Nonaqueous electrolyte and nonaqueous electrolyte secondary battery

By using a non-aqueous electrolyte with isocyanate compounds to stabilize the Ni surface in high Ni content transition metal oxide cathodes, the input resistance and stability of non-aqueous electrolyte secondary batteries are improved, addressing the surface reaction issue and enhancing battery performance.

JP7579714B2Active Publication Date: 2024-11-08MITSUBISHI CHEM CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021012987
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-29
Filing Date
2021-01-29
Publication Date
2024-11-08
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

There is a challenge in non-aqueous electrolyte secondary batteries with high Ni content transition metal oxide cathodes, where surface reactions with the electrolyte occur during charging, leading to decreased input characteristics due to unstable Ni valence changes.

Method used

Incorporating a non-aqueous electrolyte containing specific isocyanate compounds that interact with the electrolyte to stabilize the Ni surface, using a positive electrode with a transition metal oxide containing at least 40 mol% Ni and Co, and a carbon-based negative electrode to reduce input resistance.

Benefits of technology

The solution achieves low input resistance and improved stability in non-aqueous electrolyte secondary batteries with high Ni content, enhancing their performance and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579714000001
    Figure 0007579714000001
  • Figure 0007579714000002
    Figure 0007579714000002
  • Figure 0007579714000003
    Figure 0007579714000003
Patent Text Reader

Abstract

To provide: a nonaqueous electrolyte which can achieve a low input resistance in a nonaqueous electrolyte secondary battery having a positive electrode high in Ni content; and a nonaqueous electrolyte secondary battery arranged by use of such a nonaqueous electrolyte, including a positive electrode of high Ni content, and having a low input resistance.SOLUTION: A nonaqueous electrolyte hereof is to be used for a nonaqueous electrolyte secondary battery having: a positive electrode containing a transition metal oxide capable of occluding and releasing metal ions and including at least Ni and Co, in which Ni accounts for 40 mol% or more of the transition metal; a negative electrode containing a carbon-based material capable of occluding and releasing metal ions; and a nonaqueous electrolyte containing a nonaqueous solvent, and an electrolyte dissolved in the nonaqueous solvent. The nonaqueous electrolyte comprises at least one isocyanate compound selected from a compound represented by the general formula (1) below, and a compound represented by the general formula (2) below. In the formula (1), n≥2; and in the formula (2), p≥1 and s≥1.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-aqueous electrolyte and a non-aqueous electrolyte secondary battery. [Background technology]

[0002] 2. Description of the Related Art Non-aqueous electrolyte secondary batteries, such as lithium secondary batteries, have been put to practical use in a wide range of applications, such as power sources for so-called small consumer devices, such as mobile phones such as smartphones and laptop computers, and on-board power sources for driving electric vehicles and the like.

[0003] As a means for improving the battery characteristics of non-aqueous electrolyte batteries, many studies have been conducted in the fields of positive and negative electrode active materials and additives for non-aqueous electrolytes.

[0004] For example, Patent Document 1 discloses a non-aqueous electrolyte consisting of a non-aqueous solvent containing a compound containing an isocyanato group and an electrolyte, and a secondary battery using this electrolyte, with the aim of providing a non-aqueous electrolyte having excellent battery life and a secondary battery using the same. In the examples, a LiCoO2 electrode is used as the positive electrode, graphite is used as the negative electrode, and ethylene carbonate (EC) and methacrylate are used as the electrolyte. This paper discloses the load characteristics after high-temperature storage of nonaqueous electrolyte secondary batteries in which 1,3-diisocyanato-4-methylbenzene (Examples 1 to 3), di(isocyanatonorbornyl)uretidine-2,4-dione (Examples 4 to 6), or di(isocyanatonorbornyl)1,3,5-oxadiazine-2,4,6-trione (Examples 7 to 9) are used as a compound containing an isocyanato group, and ethyl ethyl carbonate (MEC) is mixed in a ratio of EC:MEC = 4:6 (weight ratio). Patent Document 2 aims to provide a non-aqueous electrolyte battery with little gas generation and excellent battery characteristics, and describes a positive electrode having a positive electrode active material and a lithium absorption / release potential of 1.0 V (vs. L i / Li +A nonaqueous electrolyte battery having a negative electrode with a negative electrode active material more noble than LiMn2O4 and a nonaqueous electrolyte solution, in which an organic compound having an isocyanato group is added to the nonaqueous electrolyte solution, is disclosed. In the examples, the amount of gas generation, high rate characteristics, and remaining capacity rate are examined for a nonaqueous electrolyte secondary battery using a positive electrode containing LiMn2O4 as a positive electrode active material, using a nonaqueous electrolyte containing 1,6-diisocyanatohexane. Patent Document 3 discloses a nonaqueous electrolyte battery having a positive electrode, a negative electrode, an electrolyte, and a separator, the positive electrode containing 1000 ppm to 50 ppm of water, and the electrolyte containing a specific isocyanate compound and a specific aromatic compound, for the purpose of providing a battery that suppresses decomposition of a solvent and deformation of the battery and improves battery characteristics during high-temperature cycles. In the examples, the moisture concentration in the positive electrode active material layer and the type and content of the isocyanate compound are changed in a nonaqueous electrolyte battery using a positive electrode containing lithium cobalt oxide as the positive electrode active material, and the high-temperature storage capacity retention rate is examined. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-8719 A [Patent Document 2] JP 2009-54319 A [Patent Document 3] JP 2011-28860 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, there has been an increasing demand for high-capacity lithium batteries for use as on-board power sources for electric vehicles and power sources for mobile phones such as smartphones. As a high-capacity positive electrode active material, transition metal oxide positive electrodes with a high Ni content have been attracting attention. It was found that there was a problem in that a surface reaction occurred with the electrolyte during charging, resulting in a decrease in input characteristics.

[0007] In view of the above, an object of the present invention is to provide a nonaqueous electrolyte secondary battery using a positive electrode containing a transition metal oxide, the positive electrode containing at least Ni and Co, where 40 mol % or more of the transition metals are Ni, and a negative electrode containing a carbon-based material, the nonaqueous electrolyte secondary battery using such a nonaqueous electrolyte that achieves low input resistance, and a nonaqueous electrolyte secondary battery using such a nonaqueous electrolyte and comprising a positive electrode with a high Ni content and having low input resistance. [Means for solving the problem]

[0008] As a result of intensive research into solving the above-mentioned problems, the present inventors have conceived that in a nonaqueous electrolyte secondary battery comprising a positive electrode containing a transition metal oxide capable of absorbing and releasing metal ions, the transition metal oxide containing at least Ni and Co, where 40 mol % or more of the transition metals is Ni, a negative electrode containing a carbon-based material capable of absorbing and releasing metal ions, and a nonaqueous electrolyte solution containing a nonaqueous solvent and an electrolyte dissolved in the nonaqueous solvent, by using a nonaqueous electrolyte solution containing at least one compound selected from the compound represented by general formula (1) and the isocyanate compound represented by general formula (2), a low input resistance of the nonaqueous electrolyte secondary battery can be achieved, and have completed the present invention.

[0009] The present invention provides the following aspects and the like. <1> a positive electrode containing a transition metal oxide capable of absorbing and releasing metal ions, the transition metal oxide containing at least Ni and Co, the transition metal being at least 40 mol % being Ni; A non-aqueous electrolyte used in a non-aqueous electrolyte secondary battery including a negative electrode containing a carbon-based material capable of absorbing and releasing metal ions, and a non-aqueous electrolyte containing a non-aqueous solvent and an electrolyte dissolved in the non-aqueous solvent, A non-aqueous electrolyte solution comprising at least one isocyanate compound selected from the group consisting of compounds represented by the following general formula (1) and compounds represented by the following general formula (2): [ka] (In formula (1), m and n are integers that satisfy m+n=6, and n≧2. X represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom and may be the same or different from each other. Y represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 10 carbon atoms which may have a heteroatom.) [ka] (In formula (2), p, q, r, and s are integers satisfying p+q=5 and r+s=5, and p≧1 and s≧1. R may be the same or different and represent a hydrogen atom, a halogen atom, or an organic group having 1 to 10 carbon atoms which may have a heteroatom. X' represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom.) <2> The nonaqueous electrolyte solution contains a compound represented by formula (1), wherein n is 2. <1> The non-aqueous electrolyte solution according to claim 1. <3> The nonaqueous electrolyte solution contains a compound represented by formula (1), X is a methylene group or a dimethylmethylene group; <1> or <2> The non-aqueous electrolyte solution according to claim 1. <4> The nonaqueous electrolyte solution contains a compound represented by formula (2), and in formula (2), s=p=1. <1> The non-aqueous electrolyte solution according to claim 1. <5> The non-aqueous electrolyte solution contains at least one of a compound having a PF bond and a compound having an SO2 structure. <1> ~ <4> 2. The non-aqueous electrolyte solution according to claim 1 . <6> a positive electrode capable of absorbing and releasing metal ions, a negative electrode containing a carbon-based material capable of absorbing and releasing metal ions, and a nonaqueous electrolyte solution containing a nonaqueous solvent and an electrolyte dissolved in the nonaqueous solvent; A non-aqueous electrolyte secondary battery comprising: The positive electrode contains a transition metal oxide and at least Ni and Co as transition metals, and 40 mol % or more of the transition metals is Ni; The non-aqueous electrolyte solution is <1> ~ <5> 2. A non-aqueous electrolyte secondary battery comprising the non-aqueous electrolyte according to claim 1. Effect of the Invention

[0010] According to the present invention, a nonaqueous electrolyte that can realize low input resistance in a nonaqueous electrolyte secondary battery having a positive electrode with a high Ni content is provided. Also, a nonaqueous electrolyte secondary battery using the nonaqueous electrolyte and having a low input resistance and a positive electrode with a high Ni content is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described in detail. The following embodiments are examples (representative examples) of the present invention, and the present invention is not limited to these. Furthermore, the present invention can be modified and carried out as desired without departing from the scope of the present invention.

[0012] <1.Non-aqueous electrolyte> The nonaqueous electrolyte according to the present embodiment is used in a nonaqueous electrolyte secondary battery including a positive electrode containing a transition metal oxide capable of absorbing and releasing metal ions, the transition metal oxide containing at least Ni and Co, where 40 mol % or more of the transition metals is Ni, a negative electrode containing a carbon-based material capable of absorbing and releasing metal ions, and a nonaqueous electrolyte containing a nonaqueous solvent and an electrolyte dissolved in the nonaqueous solvent, and is characterized in that it contains at least one isocyanate compound selected from the compounds represented by the following general formula (1) and the compounds represented by the general formula (2). [ka] (In formula (1), m and n are integers that satisfy m+n=6, and n≧2. X represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom and may be the same or different from each other. Y represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 10 carbon atoms which may have a heteroatom.) [ka] In formula (2), p, q, r, and s are integers that satisfy p+q=5 and r+s=5, and p≧1 and s≧1. R's each may be the same or different and are a hydrogen atom, a halogen atom, or a benzene ring. X' represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a hetero atom.

[0013] The mechanism by which the use of a nonaqueous electrolyte solution containing at least one isocyanate compound selected from the group consisting of compounds represented by general formula (1) and compounds represented by general formula (2) provides a low input resistance to a nonaqueous electrolyte secondary battery having a positive electrode containing a transition metal oxide capable of absorbing and releasing metal ions, the transition metal oxide containing at least Ni and Co, and 40 mol % or more of the transition metal being Ni, is not clear, but is presumed to be as follows. In the positive electrode material, the valence change during charging is +1 for Mn, Co, and Fe, which are typical transition metals used in the positive electrode active material. In contrast, in the Ni-containing positive electrode, the valence of Ni changes from +2 to +4 during charging, but as the proportion of Ni contained increases, the unstable +3 valence increases. Since the trivalent Ni is unstable, a surface reaction with the electrolyte occurs, and it is presumed that the input characteristics are reduced by deactivating the Li insertion points on the surface. The inventors have come up with the idea of ​​reducing the surface activity of unstable Ni, which is present in large amounts, in a positive electrode with a high Ni content. In this embodiment, it is expected that by including a compound containing an aromatic ring in the electrolyte, the aromatic ring π electrons and the unstable Ni present on the surface interact with each other, preferentially adsorbing to the active points and further stabilizing them. Furthermore, it is presumed that the compound represented by formula (1) or formula (2) has two or more isocyanate (NCO) groups, and thus the NCO groups polymerize with each other starting from the nucleophile contained in the electrolyte, and the active point covering effect by the additive becomes stronger, thereby achieving the effects of the present invention. In this case, the nucleophile contained in the electrolyte is generated by the reduction of the electrolyte components, and in the present invention, a negative electrode material (typified by a carbon-based material) having a potential at which the electrolyte components can be reduced is used. Furthermore, it is presumed that by using an isocyanate compound in which the NCO group is not directly bonded to an aromatic ring but is bonded via a hydrocarbon group, the decomposition of the compound itself is suppressed while the protective effect on the active sites is more easily exerted.

[0014] <1-1. Isocyanate compounds> A non-aqueous electrolyte solution according to one embodiment of the present invention is characterized in that it contains at least one isocyanate compound selected from a compound represented by the following general formula (1) and a compound represented by the following general formula (2):

[0015] <1-1-1. Compound represented by general formula (1)> [ka] (In formula (1), m and n are integers that satisfy m+n=6, and n≧2. X represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom and may be the same or different from each other. Y represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 10 carbon atoms which may have a heteroatom.)

[0016] In the general formula (1), X represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom, and which may be the same or different. Examples of divalent organic groups having 1 to 10 carbon atoms which may have a heteroatom include hydrocarbon groups having 10 or less carbon atoms which may have a substituent; carbonyl groups; and groups consisting of two or more hydrocarbon groups which may have a substituent and at least one group selected from an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-CO-), and an amino group (-NH-).

[0017] Examples of such groups include an ether group consisting of an optionally substituted hydrocarbon group and an oxygen atom (-O-); an ester group consisting of an optionally substituted hydrocarbon group, an oxygen atom (-O-), and a carbonyl group (-CO-); a thioether group consisting of an optionally substituted hydrocarbon group and a sulfur atom (-S-); and an amide group consisting of an optionally substituted hydrocarbon group, an amino group (-NH-), and a carbonyl group (-CO-).

[0018] Specific examples of the hydrocarbon group include alkylene groups having 1 to 10 carbon atoms, such as methylene, ethylene, propylene, and butylene; alkenylene groups having 2 to 10 carbon atoms, such as vinylene; alkynylene groups having 2 to 10 carbon atoms, such as ethynylene; cycloalkenylene groups, such as cyclopentylene and cyclohexylene; and arylene groups having 6 to 10 carbon atoms, such as phenylene. Of these, from the viewpoint of the input resistance of the battery, a divalent hydrocarbon group having 1 to 10 carbon atoms which may have a substituent is preferred. When the hydrocarbon group has a substituent, the number of carbon atoms contained in the substituent is not included in the carbon number. More preferably, it is a divalent linear or branched aliphatic hydrocarbon group having 1 to 6 carbon atoms, which may have a substituent, and even more preferably, it is a divalent linear or branched aliphatic hydrocarbon group having 1 to 4 carbon atoms. Preferred examples of such hydrocarbon groups include a methylene group, a methylmethylene group, a dimethylmethylene group, an ethylmethylene group, a dimethylene group, a trimethylene group, and a tetramethylene group.

