide particles in the butanol solution used here was measured with a laser diffraction / scattering type particle size distribution measuring device and was found to be 146 nm. Next, a titanium plate (t0.5mm x 100mm x 50mm) equivalent to JIS Class 1 was immersed in acetone and ultrasonically cleaned for 10 minutes to degrease it, then treated in 8% by weight hydrofluoric acid at 20°C for 1 minute, and then treated in a 60% by weight aqueous sulfuric acid solution at 120°C for 1 minute. The titanium substrate was then treated in 0.3% by weight hydrofluoric acid at 20°C for 45 seconds. 0.13 mL of the coating solution was applied onto the surface-treated titanium substrate, which was then dried at room temperature for 5 minutes and then treated in air at 550° C. for 5 minutes. The above process was repeated six times, and without performing a post-treatment process, an electrode of Comparative Example 3 was produced in which a metal oxide consisting of 90.5 mol % tin oxide, 9.2 mol % antimony oxide, and 0.3 mol % nickel oxide was supported on a titanium substrate.
[0050] <Ozone generation efficiency> Electrolysis was performed under the following conditions using Examples 1 to 5 and Comparative Examples 1 and 2 as the anode, and the ozone generation efficiency was determined. The electrolyte used was 150 ml of an aqueous solution containing 0.25 mmol of MgSO4, 0.25 mmol of NaHCO3, 0.25 mmol of CaCl2, and 0.025 mmol of KHCO3 per 1 L. The current density was 2 A / dm 2 Electrolysis was performed for 120 seconds under constant current control at 1000V. The amount of ozone generated was then measured using the indigo method, and the ozone generation efficiency was calculated.
[0051] <Durability test> Using each of the electrodes of Examples 1 to 5 and Comparative Examples 1 to 2 as anodes, durability tests were carried out under the following conditions: The ozone generation efficiency of Examples 1 to 5 and Comparative Examples 1 and 2 was determined by the above method before and during the durability test. The results are shown in Table 1. The electrolyte used was 150 ml of an aqueous solution containing 0.25 mmol of MgSO4, 0.25 mmol of NaHCO3, 0.25 mmol of CaCl2, and 0.025 mmol of KHCO3 per 1 L. The current density was 2 A / dm 2 Electrolysis was performed under constant current control.
[0052] <Method for measuring electric double layer capacitance> Cyclic voltammetry (CV) measurements were performed using a three-electrode electrolytic cell, and the electric double layer capacity was calculated from the obtained cyclic voltammogram. Specifically, CV measurements were performed in 0.5 M sulfuric acid, using the electrodes (20 × 25 mm) from the examples and comparative examples as the working electrodes, a silver-silver chloride electrode as the reference electrode, and a Pt plate as the counter electrode, with the potential range of 0.8 to 1.3 V (vs. Ag / AgCl) and a scan rate of 50 mV / s. Half the sum of the charge and discharge electrical quantities of the obtained electric double layer was calculated, and this was then applied to an electrode with an area of 5 cm. 2 The electric double layer capacity of the electrode was calculated by dividing the electric double layer capacity (mC / cm 2 ) are listed in Table 1.
[0053] [Table 1]
Claims
1. An electrode substrate made of titanium or a titanium alloy; a catalyst layer provided on the electrode substrate, the catalyst layer being composed of, in terms of metal, 79.0 mol % to 90.0 mol % of tin oxide, 7.0 mol % to 17.0 mol % of antimony oxide, and 0.9 mol % (excluding 0.9 mol %) to 6.0 mol % of nickel oxide; An electrode for generating ozone.
2. The electric double layer capacitance is 2 to 40 (mC / cm 2 2. The electrode for generating ozone according to claim 1, characterized in that
3. A solution in which tin oxide particles and antimony oxide particles are dispersed in a lower alcohol is mixed with a solution in which a nickel compound is dissolved in a lower alcohol, 3. The method for producing an electrode for ozone generation according to claim 1, wherein the mixed solution is applied onto a titanium substrate, dried, and then heat-treated at 300° C. to 700° C. in air.
Citation Information
Patent Citations
Electrocatalyst, electrode coating and electrode for preparation of chlorine
JP2014151323A