Recording paper

A recording paper with a carboxyl group-containing resin and specific surface roughness on the base material achieves high adhesion and reduced blocking, addressing the cost and adhesion challenges of print-receiving layers.

JP7580009B2Active Publication Date: 2024-11-08株式会社ユポ
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024143299
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-31
Filing Date
2024-08-23
Publication Date
2024-11-08
Estimated Expiration
2041-11-04

AI Technical Summary

Technical Problem

Recording paper with a print-receiving layer is expensive due to the high cost of forming the layer, and achieving high adhesion to both ink and the base material while minimizing surface blocking is challenging.

Method used

A recording paper with a print-receiving layer containing a carboxyl group-containing resin with a low acid value and a base material with a specific surface roughness, combined with inorganic fillers, to enhance adhesion and reduce blocking.

Benefits of technology

The solution provides high adhesion to both ink and base material while minimizing blocking, reducing the thickness and cost of the print-receiving layer, and improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580009000003
    Figure 0007580009000003
  • Figure 0007580009000001
    Figure 0007580009000001
  • Figure 0007580009000002
    Figure 0007580009000002
Patent Text Reader

Abstract

To provide recording paper that exhibits high adhesion between a print receiving layer and an ink and a base material and that is not susceptible to blocking.SOLUTION: Recording paper has a base material and a print receiving layer on the base material. The print receiving layer contains an inorganic filler and a carboxyl group-containing resin having an acid value of 2-20 KOHmg / m2. The arithmetic mean roughness Ra of the surface of the base material on the print receiving layer side is 0.3-1.0 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a recording paper. [Background technology]

[0002] Conventionally, recording paper having a print-receiving layer containing a pigment on the surface of a substrate has been widely used. For example, the inkjet recording paper sheet disclosed in Patent Document 1 has an ink-receiving layer containing an aqueous polyester resin having an acid group. Also, the electrophotographic medium disclosed in Patent Document 2 has a toner-receiving layer containing a carboxylic acid-containing thermoplastic polymer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-247020 A [Patent Document 2] JP 2008-522241 A Summary of the Invention [Problem to be solved by the invention]

[0004] Generally, recording paper provided with a print-receiving layer is expensive. This is because it costs more to form the print-receiving layer than recording paper without a print-receiving layer. From the viewpoint of cost reduction, there is a demand for a thinner print-receiving layer. Furthermore, when the print-receiving layer is formed by a coating method, binder migration can be suppressed by making the layer thinner. Furthermore, productivity is improved by improving the drying property of the coating film, so there is a high demand for a thinner layer.

[0005] To reduce the thickness of the print-receiving layer, it is effective to use a material that has high adhesion not only to the ink but also to the substrate. However, a print-receiving layer that has high adhesion to the substrate tends to have high blocking properties on its surface, making it difficult to simultaneously improve adhesion and reduce blocking.

[0006] An object of the present invention is to provide a recording paper having a print-receiving layer that exhibits high adhesion between the ink and the substrate and that exhibits little blocking. [Means for solving the problem]

[0007] As a result of intensive research conducted by the inventors to solve the above-mentioned problems, they discovered that the above-mentioned problems can be solved by using a carboxyl group-containing resin with a very low acid value as the material for the print-receiving layer and combining it with a substrate having a surface roughness within a specific range, and thus completed the present invention. That is, the present invention is as follows.

[0008] (1) A recording paper having a print-receiving layer on a substrate, The print receiving layer comprises an inorganic filler and a polymer having an acid value of 2 to 20 KOH. mg KOH / g and a carboxyl group-containing resin, The arithmetic mean roughness Ra of the surface of the substrate on the side of the print-receiving layer is 0.3 to 1.0 μm. Recording paper.

[0009] (2) The inorganic filler contains calcium carbonate and layered silicate. The recording paper described in (1) above.

[0010] (3) The content of the carboxyl group-containing resin in the print-receiving layer is 40 to 150 parts by mass per 100 parts by mass of the inorganic filler. The recording paper described in (1) or (2) above.

[0011] (4) The print-receiving layer has a thickness of 0.2 to 10 μm. The recording paper according to any one of (1) to (3) above.

