Lithium-ion secondary battery
The lithium ion secondary battery design with controlled separation distances between electrode layers in a roll-like form addresses poor performance issues by ensuring electrolyte penetration and efficient current collection, enhancing capacity and discharge rates.
Patent Information
- Application Number
- JP2020215597
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Existing wound-type lithium ion secondary batteries with an integral sintered body structure for positive, ceramic separator, and negative electrode layers suffer from poor battery performance, including capacity and discharge rate characteristics due to insufficient gaps for electrolyte penetration.
A lithium ion secondary battery design with a roll-like form where the positive and negative electrode layers are separated by a ceramic separator, forming an integral sintered body with controlled separation distances between adjacent sheets, creating gaps for electrolyte impregnation and improved current collection.
The design enhances battery performance by improving capacity and discharge rate characteristics through effective electrolyte penetration and efficient current collection, maintaining shape retention while optimizing the separation distances between electrode layers.
Smart Images

Figure 0007579697000002 
Figure 0007579697000003 
Figure 0007579697000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a lithium ion secondary battery. [Background technology]
[0002] Lithium-ion secondary batteries are widely used in various devices that require charging. Many existing lithium-ion secondary batteries use a powder-dispersed positive electrode (so-called coated electrode) that is made by coating and drying a positive electrode mixture that contains a positive electrode active material, a conductive additive, a binder, etc.
[0003] In general, a powder-dispersed positive electrode contains a relatively large amount (for example, about 10% by weight) of components (binders and conductive assistants) that do not contribute to capacity, so the packing density of the lithium composite oxide as the positive electrode active material is low. For this reason, the powder-dispersed positive electrode has a large room for improvement in terms of capacity and charge / discharge efficiency. Therefore, attempts have been made to improve the capacity and charge / discharge efficiency by forming the positive electrode or the positive electrode active material layer from a lithium composite oxide sintered plate. In this case, since the positive electrode or the positive electrode active material layer does not contain a binder or conductive assistant (for example, conductive carbon), it is expected that a high capacity and good charge / discharge efficiency can be obtained by increasing the packing density of the lithium composite oxide. For example, Patent Document 1 (Patent Publication No. 5587052) discloses a positive electrode of a lithium ion secondary battery that includes a positive electrode collector and a positive electrode active material layer bonded to the positive electrode collector via a conductive bonding layer. The positive electrode active material layer is said to be made of a lithium composite oxide sintered plate having a thickness of 30 μm or more, a porosity of 3 to 30%, and an open pore ratio of 70% or more. In addition, Patent Document 2 (Japanese Patent No. 6374634) describes lithium cobalt oxide LiCoO 2The lithium composite oxide sintered plate has a structure in which a plurality of primary particles having a layered rock salt structure are bonded together, and has a porosity of 3 to 40%, an average pore size of 15 μm or less, an open pore ratio of 70% or more, a thickness of 15 to 200 μm, and a primary particle size, which is the average particle size of the plurality of primary particles, of 20 μm or less. The lithium composite oxide sintered plate is also said to have an average angle, i.e., an average tilt angle, between the (003) plane of the plurality of primary particles and the plate surface of the lithium composite oxide sintered plate, which is greater than 0° and less than 30°.
[0004] On the other hand, it has also been proposed to use a titanium-containing sintered plate as the negative electrode. For example, Patent Document 3 (JP Patent Publication 2015-185337 A) proposes using lithium titanate (Li 4 Ti 5 O 12 Patent Document 4 (Japanese Patent No. 6392493) discloses a lithium ion secondary battery using a sintered body of lithium titanate Li 4 Ti 5 O 12 The LTO sintered plate has a structure in which multiple primary particles are bonded together, and is said to have a thickness of 10 to 290 μm, a primary particle size, which is the average particle size of the multiple primary particles, of 1.2 μm or less, a porosity of 21 to 45%, and an open pore ratio of 60% or more.
[0005] Lithium ion secondary batteries have also been proposed that achieve both high discharge capacity and excellent charge / discharge cycle performance by adopting a configuration in which the positive electrode layer, separator, and negative electrode layer as a whole form a single integrated sintered plate. For example, Patent Document 5 (WO2019 / 221140A1) discloses a lithium ion secondary battery that includes a positive electrode layer made of a sintered body of a lithium composite oxide (e.g., lithium cobalt oxide), a negative electrode layer made of a titanium-containing sintered body (e.g., lithium titanate), a ceramic separator, and an electrolyte impregnated into the ceramic separator. In this battery, the positive electrode layer, the ceramic separator, and the negative electrode layer as a whole form a single integrated sintered plate, thereby bonding the positive electrode layer, the ceramic separator, and the negative electrode layer to each other.
[0006] Meanwhile, batteries in which a wound type battery element is housed inside an outer can are known. For example, Patent Document 6 (Japanese Patent No. 5767115) discloses a button battery provided with an electrode / separator composite that exists as a spiral roll. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 5587052 [Patent Document 2] Patent No. 6374634 [Patent Document 3] JP 2015-185337 A [Patent Document 4] Patent No. 6392493 [Patent Document 5] WO2019 / 221140A1 [Patent Document 6] Patent No. 5767115 Summary of the Invention
[0008] However, when attempts were made to fabricate a wound battery using a type of battery in which the positive electrode layer, ceramic separator, and negative electrode layer as a whole form a single integrated sintered body, it was found that the battery performance, such as capacity and discharge rate characteristics, was poor.
[0009] The present inventors have now discovered that in an integrally sintered body type wound lithium ion secondary battery in which a positive electrode layer, a ceramic separator, and a negative electrode layer as a whole form a single integral sintered body, by providing a gap between the layers and controlling the gap distance, it is possible to improve battery performance such as capacity and discharge rate characteristics.
[0010] SUMMARY OF THE PRESENT DISCLOSURE OF THE PRESENT DISCLOSURE An object of the present invention is to provide an integrally sintered body type wound lithium ion secondary battery having improved battery performance such as capacity and discharge rate characteristics.
