Laser sintered perovskite solar cell and its manufacturing method

Laser sintering addresses the inefficiencies of high-temperature processes in perovskite solar cell manufacturing by promoting crystal lattice connectivity and reducing environmental sensitivity, enhancing efficiency and reproducibility for large-scale production.

JP7579914B2Active Publication Date: 2024-11-08HUBEI WONDER SOLAR LLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023101041
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-13
Filing Date
2023-06-20
Publication Date
2024-11-08
Estimated Expiration
2043-06-20

AI Technical Summary

Technical Problem

The existing high-temperature sintering process for mesoscopic perovskite solar cells is energy-intensive, time-consuming, and prone to environmental instability, leading to poor reproducibility and device efficiency due to uneven heat application and material reactivity, which hinders large-scale industrial production.

Method used

A laser sintering method is employed to promote crystal lattice connectivity and remove organic components, utilizing a high-energy laser beam to sinter titanium dioxide, creating a mesoporous structure with improved crystal lattice connectivity and reducing processing time and environmental requirements.

Benefits of technology

Laser sintering significantly reduces energy consumption, shortens processing time, enhances manufacturing reproducibility, and improves device efficiency by promoting electron transport and reducing environmental sensitivity, facilitating large-area and flexible manufacturing of perovskite solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579914000002
    Figure 0007579914000002
  • Figure 0007579914000003
    Figure 0007579914000003
  • Figure 0007579914000004
    Figure 0007579914000004
Patent Text Reader

Abstract

To provide a laser-sintered perovskite solar battery and a method of manufacturing the same that embody manufacture of a large-area mesoporous film in an extremely short time, greatly reduce an energy consumption, shorten a processing time, improve manufacture efficiency, improve reproducibility of product manufacture, and reduce requirements for processing environment.SOLUTION: A manufacturing method includes the steps of: manufacturing a hole blocking layer 2 on a conductive base 1; manufacturing a mesoporous nanocrystal layer 3 on the hole blocking layer 2 and sintering the mesoporous nanocrystal layer 3 by a laser; manufacturing an insulation spacer layer 4 on the mesoporous nanocrystal layer 3; manufacturing a counter electrode layer 5 on the insulation spacer layer 4 and sintering the insulation spacer layer 4 and counter electrode layer 5; and applying a perovskite precursor solution over the counter electrode layer 5 to obtain a laser-sintered perovskite solar battery.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of solar cell manufacturing, in particular to laser sintered perovskite solar cells and methods for manufacturing the same. [Background technology]

[0002] Mesoscopic perovskite solar cells are solar cells that use perovskite-type organometal halide semiconductors as light-absorbing materials. The working principle is roughly as follows: First, sunlight penetrates the glass and conductive base thin film into the cell. Then, the perovskite active light-absorbing material absorbs photons to form excitons. Since exciton dissociation requires a certain amount of exciton dissociation energy, some excitons are excited to generate electron-hole pairs and become free carriers. The electrons are transported through the perovskite layer to the mesoporous nanocrystal layer and finally collected in the conductive base, while the holes are introduced through the perovskite material to the counter electrode layer for collection. Finally, the transport and transfer of carriers forms a voltage across the cell, generating a current in the external circuit.

[0003] At present, the manufacturing process of mesoscopic perovskite solar cells is mainly as follows: First, a hole blocking layer is sprayed onto the conductive glass, and then a mesoporous nanocrystal layer, an insulating spacer layer, and a counter electrode layer are printed on the hole blocking layer in sequence. After printing, the required mesoporous structure should be obtained in the thin film of each layer by sequential high-temperature sintering. Finally, the perovskite precursor solution is drop-coated on the surface of the counter electrode layer, and the perovskite precursor solution penetrates into the mesoporous structure of each layer inside the cell through capillary action, completing the perovskite crystallization and realizing the manufacture of the device.