[0019] Examples of the heteroatom include halogen atoms, phosphorus atoms, silicon atoms, oxygen atoms, and sulfur atoms. Among these, fluorine atoms are preferred from the viewpoints of lowering the input resistance of the battery and minimizing electrochemical side reactions. The heteroatom may be substituted for a carbon atom of the hydrocarbon group, or may be substituted for a hydrogen atom of the hydrocarbon group.

[0020] Here, the substituent is a cyano group, an isocyanato group, an acyl group (-(C=O)-R a), acyloxy group (-O(C=O)-R a ), alkoxycarbonyl group (-(C=O)OR a ), sulfonyl group (-SO2-R a ), sulfonyloxy group (-O(SO2)-R a ), alkoxysulfonyl group (-(SO2)-OR a ), alkoxysulfonyloxy group (-O-(SO2)-OR a ), alkoxycarbonyloxy group (-O-(C=O)-OR a ), alkoxy group (-OR a ), a halogen atom (preferably a fluorine atom), a trifluoromethyl group, etc. a R represents an alkyl group having 1 to 10 carbon atoms, an alkylene group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms. a When is an alkylene group, it may be bonded to a part of the hydrocarbon group which substitutes it to form a ring. Among these substituents, a cyano group, an isocyanato group, an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), or a trifluoromethyl group, and more preferably an isocyanato group or an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), a trifluoromethyl group, and particularly preferably an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), or a trifluoromethyl group.

[0021] In terms of increasing the coating density on the positive electrode surface, X in general formula (1) is more preferably a single bond, a methylene group, or a dimethylmethylene group, which has a shorter distance between the aromatic ring and the NCO group, and is particularly preferably a methylene group or a dimethylmethylene group in terms of the protective effect on the active site while suppressing decomposition of the compound represented by general formula (1) itself. The X's in the general formula (1) may be the same or different, but are preferably the same in terms of ease of synthesis of the compound. From the viewpoint of sufficiently lowering the input resistance of a nonaqueous electrolyte secondary battery, a diisocyanate compound in which n is 2 in formula (1) is particularly preferred.

[0022] In the general formula (1), Y represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 10 carbon atoms which may have a heteroatom. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Of these, a fluorine atom is preferred from the viewpoint of reducing electrochemical side reactions. Examples of the monovalent organic group having 1 to 10 carbon atoms which may have a heteroatom include hydrocarbon groups which may have a substituent, and more specific examples thereof include linear or branched aliphatic hydrocarbon groups which may have a substituent, and aromatic hydrocarbon groups which may have a substituent. The hydrocarbon group having 1 to 10 carbon atoms is preferably a hydrocarbon group having 1 to 6 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 4 carbon atoms. Specific examples of the hydrocarbon group include an alkyl group, an alkenyl group, an alkynyl group, and an aryl group.

[0023] Specific examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups. Among them, preferred are methyl, ethyl, n-propyl, n-butyl, tert-butyl, n-pentyl, and hexyl groups, more preferred are methyl, ethyl, n-propyl, n-butyl, tert-butyl, and n-pentyl groups, and particularly preferred are methyl, ethyl, n-butyl, and tert-butyl groups. The above-mentioned alkyl groups are preferred because the compound represented by the general formula (A) tends to be localized near the surface of the positive electrode active material and / or the negative electrode active material.

[0024] Specific examples of the alkenyl group include vinyl, allyl, methallyl, 2-butenyl, 3-methyl-2-butenyl, 3-butenyl, and 4-pentenyl groups. Among them, vinyl, allyl, methallyl, and 2-butenyl groups are preferred, vinyl, allyl, and methallyl groups are more preferred, and vinyl or allyl groups are particularly preferred. The above-mentioned alkenyl groups are preferred because the compound represented by general formula (1) tends to be localized near the surface of the positive electrode active material.

[0025] Specific examples of the alkynyl group include an ethynyl group, a 2-propynyl group, a 2-butynyl group, a 3-butynyl group, a 4-pentynyl group, and a 5-hexynyl group. Among these, an ethynyl group, a 2-propynyl group, a 2-butynyl group, and a 3-butynyl group are preferred, a 2-propynyl group and a 3-butynyl group are more preferred, and a 2-propynyl group is particularly preferred. The above-mentioned alkynyl group is preferred because the compound represented by the general formula (1) tends to be localized near the surface of the positive electrode active material and / or the negative electrode active material.

[0026] Specific examples of the aryl group include a phenyl group, a tolyl group, a benzyl group, a phenethyl group, etc. Among them, a phenyl group is preferred from the viewpoint that the compound represented by the general formula (1) tends to be localized near the surface of the positive electrode active material. Examples of the heteroatom include a halogen atom, a phosphorus atom, a silicon atom, an oxygen atom, and a sulfur atom. Among these, a fluorine atom is preferred from the viewpoint of causing fewer electrochemical side reactions. The heteroatom may be substituted for a carbon atom of the hydrocarbon group, or may be substituted for a hydrogen atom of the hydrocarbon group. Here, the substituent is a cyano group, an isocyanato group, an acyl group (-(C=O)-R a ), acyloxy group (-O(C=O)-R a ), alkoxycarbonyl group (-(C=O)OR a ), sulfonyl group (-SO2-R a ), sulfonyloxy group (-O(SO2)-R a ), alkoxysulfonyl group (-(SO2)-ORa ), alkoxysulfonyl The oxy group (-O-(SO2)-OR a ), alkoxycarbonyloxy group (-O-(C=O)-OR a ), alkoxy group (-OR a ), a halogen atom (preferably a fluorine atom), a trifluoromethyl group, etc. a R represents an alkyl group having 1 to 10 carbon atoms, an alkylene group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms. a When is an alkylene group, it may be bonded to a part of the hydrocarbon group which substitutes it to form a ring. Among these substituents, a cyano group, an isocyanato group, an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), or a trifluoromethyl group, and more preferably an isocyanato group or an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), a trifluoromethyl group, and particularly preferably an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), or a trifluoromethyl group. From the viewpoint of sufficiently lowering the input resistance of the nonaqueous electrolyte secondary battery, Y is preferably a hydrogen atom, a methyl group, or an ethyl group, and particularly preferably a hydrogen atom or a methyl group.

[0027] Specific examples of the compound represented by formula (1) include 1,3-xylylene diisocyanate, 1,3-bis(2-isocyanato-2-propyl)benzene, toluene diisocyanate, and phenylene diisocyanate. Among them, 1,3-xylylene diisocyanate, 1,3-bis(2-isocyanato-2-propyl)benzene, and toluene diisocyanate are preferred from the viewpoint of lowering the input resistance of the battery. In addition, 1,3-xylylene diisocyanate and 1,3-bis(2-isocyanato-2-propyl)benzene are preferred because they suppress the decomposition of the compound itself while making it easier to exert a protective effect on the active sites.

[0028] <1-1-2. Compound represented by general formula (2)> [ka] (In formula (2), p, q, r, and s are integers satisfying p+q=5 and r+s=5, and p≧1 and s≧1. R may be the same or different and represent a hydrogen atom, a halogen atom, or an organic group having 1 to 10 carbon atoms which may have a heteroatom. X' represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom.)

[0029] In the general formula (2), R's may be the same or different and represent a hydrogen atom, a halogen atom, or an organic group having 1 to 10 carbon atoms which may have a heteroatom. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, etc. A fluorine atom is preferable because it causes fewer electrochemical side reactions. Examples of the heteroatom in the organic group having 1 to 10 carbon atoms which may have a heteroatom include a halogen atom, a phosphorus atom, a silicon atom, an oxygen atom, and a sulfur atom. Examples of the organic group having 1 to 10 carbon atoms which may have a heteroatom include a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, an alkoxy group having 1 to 10 carbon atoms which may have a substituent, an amino group, and an amide group. Of these, a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent or an alkoxy group having 1 to 10 carbon atoms which may have a substituent is preferred. When the hydrocarbon group has a substituent, the number of carbon atoms contained in the substituent is also included in this carbon number. The hydrocarbon group may be a hydrocarbon group having 2 to 10 carbon atoms and a carbon-carbon unsaturated bond. The hydrocarbon group having 2 to 10 carbon atoms and a carbon-carbon unsaturated bond is an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms, which will be described later. Examples of such groups include When there are a plurality of R's in the general formula (2), they may be the same or different, but it is preferable that they are the same in terms of ease of synthesis of the compound. The hydrocarbon group having 1 to 10 carbon atoms is preferably a hydrocarbon group having 1 to 6 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 4 carbon atoms. Specific examples of the hydrocarbon group include an alkyl group, an alkenyl group, an alkynyl group, and an aryl group. Specific examples of the alkyl group include the same groups as those exemplified in the description of the compound represented by formula (1). Preferred are methyl, ethyl, n-propyl, n-butyl, tert-butyl, n-pentyl, and hexyl groups, more preferred are methyl, ethyl, n-propyl, n-butyl, tert-butyl, and n-pentyl groups, and particularly preferred are methyl, ethyl, n-butyl, and tert-butyl groups.

[0030] Specific examples of the alkenyl group include the same groups as those exemplified in the description of the compound represented by formula (1). Among them, vinyl group, allyl group, methallyl group, and 2-butenyl group are preferred, vinyl group, allyl group, and methallyl group are more preferred, and vinyl group or allyl group is particularly preferred. The above-mentioned alkenyl group is preferred because the compound represented by formula (2) tends to be localized near the surface of the positive electrode active material.

[0031] Specific examples of the alkynyl group include the same groups as those exemplified in the description of the compound represented by formula (1). Among them, preferred are ethynyl, 2-propynyl, 2-butynyl, and 3-butynyl groups, more preferred are 2-propynyl and 3-butynyl groups, and particularly preferred are 2-propynyl groups. The above-mentioned alkynyl groups are preferred because the compound represented by formula (2) tends to be localized near the surface of the positive electrode active material.

[0032] Specific examples of the aryl group include the same groups as those exemplified in the description of the compound represented by formula (1). Among them, a phenyl group is preferred from the viewpoint that the compound represented by general formula (2) tends to be localized near the surface of the positive electrode active material. The alkoxy group having 1 to 10 carbon atoms is preferably an alkoxy group having 1 to 6 carbon atoms, and particularly preferably an alkoxy group having 1 to 4 carbon atoms. Specific examples of the alkoxy group having 1 to 10 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, an isopropoxy group, and a methoxyethoxy group, etc. Among these, a methoxy group and an ethoxy group are preferred in that they cause less steric hindrance to the compound represented by the general formula (1) and are suitably concentrated on the surface of the active material.

[0033] Here, the substituent is a cyano group, an isocyanato group, an acyl group (-(C=O)-R a ), acyloxy group (-O(C=O)-R a ), alkoxycarbonyl group (-(C=O)OR a ), sulfonyl group (-SO2-R a ), sulfonyloxy group (-O(SO2)-R a ), alkoxysulfonyl group (-(SO2)-OR a ), alkoxysulfonyloxy group (-O-(SO2)-OR a ), alkoxycarbonyloxy group (-O-(C=O)-OR a ), alkoxy group (-OR a ), a halogen atom (preferably a fluorine atom), a trifluoromethyl group, etc. a R represents an alkyl group having 1 to 10 carbon atoms, an alkylene group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms. a When is an alkylene group, it may be bonded to a part of the hydrocarbon group which substitutes it to form a ring. Among these substituents, a cyano group, an isocyanato group, an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), or a trifluoromethyl group, and more preferably an isocyanato group or an acyloxy group (-O(C=O)-R a ), a halogen atom (preferably a fluorine atom), a trifluoromethyl group, and particularly preferably an acyloxy group (-O(C=O)-R a), halogen atoms (preferably fluorine atoms ) and a trifluoromethyl group. Specific examples of the compound represented by formula (2) include 4,4'-diphenylmethane diisocyanate and bis(4-isocyanatophenyl)dimethylmethane. From the viewpoint of reducing the force resistance, 4,4'-diphenylmethane diisocyanate is preferred.

[0034] The total content of the compound represented by general formula (1) and the isocyanate compound represented by formula (2) relative to the total amount of the nonaqueous electrolyte solution according to one embodiment of the present invention is usually 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.2 mass% or more, and is usually 10 mass% or less, preferably 8 mass% or less, more preferably 6.0 mass% or less, even more preferably 4.0 mass% or less, especially preferably 3.0 mass% or less, particularly preferably 2.0 mass% or less, and most preferably 1.0 mass% or less. When the total content of the isocyanate compounds represented by general formula (1) or (2) relative to the total amount of the nonaqueous electrolyte is within the above-mentioned range, the polymerization of the NCO groups proceeds favorably, the active site covering effect on the positive electrode is sufficiently obtained, and a nonaqueous electrolyte secondary battery with low input resistance can be produced. The method of adding the compound represented by the general formula (1) or the compound represented by the formula (2) to the electrolyte of the present invention is not particularly limited. In addition to the method of directly adding the compound to the electrolyte, the method of generating the compound in the battery or the electrolyte can be mentioned.

[0035] <1-2. Electrolytes> The non-aqueous electrolyte of the present embodiment, like a general non-aqueous electrolyte, usually contains an electrolyte as a component. There is no particular limitation on the electrolyte used in the non-aqueous electrolyte of the present embodiment, and any known electrolyte can be used. Specific examples of the electrolyte will be described in detail below.

[0036] <1-2-1. Lithium salts> When the non-aqueous electrolyte secondary battery using the non-aqueous electrolyte according to the present embodiment is a lithium ion secondary battery, a lithium salt is usually used as the electrolyte. The lithium salt is not particularly limited as long as it is known to be used for this purpose, and one or more of any lithium salts can be used, and specifically, the following can be mentioned.

[0037] For example, inorganic lithium salts such as LiBF4, LiClO4, LiAlF4, LiSbF6, LiTaF6, LiWF7, etc.; Lithium fluorophosphates such as LiPF6; Lithium tungstate salts such as LiWOF5; Lithium carboxylates such as CF3CO2Li; Lithium sulfonate salts such as CH3SO3Li; Lithium imide salts such as LiN(FSO2)2, LiN(CF3SO2)2; Lithium methide salts such as LiC(FSO2)3; Lithium oxalate salts such as lithium bisoxalatoborate and lithium difluorooxalatoborate; Other fluorine-containing organic lithium salts such as LiPF4(CF3)2; etc.

[0038] In order to further enhance the effects of improving the charge / discharge rate characteristics and the impedance characteristics, in addition to the durability improving effect obtained by the present invention, the lithium salt is preferably selected from inorganic lithium salts, lithium fluorophosphate salts, lithium sulfonate salts, lithium imide salts, and lithium oxalate salts, and in order to improve the charge / discharge characteristics, inorganic lithium salts, lithium imide salts, and lithium oxalate salts are more preferable.

[0039] The total concentration of these electrolytes in the non-aqueous electrolyte solution may be any concentration as long as it does not significantly impair the effects of the present invention. There is no limitation, but the lithium salt content is preferably 0.5 mol / L or more, more preferably 0.6 mol / L or more, and even more preferably 0.7 mol / L or more, based on the total amount of the nonaqueous electrolyte, and is preferably 3 mol / L or less, more preferably 2 mol / L or less, and even more preferably 1.8 mol / L or less. By having the lithium salt content within the above range, the ion conductivity can be appropriately increased. When the total concentration of the electrolyte is within the above range, the electrical conductivity becomes appropriate for the operation of the battery, and sufficient output characteristics tend to be obtained. The method for measuring the content of the lithium salts described above is not particularly limited, and any known method can be used, such as ion chromatography, nuclear magnetic resonance spectroscopy, etc.