[0012] (5) The carboxyl group-containing resin is an acrylic resin. The recording paper according to any one of (1) to (4) above.

[0013] (6) The substrate is a thermoplastic resin film. The recording paper according to any one of (1) to (5) above.

[0014] (7) The thermoplastic resin film contains a filler. The recording paper described in (6) above. Effect of the Invention

[0015] According to the present invention, it is possible to provide a recording paper having high adhesion between the print-receiving layer and the ink and the base material, and having little blocking. [Brief description of the drawings]

[0016]

Figure 1

[0017] The recording paper of the present invention will be described in detail below. The following description is one example (representative example) of the present invention, and the present invention is not limited to these contents. In the following description, the term "(meth)acrylic" refers to both acrylic and methacrylic. Furthermore, the term "(co)polymer" refers to both homopolymer and copolymer.

[0018] [Recording paper] The recording paper of the present invention has a substrate and a print-receiving layer. FIG. 1 shows a recording paper 1 as a specific example. 1 has a substrate 11 and a print-receiving layer 12. The print-receiving layer 12 is laminated on one surface of the substrate 11.

[0019] In the present invention, the print-receiving layer is made of an inorganic filler and a cellulose acetate having an acid value of 2 to 20. mg KOH / gThe arithmetic mean roughness Ra of the surface of the print-receiving layer side of the substrate 11 is 0.3 to 1.0 μm. Usually, in order to improve the adhesion of the print-receiving layer to the ink, it is necessary to thicken the print-receiving layer and increase the amount of active ingredients in the layer. However, by providing a print-receiving layer containing a carboxyl group-containing resin with a very low acid value on the surface of a substrate having a surface roughness in a specific range as in the present invention, not only high adhesion to the ink but also high adhesion to the substrate can be achieved. Since it is not necessary to thicken the print-receiving layer to improve adhesion and it is possible to make it thin, the cost required for forming the print-receiving layer can be reduced and the productivity can be improved.

[0020] Generally, a print-receiving layer that has high adhesion to a substrate also has high adhesion to the substrate when other recording paper is overlaid, and is therefore prone to blocking between the print-receiving layer and the other recording paper. However, in the present invention, by disposing the print-receiving layer on the surface of a substrate having a surface roughness within a specific range, it is possible to reduce blocking that occurs when other recording paper is overlaid on the surface of the print-receiving layer. Therefore, it is possible to provide a recording paper that has high adhesion between the print-receiving layer and the ink and substrate, and is less prone to blocking. Each layer of the recording paper will now be described in detail.

[0021] (print receiving layer) The print-receiving layer has high adhesion to ink and improves the printability of the recording paper. The print-receiving layer also has high adhesion to the substrate. As described above, the print-receiving layer contains a carboxyl group-containing resin and an inorganic filler.

[0022] <Carboxy group-containing resin> The carboxyl group-containing resin not only enhances the adhesion between the print-receiving layer and the ink, but also has the function of dispersing the inorganic filler uniformly in the print-receiving layer. The carboxyl group-containing resin can improve the water resistance of the print-receiving layer by reacting with a crosslinking agent described later. The carboxyl group-containing resin can also improve the adhesion between the inorganic filler and the substrate, and therefore can also improve the water abrasion resistance of the recording paper.

[0023] <<Acid value>> Carboxylic acid-containing resin: 2~20KOH mg KOH / g The acid value is expressed as the mass (mg) of potassium hydroxide required to neutralize the acid groups contained in 1 g of resin, and is measured in accordance with JIS K0070. From the viewpoint of improving the adhesion between the print-receiving layer and the substrate, and between the print-receiving layer and the ink, the acid value of the carboxyl group-containing resin is set to 5. mg KOH / g From the viewpoint of suppressing the deterioration of the water-resistant adhesion between the print-receiving layer and the ink due to an excessively high acid value and suppressing the increase in viscosity over time of the composition for forming the print-receiving layer, the acid value is preferably 15 or more. mg KOH / g The following is preferred:

[0024] The carboxyl group-containing resin that can be used in the print-receiving layer has an acid value of 2 to 20. mg KOH / g As long as the resin is not particularly limited, preferred examples of the resin include acrylic resins, styrene resins, styrene-acrylic resins such as styrene-acrylate copolymers and styrene-methacrylate copolymers, polyurethane resins, urethane resins such as urethane-vinyl hybrid polymers, and mixtures thereof.