[0004] In the above manufacturing process, the formation of the mesoporous structure is realized by high-temperature sintering, but the current mesoporous process of thin films has many limitations. Take the mesoporous nanocrystalline titanium dioxide layer as an example, the conventional high-temperature hot-stage sintering only removes organic components such as pore-forming agents and solvents, but does not form high-quality crystal lattice connections between titanium dioxide particles. In addition, the required mesoporous structure can only be obtained by sintering the thin film at high temperatures for a long time, which consumes a lot of energy, has low manufacturing efficiency, and requires a long process time to increase and decrease the temperature of the sintering furnace. In addition, high-temperature sintering must maintain temperature stability for a long time, so the requirements for the processing environment are relatively high. It is relatively difficult to achieve an absolute temperature stability state, and temperature fluctuations will cause uneven heat during thin film annealing, generating internal stress, which will affect the reproducibility of device manufacturing. In addition, the thin film itself is prone to reacting with moisture and oxygen in the air, and the reaction will become more intense under high temperature conditions for a long time, greatly hindering the improvement of device efficiency. These problems become more pronounced when the device area is expanded, and are issues that must be resolved urgently in order to transition mesoscopic perovskite solar cell devices to an industrial scale. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a laser sintered perovskite solar cell and a manufacturing method thereof, which promotes the melting and bonding between titanium dioxide crystal grains by a high energy laser beam, realizes better crystal lattice connection of titanium dioxide, and thus establishes an electrical interconnection structure between crystal grains to promote efficient carrier transfer, while at the same time removing organic components such as solvent and binder present in the paste by laser sintering to ensure a mesoporous structure of the thin film, thereby solving the technical problems of the existing high temperature sintering process, such as long thin film sintering time, high energy consumption, low manufacturing efficiency, high processing environment requirements, poor manufacturing reproducibility, and serious device charge recombination.

[0006] In order to solve the above technical problems, the technical solution of the present invention is as follows:

[0007] A method for producing a laser sintered perovskite solar cell, comprising the steps of: (1) forming a hole blocking layer on a conductive base; (2) preparing a mesoporous nanocrystal layer on the hole blocking layer obtained in step (1) and sintering the mesoporous nanocrystal layer with a laser; (3) preparing an insulating spacer layer on the mesoporous nanocrystalline layer obtained in step (2); (4) producing a counter-electrode layer on the insulating spacer layer obtained in step (3) and sintering the insulating spacer layer and the counter-electrode layer; (5) applying a perovskite precursor solution onto the counter electrode layer obtained in step (4) to obtain a laser sintered perovskite solar cell; Preferably, in step (2), laser sintering is performed using any one of an ultraviolet laser, an infrared laser, and a visible laser.

[0008] Preferably, in step (2), the laser wavelength of the laser sintering is 0.35 to 10.8 μm; Optionally, the laser power of the laser sintering is 0.08 to 275 W; Optionally, the laser sintering focal length is 600±40 mm; Optionally, the filling manner of the laser etched lines of the laser sintering is one of parallel same direction, parallel opposite direction, arcuate connection, and cross connection; Optionally, the fill spacing of the laser sintered laser etched lines is 0.008 to 0.05 mm; Optionally, the laser sintering laser output power percentage is 25-75%; Optionally, the laser frequency of the laser sintering is 10 to 85 kHz; Optionally, the laser scanning speed of the laser sintering is 20 to 8000 mm / s; Optionally, the laser scanning number of the laser sintering is 1 to 10; Optionally, the laser scanning area of ​​the laser sintering is 0.8 to 1024 cm 2 It is.

[0009] It should be noted that the laser wavelength, laser power, focal length, laser output power percentage, filling interval, scanning speed, and laser frequency have a relatively large effect on the effect of laser sintering.

[0010] Preferably, in step (2), laser sintering is performed with a volume fraction of oxygen or ozone of 45 to 99%.

[0011] Preferably, in step (1), a hole blocking layer is formed on a conductive base by spray coating; the conductive base is one or more of a conductive glass, a metal oxide, a carbon nanomaterial, and a conductive polymer; and the hole blocking layer is one or more of titanium dioxide, aluminum oxide; Optionally, the hole blocking layer has a thickness of 1 to 50 nm.

[0012] Preferably, in step (2), preparing the mesoporous nanocrystal layer includes printing a mesoporous nanocrystal layer paste on the hole blocking layer by silk screen and drying to obtain a mesoporous nanocrystal layer; the mesoporous nanocrystalline layer paste is one or more of titanium dioxide, tin dioxide, zinc oxide, barium stannate, strontium titanate, nickel oxide; Optionally, the mesoporous nanocrystalline layer has a thickness of from 10 to 8000 nm.

[0013] Preferably, in step (3), preparing the insulating spacer layer includes printing an insulating spacer layer paste onto the mesoporous nanocrystalline layer by silkscreening and drying to obtain an insulating spacer layer; The insulating spacer layer paste is one or more of zirconium dioxide, aluminum oxide, and silicon dioxide; Optionally, the insulating spacer layer has a thickness of 1 to 100 μm.

[0014] Preferably, in step (4), preparing the counter electrode layer includes printing the counter electrode layer paste on the insulating spacer layer by silk screen and drying to obtain the counter electrode layer; The counter electrode layer paste is one or more of carbon black, graphite, carbon nanotubes, activated carbon, graphene, and graphene; Optionally, the counter electrode layer has a thickness of 1 to 100 μm; Optionally, in step (4), the insulating spacer layer and the counter electrode layer are sintered at 300-400° C. for 30-50 minutes.