[0040] <1-3.Non-aqueous solvents> The non-aqueous electrolyte used in this embodiment, like a general non-aqueous electrolyte, usually contains a non-aqueous solvent that dissolves the electrolyte described below as its main component. There is no particular limitation on the non-aqueous solvent used here, and a known organic solvent can be used. The organic solvent is preferably at least one selected from saturated cyclic carbonates, chain carbonates, chain carboxylic acid esters, cyclic carboxylic acid esters, ether compounds, and sulfone compounds, but is not particularly limited thereto. These can be used alone or in combination of two or more.

[0041] <1-3-1. Saturated cyclic carbonates> Examples of the saturated cyclic carbonate include those having an alkylene group having 2 to 4 carbon atoms. Specifically, examples of the saturated cyclic carbonate having 2 to 4 carbon atoms include ethylene carbonate, propylene carbonate, butylene carbonate, etc. Among them, ethylene carbonate and propylene carbonate are preferred from the viewpoint of improving the battery characteristics due to the improvement of the degree of dissociation of lithium ions. The saturated cyclic carbonate may be used alone or in any combination and ratio of two or more kinds.

[0042] The content of the saturated cyclic carbonate is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but the lower limit is usually 3% by volume or more, preferably 5% by volume or more, in 100% by volume of the nonaqueous solvent. By setting it in this range, the decrease in electrical conductivity due to the decrease in the dielectric constant of the nonaqueous electrolyte can be avoided, and the large current discharge characteristics, stability to the negative electrode, and cycle characteristics of the nonaqueous electrolyte secondary battery can be easily set in a good range. The upper limit is usually 90% by volume or less, preferably 85% by volume or less, and more preferably 80% by volume or less. By setting it in this range, the viscosity of the nonaqueous electrolyte can be set in an appropriate range, the decrease in ion conductivity can be suppressed, and the input / output characteristics of the nonaqueous electrolyte secondary battery can be further improved, and durability such as cycle characteristics and storage characteristics can be further improved, which is preferable.

[0043] <1-3-2. Chain carbonate> The chain carbonate preferably has 3 to 7 carbon atoms. Specifically, examples of the chain carbonate having 3 to 7 carbon atoms include dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propyl isopropyl carbonate, ethyl methyl carbonate, methyl-n-propyl carbonate, n-butyl methyl carbonate, isobutyl methyl carbonate, t-butyl methyl carbonate, ethyl-n-propyl carbonate, n-butyl ethyl carbonate, isobutyl ethyl carbonate, t-butyl ethyl carbonate, etc. Among these, dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propyl isopropyl carbonate, ethyl methyl carbonate, and methyl-n-propyl carbonate are preferred, and dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate are particularly preferred.

[0044] In addition, chain carbonates having fluorine atoms (hereinafter, sometimes abbreviated as "fluorinated chain carbonate") can also be suitably used. The number of fluorine atoms in the fluorinated chain carbonate is not particularly limited as long as it is 1 or more, but is usually 6 or less, and preferably 4 or less. When the fluorinated chain carbonate has multiple fluorine atoms, they may be bonded to the same carbon or different carbons. Examples of the fluorinated chain carbonate include fluorinated dimethyl carbonate derivatives, fluorinated ethyl methyl carbonate derivatives, and fluorinated diethyl carbonate derivatives.

[0045] The chain carbonate may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0046] The content of the chain carbonate is not particularly limited, but is usually 15% by volume or more, preferably 20% by volume or more, more preferably 25% by volume or more, in 100% by volume of the nonaqueous solvent. Also, it is usually 90% by volume or less, preferably 85% by volume or less, more preferably 80% by volume or less. By setting the content of the chain carbonate in the above range, the viscosity of the nonaqueous electrolyte is set to an appropriate range, the decrease in ion conductivity is suppressed, and the input / output characteristics and charge / discharge rate characteristics of the nonaqueous electrolyte secondary battery are easily set to a good range. In addition, the decrease in electrical conductivity due to the decrease in the dielectric constant of the nonaqueous electrolyte is avoided, and the input / output characteristics and charge / discharge rate characteristics of the nonaqueous electrolyte secondary battery are easily set to a good range.

[0047] <1-3-3. Chain carboxylate ester> Examples of the chain carboxylate ester include those having a total carbon number of 3 to 7 in the structural formula. Specific examples include methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, n-propyl propionate, isopropyl propionate, n-butyl propionate, isobutyl propionate, t-butyl propionate, methyl butyrate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, methyl isobutyrate, ethyl isobutyrate, n-propyl isobutyrate, isopropyl isobutyrate, etc. Among these, methyl acetate, ethyl acetate, n-propyl acetate, n-butyl acetate, methyl propionate, ethyl propionate, n-propyl propionate, isopropyl propionate, methyl butyrate, ethyl butyrate, etc. are preferred from the viewpoints of improving ion conductivity by reducing viscosity and suppressing battery swelling during durability tests such as cycles and storage. The content of the chain carboxylate as the non-aqueous solvent is not particularly limited, but is usually 5% by volume or more, and usually 50% by volume or less, preferably 30% by volume or less, and more preferably 20% by volume or less, in 100% by volume of the non-aqueous solvent. The chain carboxylate can also be used as an additive in an amount of less than 5% by volume in 100% by volume of the non-aqueous solvent.

[0048] <1-3-4. Cyclic carboxylate ester> Examples of the cyclic carboxylate include those having a total carbon atom number of 3 to 12 in the structural formula. Specific examples include gamma-butyrolactone, gamma-valerolactone, gamma-caprolactone, epsilon-caprolactone, and the like. Among these, gamma-butyrolactone is particularly preferred in terms of improving the battery characteristics due to the improvement in the degree of dissociation of lithium ions. The content of the cyclic carboxylate as the non-aqueous solvent is not particularly limited, but is usually 5% by volume or more, and usually 50% by volume or less, preferably 30% by volume or less, and more preferably 20% by volume or less, in 100% by volume of the non-aqueous solvent. The cyclic carboxylate can also be used as an additive in an amount of less than 5% by volume in 100% by volume of the non-aqueous solvent.

[0049] <1-3-5. Ether compounds> The ether compounds include chain ethers having 3 to 10 carbon atoms and cyclic ethers having 3 to 6 carbon atoms. Ethers are preferred.

[0050] Examples of the chain ether having 3 to 10 carbon atoms include diethyl ether, di(2-fluoroethyl)ether, di(2,2-difluoroethyl)ether, di(2,2,2-trifluoroethyl)ether, ethyl(2-fluoroethyl)ether, ethyl(2,2,2-trifluoroethyl)ether, ethyl(1,1,2,2-tetrafluoroethyl)ether, (2-fluoroethyl)(2,2,2-trifluoroethyl)ether, (2-fluoroethyl)(1,1,2,2-tetrafluoroethyl)ether, and (2,2,2-trifluoroethyl). Ethyl)(1,1,2,2-tetrafluoroethyl)ether, ethyl-n-propyl ether, ethyl(3-fluoro-n-propyl)ether, ethyl(3,3,3-trifluoro-n-propyl)ether, ethyl(2,2,3,3-tetrafluoro-n-propyl)ether, ethyl(2,2,3,3,3-pentafluoro-n-propyl)ether, 2-fluoroethyl-n-propyl ether, (2-fluoroethyl)(3-fluoro-n-propyl)ether, (2-fluoroethyl)(3,3,3-trifluoro-n-propyl pyl) ether, (2-fluoroethyl)(2,2,3,3-tetrafluoro-n-propyl) ether, (2-fluoroethyl)(2,2,3,3,3-pentafluoro-n-propyl) ether, 2,2,2-trifluoroethyl-n-propyl ether, (2,2,2-trifluoroethyl)(3-fluoro-n-propyl) ether, (2,2,2-trifluoroethyl)(3,3,3-trifluoro-n-propyl) ether, (2,2,2-trifluoroethyl)(2,2,3,3-tetrafluoro-n-propyl) ether , (2,2,2-trifluoroethyl)(2,2,3,3,3-pentafluoro-n-propyl)ether, 1,1,2,2-tetrafluoroethyl-n-propyl ether, (1,1,2,2-tetrafluoroethyl)(3-fluoro-n-propyl)ether, (1,1,2,2-tetrafluoroethyl)(3,3,3-trifluoro-n-propyl)ether, (1,1,2,2-tetrafluoroethyl)(2,2,3,3-tetrafluoro-n-propyl)ether, (1,1,2,2-tetrafluoroethyl)(2,2,3,3-tetrafluoro-n-propyl)ether, (1,1,2,2-tetrafluoroethyl)(2,2,3,3,3-Pentafluoro-n-propyl)ether, di-n-propyl ether, (n-propyl)(3-fluoro-n-propyl)ether, (n-propyl)(3,3,3-trifluoro-n-propyl)ether, (n-propyl)(2,2,3,3-tetrafluoro-n-propyl)ether, (n-propyl)(2,2,3,3,3-pentafluoro-n-propyl)ether, di(3-fluoro-n-propyl)ether, (3-fluoro-n-propyl)(3,3,3-trifluoro-n-propyl)ether, (3 -fluoro-n-propyl)(2,2,3,3-tetrafluoro-n-propyl) ether, (3-fluoro-n-propyl)(2,2,3,3,3-pentafluoro-n-propyl) ether, di(3,3,3-trifluoro-n-propyl) ether, (3,3,3-trifluoro-n-propyl)(2,2,3,3-tetrafluoro-n-propyl) ether, (3,3,3-trifluoro-n-propyl)(2,2,3,3,3-pentafluoro-n-propyl) ether, di(2,2,3,3-tetrafluoro-n-propyl) (2,2,3,3-tetrafluoro-n-propyl) ether, (2,2,3,3-pentafluoro-n-propyl) ether, di(2,2,3,3,3-pentafluoro-n-propyl) ether, di-n-butyl ether, dimethoxymethane, methoxyethoxymethane, methoxy(2-fluoroethoxy)methane, methoxy(2,2,2-trifluoroethoxy)methane, methoxy(1,1,2,2-tetrafluoroethoxy)methane, diethoxymethane, ethoxy(2-fluoroethoxy)methane, ethoxy( 2,2,2-trifluoroethoxy)methane, ethoxy(1,1,2,2-tetrafluoroethoxy)methane, di(2-fluoroethoxy)methane, (2-fluoroethoxy)(2,2,2-trifluoroethoxy)methane, (2-fluoroethoxy)(1,1,2,2-tetrafluoroethoxy)methane di(2,2,2-trifluoroethoxy)methane, (2,2,2-trifluoroethoxy)(1,1,2,2-tetrafluoroethoxy)methane, di(1,1,2,2-tetrafluoroethoxy)methane, dimethoxyethane, , methoxyethoxyethane, methoxy(2-fluoroethoxy)ethane, methoxy(2,2,2-trifluoroethoxy)ethane, methoxy(1,1,2,2-tetrafluoroethoxy)ethane, diethoxyethane, ethoxy(2-fluoroethoxy)ethane, ethoxy(2,2,2-trifluoroethoxy)ethane, ethoxy(1,1,2,2-tetrafluoroethoxy)ethane, di(2-fluoroethoxy)ethane, (2-fluoroethoxy)(2,2,2-trifluoroethoxy)ethane (2-fluoroethoxy)(1,1,2,2-tetrafluoroethoxy)ethane, di(2,2,2-trifluoroethoxy)ethane, (2,2,2-trifluoroethoxy)(1,1,2,2-tetrafluoroethoxy)ethane, di(1,1,2,2-tetrafluoroethoxy)ethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, diethylene glycol dimethyl ether, and the like.

[0051] Examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, 1,3-dioxane, 2-methyl-1,3-dioxane, 4-methyl-1,3-dioxane, 1,4-dioxane, and fluorinated compounds thereof. Among these, dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether are preferred in terms of their high solvation ability to lithium ions and their improved lithium ion dissociation ability. Particularly preferred are dimethoxymethane, diethoxymethane, and ethoxymethoxymethane, which have low viscosity and provide high ionic conductivity. The content of the cyclic ether as the non-aqueous solvent is not particularly limited, but is usually 5% by volume or more, and usually 50% by volume or less, preferably 30% by volume or less, and more preferably 20% by volume or less, in 100% by volume of the non-aqueous solvent. The cyclic ether can also be used as an additive in an amount of less than 5% by volume in 100% by volume of the non-aqueous solvent.

[0052] <1-3-6. Sulfone compounds> The sulfone-based compound is preferably a cyclic sulfone having 3 to 6 carbon atoms, or a chain sulfone having 2 to 6 carbon atoms. The number of sulfonyl groups in one molecule is preferably 1 or 2.

[0053] Examples of cyclic sulfones include monosulfone compounds such as trimethylene sulfones, tetramethylene sulfones, and hexamethylene sulfones; and disulfone compounds such as trimethylene disulfones, tetramethylene disulfones, and hexamethylene disulfones. Among these, from the viewpoint of dielectric constant and viscosity, tetramethylene sulfones, tetramethylene disulfones, hexamethylene sulfones, and hexamethylene disulfones are more preferred, and tetramethylene sulfones (sulfolanes) are particularly preferred.

[0054] The sulfolane is preferably sulfolane and / or a sulfolane derivative (hereinafter, sulfolane may be abbreviated as "sulfolane") The sulfolane derivative is preferably one in which one or more hydrogen atoms bonded to the carbon atom constituting the sulfolane ring are substituted with a fluorine atom or an alkyl group.

[0055] Among these, 2-methylsulfolane, 3-methylsulfolane, 2-fluorosulfolane, 3-fluorosulfolane, 2,2-difluorosulfolane, 2,3-difluorosulfolane, 2,4-difluorosulfolane, 2,5-difluorosulfolane, 3,4-difluorosulfolane, 2-fluoro-3-methylsulfolane, 2-fluoro-2-methylsulfolane, 3-fluoro-3-methylsulfolane, 3-fluoro-2-methylsulfolane, 4-fluoro-3-methylsulfolane, 4-fluoro-2-methylsulfolane, 5-fluoro-3-methylsulfolane, 5-fluoro-2-methylsulfolane, 2-fluoromethylsulfolane, 3-fluoromethylsulfolane, 2-difluoromethylsulfolane, 3-Difluoromethylsulfolane, 2-trifluoromethylsulfolane, 3-trifluoromethylsulfolane, 2-fluoro-3-(trifluoromethyl)sulfolane, 3-fluoro-3-(trifluoromethyl)sulfolane, 4-fluoro-3-(trifluoromethyl)sulfolane, 5-fluoro-3-(trifluoromethyl)sulfolane, and the like are preferred because they have high ionic conductivity and high input / output.