[0011] According to one aspect of the present invention, (a) A battery element having a roll-like form in which a power generating sheet including a ceramic positive electrode layer, a ceramic separator, a ceramic negative electrode layer, and a ceramic insulating layer is wound, and which forms a single integral sintered body as a whole, an opposing portion that constitutes a main portion of the roll away from both side ends and where the ceramic positive electrode layer and the ceramic negative electrode layer face each other via the ceramic separator; a non-facing portion that constitutes an outer circumferential portion along both side ends of the roll, the non-facing portion including either the ceramic positive electrode layer or the ceramic negative electrode layer but not including the other, such that the ceramic positive electrode layer and the ceramic negative electrode layer do not face each other alternately; A battery element having (b) an electrolyte impregnated in the battery element; (c) an exterior body that houses the battery element and the electrolyte; A lithium ion secondary battery comprising: The battery element includes a lithium ion secondary battery in which adjacent power generating sheets are spaced apart to form a gap, and the separation distance X between the adjacent power generating sheets in the non-facing portion is greater than the separation distance Y between the adjacent power generating sheets in the facing portion. [Brief description of the drawings]
[0012] [Figure 1A] FIG. 1 is a schematic cross-sectional view conceptually illustrating an example of a lithium ion secondary battery of the present invention. [Figure 1B] FIG. 1B is a schematic cross-sectional view of the electrode element shown in FIG. 1A. [Diagram 2] 1 is a SEM image showing an example of a cross section perpendicular to the layer surface of an oriented positive electrode layer. [Diagram 3] 3 is an EBSD image of a cross section of the oriented positive electrode layer shown in FIG. 2. [Figure 4] FIG. 4 is a histogram showing the distribution of orientation angles of primary particles in the EBSD image of FIG. 3 on an area basis. [Figure 5A] FIG. 2 is a perspective view of the green sheet laminate produced in Examples 1 to 4. [Figure 5B] 5B is a cross-sectional view of the green sheet laminate shown in FIG. 5A taken along line 5B-5B. [Figure 5C] FIG. 6 is a diagram showing a cross-sectional structure of the green sheet laminate shown in FIGS. 5A and 5B after cutting. [Figure 6A] 1 is a photograph of the battery element (roll-shaped integrated sintered body) produced in Example 1. [Figure 6B] 1 is a cross-sectional SEM image of a battery element (roll-shaped integrated sintered body) produced in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] 1A and 1B show an example of the lithium ion secondary battery of the present invention. The lithium ion secondary battery 10 shown in FIG. 1A and 1B is in the form of a coin-shaped battery, but the present invention is not limited thereto, and may be a battery in other forms such as a button-shaped battery, a cylindrical battery, or a pack-shaped battery. The lithium ion secondary battery 10 includes a battery element 12, an electrolyte 24 impregnated in the battery element 12, and an exterior body 26 in which the battery element 12 and the electrolyte 24 are accommodated. The battery element 12 has a roll-like form in which a power generating sheet 22 including a ceramic positive electrode layer 14, a ceramic separator 16, a ceramic negative electrode layer 18, and a ceramic insulating layer 20 is wound, and forms an integral sintered body as a whole. The battery element 12 has an opposing portion 12y and a non-opposing portion 12x. The opposing portion 12y constitutes a main portion away from both side ends of the roll, and is a portion where the ceramic positive electrode layer 14 and the ceramic negative electrode layer 18 face each other via the ceramic separator 16. On the other hand, the non-facing portion 12x constitutes an outer peripheral portion along both side ends of the roll, and includes either the ceramic positive electrode layer 14 or the ceramic negative electrode layer 18, but does not include the other, so that the ceramic positive electrode layer 14 and the ceramic negative electrode layer 18 do not face each other alternately. In the battery element 12, the adjacent power generating sheets 22 are separated to form a gap G, and the separation distance X between the adjacent power generating sheets 22 in the non-facing portion is larger than the separation distance Y between the adjacent power generating sheets 22 in the facing portion. In this way, in an integrated sintered body type wound lithium ion secondary battery in which the ceramic positive electrode layer 14, the ceramic separator 16, and the ceramic negative electrode layer 18 form a single integrated sintered body as a whole, the gap G is provided between the power generating sheets 22, and the separation distances X and Y are controlled, thereby improving the battery performance such as the capacity and the discharge rate characteristics.
[0014] As described above, a lithium-ion secondary battery has been proposed that achieves both high discharge capacity and excellent charge / discharge cycle performance by adopting a configuration in which the positive electrode layer, the separator, and the negative electrode layer form a single integrated sintered plate as a whole (see, for example, Patent Document 5 (WO2019 / 221140A1)). However, when an attempt was made to manufacture a wound battery using a type of battery in which the positive electrode layer, the ceramic separator, and the negative electrode layer form a single integrated sintered body as a whole, it was found that the battery performance, such as capacity and discharge rate characteristics, was poor. This problem is conveniently solved by the present invention. The reason for this is considered to be as follows. That is, if there are few gaps in the wound battery elements, it becomes difficult for the electrolyte to penetrate, and the battery performance deteriorates. Therefore, by providing a gap G between the power generation sheets 22 and controlling the separation distances X and Y, the electrolyte 24 becomes more likely to penetrate into the gap G, and as a result, the battery performance, such as capacity and discharge rate characteristics, can be improved. In this regard, in the case of coated electrodes (containing active material paste rather than sintered electrodes) that have been used in conventional wound batteries, if the winding is loosened to form gaps, problems such as poor shape retention, reduced performance, and increased volume arise. However, the integrally sintered wound battery of the present invention has good shape retention and does not suffer from such problems.
[0015] As described above, in the battery element 12, adjacent power generating sheets 22 are spaced apart to form a gap G, and the separation distance X between adjacent power generating sheets 22 in the non-facing portions 12x is greater than the separation distance Y between adjacent power generating sheets 22 in the facing portions 12y. Specifically, the ratio of the separation distance X between adjacent power generating sheets in the non-facing portions to the separation distance Y between adjacent power generating sheets in the facing portions is preferably 1.3 to 10, more preferably 2 to 9, even more preferably 3 to 8, particularly preferably 4 to 7, and most preferably 5 to 6. In addition, the separation distance X between adjacent power generating sheets 22 in the non-facing portions 12x is preferably 20 μm or less, more preferably 1 to 18 μm, even more preferably 2 to 16 μm, particularly preferably 3 to 14 μm, and most preferably 4 to 13 μm. As described in the examples below, the separation distance X or Y can be determined by adding up the distances of all the gaps G in each non-facing portion 12x or facing portion 12y by cross-sectional SEM observation, dividing the total value by the number of gaps G (the number of stacked power generating sheets 22 minus 1) to calculate the average value. Note that in both the separation distance X and the separation distance Y, the internal space corresponding to the roll core portion is not considered to be a gap G. Note that, when there are two or more non-facing portions 12x as shown in FIG. 1B, it is sufficient that the separation distance X in at least one non-facing portion 12 satisfies the above condition, but it is preferable that the separation distance X in all of the two or more non-facing portions 12x satisfies the above condition.
[0016] Typically, the non-facing portion 12x includes a first non-facing portion 12x constituting a first outer periphery along one side end of the roll, and a second non-facing portion 12x constituting a second outer periphery along the other side end of the roll. In this case, it is preferable that the first non-facing portion 12x includes the ceramic positive electrode layer 14 and does not include the ceramic negative electrode layer 18, and the second non-facing portion 12x includes the ceramic negative electrode layer 18 and does not include the ceramic positive electrode layer 14. Specifically, it is preferable that a ceramic insulating layer 20, or a ceramic separator 16 and a ceramic insulating layer 20 are interposed between adjacent ceramic positive electrode layers 14 in the first non-facing portion 12x. It is also preferable that a ceramic insulating layer 20, or a ceramic separator 16 and a ceramic insulating layer 20 are interposed between adjacent ceramic negative electrode layers 18 in the second non-facing portion 12x. This makes it easier to collect current from the ceramic positive electrode layer 14 at the first non-facing portion 12x, while making it easier to collect current from the ceramic negative electrode layer 18 at the second non-facing portion 12x opposite the first non-facing portion 12x.
[0017] The facing portion 12y preferably has a layer structure in which stacking units, each having a ceramic separator 16 interposed between a ceramic positive electrode layer 14 and a ceramic negative electrode layer 18, are repeated in the roll radial direction with a ceramic insulating layer 20 interposed between adjacent stacking units. This allows a repeating positive electrode / separator / negative electrode cell structure, resulting in a desirable wound cell stack (multilayer cell) structure. As a result, it is possible to more effectively achieve both high voltage and large current and improved rate characteristics.
[0018] It is preferable that a ceramic insulating layer 20 is positioned as the outermost layer on the outer circumferential surface of the roll of the battery element 12. This makes it difficult for electrical short circuits to occur.
[0019] The battery element 12 has a roll-like form in which a power generating sheet 22 is wound. For convenience of explanation, the battery element 12 shown in FIG. 1A is drawn with two turns per roll, but the number of turns per roll is preferably 3 or more, more preferably 4 or more, even more preferably 5 or more, and particularly preferably 6 or more. The power generating sheet 2 includes a ceramic positive electrode layer 14, a ceramic separator 16, a ceramic negative electrode layer 18, and a ceramic insulating layer 20. The thickness of the power generating sheet 22 is preferably 22 to 1080 μm, more preferably 25 to 500 μm, even more preferably 30 to 300 μm, and particularly preferably 40 to 200 μm.
[0020] The ceramic positive electrode layer 14 (hereinafter referred to as the positive electrode layer 14 or the oriented positive electrode layer 14) is preferably made of a lithium composite oxide sintered body. The fact that the positive electrode layer 14 is made of a sintered body means that the positive electrode layer 14 does not contain a binder or a conductive assistant. This is because even if the green sheet contains a binder, the binder will disappear or be burned away during firing. Furthermore, the fact that the positive electrode layer 14 does not contain a binder has the advantage that deterioration of the positive electrode due to the electrolyte 24 can be avoided. The lithium composite oxide that constitutes the sintered body is lithium cobalt oxide (typically LiCoO 2 (hereinafter, sometimes abbreviated as LCO) is particularly preferable. Various lithium composite oxide sintered plates or LCO sintered plates are known, and for example, those disclosed in Patent Document 1 (Japanese Patent No. 5587052) and Patent Document 2 (Japanese Patent No. 6374634) can be referred to.