[0015] The present invention further provides a laser sintered perovskite solar cell obtained by the method for producing a laser sintered perovskite solar cell.

[0016] Preferably, the laser sintered perovskite solar cell comprises, in sequence, a conductive base, a hole blocking layer, a mesoporous nanocrystal layer, an insulating spacer layer, and a counter electrode layer, and the perovskite crystals are located within the mesoporous nanocrystal layer, the insulating spacer layer, and the counter electrode layer.

[0017] The above solution of the present invention includes at least the following beneficial effects:

[0018] (1) A method for producing a laser-sintered perovskite solar cell of the present invention includes the steps of producing a hole-blocking layer on a conductive base, producing a mesoporous nanocrystal layer on the hole-blocking layer and sintering the mesoporous nanocrystal layer with a laser, producing an insulating spacer layer on the mesoporous nanocrystal layer, producing a counter-electrode layer on the insulating spacer layer and sintering the insulating spacer layer and the counter-electrode layer, and applying a perovskite precursor solution onto the counter-electrode layer to obtain a laser-sintered perovskite solar cell. The manufacturing method of the laser sintered perovskite solar cell of the present invention utilizes the instantaneous high temperature generated by the laser to promote interfacial adhesion between mesoporous nanocrystals, thereby realizing a crystal lattice connection structure between crystal particles, and at the same time removing the solvent and organic binder present in the paste, which can realize the production of a large-area mesoporous film in an extremely short time, replacing high-temperature sintering, thereby greatly reducing energy consumption, shortening the processing time, improving the preparation efficiency, improving the reproducibility of product manufacturing, reducing the processing environment requirements, better facilitating the large-area and flexible manufacturing of devices, and further promoting the industrialization of mesoscopic perovskite solar cells.

[0019] Specifically, the energy consumption required for laser excitation and generation is low, high-energy laser can be generated with relatively low energy, energy utilization is high, no warm-up or preparation time is required for laser excitation and generation and shut-off, and sufficient sintering of mesoporous film can be achieved in an extremely short time due to the instantaneous high temperature of the laser, which greatly shortens the required processing time. The laser output stability is strong and the manufacturing speed is fast, so the reproducibility of product manufacturing is guaranteed. The laser sintering method abandons the use of the traditional high-temperature hot stage, and can generate instantaneous high temperature by laser, and the manufacturing speed is fast, so the operating range of the temperature and humidity of the device manufacturing environment is increased, breaking through the solid-based limitations of perovskite solar cells, the range affected by heat is small, and the environmental requirements for processing are reduced, so it is very suitable for the application and manufacturing of flexible-based devices, and therefore the manufacturing of all low-temperature flexible devices can be realized in a breakthrough way. The concentration of the laser beam and high processing accuracy are more suitable for the processing of thin films, and laser sintering is a clean, energy-saving, time-saving, highly efficient, and non-contact method, so contact with pollutants during sintering can be avoided.

[0020] (2) In the manufacturing method of the laser-sintered perovskite solar cell of the present invention, the mesoporous nanocrystal layer is sintered by a laser, and due to the instantaneous nature of the laser, the crystal grains of the mesoporous nanocrystal layer are rapidly sintered to form an oxygen-deficient state (metallization), which increases the electron cloud density of the crystal grains and promotes carrier transport.

[0021] (3) In the method for producing laser sintered perovskite solar cells of the present invention, when the mesoporous nanocrystal layer is titanium dioxide, the titanium dioxide TiO2 crystal particles are not completely melted when the laser sweeps across a light spot, so that the TiO2 crystal particles form a solidified body (oxygen-deficient state) containing a particle core structure that is not melted (crystalline state), thereby realizing the adjustment of the energy level position of the TiO2 crystal particles. When oxygen or ozone is introduced during laser sintering, the outermost layer of the particle core structure returns to the initial crystalline state by controlling the oxygen / ozone partial pressure, thus changing the position distribution of the oxygen-deficient state of the TiO2 particle shell layer, and forming an ideal multi-layered spherical shell structure of the TiO2 crystal particles with an inner crystalline state, an intermediate oxygen-deficient state, and an outer crystalline state.