[0056] Examples of the chain sulfone include dimethyl sulfone, ethyl methyl sulfone, diethyl sulfone, n-propyl methyl sulfone, n-propyl ethyl sulfone, di-n-propyl sulfone, isopropyl methyl sulfone, isopropyl ethyl sulfone, diisopropyl sulfone, n-butyl methyl sulfone, n-butyl ethyl sulfone, t-butyl methyl sulfone, t-butyl ethyl sulfone, monofluoromethyl methyl sulfone, difluoromethyl methyl sulfone, trifluoromethyl methyl sulfone, monofluoroethyl methyl sulfone, difluoroethyl methyl sulfone, trifluoroethyl methyl sulfone, pentafluoroethyl methyl sulfone, ethyl monofluoromethyl sulfone, ethyl difluoromethyl sulfone, ethyl trifluoromethyl sulfone, perfluoroethyl methyl sulfone, ethyl trifluoroethyl sulfone, ethyl ethyl pentafluoroethyl sulfone, di(trifluoroethyl)sulfone, perfluorodiethyl sulfone, fluoromethyl-n-propyl sulfone, difluoromethyl-n-propyl sulfone, trifluoromethyl-n-propyl sulfone, fluoromethyl isopropyl sulfone, difluoromethyl isopropyl sulfone, trifluoromethyl isopropyl sulfone, trifluoroethyl-n-propyl sulfone, trifluoromethyl-n-butyl sulfone, trifluoromethyl-t-butyl sulfone, trifluoroethyl isopropyl sulfone, pentafluoroethyl-n-propyl sulfone, pentafluoroethyl isopropyl sulfone, trifluoroethyl-n-butyl sulfone, trifluoroethyl-t-butyl sulfone, pentafluoroethyl-n-butyl sulfone, pentafluoroethyl-t-butyl sulfone, and the like.

[0057] Among these, dimethyl sulfone, ethyl methyl sulfone, diethyl sulfone, n-propyl methyl sulfone, isopropyl methyl sulfone, n-butyl methyl sulfone, t-butyl methyl sulfone, monofluoromethyl methyl sulfone, difluoromethyl methyl sulfone, trifluoromethyl methyl sulfone, monofluoroethyl methyl sulfone, difluoroethyl methyl sulfone, trifluoroethyl methyl sulfone, pentafluoroethyl methyl sulfone, ethyl monofluoromethyl sulfone, ethyl difluoromethyl sulfone, ethyl trifluoromethyl sulfone, ethyl trifluoroethyl sulfone, ethyl pentafluoroethyl sulfone, trifluoromethyl-n-propyl sulfone, trifluoromethyl isopropyl sulfone, trifluoroethyl-n-butyl sulfone, trifluoroethyl-t-butyl sulfone, trifluoromethyl-n-butyl sulfone, trifluoromethyl-t-butyl sulfone, and the like are preferred in terms of high ionic conductivity and high input / output.

[0058] The content of the sulfone-based compound as the non-aqueous solvent is not particularly limited, but is usually 10% by volume or more, and usually 50% by volume or less, preferably 30% by volume or less, and more preferably 20% by volume or less, in 100% by volume of the non-aqueous solvent. The sulfone-based compound can also be used as an additive in an amount of less than 10% by volume in 100% by volume of the non-aqueous solvent.

[0059] <1-4. Additives> The nonaqueous electrolyte used in this embodiment contains, in addition to the various compounds listed above, Unsaturated cyclic carbonates such as vinylene carbonate, vinyl ethylene carbonate, or ethynyl ethylene carbonate; Fluorinated cyclic carbonates such as monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, and 4,5-difluoro-4,5-dimethylethylene carbonate; Carbonate compounds such as methoxyethyl-methyl carbonate; Spiro compounds such as methyl-2-propynyl oxalate; Isocyanate compounds such as diisocyanates having a cycloalkylene group, such as 1,3-bis(isocyanatomethyl)cyclohexane; Nitrogen-containing compounds such as 1-methyl-2-pyrrolidinone; Hydrocarbon compounds such as cycloheptane; Fluorinated aromatic compounds such as fluorobenzene; Silane compounds such as tris(trimethylsilyl) borate, tris(trimethylsilyl) phosphate, and tetravinylsilane; Ester compounds such as 2-propynyl 2-(methanesulfonyloxy)propionate; Lithium salts such as lithium ethylmethyloxycarbonylphosphonate; Isocyanate esters such as triallyl isocyanurate; Compounds having a cyano group, such as malononitrile, succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, azelanitrile, sebaconitrile, undecanedinitrile, dodecanedinitrile, and hexanetricarbonitrile; Carboxylic acid anhydride compounds such as acrylic anhydride, 2-methylacrylic anhydride, 3-methylacrylic anhydride, benzoic anhydride, 2-methylbenzoic anhydride, 4-methylbenzoic anhydride, 4-tert-butylbenzoic anhydride, 4-fluorobenzoic anhydride, 2,3,4,5,6-pentafluorobenzoic anhydride, methoxyformic anhydride, ethoxyformic anhydride, succinic anhydride, and maleic anhydride; Compounds with an SO2 structure, such as lithium fluorosulfonate (LiFSO3), lithium bis(fluorosulfonyl)imide (LiN(FSO2)2), methyl methanesulfonate, 1,3-propane sultone, dimethyl sulfate, and ethylene sulfate; Compounds having a PF bond such as lithium difluorophosphate may be added. However, although the lithium difluorophosphate mentioned here corresponds to a lithium salt, it is not treated as an electrolyte from the viewpoint of the degree of ionization with respect to the non-aqueous solvent used in the non-aqueous electrolyte, but is positioned as an additive. In addition, various additives such as cyclohexylbenzene, t-butylbenzene, t-amylbenzene, biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, diphenyl ether, and dibenzofuran may be blended as an overcharge inhibitor within a range that does not significantly impair the effects of the present invention. These compounds may be used in appropriate combination.

[0060] In the non-aqueous electrolyte used in this embodiment, particularly preferred additives that have a particularly high additive effect and exhibit a synergistic effect include (A) a compound having a PF bond and (B) a compound having an SO2 structure. These are incorporated in the polymerization process of the isocyanate compound represented by formula (1) or formula (2), and are considered to suppress input resistance while further suppressing side reactions at the positive electrode, thereby improving the initial charge / discharge efficiency.

[0061] <1-4-1.(A) Compounds with PF bonds> (A) The compound having a PF bond is not particularly limited as long as it has a PF bond in the molecule, and any compound can be used as long as it does not significantly impair the effects of the present invention. Among them, a phosphate having a PF bond is preferred. There is no particular limitation on the counter cation of the phosphate having a PF bond, but lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, barium, and NR 13 R 14 R 15 R 16 (In the formula, R 13 ~R 16Each of the groups independently represents a hydrogen atom or an organic group having 1 to 12 carbon atoms. Examples of the ammonium represented by the formula: are listed below. Among these, lithium is particularly preferred. In addition, the number of PF bonds contained in the molecule is preferably 2 or more, since the oxidation potential increases. Specifically, lithium difluorobis(oxalato)phosphate and lithium difluorophosphate are particularly preferred. The compounds having a PF bond may be used alone or in any combination of two or more. The content of the compound having a PF bond is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but is usually 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and is usually 10% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and most preferably 1% by mass or less, in 100% by mass of the nonaqueous electrolyte solution. If the content of the compound having a PF bond is within this range, it is possible to increase the initial charge / discharge efficiency while suppressing the input resistance of the nonaqueous electrolyte secondary battery.

[0062] <1-4-2.(B) Compounds with SO2 structure> (B) The compound having an SO2 structure is not particularly limited as long as it has an SO2 structure in the molecule, and any compound can be used as long as it does not significantly impair the effects of the present invention. Among them, a lithium salt having an SO2 structure or an ester compound having an SO2 structure is preferred. Examples of lithium salts having an SO2 structure include: Lithium fluorosulfonate (LiFSO3); Lithium bis(fluorosulfonyl)imide (LiN(FSO2)2), LiN(F S Lithium salts of fluorosulfonylimides such as LiN(CF3SO2)2, LiN(CF3SO2)2, etc.; Lithium salts of fluorosulfonylmethides such as LiC(FSO2)3; Lithium fluorosulfonylborates such as LiBF3(FSO3) and LiB(FSO2)4; Among the compounds having an SO2 structure, Li salts having an FS bond are preferred. Among them, LiFSO3 and LiN(FSO2)2 are particularly preferred because they have a small molecular structure and are easily accessible to the positive electrode. Examples of esters having an SO2 structure include: Chain sulfonate esters such as methyl methanesulfonate and ethyl methanesulfonate; Cyclic sulfonic acid esters such as 1,3-propane sultone, 1-propene 1,3-sultone; Chain sulfate esters such as dimethyl sulfate and diethyl sulfate; cyclic sulfate esters such as ethylene sulfate, propylene sulfate, etc.; Of the compounds having an SO2 structure, those having 2 to 10 carbon atoms are preferred, and further, from the viewpoint of small molecular structure and easy access to the positive electrode, chain sulfonate esters having 2 to 4 carbon atoms and chain sulfate esters having 2 to 4 carbon atoms are particularly preferred, and from the viewpoint of structural stability, cyclic sulfonate esters having 3 to 4 carbon atoms and cyclic sulfate esters having 2 to 3 carbon atoms are particularly preferred. More preferred are cyclic sulfonate esters having 3 to 4 carbon atoms and cyclic sulfate esters having 2 to 3 carbon atoms, specifically 1,3-propane sultone and ethylene sulfate. The compound having SO2 structure may be used alone or in any combination and ratio of two or more. The content of the compound having SO2 structure is not particularly limited and may be any as long as it does not significantly impair the effect of the present invention, but is usually 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 2 mass% or less, and most preferably 1 mass% or less in 100 mass% of non-aqueous electrolyte solution. If the content of the compound having an SO2 structure is within this range, it is possible to increase the initial charge / discharge efficiency while suppressing the input resistance of the nonaqueous electrolyte secondary battery. However, LiN(FSO2)2 may be used as a main salt, in which case the above content is not limited. Also, for example, a compound having an SO2 structure, such as a sulfone-based compound, may be used as a non-aqueous solvent, in which case the above content is not limited.

[0063] As described above, the nonaqueous electrolyte according to this embodiment comprises: (A) a compound having a PF bond; It is preferable to include at least one compound having a (B) SO2 structure, and the compound having a (A) PF bond and the compound having a (B) SO2 structure may be used in combination of two or more. When at least one compound having a (A) PF bond and at least one compound having a (B) SO2 structure are combined, the effect of increasing the initial charge / discharge efficiency of the non-aqueous electrolyte battery becomes more pronounced, which is preferable. In addition, in the nonaqueous electrolyte solution according to this embodiment, the use of one or more selected from unsaturated cyclic carbonates and cyclic carbonates having fluorine atoms in combination is preferable in that gas generation during initial conditioning is further suppressed, resulting in a battery that is less prone to swelling. The "unsaturated cyclic carbonate" and the "fluorinated cyclic carbonate" will be described in detail below.

[0064] <1-4-3. Unsaturated cyclic carbonates> In this specification, the term "unsaturated cyclic carbonate" refers to a cyclic carbonate having a carbon-carbon unsaturated bond, and is not particularly limited as long as it is a carbonate having a carbon-carbon unsaturated bond such as a carbon-carbon double bond or a carbon-carbon triple bond, and any unsaturated cyclic carbonate can be used. Examples of unsaturated cyclic carbonates include vinylene carbonates and ethylene carbonates substituted with a substituent having a carbon-carbon unsaturated bond. Specific examples of vinylene carbonates include vinylene carbonate, methylvinylene carbonate, and 4,5-dimethylvinylene carbonate. Specific examples of ethylene carbonates substituted with a substituent having a carbon-carbon unsaturated bond include vinyl ethylene carbonate, 4,5-divinyl ethylene carbonate, ethynyl ethylene carbonate, and propargyl ethylene carbonate. Among these, vinylene carbonate, vinyl ethylene carbonate, and ethynyl ethylene carbonate are preferred, and vinylene carbonate is particularly preferred because it can contribute to the formation of a stable film-like structure. The molecular weight of the unsaturated cyclic carbonate is not particularly limited and may be any value as long as it does not significantly impair the effects of the present invention, but is usually at least 50, preferably at least 80, and usually at most 250, preferably at most 150. Within this range, the solubility of the unsaturated cyclic carbonate in the nonaqueous electrolyte is easily ensured, and the effects of the present invention are easily exhibited. The unsaturated cyclic carbonate may be used alone or in any combination and ratio of two or more. The content of the unsaturated cyclic carbonate is not particularly limited and may be any as long as it does not significantly impair the effects of the present invention, but the content of the unsaturated cyclic carbonate is usually 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.2 mass% or more, and is usually 10 mass% or less, preferably 8 mass% or less, and more preferably 5 mass% or less, in 100 mass% of the nonaqueous electrolyte. If the content of the unsaturated cyclic carbonate is within the above range, the nonaqueous electrolyte secondary battery is likely to exhibit sufficient high-temperature storage characteristics and cycle characteristic improvement effects.

[0065] <1-4-4. Fluorinated cyclic carbonates> As used herein, a "fluorinated cyclic carbonate" is a cyclic carbonate having a fluorine atom. The fluorinated cyclic carbonate may be a derivative of a cyclic carbonate having an alkylene group having 2 to 6 carbon atoms, such as an ethylene carbonate derivative. The ethylene carbonate derivative may be, for example, a fluorinated product of ethylene carbonate or ethylene carbonate substituted with an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms), and among these, those having 1 to 8 fluorine atoms are preferred. Specifically, monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4-fluoro-4-methylethylene carbonate, 4,5-difluoro-4-methylethylene carbonate, 4-fluoro- Examples of the ethylene carbonate include 5-methylethylene carbonate, 4,4-difluoro-5-methylethylene carbonate, 4-(fluoromethyl)-ethylene carbonate, 4-(difluoromethyl)-ethylene carbonate, 4-(trifluoromethyl)-ethylene carbonate, 4-(fluoromethyl)-4-fluoroethylene carbonate, 4-(fluoromethyl)-5-fluoroethylene carbonate, 4-fluoro-4,5-dimethylethylene carbonate, 4,5-difluoro-4,5-dimethylethylene carbonate, and 4,4-difluoro-5,5-dimethylethylene carbonate. Among these, at least one selected from the group consisting of monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, and 4,5-difluoro-4,5-dimethylethylene carbonate is more preferred in that it provides high ion conductivity and favorably forms an interface protective coating. The fluorinated cyclic carbonates may be used alone or as a mixture of two or more kinds in any combination and in any ratio. The fluorinated cyclic carbonate may be used as an additive to the non-aqueous electrolyte or as a non-aqueous solvent. The content of the fluorinated cyclic carbonate when used as a non-aqueous solvent is usually 8% by mass or more, preferably 10% by mass or more, more preferably 12% by mass or more, and usually 85% by mass or less, preferably 80% by mass or less, and more preferably 75% by mass or less, in 100% by mass of the non-aqueous electrolyte. In this range, the non-aqueous electrolyte secondary battery is likely to exhibit a sufficient cycle characteristic improvement effect, and it is easy to avoid a decrease in the discharge capacity retention rate. The content of the fluorinated cyclic carbonate when used as an additive is usually 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more, in 100% by mass of the non-aqueous electrolyte. It is usually 10% by mass or less, preferably 8% by mass or less, and more preferably 5% by mass or less. When the content of the fluorinated cyclic carbonate is within the above range, the nonaqueous electrolyte secondary battery is likely to exhibit sufficient high-temperature storage characteristics and improved cycle characteristics. In the nonaqueous electrolyte according to one embodiment of the present invention, the unsaturated cyclic carbonate or fluorinated cyclic carbonate is preferably at least one selected from the group consisting of vinylene carbonate, vinyl ethylene carbonate, ethynyl ethylene carbonate, and fluoroethylene carbonate.

