Thermoforming of fiberboard.
The thermoforming of a laminate of polyester and polyolefin fibers forms micropores naturally, addressing the challenges of pore blocking and cumbersome micropore creation in polyester resin films, resulting in improved sound absorption.
Patent Information
- Application Number
- JP2020135293
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-08-07
AI Technical Summary
Conventional methods of creating micropores in polyester resin films for sound absorption are cumbersome and prone to pore blocking during heat-molding, leading to suboptimal sound absorption characteristics in molded articles.
A thermoforming process is applied to a laminate of specific nonwoven bodies, including polyester and polyolefin fibers, where polyolefin fibers melt along core-sheath composite fibers to form micropores without pre-drilling, using a controlled heating and pressure process.
The method produces a molded article with excellent sound absorption properties by forming micropores naturally during thermoforming, enhancing sound absorption without the need for drilling and minimizing pore blocking.
Smart Images

Figure 0007579560000001 
Figure 0007579560000002 
Figure 0007579560000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for thermoforming a fiberboard, and more particularly to a method for thermoforming a fiberboard to obtain a molded article having excellent sound absorbing properties for use in the exterior or interior of an automobile. [Background technology]
[0002] Conventionally, fiber boards made of recycled fibers, glass fibers, etc. have been adopted as sound-absorbing materials for automobiles, etc. Also, in order to improve sound-absorbing properties, it has been proposed to use a fiber structure made by laminating a polyester resin film on a nonwoven fabric made of accumulated polyester fibers as a sound-absorbing material (Patent Document 1). However, since polyester resin films tend to reflect sound, Patent Document 1 also proposes opening micropores of several μm to several tens of μm in the polyester resin film in order to further improve sound-absorbing properties.
[0003] However, it is troublesome to make micropores in a polyester resin film. In addition, when the fiber structure described in Patent Document 1 is heated and molded to obtain a molded product, the micropores may be blocked due to softening or melting of the polyester resin film. Therefore, the molded product may not have the desired sound absorbing properties.
[0004] [Patent Document 1] JP 2019-209569 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] The present invention aims to obtain a molded article having excellent sound absorbing properties by thermoforming while eliminating the need for the step of drilling microholes. [Means for solving the problem]
[0006] The present invention has solved the above-mentioned problems by subjecting a fiberboard made of a specific laminate to a specific heat forming process. That is, the present invention provides a first nonwoven body made of polyester fibers, a second nonwoven body made of polyolefin fibers, a third nonwoven body made of core-sheath type composite fibers A having a core component of a polyester polymer and a sheath component of a polyolefin polymer, and a fourth nonwoven body made of polyester fibers. In this order: The laminated fiberboard is heated to a temperature higher than the melting point of the polyolefin fiber. and less than the melting point of the polyester polymer The present invention relates to a method for thermoforming a fiberboard, which comprises carrying out thermoforming under temperature conditions of
[0007] The first nonwoven body 1 used in the present invention is made of accumulated polyester fibers. The fineness of the polyester fibers is about 1 to 10 decitex. The first nonwoven body 1 may be made of simply accumulated polyester fibers, but generally, it is preferable that the polyester fibers are bonded or entangled with each other to have a predetermined strength and to be easy to handle. In particular, it is preferable that the first nonwoven body 1 is a needle-punched nonwoven body in which the accumulated polyester fibers are entangled with each other by needle punching. When needle punching is performed, the punch density is 10 or more / cm. 2 The weight of the first nonwoven body 1 is preferably 100 to 2000 g / m 2 If the weight of the first nonwoven body 1 is too low, the function of protecting the film having micropores obtained after thermoforming is reduced, and the sound absorption properties of the obtained molded body tend to decrease. Also, if the weight of the first nonwoven body 1 is too high, the obtained molded body becomes heavy and difficult to handle, which is not reasonable.