[0022] (4) In the method for producing a laser sintered perovskite solar cell of the present invention, the mesoporous nanocrystal layer is sintered by a laser, and the laser has a small transmission ability, and the laser sintering has selectivity for the sintered object, and the absorption ability of different materials for a specific wavelength laser is different, and the sintering of a specified area can be realized by adjusting parameters without affecting other parts. Therefore, the lower layer thin film is not affected during the sintering production of the upper layer, which is beneficial for the construction of a three-layer mesoporous film structure of a mesoscopic perovskite solar cell device. At the same time, the high-energy beam can realize the melt adhesion between TiO2 crystal particles (external crystalline state), which improves the electron extraction and transport ability of the mesoporous TiO2 layer, and is beneficial for the transfer of carriers. The present invention applies the method of laser point scanning control to realize the formation of a topological structure of a thin film wavy surface, which is beneficial for realizing three-dimensional interface contact between film layers, which improves the electron extraction and transmission ability of the mesoporous TiO2 layer, and thus a TiO2 thin film with high mesoporosity and high conductivity is obtained, which is beneficial for improving the device efficiency.

[0023] (5) In the method for producing a laser sintered perovskite solar cell of the present invention, the mesoporous nanocrystal layer is sintered by laser sintering, and the unique anisotropic shrinkage behavior of the semiconductor material during laser sintering can reduce the residual stress in the thin film, thus reducing the thickness of the thin film, greatly increasing the porosity of the thin film, and promoting the effective filling and adhesion of the perovskite material.

[0024] (6) In the method for producing the laser sintered perovskite solar cell of the present invention, the hole blocking layer is produced in step (1), the insulating spacer layer is sintered in step (4), and the counter electrode layer can all be sintered by laser, thereby realizing the production of flexible perovskite solar cells by low temperature and all laser sintering. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a structural schematic diagram of a laser sintered perovskite solar cell of the present invention. [Diagram 2] FIG. 2 is a locally enlarged schematic diagram of a mesoporous nanocrystal layer of a high-temperature hot-stage sintered perovskite solar cell obtained in Comparative Example 2 of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing a local enlargement of a mesoporous nanocrystal layer of the laser sintered perovskite solar cell obtained in Example 1 of the present invention. [Figure 4] FIG. 2 is a schematic diagram of a locally enlarged grain of a mesoporous nanocrystal layer of the laser sintered perovskite solar cell obtained in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, exemplary embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. It should be understood that, although exemplary embodiments of the present disclosure are shown in the drawings, the present disclosure can be embodied in various forms and should not be limited by the embodiments described herein. Rather, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.

[0027] <Example 1> The manufacturing method of the laser sintered perovskite solar cell of this embodiment includes the following steps.

[0028] (1) Take the conductive base, place it on a high-temperature hot stage and heat it to 450℃, and then spray-coat the hole-blocking layer on the conductive base. The conductive base is FTO conductive glass. The hole-blocking layer is titanium dioxide with a thickness of 1nm.

[0029] (2) preparing a mesoporous nanocrystal layer on the hole blocking layer obtained in step (1), printing a mesoporous nanocrystal layer paste on the hole blocking layer and drying to obtain a mesoporous nanocrystal layer, and then laser sintering the mesoporous nanocrystal layer with an oxygen volume fraction of 45%.

[0030] The mesoporous nanocrystal layer paste is titanium dioxide. The laser wavelength of the laser sintering is 9.2 μm. The laser power of the laser sintering is 275 W, the focal length of the laser sintering is 600±40 mm, and the filling manner of the laser etched lines of the laser sintering is parallel and reverse. The filling interval of the laser etched lines of the laser sintering is 0.008 mm, and the laser output power percentage of the laser sintering is 25%. The laser frequency of the laser sintering is 60 kHz, and the laser scanning speed of the laser sintering is 3000 mm / s. The number of laser scans of the laser sintering is 2. The laser scanning area of ​​the laser sintering is 0.8 cm 2 It is.

[0031] In addition, the laser sintering can be performed using any one of an ultraviolet laser, an infrared laser, and a visible light laser. In terms of achieving the object of the present invention, the filling method of the laser etching line of the laser sintering, the number of laser scans of the laser sintering, and the laser scan area of ​​the laser sintering are not unique, and those skilled in the art can select an appropriate implementation method according to the situation (not described again below).

[0032] (3) Printing an insulating spacer layer on the mesoporous nanocrystal layer obtained in step (2), the insulating spacer layer paste being zirconium dioxide.

[0033] (4) A counter electrode layer is printed on the insulating spacer layer obtained in step (3), dried, and then sintered at 300°C for 50 minutes to form a mesoporous structure in the insulating spacer layer and the counter electrode layer.

[0034] The counter electrode layer paste is a mixture of carbon black and graphite, and the carbon black and graphite are mixed in a mass ratio of 1:1.