[0021] According to a preferred embodiment of the present invention, the positive electrode layer 14, i.e., the lithium composite oxide sintered body plate, is an oriented positive electrode layer that includes a plurality of primary particles composed of a lithium composite oxide, and the plurality of primary particles are oriented at an average orientation angle of more than 0° and not more than 30° with respect to the layer surface of the positive electrode layer. In the present invention, since the battery element 12 is in a roll shape, the positive electrode layer 14 also has a curved surface, but the layer surface of the positive electrode layer that is the reference (0°) of the average orientation angle is flat when viewed in a direction parallel to the roll axis, so that the average orientation angle can be accurately determined by observing a cross section parallel to the roll axis of the positive electrode layer 14. FIG. 2 shows an example of a cross-sectional SEM image perpendicular to the layer surface of the oriented positive electrode layer 14, while FIG. 3 shows an electron backscatter diffraction (EBSD) image of a cross section perpendicular to the layer surface of the oriented positive electrode layer 14. FIG. 4 shows a histogram showing the distribution of the orientation angles of the primary particles 11 in the EBSD image of FIG. 3 on an area basis. In the EBSD image shown in FIG. 3, discontinuity of the crystal orientation can be observed. In Fig. 3, the orientation angle of each primary particle 11 is indicated by a shade of color, and the darker the color, the smaller the orientation angle. The orientation angle is the inclination angle of the (003) plane of each primary particle 11 with respect to the layer surface direction. In Figs. 2 and 3, the areas shown in black inside the oriented positive electrode layer 14 are pores.
[0022] The oriented positive electrode layer 14 is an oriented sintered body composed of a plurality of primary particles 11 bonded to each other. Each primary particle 11 is mainly plate-shaped, but may also be formed into a rectangular parallelepiped, cubic, spherical, or other shape. The cross-sectional shape of each primary particle 11 is not particularly limited, and may be rectangular, a polygonal shape other than a rectangle, a circle, an ellipse, or any other complex shape.
[0023] Each primary particle 11 is composed of a lithium composite oxide. x MO 2It is an oxide represented by (0.05 < x < 1.10, where M is at least one transition metal, and M typically includes one or more of Co, Ni, and Mn). The lithium composite oxide has a layered rock salt structure. The layered rock salt structure refers to a crystal structure in which lithium layers and transition metal layers other than lithium are alternately stacked with oxygen layers in between, that is, a crystal structure in which transition metal ion layers and single lithium layers are alternately stacked via oxide ions (typically the
[0111] axis direction of the α-NaFeO 2 type structure, that is, a structure in which transition metals and lithium are regularly arranged in the
[0111] axis direction of the cubic rock salt type structure). Examples of the lithium composite oxide include Li x CoO 2 (lithium cobalt oxide), Li x NiO 2 (lithium nickel oxide), Li x MnO 2 (lithium manganate), Li x NiMnO 2 (lithium nickel manganate), Li x NiCoO 2 (lithium nickel cobalt oxide), Li x CoNiMnO 2 (lithium cobalt nickel manganate), Li x CoMnO 2 (lithium cobalt manganate), etc. Particularly preferred is Li x CoO 2 (lithium cobalt oxide, typically LiCoO 2 ). The lithium composite oxide may contain one or more elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, Ag, Sn, Sb, Te, Ba, Bi, and W.
[0024] As shown in Figs. 3 and 4, the average value of the orientation angles of the primary particles 11, that is, the average orientation angle, is more than 0° and not more than 30°. This brings about various advantages as follows. First, since each primary particle 11 is in a state of lying inclined with respect to the thickness direction, the adhesion between each primary particle can be improved. As a result, the lithium ion conductivity between a certain primary particle 11 and other primary particles 11 adjacent to both sides of the primary particle 11 in the longitudinal direction can be improved, so that the rate characteristics can be improved. Secondly, the rate characteristics can be further improved. This is because, as described above, in the oriented positive electrode layer 14, expansion and contraction in the thickness direction is dominant over the layer surface direction when lithium ions enter and exit, so that the expansion and contraction of the oriented positive electrode layer 14 becomes smooth, and accordingly, the entry and exit of lithium ions also becomes smooth. Thirdly, the expansion and contraction of the oriented positive electrode layer 14 accompanying the entry and exit of lithium ions occurs predominantly in the direction perpendicular to the layer surface, so that stress is less likely to occur at the bonding interface between the oriented positive electrode layer 14 and the ceramic separator 16, making it easier to maintain good bonding at the interface.
[0025] The average orientation angle of the primary particles 11 is obtained by the following method. First, in an EBSD image of a rectangular region of 95 μm×125 μm observed at a magnification of 1000 times as shown in FIG. 3, three horizontal lines are drawn to divide the oriented positive electrode layer 14 into four equal parts in the thickness direction, and three vertical lines are drawn to divide the oriented positive electrode layer 14 into four equal parts in the layer surface direction. Next, the average orientation angle of the primary particles 11 is obtained by arithmetically averaging the orientation angles of all the primary particles 11 that intersect with at least one of the three horizontal lines and the three vertical lines. From the viewpoint of further improving the rate characteristics, the average orientation angle of the primary particles 11 is preferably 30° or less, more preferably 25° or less. From the viewpoint of further improving the rate characteristics, the average orientation angle of the primary particles 11 is preferably 2° or more, more preferably 5° or more.
[0026] As shown in FIG. 4, the orientation angle of each primary particle 11 may be widely distributed from 0° to 90°, but it is preferable that the majority of the orientation angles are distributed in the region of more than 0° and less than 30°. That is, when the cross section of the oriented sintered body constituting the oriented positive electrode layer 14 is analyzed by EBSD, the total area of the primary particles 11 (hereinafter referred to as low-angle primary particles) having an orientation angle of more than 0° and less than 30° with respect to the layer surface of the oriented positive electrode layer 14 among the primary particles 11 contained in the analyzed cross section is preferably 70% or more, more preferably 80% or more, relative to the total area of the primary particles 11 contained in the cross section (specifically, the 30 primary particles 11 used to calculate the average orientation angle). This makes it possible to increase the proportion of primary particles 11 with high mutual adhesion, thereby further improving the rate characteristics. In addition, it is more preferable that the total area of the low-angle primary particles having an orientation angle of 20° or less is 50% or more relative to the total area of the 30 primary particles 11 used to calculate the average orientation angle. Furthermore, the total area of the low-angle primary particles having an orientation angle of 10° or less is more preferably 15% or more of the total area of the 30 primary particles 11 used to calculate the average orientation angle.
[0027] Since each primary particle 11 is mainly plate-like, as shown in Figs. 2 and 3, the cross section of each primary particle 11 extends in a predetermined direction and is typically approximately rectangular. That is, when the cross section of the oriented sintered body is analyzed by EBSD, the total area of the primary particles 11 having an aspect ratio of 4 or more among the primary particles 11 included in the analyzed cross section is preferably 70% or more, more preferably 80% or more, of the total area of the primary particles 11 included in the cross section (specifically, the 30 primary particles 11 used to calculate the average orientation angle). Specifically, in the EBSD image shown in Fig. 3, this can further improve the mutual adhesion between the primary particles 11, and as a result, the rate characteristics can be further improved. The aspect ratio of the primary particles 11 is the value obtained by dividing the maximum Feret diameter of the primary particles 11 by the minimum Feret diameter. The maximum Feret diameter is the maximum distance between two parallel straight lines when the primary particle 11 is sandwiched between the two parallel straight lines on the EBSD image when the cross section is observed. The minimum Feret diameter is the minimum distance between two parallel lines when the primary particle 11 is sandwiched between the lines on an EBSD image.