[0008] The polyester fibers constituting the first nonwoven body 1 may be long fibers or short fibers obtained by melt spinning a conventionally known polyester polymer. In the present invention, it is preferable to use, as the polyester fibers, core-sheath type conjugated long fibers B having a core component made of polyethylene terephthalate with a high melting point and a sheath component made of a polyester polymer with a low melting point. This is because the long fibers give a molded product with higher rigidity. Such core-sheath type conjugated long fibers B can be obtained by a known method of supplying the polyethylene terephthalate core component and the polyester polymer sheath component to a spinning device having a conjugated spinning hole and melt spinning them.
[0009] The polyethylene terephthalate forming the core component is a polyester obtained by dehydration condensation of ethylene glycol as a diol component and terephthalic acid as a dicarboxylic acid component, but a small amount of other dicarboxylic acid components such as isophthalic acid may be mixed as the dicarboxylic acid component. The melting point of such polyethylene terephthalate is about 260°C, and the glass transition point is preferably about 70 to 80°C.
[0010] As the polyester polymer forming the sheath component, it is preferable to adopt a copolymer polyester obtained by dehydration condensation of ethylene glycol as a diol component, and adipic acid and terephthalic acid as dicarboxylic acid components. The mixing ratio of adipic acid and terephthalic acid as dicarboxylic acid components is arbitrary, but is about adipic acid:terephthalic acid=1:1-10 (molar ratio). As the diol component, it is preferable to mix a small amount of diethylene glycol. The mixing amount of diethylene glycol is about 0.5-5.0 mol % in the diol component. Also, as the dicarboxylic acid component, it is preferable to mix a small amount of isophthalic acid. The mixing amount of isophthalic acid is about 2.0-5.0 mol % in the dicarboxylic acid component. The reason for mixing a small amount of diethylene glycol or isophthalic acid is to appropriately adjust the rigidity of the obtained fiber. The melting point of the polyester polymer constituting the sheath component is about 200°C, and the glass transition point is preferably about 40-50°C.
[0011] The weight ratio of the core component to the sheath component is about core component:sheath component=0.3 to 5:1 (weight ratio). If the weight ratio of the core component is too low, the strength and rigidity of the molded body obtained by thermoforming tend to decrease. If the weight ratio of the core component is too high, the core component is difficult to integrate during thermoforming, and fuzz tends to occur on the surface of the obtained molded body. The core component and the sheath component may be arranged concentrically or eccentrically. However, if they are arranged eccentrically, shrinkage is likely to occur during thermoforming, so it is preferable to arrange them concentrically.
[0012] The second nonwoven body 2 used in the present invention is formed by accumulating polyolefin fibers. The weight of the second nonwoven body 2 is 20 to 70 g / m 2 The weight of the second nonwoven body 2 is about 100%. If the weight of the second nonwoven body 2 is too low, it tends to be difficult to form a film during thermoforming. If the weight of the second nonwoven body 2 is too high, it is difficult to form a film having micropores during thermoforming. The polyolefin fibers constituting the second nonwoven body 2 may be short fibers or long fibers. Polypropylene fibers are generally used as the polyolefin fibers. The polypropylene fibers may be polypropylene fibers or copolymer fibers in which propylene is copolymerized with an olefin such as ethylene or butylene. The melting point of the polypropylene fibers is less than 200°C, and the melting point of the polypropylene fibers is about 160 to 170°C. As the polyolefin fibers, it is preferable to use ultrafine fibers having a smaller fiber diameter than the fibers constituting the other nonwoven bodies. This is because they are easily melted during thermoforming, and a film having micropores is easily formed. The fiber diameter of the ultrafine fibers is preferably about 0.5 μm to 7 μm.