[0035] (5) A perovskite precursor solution is applied onto the counter electrode layer obtained in step (4), and the perovskite precursor solution penetrates into the mesoporous nanocrystal layer having a mesoporous structure, the insulating spacer layer, and the counter electrode layer by capillary action, and grows and crystallizes, thereby obtaining a laser sintered perovskite solar cell.

[0036] The solute of the perovskite precursor solution has the following general formula: ABX 3、 The A is methylamine, the B is lead, and the X is iodine.

[0037] The laser-sintered perovskite solar cell obtained by the manufacturing method of the laser-sintered perovskite solar cell described in this embodiment includes a conductive base 1, a hole-blocking layer 2, a mesoporous nanocrystal layer 3, an insulating spacer layer 4, and a counter electrode layer 5, which are arranged in this order, as shown in FIG. 1, and the perovskite crystals are located in the mesoporous nanocrystal layer, the insulating spacer layer, and the counter electrode layer.

[0038] <Example 2> The manufacturing method of the laser sintered perovskite solar cell of this embodiment includes the following steps.

[0039] (1) Take a conductive base, place it on a high-temperature hot stage, and heat it to 450℃, and then spray-coat a hole-blocking layer on the conductive base. The conductive base is ITO conductive glass, and the hole-blocking layer is aluminum oxide.

[0040] (2) A mesoporous nanocrystal layer is prepared on the hole blocking layer obtained in step (1) by silk screen printing, and after drying, the mesoporous nanocrystal layer is laser sintered in an ozone atmosphere with a volume fraction of 99%.

[0041] The mesoporous nanocrystalline layer paste is titanium dioxide, the laser wavelength of the laser sintering is 10.8 μm, the laser power of the laser sintering is 0.08 W, the focal length of the laser sintering is 600±40 mm, the filling manner of the laser etching lines of the laser sintering is parallel and unidirectional, the filling interval of the laser etching lines of the laser sintering is 0.05 mm, the laser output power percentage of the laser sintering is 35%, the laser frequency of the laser sintering is 20 kHz, the laser scanning speed of the laser sintering is 3000 mm / s, the laser scanning number of the laser sintering is 10, and the laser scanning area of ​​the laser sintering is 1024 cm 2 It is.

[0042] The laser sintering can be performed using any one of an ultraviolet laser, an infrared laser, and a visible light laser.

[0043] (3) preparing an insulating spacer layer on the mesoporous nanocrystal layer obtained in step (2) by silk screen printing and drying, the insulating spacer layer paste being aluminum oxide;

[0044] (4) Preparing a counter electrode layer on the insulating spacer layer obtained in step (3) by silk screen printing, drying it, and then sintering it at 400°C for 30 minutes to form a mesoporous structure in the insulating spacer layer and the counter electrode layer.

[0045] The counter electrode layer paste is a mixture of activated carbon and graphite, with the carbon black and graphite being mixed in a mass ratio of 2:1.

[0046] (5) A perovskite precursor solution is applied onto the counter electrode layer obtained in step (4), and the perovskite precursor solution penetrates into the mesoporous nanocrystal layer having a mesoporous structure, the insulating spacer layer, and the counter electrode layer by capillary action, and grows and crystallizes, thereby obtaining a laser sintered perovskite solar cell.

[0047] The solute of the perovskite precursor solution has the following general formula: ABX 3、 The A is formamidine, the B is lead, and the X is iodine.

[0048] <Example 3> The manufacturing method of the laser sintered perovskite solar cell of this embodiment includes the following steps.

[0049] (1) Take the conductive base, place it on a high-temperature hot stage, and heat it to 450℃, and then spray-coat the hole-blocking layer on the conductive base. The conductive base is FTO conductive glass, and the hole-blocking layer is titanium dioxide.

[0050] (2) A mesoporous nanocrystal layer is produced on the hole blocking layer obtained in step (1) by silk screen printing, and after drying, the mesoporous nanocrystal layer is laser sintered in an oxygen volume fraction of 72%.

[0051] The mesoporous nanocrystalline layer paste is zinc oxide, the laser wavelength of the laser sintering is 0.35 μm, the laser power of the laser sintering is 142 W, the focal length of the laser sintering is 600±40 mm, the filling manner of the laser etched lines of the laser sintering is arcuate connection, the filling interval of the laser etched lines of the laser sintering is 0.03 mm, the laser output power percentage of the laser sintering is 45%, the laser frequency of the laser sintering is 50 kHz, the laser scanning speed of the laser sintering is 4000 mm / s, the laser scanning number of the laser sintering is 5, and the laser scanning area of ​​the laser sintering is 512 cm 2 It is.

[0052] The laser sintering can be performed using any one of an ultraviolet laser, an infrared laser, and a visible light laser.