[0028] The average particle size of the primary particles constituting the oriented sintered body is preferably 5 μm or more. Specifically, the average particle size of the 30 primary particles 11 used to calculate the average orientation angle is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 12 μm or more. This reduces the number of grain boundaries between the primary particles 11 in the direction in which lithium ions are conducted, improving the overall lithium ion conductivity, and thus improving the rate characteristics. The average particle size of the primary particles 11 is the arithmetic average of the circle-equivalent diameters of the primary particles 11. The circle-equivalent diameter is the diameter of a circle having the same area as each primary particle 11 on an EBSD image.
[0029] The positive electrode layer 14 preferably contains pores. When the sintered body contains pores, particularly open pores, the electrolyte can penetrate into the sintered body when the sintered body is incorporated into a battery as a positive electrode plate, and as a result, the lithium ion conductivity can be improved. This is because the conduction of lithium ions in the sintered body is by far faster than the conduction through the electrolyte in the pores, although there are two types of conduction: through the constituent particles of the sintered body and through the electrolyte in the pores.
[0030] The positive electrode layer 14, i.e., the lithium composite oxide sintered body, preferably has a porosity of 20 to 60%, more preferably 25 to 55%, further preferably 30 to 50%, and particularly preferably 30 to 45%. The pores are expected to provide a stress relief effect and a high capacity, and the mutual adhesion between the primary particles 11 can be further improved, thereby further improving the rate characteristics. The porosity of the sintered body is calculated by polishing the cross section of the positive electrode layer with a CP (cross section polisher) and then observing the SEM at 1000 magnifications, and binarizing the obtained SEM image. The average circle equivalent diameter of each pore formed inside the oriented sintered body is not particularly limited, but is preferably 8 μm or less. The smaller the average circle equivalent diameter of each pore, the more the mutual adhesion between the primary particles 11 can be further improved, and as a result, the rate characteristics can be further improved. The average circle equivalent diameter of the pores is the arithmetic average of the circle equivalent diameters of 10 pores on the EBSD image. The circle equivalent diameter is the diameter of a circle having the same area as each pore on the EBSD image. Each pore formed inside the oriented sintered body is preferably an open pore that communicates with the outside of the positive electrode layer 14.
[0031] The average pore size of the positive electrode layer 14, i.e., the lithium composite oxide sintered body, is preferably 0.1 to 10.0 μm, more preferably 0.2 to 5.0 μm, and further preferably 0.25 to 3.0 μm. Within the above range, local stress concentration in large pores is suppressed, and stress in the sintered body is easily released uniformly.
[0032] The thickness of the positive electrode layer 14 is preferably 10 to 500 μm, more preferably 15 to 250 μm, and further preferably 20 to 100 μm. Within such a range, the active material capacity per unit area is increased to improve the energy density of the lithium-ion secondary battery 10, and deterioration of the battery characteristics (particularly an increase in the resistance value) due to repeated charging and discharging can be suppressed.
[0033] The negative electrode layer 18 is preferably made of a titanium-containing sintered body. The titanium-containing sintered body is preferably lithium titanate Li 4 Ti 5 O 12 (hereinafter referred to as LTO) or niobium titanium composite oxide Nb 2 TiO 7 Preferably, the battery contains Li, more preferably LTO. Although LTO is typically known to have a spinel structure, it can also have other structures during charging and discharging. For example, LTO contains Li 4 Ti 5 O 12 (spinel structure) and Li 7 Ti 5 O 12 The reaction proceeds in the coexistence of two phases, i.e., spinel and tetrahydrofuran (rock salt structure). Therefore, LTO is not limited to a spinel structure.
[0034] The negative electrode layer 18 being made of a sintered body means that the negative electrode layer 18 does not contain a binder or a conductive additive. This is because even if the green sheet contains a binder, the binder will disappear or be burned away during firing. Since the negative electrode layer does not contain a binder, the negative electrode active material (e.g., LTO or Nb 2 TiO 7 By increasing the packing density of the LTO sintered body, it is possible to obtain a high capacity and good charge / discharge efficiency. The LTO sintered body can be produced according to the methods described in Patent Document 3 (JP Patent Publication 2015-185337 A) and Patent Document 4 (JP Patent No. 6392493 A).
[0035] The negative electrode layer 18, i.e., the titanium-containing sintered body, has a structure in which a plurality (i.e., a large number) of primary particles are bonded together. 2 TiO 7 It is preferable that the ion exchange membrane 100 is composed of the following:
[0036] The thickness of the negative electrode layer 18 is preferably 10 to 500 μm, more preferably 15 to 250 μm, and further preferably 20 to 100 μm. The thicker the negative electrode layer 18, the easier it is to realize a battery with a high capacity and high energy density. The thickness of the negative electrode layer 18 can be obtained, for example, by measuring the distance between layer surfaces observed to be approximately parallel when a cross section of the negative electrode layer 18 is observed by SEM (scanning electron microscope).
[0037] The primary particle size, which is the average particle size of the multiple primary particles constituting the negative electrode layer 18, is preferably 1.2 μm or less, more preferably 0.02 to 1.2 μm, and further preferably 0.05 to 0.7 μm. Within such a range, it is easy to achieve both lithium ion conductivity and electronic conductivity, which contributes to improving the rate performance.
[0038] The negative electrode layer 18 preferably contains pores. When the sintered body contains pores, particularly open pores, and is incorporated into a battery as a negative electrode layer, the electrolyte can penetrate into the sintered body, thereby improving the lithium ion conductivity. This is because the conduction of lithium ions in the sintered body is by far faster than the conduction through the electrolyte in the pores, although there are two types of conduction: through the constituent particles of the sintered body and through the electrolyte in the pores.
[0039] The porosity of the negative electrode layer 18 is preferably 20 to 60%, more preferably 30 to 55%, and further preferably 35 to 50%. Within such a range, it is easy to achieve both lithium ion conductivity and electronic conductivity, which contributes to improving the rate performance.
[0040] The average pore size of the negative electrode layer 18 is 0.08 to 5.0 μm, preferably 0.1 to 3.0 μm, and more preferably 0.12 to 1.5 μm. Within such a range, it is easy to achieve both lithium ion conductivity and electronic conductivity, which contributes to improving the rate performance.
[0041] The ceramic separator 16 is a microporous film made of ceramic. The ceramic separator 16 is advantageous in that it can be manufactured as a single integrated sintered body together with the positive electrode layer 14, the negative electrode layer 18, and the current collecting layer 21, as well as having excellent heat resistance. The ceramics contained in the ceramic separator 16 are MgO, Al 2 O 3 , ZrO 2 , SiC, Si 3 N 4 , AlN, and cordierite, and more preferably MgO, Al 2 O 3 , and ZrO 2 At least one selected from the following. The thickness of the ceramic separator 16 is preferably 1 to 40 μm, more preferably 2 to 30 μm, and further preferably 3 to 20 μm. The porosity of the ceramic separator 16 is preferably 30 to 85%, and more preferably 40 to 80%.
[0042] The ceramic separator 16 may contain a glass component from the viewpoint of improving the adhesion between the positive electrode layer 14 and the negative electrode layer 18. In this case, the content of the glass component in the ceramic separator 16 is preferably 0.1 to 50% by weight, more preferably 0.5 to 40% by weight, and further preferably 0.5 to 30% by weight, based on the total weight of the ceramic separator 16. The glass component is preferably added to the ceramic separator 16 by adding glass frit to the raw material powder of the ceramic separator. However, as long as the desired adhesion between the ceramic separator 16 and the positive electrode layer 14 and the negative electrode layer 18 can be ensured, it is not particularly necessary for the ceramic separator 16 to contain a glass component.