[0013] As the second nonwoven body 2, it is preferable to use a laminated structure in the order of a first long fiber nonwoven fabric made of polypropylene long fibers, an ultrafine fiber nonwoven fabric made of ultrafine fibers whose fiber diameter is smaller than that of the polypropylene long fibers, and a second long fiber nonwoven fabric made of polypropylene long fibers. That is, it is preferable to use a laminated structure in which an ultrafine fiber nonwoven fabric is sandwiched between two long fiber nonwoven fabrics. This is because the ultrafine fiber nonwoven fabric alone has low strength and is difficult to handle. The fiber diameter of the long fibers constituting the first and second long fiber nonwoven fabrics is preferably about 10 μm to 50 μm. As the long fiber nonwoven fabric, a nonwoven fabric obtained by a spunbond method is used, and as the ultrafine fiber nonwoven fabric, a nonwoven fabric obtained by a melt-blowing method is often used, and such laminated nonwoven fabrics are called SMS nonwoven fabrics. Therefore, it is preferable to use an SMS nonwoven fabric as the second nonwoven body 2. In the case of SMS nonwoven fabrics, the weight of the first and second long fiber nonwoven fabrics is generally 1 to 30 g / m 2 The weight of the ultrafine fiber nonwoven fabric is approximately 0.1 to 7 g / m 2 It is.
[0014] The third nonwoven body 3 used in the present invention is formed by accumulating core-sheath type composite fibers A, the core component of which is a polyester polymer and the sheath component of which is a polyolefin polymer. The fineness of the core-sheath type composite fibers A is about 1 to 10 decitex. The weight of the third nonwoven body 3 is 20 to 70 g / m 2 The weight of the third nonwoven body 3 is preferably about the same as that of the second nonwoven body 2. This is because the third nonwoven body 3 makes it easier to melt the polyolefin fibers of the second nonwoven body 2 along the surface of the core-sheath type composite fibers A during thermoforming. but If the temperature is too low, the amount of molten polyolefin fibers becomes excessive, which tends to make it difficult to form a membrane with micropores. but If the temperature is too high, the membrane itself tends to be difficult to form. The core-sheath type composite fiber A may be a long fiber or a short fiber, but is preferably a long fiber that can realize high strength.
[0015] The polyester polymer forming the core component of the sheath-core composite fiber A is preferably polyethylene terephthalate. That is, it is a polyester obtained by dehydration condensation of ethylene glycol as a diol component and terephthalic acid as a dicarboxylic acid component, but a small amount of other dicarboxylic acid components such as isophthalic acid may be mixed as the dicarboxylic acid component. In addition, the sheath component is preferably a polyolefin such as polyethylene. By using a polyolefin as the sheath component, the polyolefin fiber in the second nonwoven body 2 can be melted along the surface of the sheath-core composite fiber A during thermoforming. If the sheath component is not a polyolefin but a polymer such as polyester, it has poor compatibility with the polyolefin fiber in the second nonwoven body 2, and it is difficult to melt the sheath-core composite fiber A along the surface. The weight ratio of the core and the arrangement of the core and the sheath of the core of the sheath-core composite fiber A may be the same as those of the core and the sheath composite fiber B.
[0016] The fourth nonwoven body 4 used in the present invention is formed by accumulating polyester-based fibers. The fourth nonwoven body 4 is preferably of the same type as the first nonwoven body 1. Of course, the fourth nonwoven body 4 may be of a different type from the first nonwoven body 1, so long as the fourth nonwoven body 4 is an accumulated polyester-based fiber.
[0017] A laminate is obtained by laminating the first nonwoven body 1, the second nonwoven body 2, the third nonwoven body 3, and the fourth nonwoven body 4 in this order. This laminate may be simply laminated to form a fiberboard, but it is preferable to bond and integrate the first nonwoven body 1, the second nonwoven body 2, the third nonwoven body 3, and the fourth nonwoven body 4 to form a fiberboard. This is because it is easier to handle when integrated. A preferred method of integration is to laminate the first nonwoven body 1, the second nonwoven body 2, the third nonwoven body 3, and the fourth nonwoven body 4, and then needle punch them. The needle punching entangles the fibers constituting each nonwoven body, and firmly integrates them. The punch density is arbitrary, but is generally 10 or more / cm. 2 It is preferable that the punch density is less than 10 punches / cm 2 If the weight of the fiberboard is less than 300g / m2, the degree of integration is low and the handling property tends to be deteriorated. 2The weight of the fiberboard is about 300g / m 2 If the weight of the fiberboard is less than 2500 g / m, sound absorption tends to be difficult to improve. 2 If it exceeds this limit, the weight becomes too heavy and handling tends to deteriorate.