[0053] (3) preparing an insulating spacer layer on the mesoporous nanocrystal layer obtained in step (2) by silk screen printing and drying, the insulating spacer layer paste is silicon dioxide.

[0054] (4) Preparing a counter electrode layer on the insulating spacer layer obtained in step (3) by silk screen printing, drying it, and then sintering it at 350°C for 40 minutes to form a mesoporous structure in the insulating spacer layer and the counter electrode layer.

[0055] The counter electrode layer paste is a mixture of carbon black and graphite, where the carbon black and graphite are mixed in a mass ratio of 1:3.

[0056] (5) A perovskite precursor solution is applied onto the counter electrode layer obtained in step (4), and the perovskite precursor solution penetrates into the mesoporous nanocrystal layer having a mesoporous structure, the insulating spacer layer, and the counter electrode layer by capillary action, and grows and crystallizes, thereby obtaining a laser sintered perovskite solar cell.

[0057] The solute of the perovskite precursor solution has the general formula: ABX3, where A is cesium, B is lead, and X is chlorine.

[0058] <Example 4> The manufacturing method of the laser sintered perovskite solar cell of this embodiment includes the following steps.

[0059] (1) Take the conductive base, place it on a high-temperature hot stage, and heat it to 450℃, and then spray-coat the hole-blocking layer on the conductive base. The conductive base is FTO conductive glass, and the hole-blocking layer is titanium dioxide.

[0060] A mesoporous nanocrystal layer is prepared on the hole blocking layer obtained in step (1), and the mesoporous nanocrystal layer paste is silkscreen printed on the hole blocking layer through a 200 mesh plate and dried to obtain a mesoporous nanocrystal layer, which is then laser sintered with an oxygen volume fraction of 72%.

[0061] The mesoporous nanocrystalline layer paste is titanium dioxide, the laser wavelength of the laser sintering is 10 μm, the laser power of the laser sintering is 142 W, the focal length of the laser sintering is 600±40 mm, the filling manner of the laser etched lines of the laser sintering is arcuate connection, the filling interval of the laser etched lines of the laser sintering is 0.03 mm, the laser output power percentage of the laser sintering is 50%, the laser frequency of the laser sintering is 50 kHz, the laser scanning speed of the laser sintering is 1000 mm / s, the laser scanning number of the laser sintering is 3, and the laser scanning area of ​​the laser sintering is 1.3 cm 2 It is.

[0062] The laser sintering can be performed using any one of an ultraviolet laser, an infrared laser, and a visible light laser.

[0063] (3) preparing an insulating spacer layer on the mesoporous nanocrystal layer obtained in step (2) by silk screen printing and drying, the insulating spacer layer paste being zirconium dioxide;

[0064] (4) Preparing a counter electrode layer on the insulating spacer layer obtained in step (3) by silk screen printing, drying it, and then sintering it at 350°C for 40 minutes to form a mesoporous structure in the insulating spacer layer and the counter electrode layer.

[0065] The counter electrode layer paste is a mixture of carbon black, graphite, and activated carbon, and the carbon black, graphite, and activated carbon are mixed in a mass ratio of 1:3:1.

[0066] (5) A perovskite precursor solution is applied onto the counter electrode layer obtained in step (4), and the perovskite precursor solution penetrates into the mesoporous nanocrystal layer having a mesoporous structure, the insulating spacer layer, and the counter electrode layer by capillary action, and grows and crystallizes, thereby obtaining a laser sintered perovskite solar cell.

[0067] The perovskite precursor solution solute has the general formula: ABX3, where A is methylamine, B is lead, and X is iodine.

[0068] As shown in Fig. 3, a schematic diagram of a local enlargement of the particles of the mesoporous nanocrystal layer of the laser sintered perovskite solar cell of this example is shown. As shown in Fig. 4, a schematic diagram of a local enlargement of the particles of the mesoporous nanocrystal layer of the laser sintered perovskite solar cell obtained in this example is shown.

[0069] <Example 5> In this example, the same method as in Example 4 is used to fabricate a laser sintered perovskite solar cell, with the only difference being that in step (1), a conductive base is taken, and a hole blocking layer is fabricated on the conductive base by spray coating, and then laser sintering is performed.

[0070] The specific conditions for the laser sintering in step (1) are as follows: the laser wavelength of the laser sintering is 10 μm, the laser power of the laser sintering is 142 W, the focal length of the laser sintering is 600±40 mm, the filling manner of the laser etched lines of the laser sintering is arcuate connection, the filling interval of the laser etched lines of the laser sintering is 0.03 mm, the laser output power percentage of the laser sintering is 50%, the laser frequency of the laser sintering is 50 kHz, the laser scanning speed of the laser sintering is 1000 mm / s, the number of laser scans of the laser sintering is 3, and the laser scanning area of ​​the laser sintering is 1.3 cm 2 It is.