[0066] As the fluorinated cyclic carbonate, a cyclic carbonate having an unsaturated bond and a fluorine atom (hereinafter, sometimes abbreviated as "fluorinated unsaturated cyclic carbonate") can be used. The fluorinated unsaturated cyclic carbonate is not particularly limited. Among them, those having one or two fluorine atoms are preferable. The method for producing the fluorinated unsaturated cyclic carbonate is not particularly limited, and it is possible to produce it by arbitrarily selecting a known method. Examples of the fluorinated unsaturated cyclic carbonate include vinylene carbonate derivatives and ethylene carbonate derivatives substituted with a substituent having an aromatic ring or a carbon-carbon unsaturated bond. Examples of the vinylene carbonate derivatives include 4-fluorovinylene carbonate, 4-fluoro-5-methylvinylene carbonate, 4-fluoro-5-phenylvinylene carbonate, and 4,5-difluoroethylene carbonate. Examples of ethylene carbonate derivatives substituted with a substituent having an aromatic ring or a carbon-carbon unsaturated bond include 4-fluoro-4-vinylethylene carbonate, 4-fluoro-5-vinylethylene carbonate, 4,4-difluoro-4-vinylethylene carbonate, 4,5-difluoro-4-vinylethylene carbonate, 4-fluoro-4,5-divinylethylene carbonate, 4,5-difluoro-4,5-divinylethylene carbonate, 4-fluoro-4-phenylethylene carbonate, 4-fluoro-5-phenylethylene carbonate, 4,4-difluoro-5-phenylethylene carbonate, and 4,5-difluoro-4-phenylethylene carbonate. The molecular weight of the fluorinated unsaturated cyclic carbonate is not particularly limited, and the effect of the present invention can be significantly improved. The value may be any value as long as it does not impair the electrochemical properties, but is usually at least 50, preferably at least 80, and is usually at most 250, preferably at most 150. Within this range, the solubility of the fluorinated cyclic carbonate in the nonaqueous electrolyte solution is easily ensured, and the effects of the present invention are easily achieved. The fluorinated unsaturated cyclic carbonate may be used alone or in any combination and ratio of two or more. The amount of the fluorinated unsaturated cyclic carbonate is not particularly limited and may be any amount as long as it does not significantly impair the effects of the present invention, but is usually 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and is usually 5% by mass or less, preferably 4% by mass or less, more preferably 3% by mass or less, in 100% by mass of the non-aqueous electrolyte. Within this range, the non-aqueous electrolyte secondary battery is likely to exhibit a sufficient effect of improving cycle characteristics.

[0067] The content of the additives other than the (A) compound having a PF bond, (B) compound having an SO2 structure, unsaturated cyclic carbonate and fluorinated cyclic carbonate is not particularly limited and can be any amount as long as it does not significantly impair the effects of the present invention, but is usually 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and is usually 5% by mass or less, preferably 3% by mass or less, more preferably 1% by mass or less, based on the total amount of the non-aqueous electrolyte. Within this range, the effects of the other additives are easily exerted, and high-temperature storage stability tends to be improved. When two or more additives other than the (A) compound having a PF bond, (B) compound having an SO2 structure, unsaturated cyclic carbonate and fluorinated cyclic carbonate are used in combination, the total amount of the additives should be set to satisfy the above range.

[0068] In this specification, the composition of the nonaqueous electrolyte means the composition at the time of production of the nonaqueous electrolyte, at the time of injection of the nonaqueous electrolyte into a battery, or at the time of shipment of the battery. That is, the nonaqueous electrolyte may be mixed so that the ratio of each component is a predetermined composition when preparing the nonaqueous electrolyte. After preparing the nonaqueous electrolyte, the nonaqueous electrolyte itself can be subjected to analysis to confirm the composition. The nonaqueous electrolyte may be collected from the completed nonaqueous electrolyte secondary battery and subjected to analysis. Examples of a method for collecting the nonaqueous electrolyte include a method in which the battery container is partially or entirely opened or a hole is provided in the battery container to collect the electrolyte. The opened battery container may be centrifuged to collect the electrolyte, or an extraction solvent (for example, acetonitrile dehydrated to a water content of 10 ppm or less is preferable) may be placed in the opened battery container or the extraction solvent may be brought into contact with the battery element to extract the electrolyte. The nonaqueous electrolyte collected by such a method can be subjected to analysis. The collected nonaqueous electrolyte may be diluted to provide conditions suitable for analysis and subjected to analysis.

[0069] Specific examples of the method for analyzing non-aqueous electrolytes include nuclear magnetic resonance (hereinafter sometimes abbreviated as NMR) and liquid chromatography such as gas chromatography and ion chromatography. The analysis method using NMR will be described below. In an inert atmosphere, the non-aqueous electrolyte is dissolved in a deuterated solvent that has been dehydrated to 10 ppm or less, and then placed in an NMR tube to perform NMR measurement. Alternatively, a double tube may be used as the NMR tube, with the non-aqueous electrolyte placed in one tube and the deuterated solvent placed in the other tube to perform NMR measurement. Examples of deuterated solvents include deuterated acetonitrile and deuterated dimethyl sulfoxide. When determining the concentration of the components of the non-aqueous electrolyte, a specified amount of a standard substance is dissolved in the deuterated solvent, and the concentration of each component can be calculated from the ratio of the spectra. Alternatively, the concentration of one or more components that make up the non-aqueous electrolyte can be determined in advance by another analytical method such as gas chromatography, and the concentration can be calculated from the spectral ratio of the component with a known concentration to the other components. The nuclear magnetic resonance analyzer used is preferably one that has a magnetic field of 400 MHz or more. The nuclides to be measured are as follows: 1 H, 31 P, 19 Examples include F. These analytical techniques may be used alone or in combination of two or more.

[0070] <2. Non-aqueous electrolyte secondary battery> A nonaqueous electrolyte secondary battery according to one embodiment of the present invention is a nonaqueous electrolyte secondary battery comprising a positive electrode capable of absorbing and releasing metal ions, a negative electrode capable of absorbing and releasing metal ions, and a nonaqueous electrolyte solution containing a nonaqueous solvent and an electrolyte dissolved in the nonaqueous solvent, wherein the positive electrode contains a transition metal oxide and at least Ni and Co as transition metals, with at least 40 mol % of the transition metals being Ni, the negative electrode contains a carbon-based material, and the nonaqueous electrolyte solution contains at least one isocyanate compound selected from the compounds represented by the above-mentioned general formula (1) and the compounds represented by the general formula (2).

[0071] <2-1. Battery configuration> The nonaqueous electrolyte secondary battery of this embodiment has the same configuration as that of a conventional nonaqueous electrolyte secondary battery except for the nonaqueous electrolyte, the positive electrode, and the negative electrode. Usually, the positive electrode and the negative electrode are laminated through a porous membrane (separator) impregnated with the nonaqueous electrolyte, and these are housed in a case (exterior body). Therefore, the shape of the nonaqueous electrolyte secondary battery of this embodiment is not particularly limited, and may be any of a cylindrical type, a square type, a laminate type, a coin type, a large type, etc.

[0072] <2-2. Non-aqueous electrolyte> As the non-aqueous electrolyte solution, the non-aqueous electrolyte solution according to the embodiment of the present invention is used. Note that, within the scope of the present invention, it is also possible to mix other non-aqueous electrolyte solutions with the non-aqueous electrolyte solution.

[0073] <2-3. Positive electrode> In one embodiment of the present invention, the positive electrode has a current collector and a positive electrode active material layer provided on the current collector. The positive electrode used in the nonaqueous electrolyte secondary battery of this embodiment will be described in detail below.

[0074] <2-3-1. Positive electrode active material> The positive electrode active material used in the positive electrode will be described below. (1) Composition The positive electrode active material is a transition metal oxide capable of absorbing and releasing metal ions, and contains at least Ni and Co as transition metals, with 40 mol % or more of the transition metals being Ni. For example, a material capable of electrochemically absorbing and releasing lithium ions is preferred, and contains lithium and at least Ni and Co, with 50 mol % or more of the transition metals being Ni, and more preferably 60 mol % or more of Ni. This is because Ni and Co have oxidation-reduction potentials suitable for use as positive electrode materials for secondary batteries, and are suitable for high-capacity applications.

[0075] The transition metal components of the lithium transition metal oxide include Ni and Co as essential elements, and other metals include Mn, V, Ti, Cr, Fe, Cu, Al, Mg, Zr, Er, etc., with Mn, Ti, Fe, Al, Mg, Zr, etc. being preferred. Specific examples of lithium transition metal oxides include LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.1 O 2、 , LiNi 0.7 Co 0.15 Mn 0.15 O 2、 , LiNi 0.6 Co 0.2 Mn 0.2 O 2、 LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.5 Co 0.3 Mn 0.2 O2, Li 1.05 Ni 0.50 Co 0.21 Mn 0.29 O2, LiNi 0.5 Co 0.3 Mn 0.2 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, etc.

[0076] Among these, a preferred embodiment is a transition metal oxide represented by the following composition formula (α). Li a1 Ni b1 Co c1 M d1 O2 (α) (In the above formula (α), a1, b1, c1, and d1 satisfy 0.90≦a1≦1.10, 0.4≦b1<1.0, and b1+c1+d1=1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) In the composition formula (α), it is preferable that d1 satisfies 0.10≦d1<0.40, and it is also preferable that b1 satisfies 0.50≦b1≦0.96. This is because, since the main components are Ni and Co and the composition ratio of Ni is greater than the composition ratio of Co, when used as a positive electrode of a non-aqueous electrolyte battery, it is stable and it is possible to extract a high capacity.

[0077] Among these, a transition metal oxide represented by the following composition formula (β) is preferred. Li a2 Ni b2 Co c2 M d2 O2 (β) (In formula (β), the numerical values ​​are 0.90≦a2≦1.10, 0.50≦b2≦0.94, 0.05≦c2≦0.2, and 0.01≦d2≦0.3, and b2+c2+d2=1 is satisfied. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) In the composition formula (β), it is preferable that the value 0.10≦d2≦0.3 is indicated. This is because, with the above composition, it becomes possible to obtain a particularly high capacity when used as the positive electrode of a non-aqueous electrolyte secondary battery.

[0078] In addition, two or more of the above positive electrode active materials may be mixed and used. Similarly, at least one of the above positive electrode active materials may be mixed and used with another positive electrode active material. Examples of the other positive electrode active materials include transition metal oxides, transition metal phosphate compounds, transition metal silicate compounds, and transition metal borate compounds not listed above. Among them, lithium manganese composite oxides having a spinel structure and lithium-containing transition metal phosphate compounds having an olivine structure are preferred. Specifically, lithium manganese composite oxides having a spinel structure include LiMn2O4, LiMn 1.8 Al 0.2 O4, LiMn 1.5 Ni 0.5 Among them, O4 has the most stable structure, is less likely to release oxygen even in the event of an abnormality in the non-aqueous electrolyte battery, and is therefore excellent in safety. In addition, the transition metal of the lithium-containing transition metal phosphate compound is preferably V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc., and specific examples include iron phosphates such as LiFePO4, Li3Fe2(PO4)3, LiFeP2O7, cobalt phosphates such as LiCoPO4, manganese phosphates such as LiMnPO4, and lithium transition metal phosphate compounds in which a part of the transition metal atoms that constitute the main part of these lithium transition metal phosphate compounds has been replaced with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Si, Nb, Mo, Sn, W, etc. Among them, lithium iron phosphate compounds are preferred because iron is an abundant and extremely inexpensive metal and is less harmful. That is, among the above specific examples, LiFePO4 can be cited as a more preferred specific example.

[0079] In one embodiment of the present invention, the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 40 mol % or more, and more preferably 50 mol % or more, from the viewpoint of increasing the capacity of the nonaqueous electrolyte secondary battery. In this specification, the NMC positive electrode refers to a positive electrode in which the positive electrode active material contains nickel-manganese-cobalt (NMC) and is a material represented by the following formula (I). Li a Ni b Co c Mn d O2···(I) (In the above formula (I), a, b, c, and d satisfy 0.90≦a≦1.10, 0.40≦b<1.0, and b+c+d=1.)

[0080] (2) Surface coating The surface of the positive electrode active material is coated with a substance having a different composition from the substance constituting the main positive electrode active material. It is also possible to use a material having a surface-attached substance (hereinafter, appropriately referred to as "surface-attached substance") attached thereto. Examples of surface-attached substances include oxides such as aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; and carbon.

[0081] These surface-attaching substances can be attached to the surface of the positive electrode active material by, for example, a method of dissolving or suspending the substance in a solvent, impregnating the positive electrode active material with the substance, and then drying the substance, a method of dissolving or suspending a surface-attaching substance precursor in a solvent, impregnating the positive electrode active material with the substance, and then reacting the substance by heating or the like, a method of adding the substance to a positive electrode active material precursor and simultaneously baking the substance, etc. When carbon is attached, a method of mechanically attaching the carbonaceous material, for example, in the form of activated carbon, etc., after the surface-attaching substance is attached can also be used.

[0082] The mass of the surface-attached substance attached to the surface of the positive electrode active material is preferably 0.1 ppm or more, more preferably 1 ppm or more, and even more preferably 10 ppm or more, relative to the mass of the positive electrode active material, and is preferably 20% or less, more preferably 10% or less, and even more preferably 5% or less. The surface-attached substance can suppress the oxidation reaction of the non-aqueous electrolyte on the surface of the positive electrode active material, thereby improving the battery life. In addition, when the amount of the attached substance is within the above range, the effect can be fully exerted, and the inflow and outflow of lithium ions is not hindered, and the resistance is not likely to increase.

[0083] (3) Shape The positive electrode active material particles may have a conventional shape such as a block, polyhedron, sphere, oval sphere, plate, needle, column, etc. Primary particles may be aggregated to form secondary particles, and the secondary particles may have a spherical or oval sphere shape.

[0084] (4) Manufacturing method of positive electrode active material The method for producing the positive electrode active material is not particularly limited as long as it does not deviate from the gist of the present invention. Several methods can be mentioned, and a general method for producing an inorganic compound can be used. In particular, various methods can be considered for producing spherical or ellipsoidal active materials. One example is a method in which transition metal raw materials such as transition metal nitrates or sulfates, and, if necessary, raw materials of other elements, are dissolved or crushed and dispersed in a solvent such as water, and the pH is adjusted while stirring to produce and recover a spherical precursor, which is then dried if necessary, and a Li source such as LiOH, Li2CO3, or LiNO3 is added and the mixture is fired at high temperature to obtain the active material.

[0085] Another example of the method is to dissolve or pulverize and disperse transition metal raw materials such as transition metal nitrates, sulfates, hydroxides, and oxides, and, if necessary, raw materials of other elements, in a solvent such as water, and then dry and mold the resulting mixture using a spray dryer or the like to form a spherical or ellipsoidal precursor. To this, a Li source such as LiOH, Li2CO3, or LiNO3 is added, and the mixture is fired at high temperature to obtain an active material.

[0086] As yet another example of the method, a transition metal raw material such as a transition metal nitrate, sulfate, hydroxide, or oxide, a Li source such as LiOH, Li2CO3, or LiNO3, and, if necessary, raw materials of other elements are dissolved or pulverized and dispersed in a solvent such as water, and then dried and molded using a spray dryer or the like to form a spherical or ellipsoidal precursor, which is then fired at a high temperature to obtain the active material.

[0087] <2-3-2. Positive electrode structure and manufacturing method> The configuration of the positive electrode used in the present invention and the method for producing the same will be described below. (Method of making positive electrode) The positive electrode is produced by forming a positive electrode active material layer containing positive electrode active material particles and a binder on a current collector. The positive electrode using the positive electrode active material can be produced by any known method. For example, the positive electrode active material and the binder, and if necessary, a conductive material and a thickener, etc. are mixed in a dry state to form a sheet, which is then pressed onto the positive electrode current collector, or these materials are dissolved or dispersed in a liquid medium to form a slurry, which is then applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector, thereby obtaining a positive electrode.