[0043] The ceramic insulating layer 20 can have the same structure as the ceramic separator 16. Therefore, the ceramic contained in the ceramic insulating layer 20 is MgO, Al 2 O 3 , ZrO 2 , SiC, Si 3 N 4 , AlN, and cordierite, and more preferably MgO, Al 2 O 3 , and ZrO 2 At least one selected from the following. The ceramic insulating layer 20 has a thickness of preferably 10 to 500 μm, more preferably 15 to 250 μm, and further preferably 20 to 100 μm. The insulating layer 20 has a porosity of preferably 30 to 85%, and more preferably 40 to 80%.
[0044] The battery element 12 preferably further includes a current collecting layer 21 on the surface of the ceramic negative electrode layer 18 opposite to the ceramic positive electrode layer 14. The current collecting layer 21 is not particularly limited as long as it is a layer containing a conductive material, but it is preferable that the current collecting layer 21 contains at least one selected from the group consisting of Au, Pt, Pd, and Cu. The thickness of the current collecting layer 21 is preferably 0.05 to 10 μm, more preferably 0.1 to 5 μm, and even more preferably 0.1 to 3 μm. The current collecting layer 21 is essential on the negative electrode layer 18 side, but the current collecting layer 21 may or may not be present on the positive electrode layer 14 side. For example, when the positive electrode layer 14 is an oriented positive electrode layer, it has excellent electronic conductivity, so that the positive electrode layer 14 itself can have a current collecting function without using the current collecting layer 21.
[0045] The electrolyte 24 is not particularly limited, and may be a lithium salt (e.g., LiPF ) in a non-aqueous solvent of an organic solvent (e.g., a mixed solvent of ethylene carbonate (EC) and methyl ethyl carbonate (MEC), a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC), or a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC)). 6 A commercially available electrolyte for lithium batteries, such as a solution containing Cr-Cr salt, may be used.
[0046] In order to obtain a lithium ion secondary battery having excellent heat resistance, the electrolyte 24 is a non-aqueous solvent containing lithium borofluoride (LiBF 4 In this case, the preferred non-aqueous solvent is at least one selected from the group consisting of γ-butyrolactone (GBL), ethylene carbonate (EC) and propylene carbonate (PC), more preferably a mixed solvent of EC and GBL, a single solvent of PC, a mixed solvent of PC and GBL, or a single solvent of GBL, and particularly preferably a mixed solvent of EC and GBL or a single solvent of GBL. By including γ-butyrolactone (GBL), the boiling point of the non-aqueous solvent is increased, resulting in a significant improvement in heat resistance. From this viewpoint, the volume ratio of EC:GBL in the non-aqueous solvent containing EC and / or GBL is preferably 0:1 to 1:1 (GBL ratio of 50 to 100 volume%), more preferably 0:1 to 1:1.5 (GBL ratio of 60 to 100 volume%), further preferably 0:1 to 1:2 (GBL ratio of 66.6 to 100 volume%), and particularly preferably 0:1 to 1:3 (GBL ratio of 75 to 100 volume%). Lithium borofluoride (LiBF 4 ) is an electrolyte with a high decomposition temperature, which also leads to a significant improvement in heat resistance. 4 The concentration is preferably 0.5 to 2 mol / L, more preferably 0.6 to 1.9 mol / L, further preferably 0.7 to 1.7 mol / L, and particularly preferably 0.8 to 1.5 mol / L.
[0047] The electrolyte solution 24 may further contain vinylene carbonate (VC) and / or fluoroethylene carbonate (FEC) and / or vinyl ethylene carbonate (VEC) as an additive. Both VC and FEC have excellent heat resistance. Therefore, by including such an additive in the electrolyte solution 24, an SEI film having excellent heat resistance can be formed on the surface of the negative electrode layer 18.
[0048] Also, a solid electrolyte or a polymer electrolyte may be used instead of the electrolytic solution 24 (in other words, a solid electrolyte or a polymer electrolyte may be used as the electrolyte in addition to the electrolytic solution 24). In that case, similar to the case of the electrolytic solution 24, it is preferable that the electrolyte is impregnated at least into the pores of the ceramic separator 16. The impregnation method is not particularly limited, but examples include a method of melting the electrolyte and infiltrating it into the pores of the ceramic separator 16, a method of pressing a powder compact of the electrolyte against the ceramic separator 16, and the like.
[0049] The exterior body 26 has a sealed space, and the battery element 12 and the electrolyte 24 are accommodated in this sealed space. The exterior body 26 may be appropriately selected according to the type of the lithium ion secondary battery 10. For example, when the lithium ion secondary battery is in the form of a coin-shaped battery as shown in FIG. 1A, the exterior body 26 typically has a positive electrode can 26a, a negative electrode can 26b, and a gasket 26c, and the positive electrode can 26a and the negative electrode can 26b are crimped via the gasket 26c to form a sealed space. The positive electrode can 26a and the negative electrode can 26b may be made of a metal such as stainless steel, and are not particularly limited. The gasket 26c may be a ring-shaped member made of an insulating resin such as polypropylene, polytetrafluoroethylene, or PFA resin, and are not particularly limited.
[0050] Manufacturing method of integral sintered body The roll-shaped integrated sintered body (i.e., battery element 12) composed of the ceramic positive electrode layer 14, the ceramic separator 16, the ceramic negative electrode layer 18, the ceramic insulating layer 20, and the current collecting layer 21 may be manufactured by any method, but is preferably manufactured by: (1) preparing green sheets corresponding to each of the ceramic positive electrode layer 14, the ceramic separator 16, the ceramic negative electrode layer 18, and the ceramic insulating layer 20, (2) forming the current collecting layer 21 on one side of the positive electrode green sheet and / or the negative electrode green sheet, (3) stacking these green sheets so that the current collecting layer 21 is on the outside, and (4) rolling and firing the obtained green sheet stack.
[0051] (1) Preparation of various green sheets (1a) Preparation of positive electrode green sheet The lithium composite oxide-containing green sheet as the positive electrode green sheet can be produced as follows. First, a raw material powder composed of a lithium composite oxide is prepared. This powder is LiMO 2 Pre-synthesized plate-like particles (e.g., LiCoO 2 The volumetric D50 particle size of the raw material powder is preferably 0.3 to 30 μm. For example, LiCoO 2 The plate-like particles can be prepared as follows. 3 O 4 Raw powder and Li 2 CO 3 The raw material powder is mixed and sintered (500-900°C, 1-20 hours) to obtain LiCoO 2 The powder was synthesized. The obtained LiCoO 2 The powder was pulverized in a pot mill to a volumetric D50 particle size of 0.2 μm to 10 μm, forming plate-like LiCoO particles that can conduct lithium ions parallel to the plate surface. 2 Such LiCoO particles are obtained. 2 The particles are LiCoO 2 It can also be obtained by a method of growing grains from a green sheet using a powder slurry and then crushing it, or by a method of synthesizing plate-like crystals such as the flux method, hydrothermal synthesis, single crystal growth using a melt, and the sol-gel method. 2 The particles are in a state where they can be easily cleaved along the cleavage plane. LiCoO 2 The particles are cleaved by crushing to obtain LiCoO 2 Plate-like particles can be produced.
[0052] The plate-like particles may be used alone as a raw material powder, or the plate-like powder may be used together with other raw material powders (e.g., Co 3 O 4 In the latter case, the plate-like powder functions as a template particle for providing orientation, and the other raw powder (e.g., Co 3 O 4It is preferable to make the template particles (particles) function as matrix particles that can grow along the template particles. In this case, it is preferable to use a powder in which the template particles and the matrix particles are mixed in a ratio of 100:0 to 3:97 as the raw material powder. 3 O 4 When raw powder is used as matrix particles, Co 3 O 4 The volumetric D50 particle size of the raw material powder is not particularly limited and can be, for example, 0.1 to 1.0 μm. 2 The matrix particles are preferably smaller than the volumetric D50 particle size of the template particles. 2 It can also be obtained by heat treating the raw material at 500 to 800 °C for 1 to 10 hours. 3 O 4 In addition, Co(OH) 2 Particles may be used, or LiCoO 2 Particles may also be used.
