All-solid-state lithium secondary battery and method for producing same

A laminated electrode body with a solid electrolyte-containing sheet covering the electrode edges addresses the challenge of short circuits and thickness adjustment in all-solid-state lithium secondary batteries, ensuring high capacity and energy density.

JP7579643B2Active Publication Date: 2024-11-08MAXELL LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020049813
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-19
Publication Date
2024-11-08
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Existing methods for forming solid electrolyte layers in all-solid-state lithium secondary batteries face challenges in adjusting the thickness and preventing short circuits at the outer peripheral edges of the electrodes, particularly when forming thin layers to increase battery capacity.

Method used

The use of a laminated electrode body with a solid electrolyte-containing sheet that includes an insulating porous base material and a solid electrolyte, where the peripheral edge of the sheet covers the outer peripheral side surface of the electrodes, and the thickness is set between 5 to 200 μm, ensuring flexibility and adherence.

Benefits of technology

This approach prevents short circuits at the electrode edges while maintaining high capacity and energy density, allowing for a reliable and efficient battery construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579643000001
    Figure 0007579643000001
  • Figure 0007579643000002
    Figure 0007579643000002
Patent Text Reader

Abstract

To provide an all-solid-state lithium secondary battery that prevents a short circuit from occurring at the outer peripheral ends of a positive electrode and a negative electrode, and has a high capacity and a high energy density even when the thickness of a solid electrolyte layer is reduced.SOLUTION: An all-solid-state lithium secondary battery disclosed in the present application includes a laminated electrode body including a positive electrode, a negative electrode, and a solid electrolyte-containing sheet arranged between the positive electrode and the negative electrode, and the solid electrolyte-containing sheet includes an insulating porous base material and a solid electrolyte filled in the insulating porous base material, and the peripheral portion of the solid electrolyte-containing sheet covers the outer peripheral side surface of the positive electrode or the negative electrode. The thickness of the solid electrolyte-containing sheet is 5 to 200 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high-capacity all-solid-state lithium secondary battery using a solid electrolyte and a method for producing the same. [Background technology]

[0002] Currently, organic electrolyte solutions used in lithium ion secondary batteries contain organic solvents, which are flammable substances, and therefore there is a possibility that the organic electrolyte solution will generate abnormal heat when an abnormality such as a short circuit occurs in the battery. In addition, with the recent trend toward higher energy density of lithium ion secondary batteries and an increasing amount of organic solvent in the organic electrolyte solution, there is an even greater demand for safety and reliability of lithium ion secondary batteries.

[0003] In the above circumstances, all-solid-state lithium secondary batteries that do not use organic solvents have attracted attention. All-solid-state lithium secondary batteries use a molded body of a solid electrolyte that does not use an organic solvent instead of the conventional organic solvent-based electrolyte, and are highly safe without the risk of abnormal heat generation of the solid electrolyte.

[0004] In general, all-solid-state lithium secondary batteries use a laminated electrode body in which a solid electrolyte layer is disposed between a positive electrode and a negative electrode. The laminated electrode body can be produced by a method of forming a laminated film by applying a paint in which each component material (active material, solid electrolyte) is dispersed in a solvent, or by a method of filling a mold with powder of each component material as it is and pressing it to form a pellet.

[0005] Currently, development of coin-type solid electrolyte batteries is underway as batteries for use in small electronic devices. In the case of coin-type batteries, however, pellets of a laminated electrode body are typically produced and then housed in a battery container to assemble the battery.

[0006] When the laminated electrode body of a coin-type battery is produced as a pellet, the powders of the respective constituent materials are pressure-molded in a mold, so that the whole is formed as a cylindrical laminate, and the area of ​​the positive electrode and the negative electrode is the same as the area of ​​the solid electrolyte layer. Therefore, when the active material particles are detached from the end of the positive electrode or the negative electrode, the outer peripheral end of the positive electrode and the outer peripheral end of the negative electrode come into contact with each other, which may easily cause a short circuit. In particular, when an attempt is made to form a thin solid electrolyte layer that is not related to the battery capacity in order to increase the capacity of the battery, the above-mentioned short circuit is more likely to occur.

[0007] In order to solve this problem, Patent Document 1 proposes that at least one of the positive and negative electrodes is covered with a solid electrolyte layer. By configuring the laminated electrode body as described above, the short circuit problem can be prevented. However, Patent Document 1 uses a method in which the electrode and the solid electrolyte layer, which are separately manufactured, are later integrated, making it difficult to form a thin solid electrolyte layer.