[0088] The content of the positive electrode active material in the positive electrode active material layer is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and preferably 99.9% by mass or less, more preferably 99% by mass or less. When the content of the positive electrode active material is within the above range, the electric capacity can be sufficiently ensured. Furthermore, the strength of the positive electrode is also sufficient. In addition, the positive electrode active material powder in the present invention contains at least Ni and Co as transition metals, and as long as a positive electrode having 40 mol % or more of the transition metals being Ni is produced, one type may be used alone, or two or more types having different compositions or different powder properties may be used in any combination and ratio.

[0089] <Conductive material> Any known conductive material can be used as the conductive material. Specific examples include metal materials such as copper and nickel; graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; and carbon-based materials such as amorphous carbon such as needle coke. These materials may be used alone or in any combination and ratio of two or more.

[0090] The content of the conductive material in the positive electrode active material layer is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 1% by mass or more, and is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 15% by mass or less. When the content of the conductive material is within the above range, sufficient conductivity can be ensured. Furthermore, the decrease in battery capacity is easily prevented.

[0091] <Binding agent> The binder used in producing the positive electrode active material layer is not particularly limited as long as it is a material that is stable to the nonaqueous electrolyte solution and the solvent used in producing the electrode. In the case of the coating method, there is no particular limitation as long as the material is dissolved or dispersed in the liquid medium used in the production of the electrode. Specific examples include resin-based polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, aromatic polyamide, cellulose, and nitrocellulose; rubber-like polymers such as SBR (styrene-butadiene rubber), NBR (acrylonitrile-butadiene rubber), fluororubber, isoprene rubber, butadiene rubber, and ethylene-propylene rubber; styrene-butadiene-styrene block copolymers or hydrogenated products thereof, EPDM (ethylene-propylene- Examples of suitable materials include thermoplastic elastomer-like polymers such as styrene-ethylene-butadiene-ethylene copolymers, styrene-isoprene-styrene block copolymers, and hydrogenated products thereof; soft resin-like polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, and propylene-α-olefin copolymers; fluorine-based polymers such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene, and tetrafluoroethylene-ethylene copolymers; and polymer compositions having ionic conductivity for alkali metal ions (especially lithium ions). These substances may be used alone or in any combination and ratio of two or more.

[0092] The content of the binder in the positive electrode active material layer is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and also preferably 80% by mass or less, more preferably 60% by mass or less, even more preferably 40% by mass or less, and particularly preferably 10% by mass or less. When the proportion of the binder is within the above range, the positive electrode active material can be sufficiently held, and the mechanical strength of the positive electrode can be secured, so that the battery performance such as cycle characteristics is improved. Furthermore, it also leads to avoiding a decrease in battery capacity and conductivity.

[0093] <Liquid medium> The liquid medium used in preparing the slurry for forming the positive electrode active material layer is not particularly limited in type, and either an aqueous solvent or an organic solvent may be used, so long as it is a solvent capable of dissolving or dispersing the positive electrode active material, the conductive material, the binder, and the thickener used as needed. Examples of aqueous media include water, and mixtures of alcohol and water. Examples of organic media include aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; and aprotic polar solvents such as hexamethylphosphatamide and dimethylsulfoxide. These may be used alone or in any combination and ratio of two or more.

[0094] <Thickener> When using an aqueous medium as the liquid medium for forming the slurry, it is preferable to use a thickener and a latex such as styrene-butadiene rubber (SBR) to make the slurry. The thickener is usually used to adjust the viscosity of the slurry. There are no limitations on the thickener as long as it does not significantly limit the effects of the present invention, and specific examples include carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, ethylcellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof, etc. These may be used alone or in any combination and ratio of two or more.

[0095] When a thickener is used, the ratio of the thickener to the positive electrode active material is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 0.6% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less. When the ratio of the thickener to the positive electrode active material is within the above range, the coating property of the slurry is good, and furthermore, the ratio of the active material in the positive electrode active material layer is sufficient, so that the problem of the battery capacity decreasing and the problem of the resistance between the positive electrode active materials increasing can be easily avoided.

[0096] <Consolidation> The positive electrode active material layer obtained by applying the above slurry to the current collector and drying it is preferably compacted by a hand press, roller press, or the like in order to increase the packing density of the positive electrode active material. The density of the positive electrode active material layer is 1 g cm -3 More than 1.5g cm is preferable. -3 More than 2g cm is preferable. -3 More than 4g cm is more preferable. -3 Less than 3.5 g cm is preferable. -3 Less than 3 g cm is preferable. -3 The following is even more preferred: When the density of the positive electrode active material layer is within the above range, the permeability of the non-aqueous electrolyte solution to the vicinity of the current collector / active material interface is not reduced, and the charge / discharge characteristics are good, particularly at high current densities. Furthermore, the conductivity between the active materials is less likely to decrease, and the battery resistance is less likely to increase.

[0097] <Current collector> The material of the positive electrode current collector is not particularly limited, and any known material can be used. Specific examples include metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; carbon-based materials such as carbon cloth and carbon paper; and the like. Among them, metal materials, especially aluminum, are preferred.

[0098] The shape of the current collector may be, for example, a metal foil, a metal cylinder, a metal coil, a metal plate, a metal thin film, an expanded metal, a punched metal, or a foamed metal, for example, when it is a metal material, or a carbon plate, a carbon thin film, or a carbon cylinder, for example. Of these, a metal thin film is preferred. The thin film may be formed into a mesh shape as appropriate. The thickness of the current collector is arbitrary, but is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, and is preferably 1 mm or less, more preferably 100 μm or less, even more preferably 50 μm or less. When the thickness of the current collector is within the above range, the strength required as a current collector can be sufficiently ensured. Furthermore, the handling property is also good.

[0099] The thickness ratio between the current collector and the positive electrode active material layer is not particularly limited, but (thickness of the active material layer on one side immediately before the injection of the nonaqueous electrolyte solution) / (thickness of the current collector) is preferably 150 or less, more preferably 20 or less, and particularly preferably 10 or less, and is also preferably 0.1 or more, more preferably 0.4 or more, and particularly preferably 1 or more. When the thickness ratio of the current collector to the positive electrode active material layer is within the above range, the current collector is less likely to generate heat due to Joule heat during high current density charge / discharge, and the volume ratio of the current collector to the positive electrode active material is less likely to increase, preventing a decrease in battery capacity.

[0100] <Electrode area> From the viewpoint of increasing the stability at high output and high temperature, the area of ​​the positive electrode active material layer is preferably made larger than the outer surface area of ​​the battery outer case. Specifically, the sum of the electrode areas of the positive electrodes relative to the surface area of ​​the outer case of the nonaqueous electrolyte battery is preferably 20 times or more in area ratio, and more preferably 40 times or more. In the case of a bottomed rectangular shape, the outer surface area of ​​the outer case refers to the total area calculated from the length, width, and thickness dimensions of the case part filled with the power generating element excluding the protruding part of the terminal. In the case of a bottomed cylindrical shape, it is the geometric surface area of ​​the case part filled with the power generating element excluding the protruding part of the terminal as a cylinder. The sum of the electrode areas of the positive electrodes refers to the geometric surface area of ​​the positive electrode composite layer facing the composite layer containing the negative electrode active material, and in a structure in which a positive electrode composite layer is formed on both sides via a collector foil, it refers to the sum of the areas calculated separately for each side.

[0101] <Discharge capacity> When the non-aqueous electrolyte is used, the electric capacity of the battery element housed in one battery exterior of the non-aqueous electrolyte battery (electric capacity when the battery is discharged from a fully charged state to a discharged state) is preferably 1 ampere hour (Ah) or more, since this increases the effect of improving low-temperature discharge characteristics. Therefore, the positive electrode (also called the "positive electrode plate") is designed so that the discharge capacity at full charge is preferably 3 Ah (ampere hour) or more, more preferably 4 Ah or more, and also preferably 100 Ah or less, more preferably 70 Ah or less, and particularly preferably 50 Ah or less.

[0102] Within the above range, the voltage drop due to electrode reaction resistance during drawing of a large current is not too large, and deterioration of power efficiency can be prevented. Furthermore, the temperature distribution due to heat generation inside the battery during pulse charging and discharging is not too large, and the durability of the battery during repeated charging and discharging is deteriorated, and the heat dissipation efficiency is also deteriorated against sudden heat generation during abnormality such as overcharging or internal short circuit.

[0103] <Positive electrode plate thickness> The thickness of the positive electrode plate is not particularly limited, but from the viewpoint of high capacity, high output, and high rate characteristics, the thickness of the positive electrode active material layer obtained by subtracting the thickness of the current collector from the thickness of the positive electrode plate is preferably 10 μm or more, more preferably 20 μm or more, and is preferably 200 μm or less, more preferably 100 μm or less, on one side of the current collector.

[0104] <2-4. Negative electrode> In one embodiment of the present invention, the negative electrode has a current collector and a negative electrode active material layer provided on the current collector. The negative electrode used in the nonaqueous electrolyte secondary battery of this embodiment will be described in detail below.

[0105] <2-4-1. Negative electrode active material> The negative electrode active material used in the negative electrode will be described below. The negative electrode active material includes a carbon-based material capable of electrochemically absorbing and releasing metal ions. The negative electrode active material may be used alone or in any combination of two or more.

[0106] <Carbon-based materials> Examples of the carbon-based materials include (1) natural graphite, (2) artificial graphite, (3) amorphous carbon, (4) carbon-coated graphite, (5) graphite-coated graphite, and (6) resin-coated graphite.

[0107] (1) Examples of natural graphite include scaly graphite, scaly graphite, soil graphite, and / or graphite particles obtained by subjecting these graphites to treatments such as spheroidization and densification. Among these, from the viewpoints of particle packing and charge / discharge rate characteristics, spherical or ellipsoidal graphite that has been subjected to a spheroidization treatment is particularly preferred.

[0108] The spheronization treatment can be carried out using a device that repeatedly applies mechanical actions to particles, such as compression, friction, shear force, and particle interactions, mainly impact force.

[0109] Specifically, a device having a rotor with many blades installed inside a casing, which rotates at high speed to apply mechanical actions such as impact compression, friction, shear force, etc. to the raw material natural graphite (1) introduced inside, thereby carrying out spheroidization is preferred. Also, a device having a mechanism for repeatedly applying mechanical actions by circulating the raw material is preferred.

[0110] For example, when the spheronization treatment is performed using the above-mentioned device, the peripheral speed of the rotating rotor is preferably set to 30 to 100 m / sec, more preferably 40 to 100 m / sec, and even more preferably 50 to 100 m / sec. Although the spheronization treatment can be performed by simply passing the raw material through the device, it is preferable to circulate or retain the raw material in the device for 30 seconds or more, and more preferably to circulate or retain the raw material in the device for 1 minute or more.

[0111] (2) Examples of artificial graphite include those produced by graphitizing organic compounds such as coal tar pitch, coal-based heavy oil, atmospheric residual oil, petroleum-based heavy oil, aromatic hydrocarbons, nitrogen-containing cyclic compounds, sulfur-containing cyclic compounds, polyphenylene, polyvinyl chloride, polyvinyl alcohol, polyacrylonitrile, polyvinyl butyral, natural polymers, polyphenylene silicide, polyphenylene oxide, furfuryl alcohol resin, phenol-formaldehyde resin, and imide resin at a temperature usually in the range of 2500°C or higher and usually 3200°C or lower, and then pulverizing and / or classifying as necessary.

[0112] In this case, a silicon-containing compound or a boron-containing compound may be used as a graphitization catalyst. Further, there is mentioned artificial graphite obtained by graphitizing mesocarbon microbeads separated during the heat treatment of pitch. Further, there is mentioned artificial graphite in the form of granulated particles consisting of primary particles. For example, there are mentioned mesocarbon microbeads and graphite particles obtained by mixing graphitizable carbonaceous material powder such as coke with a graphitizable binder such as tar or pitch and a graphitization catalyst, graphitizing the mixture, and pulverizing the mixture as necessary, in which a plurality of flat particles are aggregated or bonded together so that the oriented planes are non-parallel.

[0113] (3) Examples of amorphous carbon include amorphous carbon particles obtained by using graphitizable carbon precursors such as tar and pitch as raw materials and heat-treating them at least once in a temperature range in which graphitization does not occur (400 to 2200°C), and amorphous carbon particles obtained by using non-graphitizable carbon precursors such as resin as raw materials and heat-treating them.

[0114] (4) Carbon-coated graphite can be obtained as follows. Natural graphite and / or artificial graphite are mixed with a carbon precursor, which is an organic compound such as tar, pitch, or resin, and the mixture is heat-treated at least once in the range of 400 to 2300°C. The obtained natural graphite and / or artificial graphite is used as core graphite, which is then coated with amorphous carbon to obtain a carbon-graphite composite. This carbon-graphite composite can be referred to as carbon-coated graphite (4).

[0115] The composite may be in the form of a core graphite whose surface is entirely or partially covered with amorphous carbon, or a plurality of primary particles may be composited with carbon originating from the carbon precursor as a binder. The carbon-graphite composite may also be obtained by reacting natural graphite and / or artificial graphite with a hydrocarbon gas such as benzene, toluene, methane, propane, or aromatic volatile matter at high temperature to deposit carbon on the graphite surface (CVD).

[0116] (5) Graphite-coated graphite can be obtained as follows: Natural graphite and / or artificial graphite are mixed with a carbon precursor of an easily graphitizable organic compound such as tar, pitch, or resin, and the mixture is heat-treated at least once in the range of about 2400 to 3200° C. The obtained natural graphite and / or artificial graphite is used as core graphite, and the entire or part of the surface of the core graphite is coated with a graphitized material to obtain graphite-coated graphite (5).

[0117] (6) Resin-coated graphite can be obtained, for example, by mixing natural graphite and / or artificial graphite with a resin or the like, drying the mixture at a temperature of less than 400°C to obtain natural graphite and / or artificial graphite as core graphite, and then coating the core graphite with a resin or the like.

[0118] In addition, the carbon-based materials (1) to (6) described above may be used alone or in combination of two or more in any combination and ratio.

[0119] Examples of the organic compounds such as tar, pitch, and resin used in the carbon-based materials (2) to (5) above include carbonizable organic compounds selected from the group consisting of coal-based heavy oil, straight-run heavy oil, cracked petroleum heavy oil, aromatic hydrocarbons, N-ring compounds, S-ring compounds, polyphenylene, organic synthetic polymers, natural polymers, thermoplastic resins, and thermosetting resins. Further, the raw material organic compound may be dissolved in a low-molecular organic solvent for adjusting the viscosity during mixing.

[0120] In addition, as the natural graphite and / or artificial graphite used as the raw material of the nuclear graphite, spherical natural graphite subjected to spheroidization treatment is preferable.

[0121] <Negative electrode active material containing metal particles alloyable with Li and graphite particles> The negative electrode active material may contain metal particles alloyable with Li and graphite particles. In this specification, as is clear from the specifically exemplified materials, "metal particles alloyable with Li" means "particles containing a metal element and / or a metalloid element alloyable with Li". The negative electrode active material containing metal particles alloyable with Li and graphite particles may be a mixture in which the metal particles alloyable with Li and the graphite particles are mixed in a state of being independent particles of each other, or a composite in which the metal particles alloyable with Li are present on the surface and / or inside of the graphite particles.