[0025] Among them, acrylic resins are preferred because they have good adhesion to the substrate and ink, especially to ultraviolet-curable ink. Specifically, acrylic or methacrylic acid esters are mixed with one or more ethylenically unsaturated monomers having a carboxylic acid group to give a polymer having an acid value of 2 to 20. mg KOH / g Preferably, the ratio is 5 to 15. mg KOH / g Examples of the acrylic resin include those obtained by polymerizing the resin so as to obtain the above-mentioned structure.

[0026] From the viewpoint of improving adhesion to the substrate and ink, the content of the carboxyl group-containing resin in the print-receiving layer is preferably 40 parts by mass or more, and more preferably 60 parts by mass or more, relative to 100 parts by mass of the inorganic filler in the print-receiving layer, and from the viewpoint of suppressing blocking, the content is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, and even more preferably 100 parts by mass or less, relative to 100 parts by mass of the inorganic filler.

[0027] The print-receiving layer may contain a resin other than the carboxy group-containing resin as long as the effect of the present invention is not impaired.

[0028] <Inorganic filler> Inorganic fillers improve the drying properties of the ink in the print-receiving layer. In the print-receiving layer, inorganic filler particles randomly aggregate, leaving fine voids between the particles throughout the print-receiving layer. The solvent in the ink is quickly absorbed into these voids, resulting in excellent ink drying properties. When the ink in the print-receiving layer has high drying properties, gloss ghosting is less likely to occur. In addition, backing is less likely to occur when recording paper is stacked after printing, and the drying properties of overlapping colors are also high. Furthermore, the inclusion of inorganic fillers increases the surface roughness of the print-receiving layer, and the anchor effect enhances ink receptivity.

[0029] Examples of inorganic fillers that can be used in the print-receiving layer include inorganic particles such as calcium carbonate, magnesium carbonate, layered silicate, titanium oxide, silica, boric acid, zinc borate, lead borate, sodium borate (borax), expandable graphite, glass (glass balloons), shirasu (shirasu balloons), zinc oxide, zirconium oxide, alumina, silica alumina, magnesia, zeolite, aluminum hydroxide, and magnesium hydroxide. One or more of these may be used.

[0030] Among the inorganic fillers, calcium carbonate is preferred since it is easy to improve the whiteness. Examples of calcium carbonate include heavy calcium carbonate and light calcium carbonate. Among them, light calcium carbonate is preferred from the viewpoint of forming fine pores.

[0031] The inorganic filler has an average primary particle size (D50) of preferably 0.03 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more, from the viewpoint of improving the ink drying property by forming fine pores, and preferably 2.0 μm or less, more preferably 1.0 μm or less, and even more preferably 0.5 μm or less, from the viewpoint of suppressing falling off from the print-receiving layer.

[0032] The average primary particle diameter (D50) is measured by a laser light diffraction / scattering method using, for example, a Microtrac MT3300EXII (manufactured by Microtrac Bell).

[0033] When calcium carbonate is used as the inorganic filler, it is preferable to use a layered silicate in combination, since excellent antistatic properties can be obtained even under low humidity conditions. Among layered silicates, smectite is preferable because it imparts high antistatic properties to the print-receiving layer even under low humidity environments. Smectite is a type of clay mineral, and can be represented by, for example, the structural formula [(Si 8-a Al a )(Mg 6-b Al b )·O 20 (OH)4] - M + a-b It is expressed as follows: M + Na + In most cases, a b > 0.

[0034] Examples of smectite that can be used include montmorillonite, hectorite, saponite, beidellite, and nontronite. Among them, montmorillonite is preferred from the viewpoint of antistatic properties. As for montmorillonite, bentonite, which is a clay containing montmorillonite as a main component, can be used. Smectite may be either natural smectite or synthetic smectite, but synthetic smectite, which generally has a small particle size, is preferred because it has a large number of contact points between particles and can exhibit high antistatic properties.

[0035] The average particle size of the smectite is preferably 0.01 μm or more, more preferably 0.02 μm or more, from the viewpoint of antistatic performance, and is preferably 10 μm or less, more preferably 5 μm or less, from the viewpoint of preventing the smectite from falling off from the print-receiving layer.