[0008] On the other hand, Patent Documents 2 and 3 propose a method of forming a film by charging and applying powder of an active material or a solid electrolyte, and then applying pressure. With this method, the thickness of each layer can be adjusted relatively freely, so that it is possible to reduce the thickness of the solid electrolyte layer and also to fabricate a shape in which the outer peripheral surface of the electrode is covered with the solid electrolyte. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2009-64644 A [Patent Document 2] JP 2010-282803 A [Patent Document 3] JP 2019-21428 A Summary of the Invention [Problem to be solved by the invention]

[0010] However, the methods described in Patent Documents 2 and 3 only pressurize the coating film in the thickness direction, and do not impose any restrictions on the surface direction of the coating film. Therefore, when a solid electrolyte layer is formed on the outer peripheral surface of the positive electrode or negative electrode to prevent the above-mentioned short circuit, it is difficult to adjust the thickness of the solid electrolyte layer on the outer peripheral surface.

[0011] In addition, since the molded solid electrolyte layer is fragile, when a solid electrolyte layer is formed on the outer peripheral surface of a positive electrode or a negative electrode, the solid electrolyte layer formed on the outer peripheral surface of the positive electrode or a negative electrode is likely to detach during battery production, and the outer peripheral end of the positive electrode and the outer peripheral end of the negative electrode may come into contact with each other, causing a short circuit.

[0012] The present application has been made to solve the above problems, and provides an all-solid-state lithium secondary battery which prevents the occurrence of short circuits at the outer peripheral ends of the positive electrode and the negative electrode and has a high capacity by reducing the thickness of the solid electrolyte layer. [Means for solving the problem]

[0013] The all-solid-state lithium secondary battery of the present invention comprises a laminated electrode body including a positive electrode, a negative electrode, and a solid electrolyte-containing sheet disposed between the positive electrode and the negative electrode, the solid electrolyte-containing sheet including an insulating porous substrate and a solid electrolyte filled in the insulating porous substrate, the peripheral portion of the solid electrolyte-containing sheet covers the outer peripheral side portion of the positive electrode or the negative electrode, and the thickness of the solid electrolyte-containing sheet is 5 to 200 μm.

[0014] Further, a method for producing the all-solid-state lithium secondary battery of the present invention is a method for producing the all-solid-state lithium secondary battery of the present invention, and includes an electrode preparation step of preparing a positive electrode and a negative electrode, a filling step of filling an insulating porous substrate with solid electrolyte particles to prepare a solid electrolyte-containing sheet, a lamination step of laminating the positive electrode, the solid electrolyte-containing sheet, and the negative electrode in this order, and a folding step of folding back a peripheral portion of the solid electrolyte-containing sheet to the outer periphery side of one of the laminated positive electrode or the negative electrode, so as to cover an outer periphery side portion of the positive electrode or the negative electrode with the peripheral portion of the solid electrolyte-containing sheet. Effect of the Invention

[0015] According to the present application, even if the thickness of the solid electrolyte layer is thin, the occurrence of short circuits at the outer peripheral ends of the positive electrode and negative electrode can be prevented, and an all-solid-state lithium secondary battery with high capacity and high energy density can be provided. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of an all-solid-state lithium secondary battery according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a process for producing a laminated electrode body of an all-solid-state lithium secondary battery according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] (All-solid-state lithium secondary battery) An embodiment of the all-solid-state lithium secondary battery disclosed in the present application will be described. The all-solid-state lithium secondary battery of this embodiment includes a laminated electrode body including a positive electrode, a negative electrode, and a solid electrolyte-containing sheet disposed between the positive electrode and the negative electrode, the solid electrolyte-containing sheet includes an insulating porous substrate and a solid electrolyte filled in the insulating porous substrate, the peripheral portion of the solid electrolyte-containing sheet covers the outer peripheral side portion of the positive electrode or the negative electrode, and the thickness of the solid electrolyte-containing sheet is 5 to 200 μm.

[0018] In the all-solid-state lithium secondary battery of this embodiment, since the solid electrolyte is filled into the insulating porous substrate, a thin and uniform solid electrolyte layer can be formed. This makes it possible to provide an all-solid-state lithium secondary battery with high capacity and high energy density. In addition, since the peripheral portion of the solid electrolyte-containing sheet covers the outer peripheral side portion of the positive electrode or negative electrode, even if the solid electrolyte layer (solid electrolyte-containing sheet) is formed thin, it is possible to prevent the occurrence of a short circuit at the outer peripheral end portion of the positive electrode and the negative electrode.

[0019] In addition, since the thickness of the solid electrolyte-containing sheet is 200 μm or less, a certain degree of flexibility can be imparted to the solid electrolyte-containing sheet, which allows the peripheral portion of the solid electrolyte-containing sheet to be folded onto the outer peripheral side portion of the positive electrode or negative electrode, and the outer peripheral side portion of the electrode can be covered with the solid electrolyte-containing sheet in a simple manner. Furthermore, since the thickness of the solid electrolyte-containing sheet is 5 μm or more, the insulating porous substrate holds the solid electrolyte, ensuring the shape retention of the solid electrolyte-containing sheet, and allowing it to be reliably formed into a laminated electrode body by stacking it with the positive electrode and negative electrode.