[0053] The raw powder is LiCoO 2 When composed of 100% template particles or as matrix particles, LiCoO 2 When particles are used, large (e.g., 90 mm x 90 mm square) and flat LiCoO 2 A sintered layer can be obtained. Although the mechanism is unclear, LiCoO 2 Since synthesis into a sintered body is not performed, it is expected that volume change during firing or localized unevenness is unlikely to occur.
[0054] The raw material powder is mixed with a dispersion medium and various additives (binder, plasticizer, dispersant, etc.) to form a slurry. The slurry contains LiMO 2A lithium compound other than the above (e.g., lithium carbonate) may be added in an excess amount of about 0.5 to 30 mol %. It is preferable not to add a pore former to the slurry. The slurry is preferably stirred under reduced pressure to defoam it, and the viscosity is preferably adjusted to 4000 to 10000 cP. The obtained slurry is molded into a sheet to obtain a lithium composite oxide-containing green sheet. The sheet molding is preferably performed using a molding method capable of applying a shear force to plate-like particles (e.g., template particles) in the raw material powder. By doing so, the average inclination angle of the primary particles can be made to be more than 0° and 30° or less with respect to the sheet surface. As a molding method capable of applying a shear force to the plate-like particles, a doctor blade method is suitable. The thickness of the lithium composite oxide-containing green sheet may be appropriately set so that it has the desired thickness as described above after firing.
[0055] (1b) Preparation of negative electrode green sheet The titanium-containing green sheet as the negative electrode green sheet may be produced by any method. For example, the LTO-containing green sheet can be produced as follows. First, lithium titanate Li 4 Ti 5 O 12 A raw powder (LTO powder) consisting of the above is prepared. The raw powder may be a commercially available LTO powder or may be newly synthesized. For example, a powder obtained by hydrolyzing a mixture of titanium tetraisopropoxy alcohol and isopropoxy lithium may be used, or a mixture containing lithium carbonate, titania, etc. may be fired. The volumetric D50 particle size of the raw powder is preferably 0.05 to 5.0 μm, more preferably 0.1 to 2.0 μm. If the particle size of the raw powder is large, the pores tend to become large. In addition, if the raw particle size is large, a pulverization process (for example, pot mill pulverization, bead mill pulverization, jet mill pulverization, etc.) may be performed to obtain a desired particle size. Then, the raw powder is mixed with a dispersion medium and various additives (binder, plasticizer, dispersant, etc.) to form a slurry. The slurry contains LiMO for the purpose of promoting particle growth or compensating for volatile content during the firing process described later. 2A lithium compound other than the above (e.g., lithium carbonate) may be added in an excess amount of about 0.5 to 30 mol %. It is preferable not to add a pore former to the slurry. The slurry is preferably stirred under reduced pressure to defoam it, and the viscosity is preferably adjusted to 4000 to 10000 cP. The obtained slurry is formed into a sheet to obtain an LTO-containing green sheet. The sheet formation can be performed by various well-known methods, but is preferably performed by a doctor blade method. The thickness of the LTO-containing green sheet may be appropriately set so that it has the desired thickness as described above after firing.
[0056] (1c) Preparation of separator green sheets The separator green sheet can be prepared as follows. First, MgO, Al 2 O 3 , ZrO 2 , SiC, Si 3 N 4 At least one ceramic powder selected from , AlN, and cordierite is prepared. Glass frit may be added to this ceramic powder. The volumetric D50 particle size of the raw material powder is preferably 0.05 to 20 μm, more preferably 0.1 to 10 μm. If the particle size of the raw material powder is large, the pores tend to become large. If the raw material particle size is large, a pulverization process (for example, pot mill pulverization, bead mill pulverization, jet mill pulverization, etc.) may be performed to obtain a desired particle size. Then, the raw material powder is mixed with a dispersion medium and various additives (binder, plasticizer, dispersant, etc.) to form a slurry. It is preferable that no pore former is added to the slurry. The slurry is stirred under reduced pressure to defoam it, and the viscosity is preferably adjusted to 4000 to 10000 cP. The obtained slurry is formed into a sheet to obtain a separator green sheet. The sheet forming can be performed by various well-known methods, but is preferably performed by a doctor blade method. The thickness of the separator green sheet may be appropriately set so that it has the desired thickness as described above after firing.
[0057] (1d) Preparation of insulating green sheet The separator green sheets can be produced in the same manner as the separator green sheets, using the same ceramic powder. However, for the insulating green sheets for the non-facing parts 12x, which are used by being arranged in the same plane as the positive electrode green sheet or the negative electrode green sheet, the blending ratio of the binder and the plasticizer can be increased to make the separation distance X of the non-facing parts in the integrated sintered body larger than the separation distance Y of the facing parts.
[0058] (2) Formation of the current collecting layer The current collecting layer is not particularly limited as long as it is a layer containing a conductive material, but is preferably a layer that forms a metal layer by firing. The current collecting layer may be formed by applying a metal paste (e.g., Au paste, Pt paste, Pd paste, or Cu paste) to one side of the positive electrode green sheet and / or the negative electrode green sheet. The metal paste may be applied by any method, but it is preferable to apply it by printing, since it is possible to form a current collecting layer with a highly precisely controlled thickness with high productivity.
[0059] (3) Stacking and compression of green sheets Next, the positive electrode green sheet, the separator green sheet, the negative electrode green sheet, and the insulating green sheet are appropriately stacked, and the obtained laminate is pressed to pressure-bond the green sheets together. Specifically, as shown in Figs. 5A and 5B, a laminate may be formed which sequentially includes a first layer composed of the negative electrode green sheet 18' and the insulating green sheet 20b', a second layer composed of the separator green sheet 16', a third layer composed of the positive electrode green sheet 14' and the insulating green sheet 20b', and a fourth layer composed of the insulating green sheet 20a'. At this time, it is preferable that the current collecting layer 21 is disposed so as to be the outer surface of the laminate. It is also preferable that the ends of the positive electrode green sheet 14' and the negative electrode green sheet 18' are shifted from each other to form the non-facing portion 12x and the facing portion 12y. The pressing may be performed by a known method and is not particularly limited, but is preferably performed by CIP (cold isostatic pressing). A preferable pressing pressure is 10 to 5000 kgf / cm 2 and more preferably 50 to 3000 kgf / cm2 The green sheet laminate thus pressed is preferably cut into a desired shape (for example, a tape shape) or size.
[0060] (4) Winding and Firing of the Green Sheet Laminate The green sheet laminate is wound, and in this state, it is degreased as desired, and then fired to obtain a roll-shaped integrated sintered body. The degreasing is preferably carried out by holding at 300 to 600°C for 0.5 to 20 hours. The firing is preferably carried out at 650 to 900°C for 0.01 to 20 hours, and more preferably at 700 to 850°C for 0.5 to 10 hours. The temperature rise rate during firing is preferably 50 to 1500°C / h, and more preferably 200 to 1300°C / h. In particular, this temperature rise rate is preferably adopted during the temperature rise process from 600 to 900°C, and more preferably during the temperature rise process from 600 to 800°C. In this way, a roll-shaped integrated sintered body composed of the ceramic positive electrode layer 14, the ceramic separator 16, the ceramic negative electrode layer 18, the ceramic insulating layer 20, and the current collecting layer 21 is obtained. EXAMPLES
[0061] The present invention will be described more specifically by the following examples. In the following examples, LiCoO 2 is abbreviated as "LCO" and Li 4 Ti 5 O 12 shall be abbreviated as "LTO."
[0062] Example 1 (1) Preparation of LCO green sheet (positive electrode green sheet) First, Co was weighed out so that the Li / Co molar ratio was 1.01. 3 O 4 Powder (manufactured by Seido Chemical Industry Co., Ltd.) and Li 2 CO 3After mixing the powder (manufactured by Honjo Chemical Co., Ltd.), the mixture was kept at 780°C for 5 hours, and the obtained powder was pulverized in a pot mill so that the volumetric D50 was 0.4 μm to obtain a powder consisting of LCO plate-like particles. 100 parts by weight of the obtained LCO powder, 100 parts by weight of a dispersion medium (toluene: isopropanol = 1:1), 12 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The obtained mixture was stirred under reduced pressure to defoam it, and the viscosity was adjusted to 4000 cP to prepare an LCO slurry. The viscosity was measured using a Brookfield LVT type viscometer. The slurry thus prepared was formed into a sheet on a PET film by a doctor blade method to form an LCO green sheet having a thickness of 35 μm.