[0018] Fiberboard of Heat it to form it. The heating temperature is: The second nonwoven body 2 is formed The heating temperature is equal to or higher than the melting point of the polyolefin fiber and lower than the melting point of the polyester polymer that is the core component of the core-sheath type composite fiber A that constitutes the third nonwoven body 3. Specifically, the heating temperature is preferably about 200°C. During heating, pressure is generally applied to compress the fiber board. It is also preferable to apply heat and pressure using a mold to form a predetermined shape.
[0019] The molded article obtained by heating and thermoforming the fiberboard is used for various purposes, such as sound absorbing materials for automobiles and other vehicles, houses, and soundproof walls for expressways and high-speed railways. Effect of the Invention
[0020] According to the thermoforming method of the present invention, during heat forming, the polyolefin fibers in the second nonwoven body 2 melt along the surface of the core-sheath type composite fibers A in the third nonwoven body 3, so that a membrane is formed while leaving gaps between the core-sheath type composite fibers A, and these gaps become micropores. Therefore, in the obtained molded body, a membrane having micropores is formed between the first nonwoven body 1 and the fourth nonwoven body 4, and the molded body has excellent sound absorption properties. Therefore, according to the present invention, an effect is achieved in that a molded body having a membrane having micropores can be obtained without providing micropores in a resin film. EXAMPLES
[0021] Example 1 [Preparation of the first nonwoven body] As the core component, a copolymer of ethylene glycol and terephthalic acid (melting point 260°C) was prepared. As the sheath component, a copolymer of ethylene glycol, diethylene glycol, adipic acid, terephthalic acid and isophthalic acid (melting point 200°C) was prepared. The diol components were 99 mol% ethylene glycol and 1 mol% diethylene glycol, and the dicarboxylic acid components were 19 mol% adipic acid, 78 mol% terephthalic acid and 3 mol% isophthalic acid. Both the core component and the sheath component were fed to a spinning device having a composite spinning hole and melt spun to obtain a core-sheath type composite long fiber B (fineness about 3 dtex) in which the weight ratio of the core component to the sheath component was core component:sheath component = 8:2. This core-sheath type composite long fiber B was collected and accumulated on a conveyer to obtain a fiber web. This fiber web was conveyed to a needle punch device and needle punched to a punch density of 90 needles / cm. 2 Needle punched at 200g / m 2 Thus, a first nonwoven body of the above structure was obtained.
[0022] [Preparation of the second nonwoven body] Polypropylene was fed into a spinning device having a spinning hole, and a polypropylene nonwoven fabric was obtained by the spunbonding method. The weight of this polypropylene nonwoven fabric was about 22 g / m 2 The fiber diameter of the polypropylene long fibers constituting the polypropylene nonwoven fabric was about 10 μm. Ultrafine fibers were accumulated on the polypropylene nonwoven fabric by melt-blowing to obtain an ultrafine fiber nonwoven fabric. The weight of the ultrafine fiber nonwoven fabric was about 7 g / m 2 The fiber diameter of the ultrafine fibers constituting the ultrafine fiber nonwoven fabric was about 1 to 5 μm. The polypropylene nonwoven fabric was then laminated on the ultrafine fiber nonwoven fabric to obtain a fabric with a weight of about 50 g / m. 2 This SMS nonwoven fabric was used as the second nonwoven material.
[0023] [Preparation of the third nonwoven body] As the third nonwoven material, Elves (product number T0503WDO) manufactured by Unitika Ltd. was prepared. The third nonwoven material was a nonwoven fabric formed by accumulating core-sheath type composite long fibers A, the core of which was polyethylene terephthalate and the sheath of which was polyethylene. The weight of the third nonwoven material was about 50 g / m2 The fineness of the core-sheath type composite continuous fiber A is about 3 dtex.
[0024] [Preparation of the fourth nonwoven body] The first nonwoven fabric was produced in the same manner as in the first nonwoven fabric, with a weight of 600 g / m 2 Thus, a first nonwoven body of the above structure was obtained.