[0036] The content of smectite in the print-receiving layer is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, calculated as solid content, from the viewpoint of antistatic performance, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 18% by mass or less, calculated as solid content, from the viewpoint of low cost.

[0037] The content of the inorganic filler in the print-receiving layer is preferably 20% by mass or more, more preferably 30% by mass or more, from the viewpoint of pore formation and unevenness formation on the layer surface. From the viewpoint of the robustness of the print-receiving layer itself and prevention of the inorganic filler from falling off, the content is preferably 90% by mass or less, more preferably 85% by mass or less. When two or more kinds of inorganic fillers are used in combination, it is preferable that the total content of these is within the above range.

[0038] <Crosslinking agent> It is preferable that the print-receiving layer further contains a crosslinking agent, and the carboxyl group-containing resin in the print-receiving layer is crosslinked by the crosslinking agent. Crosslinking of the carboxyl group-containing resin can improve the water resistance of the print-receiving layer, and can further improve the water abrasion resistance of the printed portion of the surface of the print-receiving layer.

[0039] The crosslinking agent may be a conventionally known crosslinking agent, for example, a metal-based crosslinking agent such as ammonium zirconium carbonate, an epoxy-based crosslinking agent such as polyglycerol polyglycidyl ether, an epichlorohydrin-based crosslinking agent such as polyamide epichlorohydrin resin, polyamine epichlorohydrin resin, or epichlorohydrin adduct of polyamine polyamide, or an oxazoline-based crosslinking agent such as an oxazoline group-containing polymer.

[0040] From the viewpoint of improving the water abrasion resistance of the surface of the print-receiving layer, the print-receiving layer preferably contains one or more selected from the group consisting of the metal-based crosslinking agent, the epoxy-based crosslinking agent, the epichlorohydrin-based crosslinking agent, and the oxazoline-based crosslinking agent, and the carboxyl group-containing resin is preferably crosslinked by these crosslinking agents. Among them, the crosslinking agent is preferably one or more selected from the group consisting of the metal-based crosslinking agent and the epoxy-based crosslinking agent. In addition, from the viewpoint of improving the water-resistant adhesion of the print-receiving layer, the print-receiving layer preferably contains a metal-based crosslinking agent as a crosslinking agent, and among the metal-based crosslinking agents, ammonium zirconium carbonate is more preferable. In particular, by crosslinking the carboxyl group-containing resin with ammonium zirconium carbonate, the water abrasion resistance and water-resistant adhesion of the print-receiving layer can be further improved.

[0041] The content of the crosslinking agent in the print-receiving layer is preferably 0.8 to 12.0% by mass. Within this range, sufficient crosslinking is likely to increase water abrasion resistance. From the viewpoint of water abrasion resistance of the print-receiving layer, the content is more preferably 0.9% by mass or more, and even more preferably 1.0% by mass or more. Furthermore, from the viewpoint of adjusting the viscosity of the coating liquid for forming the print-receiving layer and obtaining good coatability, the content is more preferably 10.0% by mass or less, and even more preferably 8.0% by mass or less.

[0042] <Binder migration inhibitor> The print-receiving layer may contain isocyanate-modified polyethylene glycol to suppress binder migration, in which the carboxyl-containing resin, which is a binder component, migrates to the layer surface. By uniformly dispersing the isocyanate-modified polyethylene glycol in the print-receiving layer, even a small amount of the isocyanate-modified polyethylene glycol can sufficiently disperse the carboxyl-containing resin and suppress binder migration. The increase in viscosity of the coating liquid due to an increase in the amount of the isocyanate-modified polyethylene glycol is suppressed, and process control is also made easier.

[0043] <Surfactant> The print-receiving layer may further contain a surfactant. The surfactant can quickly attenuate the charge even if the surface of the print-receiving layer becomes charged due to friction. This can reduce transport problems such as double feeding of recording paper during printing, sticking to the printing material, paper jams, and positional deviation.

[0044] The surfactant may be any of cationic, anionic, nonionic, and amphoteric surfactants, but anionic surfactants are preferred, such as sodium dioctyl sulfosuccinate.