[0020] The all-solid-state lithium secondary battery of this embodiment will be described below with reference to the drawings. FIG. 1 is a cross-sectional view showing an example of a coin-shaped all-solid-state lithium secondary battery of this embodiment. In FIG. 1, an all-solid-state lithium secondary battery 10 has a laminated electrode body made of a negative electrode 14, a positive electrode 15, and a solid electrolyte-containing sheet 16 sealed inside an exterior body made of an exterior can 11, a sealing can 12, and a gasket 13 interposed between them. The solid electrolyte-containing sheet 16 includes an insulating porous substrate (not shown) and a solid electrolyte filled in the insulating porous substrate, and a peripheral portion 16a of the solid electrolyte-containing sheet 16 is folded back to the positive electrode 15 side to cover the outer peripheral side portion of the positive electrode 15. The peripheral portion 16a of the solid electrolyte-containing sheet 16 may be folded back to the negative electrode 14 side to cover the outer peripheral side portion of the negative electrode 14.

[0021] The sealing can 12 is fitted into the opening of the outer can 11 via a gasket 13, and the open end of the outer can 11 is tightened inward, whereby the gasket 13 abuts against the sealing can 12, sealing the opening of the outer can 11 and forming an airtight structure inside the exterior body.

[0022] Next, each of the components of the all-solid-state lithium secondary battery of this embodiment will be described.

[0023] <Solid electrolyte-containing sheet> The solid electrolyte-containing sheet in the all-solid-state lithium secondary battery of this embodiment constitutes the solid electrolyte layer of the laminated electrode body, and includes an insulating porous substrate, and a solid electrolyte and a binder filled in the insulating porous substrate.

[0024] As described above, the thickness of the solid electrolyte-containing sheet is set to 5 μm or more, preferably 10 μm or more, so that the shape retention of the solid electrolyte-containing sheet can be ensured and the sheet can be laminated with the positive and negative electrodes to reliably form a laminated electrode body. In addition, the thickness of the solid electrolyte-containing sheet is set to 200 μm or less, preferably 100 μm or less, so that the peripheral edge of the solid electrolyte-containing sheet can be folded to the outer peripheral side surface of the positive or negative electrode.

[0025] In addition, in the laminated electrode body, in order to ensure ion conductivity at the interface between the electrode and the solid electrolyte-containing sheet, the entire surface of the insulating porous substrate is made of the solid electrolyte. By quality It is preferably covered.

[0026] [Solid electrolyte] The solid electrolyte is not particularly limited as long as it has lithium ion conductivity, and for example, a sulfide-based solid electrolyte, a hydride-based solid electrolyte, an oxide-based solid electrolyte, etc. can be used.

[0027] The sulfide-based solid electrolyte is, for example, Li 2 SP 2 S 5 , Li 2 S-SiS 2 , Li 2 SP 2 S 5 -GeS 2 , Li 2 S.B. 2 S 3 In addition to sulfide-based solid electrolyte glass, Li 10 GeP 2 S 12 (LGPS series) and Li 6 P.S. 5Cl (argyrodite-based) can also be used. Among these, the argyrodite-based solid electrolyte is preferably used because it has high lithium ion conductivity and high chemical stability.

[0028] The hydride-based solid electrolyte is, for example, LiBH 4 and the following alkali metal compounds (e.g., LiBH 4 and an alkali metal compound in a molar ratio of 1:1 to 20:1. The alkali metal compound in the solid solution may be at least one selected from the group consisting of lithium halides (LiI, LiBr, LiF, LiCl), rubidium halides (RbI, RbBr, RbF, RbCl), cesium halides (CsI, CsBr, CsF, CsCl), lithium amide, rubidium amide, and cesium amide.

[0029] The oxide-based solid electrolyte may be, for example, Li 7 La 3 Zr 2 O 12 , LiTi(PO 4 ) 3 , LiGe(PO 4 ) 3 , LiLaTiO 3 etc.

[0030] Among the above-listed solid electrolytes, it is more preferable to use a sulfide-based solid electrolyte having high lithium ion conductivity.

[0031] The above solid electrolytes can be used alone, or two or more can be used in combination. The form of the above solid electrolyte is preferably particulate from the viewpoint of filling the insulating porous substrate, but may be in a form other than particulate. When two or more solid electrolytes are used in combination, the solid electrolytes may be mixed in particulate form, or may be mixed at a molecular level, or may be present in such a way that the solid electrolyte particles form different regions in the thickness direction of the solid electrolyte-containing sheet.

[0032] The average particle diameter of the solid electrolyte particles is preferably 5 μm or less, more preferably 2 μm or less, from the viewpoint of improving the filling property into the pores of the insulating porous substrate and ensuring good lithium ion conductivity. However, if the size of the solid electrolyte particles is too small, the handling property may be deteriorated or a larger amount of binder may be required, resulting in an increase in the resistance value. Therefore, the average particle diameter of the solid electrolyte particles is preferably 0.3 μm or more, more preferably 0.5 μm or more.