[0025] [Manufacturing of fiberboard] The first nonwoven body, the second nonwoven body, the third nonwoven body and the fourth nonwoven body were laminated in this order to obtain a laminate. This laminate was fed to a needle punch device and punched at a punch density of 45 needles / cm. 2 Needle punched at 1050g / m 2 Thus, a fiberboard of 1000 g was obtained.
[0026] [Thermoforming of fiberboard] The obtained fiber board was sandwiched between two hot plates heated to 200° C., and thermoformed for 30 seconds under pressure so that the distance between the hot plates was 3 mm, thereby obtaining a molded product with a thickness of 3 mm.
[0027] Comparative Example 1 The first nonwoven material and the fourth nonwoven material used in Example 1 were laminated to form a laminate, and this laminate was subjected to thermoforming under the same conditions as in Example 1 to obtain a molded product having a thickness of 3 mm.
[0028] Comparative Example 2 The first nonwoven material, the third nonwoven material, and the fourth nonwoven material used in Example 1 were laminated, and the laminate was transported to a needle punch device, and the punch density was set to 45 needles / cm. 2 This laminate was subjected to thermoforming under the same conditions as in Example 1 to obtain a molded product having a thickness of 3 mm.
[0029] Comparative Example 3 The first nonwoven fabric used in Example 1, the polyester nonwoven fabric described below, and the fourth nonwoven fabric used in Example 1 were laminated together, and the resultant was fed to a needle punch device to obtain a punch density of 45 needles / cm. 2 This laminate was subjected to thermoforming under the same conditions as in Example 1 to obtain a molded product having a thickness of 3 mm. [Polyester nonwoven fabric] A polyester nonwoven fabric formed by accumulating polyethylene terephthalate long fibers, the fineness of the polyethylene terephthalate long fibers being about 3 decitex, and the weight of the polyester nonwoven fabric being about 50 g / m 2 It is.
[0030] Comparative Example 4 The first nonwoven material, the second nonwoven material, and the fourth nonwoven material used in Example 1 were laminated, and the laminate was transported to a needle punch device, and the punch density was set to 45 needles / cm. 2 This laminate was subjected to thermoforming under the same conditions as in Example 1 to obtain a molded product having a thickness of 3 mm.
[0031] Comparative Example 5 The first nonwoven fabric and the second nonwoven fabric used in Example 1, the polyester nonwoven fabric used in Comparative Example 3, and the fourth nonwoven fabric used in Example 1 were laminated, and the laminate was transported to a needle punch device to obtain a punch density of 45 needles / cm. 2 This laminate was subjected to thermoforming under the same conditions as in Example 1 to obtain a molded product having a thickness of 3 mm.
[0032] When the layer corresponding to the first nonwoven body was peeled off from the molded product obtained in Example 1 and the surface of the remaining layer was observed by SEM photography, a membrane having micropores was formed, as shown in Figure 2. On the other hand, when the layer corresponding to the first nonwoven body was peeled off from the molded product obtained in Comparative Example 4 and the surface of the remaining layer was observed by SEM photography, a mass of molten material was present, as shown in Figure 3, and no membrane formation was observed.
[0033] The air permeability of each of the molded products obtained in Example 1 and Comparative Examples 1 to 5 was measured according to the air permeability measurement method A described in JIS L 1096. The results were as follows: The molded product obtained in Example 1 had an air permeability of 9 cc / m 2 The molded product obtained in Comparative Example 1 had a viscosity of 22 cc / m 2 The molded product obtained in Comparative Example 2 had a viscosity of 16 cc / m 2 The molded product obtained in Comparative Example 3 had a viscosity of 20 cc / m 2The molded product obtained in Comparative Example 4 had a viscosity of 16 cc / m 2 The molded product obtained in Comparative Example 5 had a viscosity of 11 cc / m 2 It was.