[0045] By incorporating a surfactant into the print-receiving layer, the frictional charge voltage on the layer surface can be attenuated, but on the other hand, the water-resistant adhesion of the layer itself tends to be reduced. In order to achieve both the frictional charge voltage attenuation of the print-receiving layer surface and the water-resistant adhesion of the print-receiving layer itself, the amount of surfactant incorporated must be kept to a minimum. Specifically, from the viewpoint of frictional charge voltage attenuation, the content of the surfactant in the print-receiving layer is preferably 0.6% by mass or more, more preferably 0.7% by mass or more. Moreover, from the viewpoint of water-resistant adhesion, the content is preferably 4.5% by mass or less, more preferably 2.3% by mass or less.

[0046] The print receiving layer may contain other additives as necessary within the range that does not impair the effects of the present invention. Examples of additives that can be used include defoamers, dispersants, thickeners, water retention agents, water resistance agents, colorants, and preservatives. For example, polycarboxylic acids can be blended as dispersants, usually in an amount of 0.05 to 5% by mass.

[0047] <Thickness> In the present invention, the print-receiving layer can be a thin film of about 0.2 to 10 μm. mg KOH / g By forming the print-receiving layer on the surface of a substrate having an arithmetic mean roughness Ra of 0.3 to 1.0 μm, the print-receiving layer contains an inorganic filler, and even when the print-receiving layer is a thin layer of 0.2 to 10 μm, it is possible to achieve good adhesion to the substrate and ink and sufficient blocking resistance. The print-receiving layer is more preferably 0.3 μm or more. In addition, since the print-receiving layer of the present invention can more effectively exhibit high adhesion to the ink and substrate, the print-receiving layer is more preferably 5 μm or less, and even more preferably 3 μm or less.

[0048] (base material) The substrate provides mechanical strength to the recording paper.

[0049] <Arithmetic mean roughness> The substrate in the present invention has an arithmetic mean roughness Ra of the surface on the print-receiving layer side in the range of 0.3 to 1.0 μm. In particular, the arithmetic mean roughness Ra is preferably 0.4 μm or more, and more preferably 0.8 μm or less. If the arithmetic mean roughness Ra is equal to or more than the above lower limit, blocking resistance can be improved. That is, when the films are stacked on top of each other or wound on a roll, adhesion between the films is suppressed. Also, if the arithmetic mean roughness Ra is equal to or less than the above upper limit, a decrease in adhesion to the print-receiving layer caused by the arithmetic mean roughness Ra being too large can be suppressed.

[0050] The arithmetic mean roughness Ra is measured in accordance with JIS-B-0601:1994. There is no particular limitation on the means for adjusting the arithmetic mean roughness Ra of the substrate surface to the specific range of the present invention. For example, the arithmetic mean roughness Ra of the substrate surface can be adjusted by providing unevenness on the surface by blending a filler described later. It can also be adjusted by surface treatments such as sandblasting, hairline treatment, matte coating, or chemical etching to provide unevenness on the surface. The matte coating is a processing method in which a coating agent containing an organic or inorganic substance is applied to the film surface to provide unevenness on the substrate surface.

[0051] In the present invention, at least the surface of the substrate on the print-receiving layer side, i.e. the surface facing the print-receiving layer, has the above-mentioned arithmetic mean roughness Ra, but both surfaces may have the above-mentioned arithmetic mean roughness Ra.

[0052] <Thermoplastic resin film> The substrate usable in the present invention is not particularly limited as long as it has a surface with an arithmetic mean roughness Ra of 0.3 to 1.0 μm, and a thermoplastic resin film or the like can be used. Generally, a thermoplastic resin film has a very smooth surface compared to pulp paper. Therefore, when a thermoplastic resin film is used as a substrate to be combined with a print-receiving layer, the present invention, which sets the surface roughness within a specific range, is particularly effective in achieving both adhesion between the substrate and the print-receiving layer and suppression of blocking.

[0053] <<Thermoplastic resin>> The thermoplastic resin used in the thermoplastic resin film is not particularly limited, and examples thereof include olefin resins, polyester resins, polyamide resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, etc. These may be used alone or in combination of two or more.