[0033] The average particle diameter of the solid electrolyte particles and other particles (positive electrode active material particles, negative electrode active material particles, etc.) referred to in this specification is a number average particle diameter measured by dispersing the particles in a medium that does not dissolve or swell the particles using, for example, a laser scattering particle size distribution meter (for example, "LA-920" manufactured by HORIBA Corporation).

[0034] [Insulating porous substrate] The insulating porous substrate is not particularly limited as long as it can be filled with and hold a solid electrolyte, but a nonwoven fabric is preferred because it is easy to handle and form into a thin film.

[0035] The porosity of the insulating porous substrate is preferably 30% by volume or more, more preferably 40% by volume or more, from the viewpoint of ensuring a certain amount of solid electrolyte and good lithium ion conductivity. However, if the porosity of the insulating porous substrate is too large, the shape retention of the solid electrolyte-containing sheet may be reduced. Therefore, from the viewpoint of further increasing the strength of the solid electrolyte-containing sheet, the porosity of the insulating porous substrate is preferably 90% by volume or less, more preferably 85% by volume or less.

[0036] As mentioned above, the entire surface of the insulating porous substrate is covered with a solid electrolyte. By quality Therefore, the thickness of the insulating porous substrate is made slightly thinner than the thickness of the solid electrolyte-containing sheet, so that the entire surface of the insulating porous substrate is covered with the solid electrolyte. By qualityThe thickness of the solid electrolyte-containing sheet in the covered state is preferably in the range of 5 to 200 μm. Therefore, the thickness of the insulating porous substrate is preferably set to 3.5 to 195 μm, and more preferably 8.5 to 137 μm.

[0037] When a nonwoven fabric is used as the insulating porous substrate, the fiber diameter of the fibrous material constituting the nonwoven fabric serving as the substrate is preferably 20 μm or less and 0.5 μm or more.

[0038] The material of the fibrous material constituting the nonwoven fabric is not particularly limited as long as it does not react with lithium metal and has insulating properties, and examples of the material that can be used include resins such as polyolefins such as polypropylene and polyethylene, polystyrene, aramid, polyamide-imide, polyimide, nylon, polyesters such as polyethylene terephthalate (PET), polyarylates, cellulose, modified cellulose, etc. Inorganic materials such as glass, alumina, silica, and zirconia can also be used.

[0039] The nonwoven fabric has a basis weight of 10 g / m2 so as to hold a sufficient amount of solid electrolyte particles to ensure good lithium ion conductivity. 2 Preferably, it is 8 g / m or less. 2 More preferably, the thickness is 3 g / m or less. Also, from the viewpoint of ensuring sufficient strength, 2 It is preferable that the content is 4 g / m or more. 2 More preferably, it is equal to or greater than this.

[0040] [Binder] The binder is preferably one that does not react with the solid electrolyte, and at least one resin selected from butyl rubber, chloroprene rubber, acrylic resin, and fluororesin is preferably used.

[0041] In addition, from the viewpoint of further improving the shape retention of the solid electrolyte-containing sheet, the content of the binder is preferably 0.5 mass % or more, and preferably 1 mass % or more, based on the total mass of the solid electrolyte and the binder. Furthermore, from the viewpoint of restricting the amount of the binder to some extent and suppressing a decrease in lithium ion conductivity, the content of the binder is preferably 5 mass % or less, and preferably 3 mass % or less.

[0042] The method for producing the solid electrolyte-containing sheet is not particularly limited, but it is preferable to produce the sheet by dispersing solid electrolyte particles together with a binder in a solvent to prepare a slurry or the like, and then filling the pores of an insulating porous substrate (such as a resin nonwoven fabric) with the slurry in a wet manner. This improves the strength of the solid electrolyte-containing sheet, making it easier to produce a large-area solid electrolyte-containing sheet.

[0043] The above-mentioned slurry is prepared by putting solid electrolyte particles and a binder into a solvent and mixing them. It is preferable to select a solvent for the slurry that is unlikely to deteriorate the solid electrolyte. In particular, since sulfide-based solid electrolytes and hydride-based solid electrolytes undergo chemical reactions with a small amount of moisture, it is more preferable to use a non-polar aprotic solvent represented by a hydrocarbon solvent such as hexane, heptane, octane, nonane, decane, decalin, toluene, or xylene, and to use it as an ultra-dehydrated solvent with a moisture content of 0.001 mass% (10 ppm) or less.

[0044] In addition, examples of the solvent that can be used include fluorine-based solvents such as "Vertrel (registered trademark)" manufactured by DuPont-Mitsui Fluorochemicals, "Zeorolla (registered trademark)" manufactured by Zeon Corporation, and "Novec (registered trademark)" manufactured by Sumitomo 3M Company, as well as non-aqueous organic solvents such as dichloromethane and diethyl ether.