[0063] (2) Preparation of LTO green sheet (negative electrode green sheet) First, 100 parts by weight of LTO powder (volume standard D50 particle size 0.06 μm, manufactured by Sigma-Aldrich Japan LLC), 100 parts by weight of dispersion medium (toluene: isopropanol = 1:1), 20 parts by weight of binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The obtained negative electrode raw material mixture was stirred and degassed under reduced pressure, and the viscosity was adjusted to 4000 cP to prepare an LTO slurry. The viscosity was measured with an LVT type viscometer manufactured by Brookfield. The slurry thus prepared was formed into a sheet shape on a PET film by the doctor blade method to form an LTO green sheet having a thickness of 35 μm.
[0064] (3) Preparation of MgO green sheets (separator green sheets and insulating green sheets A) Magnesium carbonate powder (manufactured by Konoshima Chemical Co., Ltd.) was heat-treated at 900°C for 5 hours to obtain MgO powder. The obtained MgO powder and glass frit (manufactured by Nippon Frit Co., Ltd., CK0199) were mixed at a weight ratio of 4:1. 100 parts by weight of the obtained mixed powder (volume-based D50 particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene: isopropanol = 1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The obtained raw material mixture was stirred under reduced pressure to defoam it, and the viscosity was adjusted to 4000 cP to prepare a slurry. The viscosity was measured with a Brookfield LVT type viscometer. The slurry thus prepared was formed into a sheet on a PET film by the doctor blade method to form a 35 μm thick MgO green sheet. This MgO green sheet was used not only as a separator green sheet but also as an insulating green sheet A for both the facing and non-facing parts.
[0065] (4) Preparation of MgO green sheet (insulating green sheet B) A 35 μm thick MgO green sheet was formed as insulating green sheet B for the non-facing portion in the same manner as in (3) above, except that the blending ratio of the binder, plasticizer, and dispersant in the MgO green sheet was changed to 30 parts by weight of binder, 12 parts by weight of plasticizer, and 1 part by weight of dispersant.
[0066] (5) Formation of the current collecting layer Au paste (manufactured by Tanaka Kikinzoku Co., Ltd., product name: GB-2706) was printed on one side of an LTO green sheet (negative electrode green sheet) using a printer. The thickness of the printed layer was set to 0.2 μm after firing.
[0067] (6) Lamination, compression and firing As shown in Figs. 5A and 5B, various green sheets were laminated. Specifically, the negative electrode green sheet 18' (width 6 mm x length 70 mm), the insulating green sheet B 20b' (width 4 mm x length 70 mm), and the negative electrode green sheet 18' (width 6 mm x length 70 mm) were arranged in parallel without gaps to form the first layer. At this time, the negative electrode green sheet 18' was arranged so that the current collecting layer 21 was located on the bottom surface. The separator green sheet 16' (width 16 mm x length 70 mm) was placed on the first layer to form the second layer. The insulating green sheet B 20b' (width 4 mm x length 70 mm), the positive electrode green sheet 14' (width 6 mm x length 70 mm), and the insulating green sheet B 20b' (width 4 mm x length 70 mm) were arranged in parallel without gaps on the second layer to form the third layer. The insulating green sheet A 20a' (width 16 mm x length 70 mm) was placed on the third layer. The laminates thus obtained are stacked and pressurized at 200 kgf / cm2 using CIP (cold isostatic pressing). 2 The green sheets were pressed together with a pressure, and then cut with a Thomson blade along the dotted lines shown in Figures 5A and 5B to obtain two laminated tapes (width 6 mm x length 70 mm). The laminated tape was heated on a hot plate at 60°C, wound around a reel to have an outer diameter of 10 mm and a thickness of 2.0 mm, and the ends were temporarily fixed with tape glue to obtain a rolled laminate. This rolled laminate was heated from room temperature to 600°C at a heating rate of 60°C / min and degreased for 5 hours, then heated to 800°C at a heating rate of 100°C / h and held for 10 minutes to be fired, and then cooled. In this way, a rolled integrated sintered body consisting of a positive electrode layer (LCO sintered body layer), a ceramic separator (MgO separator), a negative electrode layer (LTO sintered body layer), a current collecting layer (Au layer), and a ceramic insulating layer (MgO insulating layer) was obtained.
[0068] (7) Fabrication of lithium-ion secondary batteries A coin-type lithium-ion secondary battery 10 as shown in FIGS. 1A and 1B was fabricated as follows. A roll-shaped integrated sintered body was placed between a positive electrode can and a negative electrode can that constitute the battery case, and an electrolyte was then filled in. The positive electrode can and the negative electrode can were then crimped together via a gasket to seal the battery. In this way, a coin-cell type lithium-ion secondary battery 10 having a diameter of 12 mm and a thickness of 54 mm was fabricated. The electrolyte used in this experiment was an organic solvent in which ethylene carbonate (EC) and γ-butyrolactone (GBL) were mixed in a volume ratio of 1:3, and LiBF 4 A solution in which the above was dissolved to a concentration of 1.5 mol / L was used.
[0069] (8) Evaluation The roll-shaped integrated sintered body synthesized in (6) above and the coin-type lithium ion secondary battery fabricated in (7) above were subjected to various evaluations as shown below.
[0070] <Average orientation angle of primary particles> The LCO sintered body layer was polished with a cross-section polisher (CP) (IB-15000CP, manufactured by JEOL Ltd.), and the cross section of the positive electrode layer obtained (cross section perpendicular to the layer surface of the positive electrode layer in the direction parallel to the roll axis) was measured by EBSD at a magnification of 1000 times (125 μm × 125 μm) to obtain an EBSD image. This EBSD measurement was performed using a Schottky field emission scanning electron microscope (JSM-7800F, manufactured by JEOL Ltd.). For all particles identified in the obtained EBSD image, the angle between the (003) plane of the primary particle and the layer surface of the positive electrode layer (i.e., the inclination of the crystal orientation from (003)) was calculated as the inclination angle, and the average value of these angles was taken as the average orientation angle of the primary particles. As a result, the average orientation angle of the primary particles in the positive electrode layer was 16°.
[0071] <Layer thickness> The LCO and LTO sintered body layers and the MgO separator were polished with a cross-section polisher (CP) (IB-15000CP, manufactured by JEOL Ltd.), and the obtained cross sections were observed with an SEM (JSM6390LA, manufactured by JEOL Ltd.) to measure the thickness of each of the positive electrode layer, negative electrode layer, and separator. As a result, the thickness of the positive electrode layer was about 30 μm, the thickness of the negative electrode layer was about 30 μm, the thickness of the ceramic separator was about 20 μm, and the thickness of the independent insulating layer not in the same plane as the positive electrode layer or negative electrode layer was about 20 μm.
[0072] <Porosity> The LCO or LTO sintered body layer and the MgO separator were polished with a cross-section polisher (CP) (JEOL Ltd., IB-15000CP), and the cross section of the obtained positive electrode layer or negative electrode layer was observed with a SEM (JEOL Ltd., JSM6390LA) at a magnification of 1000 times (125 μm × 125 μm). The obtained SEM image was analyzed, and the area of all pores was divided by the area of the positive electrode or negative electrode, and the porosity (%) was calculated by multiplying the obtained value by 100. As a result, the porosity of the positive electrode layer was 45%, the porosity of the negative electrode layer was 45%, and the porosity of the ceramic separator was 50%.