[0071] <Example 6> This example uses the same method as in Example 4 to fabricate laser sintered perovskite solar cells, with the only difference being that in step (4), laser sintering is applied instead of high temperature sintering to form a mesoporous structure in the insulating spacer layer and the counter electrode layer.

[0072] The specific conditions for the laser sintering in step (4) are as follows: the laser wavelength of the laser sintering is 10 μm, the laser power of the laser sintering is 142 W, the focal length of the laser sintering is 600±40 mm, the target filling manner of the laser etching line of the laser sintering is arcuate connection, the filling interval of the laser etching line of the laser sintering is 0.03 mm, the laser output power percentage of the laser sintering is 50%, the laser frequency of the laser sintering is 50 kHz, the laser scanning speed of the laser sintering is 1000 mm / s, the laser scanning number of the laser sintering is 3, and the laser scanning area of ​​the laser sintering is 1.3 cm 2 It is.

[0073] <Example 7> This example uses the same method as in Example 4 to fabricate laser sintered perovskite solar cells, with the only difference being that laser sintering is applied in both step (1) and step (4), but The laser sintering in step (1) is the same as step (1) in Example 5, and the laser sintering in step (4) is the same as step (4) in Example 6.

[0074] <Example 8> This example uses the same method as in Example 7 to fabricate laser sintered perovskite solar cells, but the only difference is that the conductive base in step (1) is applied as poly(3,4-ethylenedioxythiophene) polystyrene sulfonate material.

[0075] <Comparative Example 1> The manufacturing method of the perovskite solar cell in this comparative example is the same as that in Example 4, with the only difference being that laser sintering is not applied in step (2).

[0076] Step (2) is specifically as follows: A mesoporous nanocrystal layer is produced on the hole blocking layer obtained in step (1) by silk screen printing, and then dried.

[0077] <Comparative Example 2> The manufacturing method of the perovskite solar cell in this comparative example is the same as that in Example 4, with the only difference being that in step (2), laser sintering is not applied, but the mesoporous nanocrystal layer is sintered at high temperature.

[0078] Step (2) is specifically as follows: A mesoporous nanocrystal layer is prepared on the hole blocking layer obtained in step (1) by silk screen printing, and then dried and sintered at a high temperature of 500° C. for 45 minutes.

[0079] FIG. 2 is a schematic diagram of a local enlargement of the mesoporous nanocrystal layer of the high-temperature sintered perovskite solar cell of this comparative example. Compared with the local enlargement of FIG. 3, the titanium dioxide crystal particles in FIG. 3 are more fused, while the fusion effect of the titanium dioxide crystal particles in FIG. 2 is relatively poor. When the fusion effect of the titanium dioxide crystal particles is good, the electrical conductivity can be improved, which is favorable for charge transport. It can be seen that laser sintering can promote the interfacial adhesion between particles and achieve better electrical interconnection between the crystal particles. In addition, the good fusion effect of the titanium dioxide crystal particles also indicates that the solvent and organic binder present in the paste can be better removed during the sintering process.

[0080] <Comparative Example of Effects> In order to verify the technical effect of the manufacturing method of the laser sintered perovskite solar cell described in the present invention, the following tests are carried out.

[0081] The laser sintered perovskite solar cells produced in Examples 1 to 8 and Comparative Examples 1 and 2 were subjected to irradiation at a room temperature of 25°C and a light intensity of 100 mW / cm -2 The JV curve (current density-photovoltage curve) under AM1.5 solar radiation was simulated, and the open circuit voltage (Voc / V) and short circuit photocurrent (Jsc / mA.cm -2 ), fill factor (FF), and photoelectric conversion efficiency (η / %) are obtained.

[0082] The results of the experiment are as follows: JPEG0007579914000001.jpg67170

[0083] A comparison of Examples 1 to 4 with Comparative Examples 1 and 2 shows that the photoelectric conversion efficiency of the obtained perovskite solar cell can be significantly improved by sintering the mesoporous nanocrystal layer with a laser. A comparison of Examples 4 to 6 shows that the photoelectric conversion efficiency of the perovskite solar cell can be improved to a certain extent by applying laser sintering not only to the mesoporous nanocrystal layer but also to the hole blocking layer, the insulating spacer layer, and the counter electrode layer. A comparison of Example 8 with Comparative Examples 1 and 2 shows that it is possible to manufacture an all-laser sintered flexible perovskite solar cell.