[0045] The method for filling the pores of the insulating porous substrate with a slurry containing solid electrolyte particles and a binder can be a coating method such as a screen printing method, a doctor blade method, or a dipping method.

[0046] After filling the pores of the insulating porous substrate with the slurry, the solvent of the slurry can be removed by drying, and if necessary, pressure molding can be performed to obtain a solid electrolyte-containing sheet.

[0047] The method for manufacturing the solid electrolyte-containing sheet is not limited to the above wet method. For example, a method of dry-filling a mixture of solid electrolyte particles and binder particles into the pores of an insulating porous substrate and then performing pressure molding may be used to manufacture the solid electrolyte-containing sheet.

[0048] <Positive electrode> As the above positive electrode, there is no particular limitation as long as it is a positive electrode used in a conventionally known lithium ion secondary battery, that is, a positive electrode containing an active material capable of occluding and releasing Li ions. For example, as the positive electrode active material, LiM x Mn 2-x O 4 (However, M is at least one element selected from the group consisting of Li, B, Mg, Ca, Sr, Ba, Ti, V, Cr, Fe, Co, Ni, Cu, Al, Sn, Sb, In, Nb, Mo, W, Y, Ru, and Rh, and 0.01 ≦ x ≦ 0.5) spinel-type lithium manganese composite oxide represented by, Li x Mn (1-y-x) Ni y M z O (2-k) F l (However, M is at least one element selected from the group consisting of Co, Mg, Al, B, Ti, V, Cr, Fe, Cu, Zn, Zr, Mo, Sn, Ca, Sr, and W, 0.8 ≦ x ≦ 1.2, 0 < y < 0.5, 0 ≦ z ≦ 0.5, k + l < 1, -0.1 ≦ k ≦ 0.2, 0 ≦ l ≦ 0.1) layered compound represented by, LiCo 1-x M x O 2 (However, M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≦ x ≦ 0.5) lithium cobalt composite oxide represented by, LiNi 1-x M x O 2(wherein M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Co, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0≦x≦0.5), lithium nickel composite oxide represented by LiM 1-x N x PO 4 (wherein M is at least one element selected from the group consisting of Fe, Mn and Co, N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb and Ba, and 0≦x≦0.5), Li 4 Ti 5 O 12 Among these, only one type may be used, or two or more types may be used in combination.

[0049] The positive electrode may have a structure in which a positive electrode mixture layer containing the positive electrode active material, a conductive assistant, and a binder is formed on one or both sides of a current collector.

[0050] As the binder for the positive electrode, for example, a fluororesin such as polyvinylidene fluoride (PVDF) can be used, and as the conductive assistant for the positive electrode, for example, a carbon material such as carbon black can be used, but the solid electrolyte used in the above-mentioned solid electrolyte-containing sheet may also be used as the conductive assistant.

[0051] As the current collector of the positive electrode, a foil of a metal such as aluminum, a punched metal, a net, an expanded metal, a foamed metal, or the like can be used.

[0052] In manufacturing the positive electrode, for example, a method can be adopted in which a positive electrode mixture-containing paste, slurry, etc., in which a positive electrode active material, a conductive assistant, a binder, etc. are dispersed in a solvent such as xylene, is applied to a current collector, dried, and then pressure-molded by calendering, etc., as necessary. As the solvent, a super-dehydrated solvent with a water content of 0.001 mass% (10 ppm) or less is preferably used.

[0053] In addition, when a conductive porous substrate such as a punched metal is used for the positive electrode current collector, the positive electrode can be manufactured, for example, by filling the pores of the conductive porous substrate with the above-mentioned positive electrode mixture-containing paste, slurry, etc., drying, and then performing pressure molding such as calendaring as necessary. A positive electrode manufactured by such a method can ensure high strength, and therefore can hold a solid electrolyte-containing sheet having a larger area.

[0054] Furthermore, instead of the above-mentioned positive electrode mixture-containing paste, slurry, or the like, a positive electrode mixture that contains a positive electrode active material, a conductive assistant, a binder, and the like and does not contain a solvent may be dry-filled into the pores of a conductive porous substrate, and the positive electrode may be produced by a method in which pressure molding such as calendaring is performed as necessary.

[0055] <Negative electrode> The negative electrode is not particularly limited as long as it is a negative electrode used in a conventionally known lithium ion secondary battery, that is, a negative electrode containing an active material capable of absorbing and releasing Li ions. For example, as the negative electrode active material, one or a mixture of two or more types of carbon-based materials capable of absorbing and releasing lithium, such as graphite, pyrolytic carbons, cokes, glassy carbons, baked bodies of organic polymer compounds, mesocarbon microbeads (MCMB), and carbon fibers, is used. In addition, simple substances, compounds, and alloys thereof containing elements such as Si, Sn, Ge, Bi, Sb, and In; compounds that can be charged and discharged at a low voltage close to that of lithium metal, such as lithium-containing nitrides or lithium-containing oxides; lithium metal; lithium / aluminum alloys, etc., can also be used as the negative electrode active material.