[0073] <Average pore diameter> The average pore diameter of the LCO or LTO sintered body layer was measured by mercury intrusion method using a mercury porosimeter (Shimadzu Corporation, Autopore IV9510). As a result, the average pore diameter of the positive electrode layer was 0.8 μm, the average pore diameter of the negative electrode layer was 0.5 μm, and the average pore diameter of the ceramic separator was 0.2 μm.
[0074] <Gap measurement> A cross section of the roll-shaped integrated sintered body cut in a direction parallel to the roll axis was observed with an SEM (JSM-IT500, manufactured by JEOL) to measure the separation distance X between adjacent power generating sheets 22 in the non-facing portion 12x and the separation distance Y between adjacent power generating sheets 22 in the facing portion 12y. Specifically, the separation distance X was calculated as an average value obtained by measuring the SEM cross section in the stacking direction at the center position (height) in the roll axis direction of each non-facing portion 12x, adding up the distances of the gaps G between all the power generating sheets 22 at that height, and dividing the total value by the number of gaps G (the number of stacked power generating sheets 22 minus 1). Similarly, the separation distance Y was calculated as an average value obtained by measuring the SEM cross section in the stacking direction at the center position (height) in the roll axis direction of the facing portion, adding up the distances of the gaps G between all the power generating sheets 22 at that height, and dividing the total value by the number of gaps G (the number of stacked power generating sheets 22 minus 1). In addition, in both the separation distance X and the separation distance Y, the internal space corresponding to the roll core portion is not included in the gap G.
[0075] <Load discharge characteristics> The lithium-ion secondary battery was charged at a constant current of 0.2 C, and when the voltage reached 2.7 V, it was switched to constant voltage charging, and was charged until the charging current was 0.01 mA or less. It was then discharged at a constant current of 0.2 C until it reached 1.5 V. The capacity at this time (i.e., the 0.2 C discharge capacity) was 2.0 mAh. From there, it was charged in the same manner as above. It was then discharged at a constant current of 1.0 C until it reached 1.5 V. The capacity at this time (i.e., the 1.0 C discharge capacity) was 1.98 mAh. The load discharge characteristic was calculated by multiplying the ratio of the 1.0 C discharge capacity to the 0.2 C discharge capacity by 100, and was 99%.
[0076] Example 2 A battery was produced and evaluated in the same manner as in Example 1, except that the blending ratio of the binder, plasticizer, and dispersant in the insulating green sheet B was changed to 20 parts by weight of binder, 8 parts by weight of plasticizer, and 1 part by weight of dispersant.
[0077] Example 3 A battery was produced and evaluated in the same manner as in Example 1, except that the blending ratio of the binder, plasticizer, and dispersant in the insulating green sheet B was changed to 10 parts by weight of binder, 2.5 parts by weight of plasticizer, and 1 part by weight of dispersant.
[0078] Example 4 (comparison) A battery was produced and evaluated in the same manner as in Example 1, except that the blending ratio of the binder, plasticizer, and dispersant in the insulating green sheet B was changed to 8 parts by weight of binder, 2 parts by weight of plasticizer, and 1 part by weight of dispersant.
[0079] result The results obtained in Examples 1 to 4 are shown in Table 1.
[0080] [Table 1] [Explanation of symbols]
[0081] 10 Lithium-ion secondary battery 11 Primary particles 12 Battery elements 12x non-opposing part 12y Opposite section 14 Ceramic positive electrode layer 14' Positive electrode green sheet 16 Ceramic separator 16' separator green sheet 18 Ceramic negative electrode layer 18' Negative electrode green sheet 20 Ceramic insulating layer 20a', 20b' Insulation green sheet 21 Current collecting layer 22 Power generation sheet 24 Electrolyte 26 Exterior body 26a Positive electrode can 26b Negative electrode can 26c Gasket G Gap X: Distance between the power generating sheets in non-facing areas Y Distance between opposing generating sheets
Claims
1. (a) A battery element having a roll-like form in which a power generating sheet including a ceramic positive electrode layer, a ceramic separator, a ceramic negative electrode layer, and a ceramic insulating layer is wound, and which forms a single integral sintered body as a whole, an opposing portion that constitutes a main portion of the roll away from both side ends and where the ceramic positive electrode layer and the ceramic negative electrode layer face each other via the ceramic separator; a non-facing portion that constitutes an outer circumferential portion along both side ends of the roll, the non-facing portion including either the ceramic positive electrode layer or the ceramic negative electrode layer but not including the other, such that the ceramic positive electrode layer and the ceramic negative electrode layer do not face each other alternately; A battery element having (b) an electrolyte impregnated in the battery element; (c) an exterior body that contains the battery element and the electrolyte; A lithium ion secondary battery comprising: the battery element has adjacent power generating sheets spaced apart to form a gap, and a separation distance X between the adjacent power generating sheets in the non-facing portion is greater than a separation distance Y between the adjacent power generating sheets in the facing portion; a ratio of a distance X between the adjacent power generating sheets in the non-facing portion to a distance Y between the adjacent power generating sheets in the facing portion is 1.3 to 10.
2. 2. The lithium ion secondary battery according to claim 1, wherein the separation distance X between the adjacent power generation sheets in the non-facing portion is 20 μm or less.
3. 3. The lithium ion secondary battery according to claim 1, wherein the ceramic positive electrode layer is made of a lithium composite oxide sintered body, and the ceramic negative electrode layer is made of a titanium-containing sintered body.
4. 4. The lithium ion secondary battery according to claim 3, wherein the lithium composite oxide is lithium cobalt oxide.
5. 5. The lithium ion secondary battery according to claim 3, wherein the titanium-containing sintered body contains lithium titanate or niobium titanium composite oxide.
6. The ceramic separator is made of MgO, Al 2 O 3 , ZrO 2 , SiC, Si 3 N 4 6. The lithium ion secondary battery according to claim 1, further comprising at least one selected from the group consisting of AlN and cordierite.
7. The lithium ion secondary battery according to any one of claims 1 to 6, wherein the power generating sheet has a thickness of 22 to 1080 µm.
8. The lithium ion secondary battery according to any one of claims 1 to 7, wherein the ceramic positive electrode layer has a thickness of 10 to 500 μm, the ceramic negative electrode layer has a thickness of 10 to 500 μm, and the ceramic separator has a thickness of 1 to 40 μm.
9. The non-facing portion is a first non-facing portion that constitutes a first outer circumferential portion along one of the side ends of the roll, the first non-facing portion including the ceramic positive electrode layer and not including the ceramic negative electrode layer; a second non-facing portion that constitutes a second outer circumferential portion along the other side end portion of the roll, the second non-facing portion including the ceramic negative electrode layer and not including the ceramic positive electrode layer; The lithium ion secondary battery according to any one of claims 1 to 8, comprising:
10. The ceramic insulating layer, or the ceramic separator and the ceramic insulating layer, are interposed between the adjacent ceramic positive electrode layers in the first non-facing portion, and The lithium ion secondary battery according to claim 9 , wherein the ceramic insulating layer, or the ceramic separator and the ceramic insulating layer, are interposed between the adjacent ceramic negative electrode layers in the second non-facing portion.
11. The lithium ion secondary battery according to any one of claims 1 to 10, wherein the facing portion has a layer configuration in which a lamination unit in which the ceramic separator is interposed between the ceramic positive electrode layer and the ceramic negative electrode layer is repeated in a roll radial direction with the ceramic insulating layer interposed between adjacent lamination units.
12. The lithium ion secondary battery according to any one of claims 1 to 11, wherein the ceramic insulating layer is located as an outermost layer on an outer peripheral surface of the roll of the battery element.
13. The lithium ion secondary battery according to any one of claims 1 to 12, wherein the battery element further comprises a current collecting layer on a surface of the ceramic negative electrode layer opposite to the ceramic positive electrode layer.
Citation Information
Patent Citations
Measuring circuit for instantaneous power
JP1980087052A
Heat treatment for hot forged parts
JP1982067115A
Spot weldable composite type vibration-damping material
JP1988074634A
Thermal transfer recording medium
JP1988092493A
Cylindrical secondary battery
JP2002110216A