[0122] The composite of metal particles capable of alloying with Li and graphite particles (also referred to as composite particles) is not particularly limited as long as it contains metal particles capable of alloying with Li and graphite particles. Preferably, it is a particle in which metal particles capable of alloying with Li and graphite particles are integrated by physical and / or chemical bonds. A more preferable form is that the metal particles capable of alloying with Li and the graphite particles are in a state where each solid component is dispersed in the particle to such an extent that they exist in at least both the surface and the bulk interior of the composite particle, and in a form where graphite particles are present in order to integrate them by physical and / or chemical bonds. A more specific preferable form is a composite material composed of at least metal particles capable of alloying with Li and graphite particles, and a composite material (negative electrode active material) characterized in that metal particles capable of alloying with Li are present in the gaps within the structure of particles having a folded structure with a curved surface, preferably natural graphite. The gaps may be voids, or substances such as amorphous carbon, graphite-like substances, or resins that buffer the expansion and contraction of metal particles capable of alloying with Li may be present in the gaps.

[0123] (Content ratio of metal particles capable of alloying with Li) The content ratio of metal particles capable of alloying with Li to the total of metal particles capable of alloying with Li and graphite particles is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1.0% by mass or more, still more preferably 2.0% by mass or more. Also, it is usually 99% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less, still more preferably 30% by mass or less, even more preferably 25% by mass or less, even more preferably 20% by mass or less, particularly preferably 15% by mass or less, and most preferably 10% by mass or less. Being within this range is preferable in that it enables control of side reactions on the Si surface and makes it possible to obtain sufficient capacity in a non-aqueous electrolyte battery.

[0124] <Metal particles capable of alloying with Li> The alloy-based material is not particularly limited, and may be any of lithium element, elemental metals and alloys that form lithium alloys, or compounds such as oxides, carbides, nitrides, silicides, sulfides, and phosphides thereof, so long as it is capable of absorbing and releasing lithium ions. The elemental metals and alloys that form lithium alloys are preferably materials that contain metal / metalloid elements of Groups 13 and 14 (i.e., excluding carbon), more preferably elemental metals such as aluminum, silicon, and tin, and alloys or compounds containing these atoms, and even more preferably those having silicon or tin as a constituent element, such as elemental metals such as silicon and tin, and alloys or compounds containing these atoms. These may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0125] When a lithium alloy-forming elemental metal and alloy, or a compound such as an oxide, carbide, nitride, silicide, sulfide, or phosphide thereof is used as the negative electrode active material, the metal capable of being alloyed with Li is in a particulate form. Examples of the particulate form include block, polyhedral, spherical, elliptical, plate-like, needle-like, and columnar forms. Primary particles may be aggregated to form secondary particles, and the shape of the secondary particles may be spherical or elliptical. Methods for confirming that the metal particles are metal particles capable of being alloyed with Li include identification of the metal particle phase by X-ray diffraction, observation and elemental analysis of the particle structure by an electron microscope, and elemental analysis by fluorescent X-rays.

[0126] Any conventionally known metal particles can be used as the metal particles capable of being alloyed with Li, but from the viewpoint of the capacity and cycle life of the non-aqueous electrolyte battery, the metal particles are preferably, for example, a metal selected from the group consisting of Fe, Co, Sb, Bi, Pb, Ni, Ag, Si, Sn, Al, Zr, Cr, P, S, V, Mn, As, Nb, Mo, Cu, Zn, Ge, In, Ti and W, or a compound thereof. In addition, when the metal particles capable of being alloyed with Li contain two or more metals, the particles may be alloy particles made of an alloy of these metals. Among these, a metal selected from the group consisting of Si, Sn, As, Sb, Al, Zn and W, or a metal compound thereof, is preferred.

[0127] Examples of compounds of metals that can be alloyed with Li include metal oxides, metal nitrides, metal carbides, etc. Further, the compound may contain two or more metals that can be alloyed with Li.

[0128] Among the metal particles that can be alloyed with Li, Si or Si-containing compounds are preferred. Si or Si-containing compounds are preferred in terms of increasing the capacity of the battery. In this specification, Si or Si-containing compounds are collectively referred to as Si compounds. Specific examples of Si compounds include SiO x , SiN x , SiC x , SiZ x O y (Z = C, N), etc. As Si compounds, silicon oxides (SiO x ) are preferred in that they have a larger theoretical capacity compared to graphite, and amorphous Si or nano-sized Si crystals are preferred in that alkali ions such as lithium ions can easily enter and exit, making it possible to obtain a high capacity.

[0129] This general formula SiO x is obtained using silicon dioxide (SiO2) and metallic Si (Si) as raw materials, where x is usually 0 < x < 2, more preferably 0.2 or more and 1.8 or less, still more preferably 0.4 or more and 1.6 or less, and particularly preferably 0.6 or more and 1.4 or less. Within this range, the battery can have a high capacity while at the same time reducing the irreversible capacity due to the bond between Li and oxygen.

[0130] (Oxygen content of metal particles that can be alloyed with Li) The oxygen content of the metal particles capable of being alloyed with Li is not particularly limited, but is usually 0.01% by mass or more and 8% by mass or less, and preferably 0.05% by mass or more and 5% by mass or less. The oxygen distribution state in the particles may be present near the surface, present inside the particles, or uniformly present inside the particles, but it is particularly preferable that the oxygen content is present near the surface. When the oxygen content of the metal particles capable of being alloyed with Li is within the above range, the strong bond between the metal particles and O (oxygen atom) suppresses volume expansion accompanying secondary charging and discharging of the non-aqueous electrolyte, and the cycle characteristics are excellent, which is preferable.

[0131] <Coverage rate> In this embodiment, the negative electrode active material may be coated with a carbonaceous material or a graphite material. Among these, it is preferable to coat with an amorphous carbonaceous material from the viewpoint of lithium ion acceptance. The coating rate is usually 0.5% to 30%, preferably 1% to 25%, more preferably 2% to 20%. The upper limit of the coating rate is preferably within the above range from the viewpoint of reversible capacity when assembled into a battery, and the lower limit of the coating rate is preferably within the above range from the viewpoint of the core carbonaceous material being uniformly coated with amorphous carbon and being strongly granulated, and from the viewpoint of the particle size of the particles obtained when pulverized after firing.

[0132] The coverage (content) of the organic compound-derived carbonized material in the final negative electrode active material can be calculated by the following formula using the amount of the negative electrode active material, the amount of the organic compound, and the carbon residue rate measured by a micro method in accordance with JIS K 2270.

[0133] Formula: Coverage rate of carbon derived from organic compound (%) = (mass of organic compound × carbon remaining rate × 100) / {mass of negative electrode active material + (mass of organic compound × carbon remaining rate)}

[0134] <Internal porosity> The internal porosity of the negative electrode active material is usually 1% or more, preferably 3% or more, more preferably 5% or more, and even more preferably 7% or more. It is usually less than 50%, preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less. If the internal porosity is too small, the amount of liquid in the particles of the negative electrode active material tends to be small in a nonaqueous electrolyte battery. On the other hand, if the internal porosity is too large, the gap between particles tends to be small when the material is used as an electrode. The lower limit of the internal porosity is preferably set to the above range from the viewpoint of charge / discharge characteristics, and the upper limit is preferably set to the above range from the viewpoint of diffusion of the nonaqueous electrolyte. In addition, as described above, the gap may be a void, or a substance that buffers the expansion and contraction of metal particles that can be alloyed with Li, such as amorphous carbon, graphite, or resin, may be present in the gap or the gap may be filled with these substances.

[0135] <2-4-2. Negative electrode structure and manufacturing method> The negative electrode (hereinafter also referred to as "negative electrode plate") can be manufactured by any known method as long as it does not significantly impair the effects of the present invention. For example, the negative electrode can be formed by adding a binder, a solvent, and, if necessary, a thickener, a conductive material, a filler, etc. to the negative electrode active material to form a slurry, applying this to a current collector, drying it, and pressing it.

[0136] In addition, the negative electrode made of the alloy-based material can be manufactured by any known method. Specifically, the manufacturing method of the negative electrode includes, for example, a method of adding a binder, a conductive material, etc. to the above-mentioned negative electrode active material, and then rolling the material to form a sheet electrode, or a method of compressing the material to form a pellet electrode. Usually, a method of forming a thin film layer (negative electrode active material layer) containing the above-mentioned negative electrode active material on a current collector for the negative electrode (hereinafter sometimes referred to as "negative electrode current collector") by a coating method, a vapor deposition method, a sputtering method, a plating method, or the like is used. In this case, a binder, a thickener, a conductive material, a solvent, etc. are added to the above-mentioned negative electrode active material to form a slurry, which is applied to the negative electrode current collector, dried, and then pressed to densify, thereby forming a negative electrode active material layer on the negative electrode current collector.

[0137] Examples of the material for the negative electrode current collector include steel, copper, copper alloy, nickel, nickel alloy, stainless steel, etc. Among these, copper foil is preferred from the viewpoints of ease of processing into a thin film and cost.

[0138] The thickness of the negative electrode current collector is usually 1 μm or more, preferably 5 μm or more, and usually 100 μm or less, preferably 50 μm or less. If the thickness of the negative electrode current collector is too thick, the capacity of the entire nonaqueous electrolyte battery may be too low, and conversely, if it is too thin, handling may be difficult.

[0139] In order to improve the bonding effect with the negative electrode active material layer formed on the surface, it is preferable to roughen the surface of the negative electrode current collector in advance. Examples of the surface roughening method include blasting, rolling with a rough-surface roll, mechanical polishing in which the current collector surface is polished with an abrasive cloth with abrasive particles fixed thereto, a grindstone, an emery buff, a wire brush equipped with a steel wire, or the like, electrolytic polishing, chemical polishing, and the like.

[0140] In addition, in order to reduce the mass of the negative electrode collector and improve the energy density per unit mass of the battery, a perforated type negative electrode collector such as an expanded metal or a punched metal can be used. The mass of this type of negative electrode collector can be freely changed by changing the aperture ratio. In addition, when a negative electrode active material layer is formed on both sides of this type of negative electrode collector, the rivet effect through the holes makes it even more difficult for the negative electrode active material layer to peel off. However, if the aperture ratio is too high, the contact area between the negative electrode active material layer and the negative electrode collector becomes small, and the adhesive strength may be reduced.

[0141] The slurry for forming the negative electrode active material layer is usually prepared by adding a binder, a thickener, etc. to the negative electrode material. In this specification, the term "negative electrode material" refers to a material in which the negative electrode active material and the conductive material are combined.

[0142] The content of the negative electrode active material in the negative electrode material is usually 70% by mass or more, preferably 75% by mass or more, and usually 97% by mass or less, preferably 95% by mass or less. If the content of the negative electrode active material is too small, the capacity of the secondary battery using the obtained negative electrode tends to be insufficient, and if it is too large, the content of the conductive material is relatively insufficient, making it difficult to ensure the electrical conductivity of the negative electrode. When two or more negative electrode active materials are used in combination, the total amount of the negative electrode active materials should be set to satisfy the above range.

[0143] Examples of the conductive material used in the negative electrode include metal materials such as copper and nickel; and carbon materials such as graphite and carbon black. These may be used alone or in any combination and ratio of two or more. In particular, it is preferable to use a carbon material as the conductive material, since the carbon material also acts as an active material. The content of the conductive material in the negative electrode material is usually 3% by mass or more, preferably 5% by mass or more, and usually 30% by mass or less, preferably 25% by mass or less. If the content of the conductive material is too small, the conductivity tends to be insufficient, and if it is too large, the content of the negative electrode active material, etc. is relatively insufficient, which tends to reduce the battery capacity and strength. When two or more conductive materials are used in combination, the total amount of the conductive materials should be set to satisfy the above range.

[0144] Any binder can be used for the negative electrode as long as it is safe against the solvent and electrolyte used in the manufacture of the electrode. Examples include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, styrene-butadiene rubber-isoprene rubber, butadiene rubber, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, etc. These may be used alone or in any combination and ratio of two or more. The content of the binder is usually 0.5 parts by mass or more, preferably 1 part by mass or more, and usually 10 parts by mass or less, preferably 8 parts by mass or less, per 100 parts by mass of the negative electrode material. If the content of the binder is too small, the strength of the resulting negative electrode tends to be insufficient, and if it is too large, the content of the negative electrode active material, etc. will be relatively insufficient, which will result in insufficient battery capacity and conductivity. When two or more binders are used in combination, the total amount of the binders should be set to satisfy the above range.

[0145] Examples of thickeners used in the negative electrode include carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, ethylcellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, etc. These may be used alone or in any combination and ratio of two or more. A thickener may be used as needed, but when used, it is preferable that the content of the thickener in the negative electrode active material layer is usually in the range of 0.5 mass% or more and 5 mass% or less.

[0146] The slurry for forming the negative electrode active material layer is prepared by mixing the negative electrode active material with a conductive material, a binder, and a thickener as necessary, and using an aqueous solvent or an organic solvent as a dispersion medium. As the aqueous solvent, water is usually used, but it is also possible to use an organic solvent such as alcohols such as ethanol and cyclic amides such as N-methylpyrrolidone in a range of 30 mass % or less based on water. In addition, examples of the organic solvent include cyclic amides such as N-methylpyrrolidone, linear amides such as N,N-dimethylformamide and N,N-dimethylacetamide, aromatic hydrocarbons such as anisole, toluene, and xylene, and alcohols such as butanol and cyclohexanol. Among them, cyclic amides such as N-methylpyrrolidone, linear amides such as N,N-dimethylformamide and N,N-dimethylacetamide are preferred. These may be used alone or in any combination of two or more in any ratio.

[0147] The obtained slurry is applied onto the above-mentioned negative electrode current collector, dried, and then pressed to form a negative electrode active material layer, thereby obtaining a negative electrode. The application method is not particularly limited, and a method known per se can be used. The drying method is also not particularly limited, and a known method such as natural drying, heat drying, and reduced pressure drying can be used.

[0148] <Electrode density> There are no particular restrictions on the structure of the electrode when the negative electrode active material is made into an electrode, but the density of the negative electrode active material layer on the current collector must be less than 1 g cm -3 More than 1.2g cm is preferable. -3 More preferably, 1.3 g cm -3 More than 2.2 g cm is particularly preferable. -3 Less than 2.1 g cm is preferable. -3 Less than 2.0 g cm is preferable. -3 Less than 1.9 g cm is more preferable. -3The following is particularly preferred. If the density of the negative electrode active material layer present on the current collector exceeds the above range, the negative electrode active material particles are destroyed, which may lead to an increase in the initial irreversible capacity of the non-aqueous electrolyte battery and a deterioration in high current density charge / discharge characteristics due to a decrease in the permeability of the non-aqueous electrolyte near the current collector / negative electrode active material interface. If the density is below the above range, the conductivity between the negative electrode active materials decreases, the battery resistance increases, and the capacity per unit volume may decrease.

[0149] <Average operating potential> As described above, it is presumed that the effect of the present invention is achieved by a reaction that brings about a higher resistance reduction effect, starting from the nucleophile generated by the reduction of the electrolyte components on the negative electrode. Therefore, in order to sufficiently advance the reduction of the electrolyte components, the average operating potential of the negative electrode (vs. Li / Li + ) is preferably 1 V or less.

[0150] <2-5. Separator> A separator is usually interposed between the positive electrode and the negative electrode to prevent short circuiting. In this case, the non-aqueous electrolyte is usually impregnated into the separator before use.