[0056] For the negative electrode, a negative electrode mixture obtained by appropriately adding a conductive assistant (carbon material such as carbon black, solid electrolyte, etc.) and a binder such as PVDF to a negative electrode active material is formed into a molded body (negative electrode mixture layer) using a current collector as a core material, or a foil of any of the above-mentioned various alloys or lithium metal is used alone or laminated on a current collector as a negative electrode mixture layer.

[0057] When a current collector is used for the negative electrode, the current collector may be made of copper or nickel foil, punched metal, net, expanded metal, foamed metal, or the like.

[0058] In manufacturing a negative electrode having a negative electrode mixture layer, for example, a method can be adopted in which a negative electrode mixture-containing paste, slurry, etc., in which a negative electrode active material, a binder, and further a conductive assistant, etc., which is used as necessary, are dispersed in a solvent such as xylene, is applied to a current collector, dried, and then pressure-molded, such as by calendaring, as necessary. As the above-mentioned solvent, a super-dehydrated solvent with a water content of 0.001 mass% (10 ppm) or less is preferably used.

[0059] In addition, when a conductive porous substrate such as a punched metal is used for the negative electrode current collector, the negative electrode can be manufactured, for example, by filling the pores of the conductive porous substrate with the above-mentioned negative electrode mixture-containing paste, slurry, etc., drying, and then, if necessary, performing pressure molding such as calendaring. A negative electrode manufactured by such a method can ensure high strength, and therefore can hold a solid electrolyte-containing sheet having a larger area.

[0060] Furthermore, instead of the above-mentioned negative electrode mixture-containing paste, slurry, or the like, a negative electrode mixture that contains a negative electrode active material, a binder, and further a conductive assistant, etc., but does not contain a solvent, may be dry-filled into the pores of a conductive porous substrate, and the negative electrode may be produced by a method in which pressure molding, such as calendaring, is performed as necessary.

[0061] <Exterior body> The materials for the exterior can and the sealing can constituting the exterior body can be, for example, stainless steel. The materials for the gasket can be polypropylene, nylon, etc., and in addition, when heat resistance is required in relation to the use of the battery, a heat-resistant resin having a melting point of more than 240°C can be used. The heat-resistant resin can be, for example, a fluororesin such as tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA); polyphenylene ether (PPE); polysulfone (PSF); polyarylate (PAR); polyethersulfone (PES); polyphenylene sulfide (PPS); polyetheretherketone (PEEK), etc. In addition, when the battery is applied to an application requiring heat resistance, a glass hermetic seal can be used for sealing the battery.

[0062] <Electrode body> The positive electrode and the negative electrode can be used in the form of a laminated electrode body in which the above-mentioned solid electrolyte-containing sheet is laminated with each other, or in the form of a wound electrode body in which this laminated electrode body is wound.

[0063] In forming the laminated electrode body, the positive electrode, the negative electrode, and the solid electrolyte-containing sheet are pressure-molded in a laminated state, and the interfaces between the positive electrode, the negative electrode, and the solid electrolyte-containing sheet are bonded and integrated. Alternatively, instead of pressing and bonding the positive electrode, the negative electrode, and the solid electrolyte-containing sheet all at once, one electrode may be bonded to the solid electrolyte-containing sheet first, and then the other electrode may be laminated and bonded to the opposite side of the solid electrolyte-containing sheet to form the laminated electrode body.

[0064] <Battery type> The form of the all-solid-state lithium secondary battery of this embodiment is not limited to one having an exterior body composed of an exterior can, a sealing can, and a gasket as shown in FIG. 1, i.e., one generally called a coin-type battery or a button-type battery, and may be, for example, one having an exterior body composed of a resin film or a metal-resin laminate film, or one having an exterior body having a cylindrical or square-tubular metallic exterior can and a sealing structure that seals the opening of the can.

[0065] (Manufacturing method of all-solid-state lithium secondary battery) Next, an embodiment of the manufacturing method of the all-solid-state lithium secondary battery disclosed in the present application will be described. A suitable aspect of the manufacturing method of the all-solid-state lithium secondary battery of this embodiment includes, as a manufacturing process of a laminated electrode body, an electrode preparation process for preparing a positive electrode and a negative electrode, a filling process for filling an insulating porous substrate with solid electrolyte particles to prepare a solid electrolyte-containing sheet, a stacking process for stacking the positive electrode, the solid electrolyte-containing sheet, and the negative electrode in this order, and a folding process for folding back the peripheral portion of the solid electrolyte-containing sheet to the outer periphery side of one of the stacked positive electrode or negative electrode, and covering the outer periphery side portion of the positive electrode or the negative electrode with the peripheral portion of the solid electrolyte-containing sheet. In the filling process, it is preferable to further fill the insulating porous substrate with a binder.