[0084] It should be noted that the above description is a preferred embodiment of the present invention, and those skilled in the art can further make some improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be regarded as within the protection scope of the present invention. [Explanation of symbols]

[0085] 1 Conductive base 2. Hole Blocking Layer 3. Mesoporous nanocrystalline layer 4 Insulating Spacer Layer 5. Counter electrode layer

Claims

1. A method for producing a laser sintered perovskite solar cell, comprising the steps of: (1) fabricating a hole blocking layer on a conductive base; (2) preparing a mesoporous nanocrystal layer on the hole blocking layer obtained in step (1) and sintering the mesoporous nanocrystal layer with a laser; (3) preparing an insulating spacer layer on the mesoporous nanocrystalline layer obtained in step (2); (4) producing a counter-electrode layer on the insulating spacer layer obtained in step (3) and sintering the insulating spacer layer and the counter-electrode layer; (5) applying a perovskite precursor solution onto the counter electrode layer obtained in step (4) to obtain a laser sintered perovskite solar cell; In step (2), laser sintering is performed using any one of an ultraviolet laser, an infrared laser, and a visible light laser; In step (2), the laser wavelength of the laser sintering is 0.35 to 10.8 μm; The laser power of the laser sintering is 0.08 to 275 W; The focal length of the laser sintering is 600±40 mm; The filling manner of the laser sintered laser etched lines is one of parallel same direction, parallel opposite direction, arcuate connection, and cross connection; The fill spacing of the laser sintered laser etched lines is 0.008-0.05 mm; The laser output power percentage of the laser sintering is 25-75%; The laser frequency of the laser sintering is 10 to 85 kHz; The laser scanning speed of the laser sintering is 20 to 8000 mm / s, The number of laser scans in the laser sintering is 1 to 10, The laser scanning area of ​​the laser sintering is 0.8 to 1024 cm2; and in step (2), the laser sintering is performed with a volume fraction of oxygen or ozone of 45 to 99%, and the mesoporous nanocrystal layer is TiO 2 In this case, the mesoporous nanocrystalline layer can be formed by controlling the oxygen / ozone partial pressure. 2 The crystal particles form a multi-layered spherical shell structure with an inner crystalline state, an intermediate oxygen-deficient state, and an outer crystalline state. Laser sintering is used to form the topological structure of thin film wavy surface by applying the method of point scanning control. A method for producing a laser sintered perovskite solar cell, wherein the hole blocking layer, the insulating spacer layer, and the counter electrode layer are all formed by laser sintering.

2. In step (1), a hole blocking layer is formed on a conductive base by spray coating; the conductive base is one or more of a conductive glass, a metal oxide, a carbon nanomaterial, and a conductive polymer; and the hole blocking layer is one or more of titanium dioxide, aluminum oxide; The method for producing a laser sintered perovskite solar cell according to claim 1, wherein the thickness of the hole blocking layer is 1 to 50 nm.

3. In step (2), preparing a mesoporous nanocrystal layer includes printing a mesoporous nanocrystal layer paste on the hole blocking layer by silk screen and drying to obtain a mesoporous nanocrystal layer; the mesoporous nanocrystalline layer paste is one or more of titanium dioxide, tin dioxide, zinc oxide, barium stannate, strontium titanate, nickel oxide; The method for producing a laser sintered perovskite solar cell according to claim 1, wherein the thickness of the mesoporous nanocrystal layer is 100 to 8000 nm.

4. In step (3), preparing the insulating spacer layer includes printing an insulating spacer layer paste on the mesoporous nanocrystal layer by silk screen and drying to obtain an insulating spacer layer; The insulating spacer layer paste is one or more of zirconium dioxide, aluminum oxide, and silicon dioxide; The method for producing a laser sintered perovskite solar cell according to claim 1, wherein the insulating spacer layer has a thickness of 2 to 100 μm.

5. In step (4), preparing the counter electrode layer includes printing the counter electrode layer paste on the insulating spacer layer by silk screen and drying to obtain a counter electrode layer; The counter electrode layer paste is one or more of carbon black, graphite, carbon nanotubes, activated carbon, graphene, and graphene; The counter electrode layer has a thickness of 10 to 80 μm; The method for producing a laser sintered perovskite solar cell according to claim 1, wherein in step (4), the insulating spacer layer and the counter electrode layer are sintered at 300-400° C. for 30-50 minutes.

Citation Information

Patent Citations

  • Mesoscopic solar cell based on perovskite light-absorbing material and method for manufacturing the same

    JP2016523453A

  • Ferroelectric-enhanced solar cell and method of manufacturing the same

    JP2020504455A