[0034] The normal incidence sound absorption coefficient of each of the molded bodies obtained in Example 1 and Comparative Examples 1 to 5 was measured using an SR-4100 B pipe (inner diameter 29 mmφ) manufactured by Ono Sokki Co., Ltd. in accordance with ISO 10534-2, with the first nonwoven side as the incident side. The normal incidence sound absorption coefficient was measured at 1000 Hz, 2000 Hz, 3000 Hz, 4000 Hz, and 5000 Hz. The results are shown in FIG. 4.
[0035] From the results of Figs. 2, 3 and 4, it is seen that the molded article obtained by the thermoforming method according to Example 1 has a film with micropores and has an improved sound absorption coefficient. [Brief description of the drawings]
[0036] [Figure 1] FIG. 2 is a schematic side view showing an example of a fiber board used in the present invention. [Diagram 2] 2 is a SEM photograph of the surface of a remaining layer after removing a layer corresponding to a first nonwoven body from the molded article obtained by the method according to Example 1. [Diagram 3] 1 is a SEM photograph of the surface of a remaining layer after removing a layer corresponding to a first nonwoven body from a molded article obtained by a method according to Comparative Example 4. [Figure 4] 1 is a graph showing the normal incident sound absorption coefficients of the molded body obtained in Example 1 and the molded bodies obtained in Comparative Examples 1 to 5. [Explanation of symbols]
[0037] 1 First nonwoven body 2 Second nonwoven body 3 Third non-woven body 4 Fourth non-woven material
Claims
1. A method for thermoforming a fiber board, comprising the steps of: heat-molding a fiber board comprising a laminate of a first nonwoven body made of accumulated polyester fibers, a second nonwoven body made of accumulated polyolefin fibers, a third nonwoven body made of accumulated core-sheath composite fibers A whose core component is a polyester polymer and whose sheath component is a polyolefin polymer, and a fourth nonwoven body made of accumulated polyester fibers, in that order, under temperature conditions equal to or higher than the melting point of the polyolefin fibers and lower than the melting point of the polyester polymer.
2. 2. A method for thermoforming a fiberboard according to claim 1, wherein the laminate is needle-punched to entangle the constituent fibers of the first nonwoven body, the second nonwoven body, the third nonwoven body and the fourth nonwoven body, thereby obtaining a fiberboard.
3. 2. The method for thermoforming a fiber board according to claim 1, wherein the polyester fibers in the first nonwoven body and the fourth nonwoven body are core-sheath type composite fibers B whose core component is a copolymer of ethylene glycol and terephthalic acid, and whose sheath component is a copolymer containing ethylene glycol, adipic acid, and terephthalic acid.
4. 4. A method for thermoforming a fiberboard according to claim 3, wherein the sheath component is a copolymer of ethylene glycol, adipic acid, terephthalic acid, and isophthalic acid and / or diethylene glycol.
5. 2. The method for thermoforming a fiber board according to claim 1, wherein the second nonwoven body is formed by laminating in this order a first long-fiber nonwoven fabric made of polypropylene-based long fibers, an ultrafine fiber nonwoven fabric made of ultrafine fibers having a fiber diameter smaller than that of the polypropylene-based long fibers, and a second long-fiber nonwoven fabric made of polypropylene-based long fibers.
6. 2. The method for thermoforming a fiber board according to claim 1, wherein the core-sheath type composite fiber A in the third nonwoven body has a core component made of polyethylene terephthalate and a sheath component made of polyethylene.
7. 4. The method for thermoforming a fiber board according to claim 1, wherein the core-sheath type composite fibers A and B are both core-sheath type composite long fibers in which a core component and a sheath component are concentrically arranged.
8. 2. A method for producing a fiber board for use in the thermoforming method of fiber board according to claim 1, characterized in that a laminate obtained by laminating in this order a first nonwoven body made of polyester-based fibers, a second nonwoven body made of polyolefin-based fibers, a third nonwoven body made of core-sheath type composite fibers A whose core component is a polyester-based polymer and whose sheath component is a polyolefin-based polymer, and a fourth nonwoven body made of polyester-based fibers is subjected to needle punching.
Citation Information
Patent Citations
Sound-absorbing nonwoven fabric and its production
JP2000199161A