[0066] The above-mentioned method for producing an all-solid-state lithium secondary battery can produce a laminated electrode body for use in the all-solid-state lithium secondary battery disclosed above. Thereafter, the laminated electrode body can be housed in the above-mentioned exterior body in a conventional manner to form a sealed structure.

[0067] Next, a method for manufacturing the laminated electrode body will be described with reference to the drawings, although the method for manufacturing the laminated electrode body is not limited to the manufacturing method described below.

[0068] FIG. 2 is a cross-sectional view showing an example of a process for manufacturing a laminated electrode body of an all-solid-state lithium secondary battery. First, as shown in FIG. 2A, for example, the above-mentioned negative electrode 14, solid electrolyte-containing sheet 16, and positive electrode 15 are sequentially placed in a mold 20. At this time, the outer periphery of the solid electrolyte-containing sheet 16 is set to be larger than the outer periphery of the positive electrode 15. Also, the size of the negative electrode 14 is set to be the same as that of the positive electrode 15. Next, as shown in FIG. 2B, the entire laminated negative electrode 14, solid electrolyte-containing sheet 16, and positive electrode 15 are pressed from above, so that the peripheral portion 16a of the solid electrolyte-containing sheet 16 is folded back to the positive electrode 15 side, and the peripheral portion 16a of the solid electrolyte-containing sheet 16 covers the outer peripheral side portion of the positive electrode 15, and the negative electrode 14, solid electrolyte-containing sheet 16, and positive electrode 15 are integrated. As a result, a laminated electrode body shown in FIG. 2C is obtained.

[0069] Thereafter, the laminated electrode body is housed in the aforementioned exterior body by a conventional method to form a sealed structure, whereby an all-solid-state lithium secondary battery can be manufactured. EXAMPLES

[0070] The all-solid-state lithium secondary battery disclosed in the present application will be described in detail below with reference to examples. However, the all-solid-state lithium secondary battery disclosed in the present application is not limited to the following examples.

[0071] Example 1 <Preparation of solid electrolyte-containing sheet> Xylene ("ultra-dehydrated" grade with a water content of 10 ppm or less) was used as the solvent, and a sulfide-based solid electrolyte (Li 6 P.S. 5 Cl) particles and an acrylic resin binder (butyl acrylate-acrylic acid copolymer) were mixed in a mass ratio of 100:3 with the above-mentioned solvent so that the solid content ratio was 40 mass%, and the mixture was stirred for 10 minutes with a Thinky mixer to prepare a uniform slurry. 2 The slurry was applied to the PET nonwoven fabric (Hirose Paper Co., Ltd., "05TH-8") by passing the slurry through the PET nonwoven fabric and then pulling it up. The slurry was then vacuum dried at 120°C for 1 hour to obtain a solid electrolyte-containing sheet having a thickness of 50 μm. The thickness of the nonwoven fabric in the produced solid electrolyte-containing sheet was 80% of the total thickness of the solid electrolyte-containing sheet. The proportion of the PET nonwoven fabric in the solid electrolyte-containing sheet was 25% by volume, and the proportion of the binder in the total mass of the solid electrolyte particles and the binder was 2.9% by mass.

[0072] Finally, the prepared solid electrolyte-containing sheet was punched out into a circle having a diameter of 11 mm, and used to prepare a laminated electrode body.

[0073] <Preparation of positive electrode> Using xylene ("ultra-dehydrated" grade with a water content of 10 ppm or less) as a solvent, LiNi with an average particle size of 3 μm, on whose surface an amorphous composite oxide of Li and Nb was formed, was0.6 Co 0.2 Mn 0.2 O 2 and sulfide-based solid electrolyte (Li 6 P.S. 5 Cl) particles, carbon nanotubes ("VGCF" (product name) manufactured by Showa Denko K.K.) as a conductive additive, and an acrylic resin binder (butyl acrylate-acrylic acid copolymer) were mixed with the above solvent in a mass ratio of 50:44:3:3 to give a solid content ratio of 50 mass%, and the mixture was stirred for 10 minutes with a Thinky mixer to prepare a uniform slurry. This slurry was applied to an Al foil with a thickness of 20 μm with an applicator leaving a gap of 200 μm, and the mixture was vacuum dried at 120°C to obtain a positive electrode.

[0074] Finally, the prepared positive electrode was punched out into a circle having a diameter of 10 mm, and used to prepare a laminated electrode body.

[0075] <Preparation of negative electrode> Xylene ("ultra-dehydrated" grade with a water content of 10 ppm or less) was used as a solvent, and graphite with an average particle size of 20 μm and a sulfide-based solid electrolyte (Li 6 P.S. 5 Cl) particles and an acrylic resin binder (butyl acrylate-acrylic acid copolymer) were mixed in a mass ratio of 50:47:3 with the above solvent so that the solid content ratio was 50 mass%, and the mixture was stirred for 10 minutes with a Thinky mixer to prepare a uniform slurry. This slurry was applied to a 20 μm-thick stainless steel foil with an applicator leaving a gap of 200 μm, and the negative electrode was obtained by vacuum drying at 120 °C.