[0151] (material) The material of the separator is not particularly limited as long as it is stable against the non-aqueous electrolyte, but preferably includes oxides such as alumina and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, sulfates such as barium sulfate and calcium sulfate, inorganic materials such as glass filters made of glass fibers, resins such as polyolefins, etc., more preferably polyolefins, and particularly preferably polyethylene or polypropylene. These materials may be used alone or in combination. The above materials may be used in a laminated form.

[0152] (Thickness) The thickness of the separator is not limited, but is usually 1 μm or more and 50 μm or less.

[0153] (form) As for the form, a thin film such as a nonwoven fabric, a woven fabric, or a microporous film is preferably used. In the thin film form, a pore size of 0.01 to 1 μm and a thickness of 5 to 50 μm are preferably used. In addition to an independent thin film form, a separator may be used in which a composite porous layer containing inorganic particles is formed on the surface layer of a positive electrode and / or a negative electrode using a resin binder. A separator made of a microporous film or nonwoven fabric is preferable because of its excellent liquid retention.

[0154] (porosity) When using a porous material such as a porous sheet or nonwoven fabric as a separator, The porosity is not limited, but is usually 20% or more and 90% or less.

[0155] (Air permeability) The air permeability of a separator can be understood by its Gurley value. The Gurley value indicates the difficulty of air passing through in the thickness direction of the film, and is expressed as the number of seconds required for 100 mL of air to pass through the film. The Gurley value of a separator is arbitrary, but is usually 10 to 1000 seconds / 100 mL.

[0156] <2-6.Battery design> [Electrode group] The electrode group may be either a laminated structure of the positive electrode plate and the negative electrode plate with the separator interposed therebetween, or a structure in which the positive electrode plate and the negative electrode plate are spirally wound with the separator interposed therebetween. The ratio of the volume of the electrode group to the internal volume of the battery (hereinafter referred to as the electrode group occupancy rate) is usually 40% or more, preferably 50% or more, and usually 90% or less, preferably 80% or less. The lower limit of the electrode group occupancy rate is preferably set to the above range from the viewpoint of the battery capacity. Also, the upper limit of the electrode group occupancy rate is preferably set to the above range in order to secure a gap space from the viewpoint of various characteristics such as the charge / discharge repeatability and high-temperature storage as a battery, and from the viewpoint of avoiding the operation of a gas release valve that releases internal pressure to the outside. If the gap space is too small, the battery will become hot, causing the components to expand or the vapor pressure of the electrolyte liquid components to increase, resulting in an increase in internal pressure. This will degrade the battery's characteristics such as repeated charge / discharge performance and high-temperature storage performance, and may even cause the gas release valve, which releases internal pressure to the outside, to operate.

[0157] [Current collection structure] Although the current collecting structure is not particularly limited, in order to more effectively realize the improvement of the discharge characteristics by the non-aqueous electrolyte, it is preferable to adopt a structure that reduces the resistance of the wiring parts and the joint parts. When the internal resistance is reduced in this way, the effect of using the non-aqueous electrolyte is particularly well exhibited.

[0158] In the case where the electrode group has the aforementioned laminated structure, a structure formed by bundling the metal core parts of each electrode layer and welding them to a terminal is preferably used. When the area of ​​one electrode becomes large, the internal resistance increases, so it is also preferably used to reduce the resistance by providing multiple terminals in the electrode. In the case where the electrode group has the aforementioned wound structure, the internal resistance can be reduced by providing multiple lead structures on each of the positive electrode and the negative electrode and bundling them to a terminal.

[0159] [Protection element] Examples of protective elements include a PTC (Positive Temperature Coefficient) element whose resistance increases with heat generation due to excessive current, etc., a temperature fuse, a thermistor, a valve (current cutoff valve) that cuts off the current flowing through the circuit due to a sudden increase in the battery's internal pressure or temperature during abnormal heat generation, etc. It is preferable to select a protective element that will not operate under normal use at high current, and from the viewpoint of high output, it is more preferable to design the battery so that abnormal heat generation or thermal runaway does not occur even without a protective element.

[0160] [Exterior body] The nonaqueous electrolyte battery of this embodiment is usually configured by housing the above-mentioned nonaqueous electrolyte, negative electrode, positive electrode, separator, etc. in an exterior body (exterior case). There are no limitations on this exterior body, and any known exterior body can be used as long as it does not significantly impair the effects of the present invention.

[0161] The material of the outer case is not particularly limited as long as it is a substance that is stable against the non-aqueous electrolyte used. Specifically, metals such as nickel-plated steel plate, stainless steel, aluminum or aluminum alloy, magnesium alloy, nickel, titanium, etc., or a combination of resin and aluminum are suitable. A laminate film with a foil is preferably used.

[0162] The exterior case using the above metals includes a sealed and sealed structure formed by welding the metals together by laser welding, resistance welding, or ultrasonic welding, or a crimped structure formed by using the above metals via a resin gasket. The exterior case using the above laminate film includes a sealed and sealed structure formed by heat fusing the resin layers together. In order to improve the sealing property, a resin different from the resin used in the laminate film may be interposed between the resin layers. In particular, when the resin layer is heat-sealed via the current collecting terminal to form a sealed structure, the joining between the metal and the resin is performed, so that a resin having a polar group or a modified resin into which a polar group has been introduced is preferably used as the interposed resin.

[0163] The shape of the exterior body may also be arbitrary, and may be, for example, cylindrical, rectangular, laminated, coin-shaped, large, or the like. EXAMPLES

[0164] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples as long as the gist of the present invention is not exceeded.

[0165] The compounds used in the present examples and comparative examples are shown below.

[0166] [ka]

[0167] [ka]

[0168] [ka]

[0169] [ka]

[0170] [ka]

[0171] [ka]

[0172] [ka]

[0173] [ka]

[0174] [ka]

[0175] [ka]

[0176] [ka]

[0177] [ka]

[0178] [ka]

[0179] <Examples 1 to 7 and Comparative Examples 10 to 13> [Preparation of positive electrode] The positive electrode active material was lithium nickel cobalt manganese composite oxide (Li 1.0 Ni 0.5 Co 0.2 Mn 0.3 90 parts by mass of O2), 7 parts by mass of acetylene black as a conductive material, and 3 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in N-methylpyrrolidone solvent with a disperser to form a slurry. This was evenly applied to both sides of a 15 μm thick aluminum foil, dried, and pressed to form a positive electrode.

[0180] <Comparative Examples 1 to 3> [Preparation of positive electrode] The positive electrode active material was lithium nickel cobalt manganese composite oxide (Li 1.0 Ni 1 / 3 Co 1 / 3 Mn 1 / 3Positive electrodes of Comparative Examples 1 to 3 were produced in the same manner as in Example 1, except that 90 parts by mass of O2) was used.

[0181] <Comparative Examples 4 to 6> Positive electrodes of Comparative Examples 4 to 6 were produced in the same manner as in Example 11, except that 90 parts by mass of lithium cobalt composite oxide (LiCoO2) was used as the positive electrode active material.

[0182] <Comparative Examples 7 to 9> Positive electrodes of Comparative Examples 7 to 9 were produced in the same manner as in Example 1, except that 90 parts by mass of lithium manganese composite oxide (LiMn2O4) was used as the positive electrode active material.

[0183] [Preparation of negative electrode] 98 parts by mass of natural graphite was mixed with 1 part by mass of an aqueous dispersion of sodium carboxymethylcellulose (concentration of sodium carboxymethylcellulose: 1% by mass) and 1 part by mass of an aqueous dispersion of styrene-butadiene rubber (concentration of styrene-butadiene rubber: 50% by mass) as a thickener and binder, and the mixture was mixed in a disperser to form a slurry. The obtained slurry was applied to one side of a 10 μm-thick copper foil, dried, and pressed to form a negative electrode.

[0184] [Preparation of non-aqueous electrolyte] In a dry argon atmosphere, 1.0 mol / L (12.3 mass%, as the concentration in the non-aqueous electrolyte) of LiPF6, which had been thoroughly dried, was dissolved as an electrolyte in a mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) (volume ratio EC:DMC:EMC=3:3:4) (hereinafter, this is referred to as reference electrolyte 1). Compounds 1 to 8 were added to reference electrolyte 1 so as to have the contents shown in Table 1 below, to prepare non-aqueous electrolytes of Examples 1 to 7 and Comparative Examples 1 to 13. In addition, the "content (mass%)" in the table is the content when the entire non-aqueous electrolyte is 100 mass%.

[0185] [Manufacturing non-aqueous electrolyte batteries] The above positive electrode, negative electrode, and polyethylene separator were laminated in the order of negative electrode, separator, and positive electrode to prepare a battery element. This battery element was inserted into a bag made of a laminate film of aluminum (thickness 40 μm) coated on both sides with a resin layer so that the positive and negative terminals were protruding, and the above prepared nonaqueous electrolyte was then injected into the bag and vacuum sealed to prepare a laminate type nonaqueous electrolyte battery.

[0186] <Evaluation of non-aqueous electrolyte batteries> [Initial conditioning] In a thermostatic chamber at 25°C, the battery was charged to 3.72V at a current equivalent to 0.05C, and then discharged to 2.8V at 0.2C. The battery was charged to 4.1V at 0.2C. Aging was then carried out at 60°C for 12 hours. The battery was then discharged to 2.8V at 0.2C at 25°C to stabilize the laminated battery. The battery was then charged to 4.3V at 0.2C, and then discharged to 2.8V at 0.2C for initial conditioning. [Input resistance measurement] The input resistance of the nonaqueous electrolyte battery that had been initially conditioned by the above method in a thermostatic bath at 25°C was measured as follows. The nonaqueous electrolyte battery after initial conditioning was charged to 3.72 V at 0.2 C. It was charged at 25 mA, 50 mA, and 100 mA at 25°C, and the voltage was measured after 10 seconds. The input resistance value (Ω) was calculated from the slope of the obtained current-voltage line.

[0187] [Table 1]

[0188] From Table 1, it can be seen that the nonaqueous electrolyte secondary batteries having a nonaqueous electrolyte solution containing a specific aromatic isocyanate compound and a positive electrode having a transition metal oxide containing at least Ni and Co as transition metals, with 40 mol % or more of the transition metals being Ni, as in Examples 1 to 7, had a significantly reduced input resistance compared to Comparative Examples 1 to 9 (nonaqueous electrolyte secondary batteries having a nonaqueous electrolyte solution containing a specific aromatic isocyanate compound but a positive electrode not containing the specific transition metal oxide) and Comparative Examples 10 to 13 (nonaqueous electrolyte secondary batteries having a positive electrode containing a specific transition metal oxide but not the specific aromatic isocyanate compound and a nonaqueous electrolyte containing a diisocyanate).

[0189] <Examples 8 to 15> A battery was prepared in the same manner as in Example 2, except that in Example 2, Compounds 9 to 13 were further added to the non-aqueous electrolyte solution as shown in Table 2, and the input resistance value and the initial charge-discharge efficiency described below were measured. The results are shown in Table 2.

[0190] [Measurement of initial charge / discharge efficiency] In the above initial conditioning, (initial discharge capacity) / (initial charge capacity) x 1 The initial charge / discharge efficiency (%) was calculated from 00.

[0191] <Examples 16 to 17> A battery was prepared in the same manner as in Example 5, except that in Example 5, Compound 9 or 13 was further added to the nonaqueous electrolyte solution as shown in Table 2, and the input resistance value and the initial charge / discharge efficiency were measured as described above. The results are shown in Table 2.

[0192] [Table 2]

[0193] From Table 2, it can be seen that, as in Examples 8 to 17, a nonaqueous electrolyte secondary battery having a positive electrode containing a nonaqueous electrolyte containing at least one of a compound having a PF bond and a compound having an SO structure in addition to a specific aromatic isocyanate compound, and a transition metal oxide containing at least Ni and Co as transition metals, with 40 mol % or more of the transition metals being Ni, not only significantly reduces the input resistance but also improves the initial charge / discharge efficiency. [Industrial Applicability]

[0194] The nonaqueous electrolyte according to the present invention is useful because it can reduce the input resistance of a nonaqueous electrolyte secondary battery and improve the deterioration of high-capacity batteries. In addition, the nonaqueous electrolyte according to the present invention and the nonaqueous electrolyte secondary battery using the same can be used in various known applications for which nonaqueous electrolyte secondary batteries are used.Specific examples include notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, mobile fax machines, mobile copiers, mobile printers, headphone stereos, video movie machines, liquid crystal televisions, handheld cleaners, portable CDs, minidiscs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, motorcycles, motorized bicycles, bicycles, lighting equipment, toys, game equipment, watches, power tools, strobes, cameras, home backup power sources, business backup power sources, load leveling power sources, and natural energy storage power sources.

Claims

1. A non-aqueous electrolyte for use in a non-aqueous electrolyte secondary battery comprising: a positive electrode containing a transition metal oxide capable of absorbing and releasing metal ions, the transition metal oxide containing at least Ni and Co, with 40 mol % or more of the transition metal being Ni; a negative electrode containing a carbon-based material capable of absorbing and releasing metal ions; and a non-aqueous electrolyte containing a non-aqueous solvent and an electrolyte dissolved in the non-aqueous solvent, A non-aqueous electrolyte solution comprising an isocyanate compound represented by the following general formula (1): [Formula 1] (In formula (1), m and n are integers satisfying m+n=6, and n is 2. X represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom and may be the same or different from each other. Y represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 10 carbon atoms which may have a heteroatom.) 2. The nonaqueous electrolyte solution according to claim 1, wherein in formula (1), X is a methylene group or a dimethylmethylene group.

3. A non-aqueous electrolyte secondary battery comprising: a positive electrode containing a transition metal oxide capable of absorbing and releasing metal ions, the transition metal oxide containing at least Ni and Co, with 40 mol % or more of the transition metal being Ni; a negative electrode containing a carbon-based material capable of absorbing and releasing metal ions; and a non-aqueous electrolyte solution containing a non-aqueous solvent and an electrolyte dissolved in the non-aqueous solvent. A non-aqueous electrolyte solution, A non-aqueous electrolyte solution comprising an isocyanate compound represented by the following general formula (2): [chemical 2] (In formula (2), p, q, r, and s are integers satisfying p+q=5 and r+s=5, and s=p=1. R's may be the same or different and represent a hydrogen atom, a halogen atom, or an organic group having 1 to 10 carbon atoms which may have a heteroatom. X' represents a single bond or a divalent organic group having 1 to 10 carbon atoms which may have a heteroatom.)

4. The non-aqueous electrolyte solution contains a compound having a P—F bond and SO 2 The non-aqueous electrolyte solution according to any one of claims 1 to 3, comprising at least one compound having a structure.

5. a positive electrode capable of absorbing and releasing metal ions, a negative electrode containing a carbon-based material capable of absorbing and releasing metal ions, and a non-aqueous electrolyte solution containing a non-aqueous solvent and an electrolyte dissolved in the non-aqueous solvent; A non-aqueous electrolyte secondary battery comprising: The positive electrode contains a transition metal oxide and at least Ni and Co as transition metals, and 40 mol % or more of the transition metals is Ni; A non-aqueous electrolyte secondary battery, wherein the non-aqueous electrolyte is the non-aqueous electrolyte according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Nonaqueous electrolyte and secondary battery using the same

    JP2002008719A

  • Nonaqueous electrolyte solution battery

    JP2009054319A

  • Nonaqueous electrolyte secondary battery, and method of manufacturing the same

    JP2011014379A

  • Nonaqueous electrolyte secondary battery

    JP2011028860A

  • Negative electrode, nonaqueous electrolyte secondary battery, and its manufacturing method

    JP2011048987A