[0076] Finally, the produced negative electrode was punched out into a circle having a diameter of 10 mm, and used to produce a laminated electrode body.

[0077] <Battery assembly> First, as shown in FIG. 2A, the prepared negative electrode, solid electrolyte-containing sheet, and positive electrode were placed in a mold so that the negative electrode mixture layer and the positive electrode mixture layer were disposed on the solid electrolyte-containing sheet side. At this time, the solid electrolyte-containing sheet was placed so that its center point was aligned with the center points of the negative electrode and the positive electrode. Next, as shown in FIG. 2B, the entire stacked negative electrode, solid electrolyte-containing sheet, and positive electrode were pressurized from above with 392 MPa (4 tf / cm 2 ) was applied to the negative electrode 14 at a pressure of 1000 V. The peripheral portion of the solid electrolyte-containing sheet was folded back toward the positive electrode side so that the peripheral portion of the solid electrolyte-containing sheet covered the outer circumferential side portion of the positive electrode, and the negative electrode, the solid electrolyte-containing sheet, and the positive electrode were integrated together to obtain the laminated electrode body shown in FIG. 2C.

[0078] Finally, as shown in FIG. 1, the laminated electrode body was housed in a stainless steel exterior body to prepare an all-solid-state lithium secondary battery of Example 1.

[0079] Comparative Example 1 The solid electrolyte-containing sheet, positive electrode, and negative electrode were all punched out into circles with a diameter of 10 mm, and the centers of each were aligned and stacked. The whole was then pressurized under a pressure of 392 MPa (4 tf / cm 2 ) to prepare a laminated electrode body. Finally, an all-solid-state lithium secondary battery of Comparative Example 1 was prepared in the same manner as in Example 1.

[0080] <Evaluation of all-solid-state lithium secondary batteries> When the voltages of the batteries of Example 1 and Comparative Example 1 were measured, 0.4 V was measured for the battery of Example 1, but no voltage could be measured for Comparative Example 1. This is believed to be because, in the laminated electrode body of Comparative Example 1, the solid electrolyte-containing sheet, the positive electrode, and the negative electrode are all formed to the same size, and the solid electrolyte-containing sheet does not cover the outer peripheral side surface of the positive electrode or the negative electrode, so that the outer peripheral end of the positive electrode comes into contact with the outer peripheral end of the negative electrode, causing a short circuit. In contrast, in the laminated electrode body of Example 1, the peripheral portion of the solid electrolyte-containing sheet is folded back to the positive electrode side, and the peripheral portion of the solid electrolyte-containing sheet covers the outer peripheral side surface of the positive electrode, so that the contact between the outer peripheral end of the positive electrode and the outer peripheral end of the negative electrode is prevented, and it is believed that no short circuit occurs. [Industrial Applicability]

[0081] The all-solid-state lithium secondary battery disclosed in the present application can prevent the occurrence of short circuits at the outer peripheral ends of the positive and negative electrodes even if the thickness of the solid electrolyte layer is thin, and can realize an all-solid-state lithium secondary battery with high capacity and high energy density, which can be preferably used as a power source for various electronic devices (particularly portable electronic devices such as mobile phones and notebook personal computers). [Explanation of symbols]

[0082] 10 All-solid-state lithium secondary battery 11 Outer can 12 Sealed cans 13 Gasket 14 Negative electrode 15 Positive electrode 16 Solid electrolyte-containing sheet 16a Periphery 20 Mold

Claims

1. an electrode preparation step of preparing a positive electrode and a negative electrode having the same size as the positive electrode; a filling step of filling an insulating porous substrate with solid electrolyte particles to prepare a solid electrolyte-containing sheet; a lamination step of laminating the positive electrode, the solid electrolyte-containing sheet, and the negative electrode in this order; and a folding step of folding back a peripheral portion of the solid electrolyte-containing sheet onto an outer periphery of one of the stacked positive electrode or negative electrode to cover an outer periphery of the positive electrode or the negative electrode with the peripheral portion of the solid electrolyte-containing sheet.

2. The method for producing an all-solid-state lithium secondary battery according to claim 1 , wherein the insulating porous substrate is further filled with a binder in the filling step.

Citation Information

Patent Citations

  • All solid lithium secondary battery

    JP2009064644A

  • Manufacturing method of all-solid lithium ion secondary battery

    JP2010282803A

  • Secondary battery

    JP2014041817A

  • Method for manufacturing all-solid battery

    JP2015153663A

  • Solid electrolyte sheet and all-solid type secondary battery

    JP2016031789A