[0054] Among them, from the viewpoints of productivity, ease of processing, water resistance, chemical resistance, recyclability and cost, olefin-based resins are preferred. Examples of olefin-based resins that can be used for the substrate layer include propylene-based resins and ethylene-based resins. Among olefin-based resins, propylene-based resins are preferred from the viewpoints of moldability and mechanical strength.

[0055] Examples of propylene-based resins include propylene homopolymers exhibiting isotactic, syndiotactic or various stereoregularities, and propylene copolymers containing propylene as the main component and α-olefins such as ethylene, butene-1, hexene-1, and heptene-1,4-methylpentene-1. The "main component" monomer means a monomer that occupies 50% by mass or more of the repeating units constituting the copolymer. The copolymer may be a binary, ternary or quaternary copolymer, and may be a random or block copolymer.

[0056] From the viewpoint of improving the adhesion between the print-receiving layer and the substrate, a random copolymer of propylene and an α-olefin is preferred, and an ethylene-propylene random copolymer is particularly preferred. In addition, a random copolymer of propylene and an α-olefin, in particular an ethylene-propylene random copolymer, has a high elongation stress, and as described below, by stretching a resin composition containing this copolymer and a filler, the unevenness caused by the filler is easily reflected on the film surface, making it preferable in that the surface roughness of the film can be easily adjusted.

[0057] When a propylene-based resin is used, from the viewpoint of improving extensibility, a thermoplastic resin having a lower melting point than the propylene-based resin, such as polyethylene, polystyrene, or an ethylene-vinyl acetate copolymer, can be used in combination in an amount of 3 to 25 mass% relative to 100 mass% of the propylene-based resin.

[0058] <Filler> From the viewpoint of adjusting the surface roughness of the substrate within the range of the present invention, the thermoplastic resin film preferably contains a filler. The filler makes it easy to form voids in the substrate, making it easy to adjust the whiteness of the recording paper. The filler can also adjust the surface roughness of the substrate.

[0059] Examples of the filler that can be used in the substrate include inorganic fillers and organic fillers. Examples of the inorganic filler include inorganic particles such as calcium carbonate, calcined clay, silica, diatomaceous earth, talc, barium sulfate, aluminum sulfate, magnesium oxide, alumina, and ultraviolet absorbing fillers. Examples of the ultraviolet absorbing filler include titanium dioxide and zinc oxide. Among these, calcium carbonate is preferred from the viewpoints of cost and pore forming ability.

[0060] When the thermoplastic resin of the substrate is an olefin-based resin, examples of the organic filler include polyethylene terephthalate, polybutylene terephthalate, polycarbonate, nylon-6, nylon-6,6, a cyclic olefin polymer, or a copolymer of a cyclic olefin and ethylene, and the like, which has a melting point higher than the melting point of the polyolefin resin used, for example, in the range of 120 to 300°C, or a glass transition temperature, for example, in the range of 120 to 280°C.

[0061] Among the above inorganic fillers or organic fillers, one may be used alone, or two or more may be combined. When two or more types are combined, the inorganic filler and the organic filler may be mixed and used.

[0062] The average particle size of the filler is preferably 0.01 to 15 μm, more preferably 0.05 to 10 μm. If the average particle size is 15 μm or less, the uniformity of the pores tends to be improved. Also, if the average particle size is 0.01 μm or more, pores of a predetermined size tend to be easily obtained. The average particle size of the filler is the average value of the measured particle sizes of 100 particles randomly sampled from the observation area of ​​a cut surface of a thermoplastic resin film in the thickness direction observed with an electron microscope. The particle size is determined from the maximum distance between two points on the contour of the particle (maximum diameter).

[0063] The content of the filler in the substrate is preferably 8% by mass or more, more preferably 14% by mass or more, while it is preferably 65% ​​by mass or less, more preferably 50% by mass or less. If the filler content is equal to or greater than the lower limit, a sufficient number of voids is easily obtained, and the recording paper tends to have a desired whiteness or opacity. If the filler content is equal to or less than the upper limit, the recording paper tends to have sufficient strength, and is less likely to break during stretch molding.

[0064] In addition, when adjusting the arithmetic mean roughness Ra of the substrate surface by blending a filler, it is effective to make the average particle size of the filler in the substrate relatively large. Therefore, from the viewpoint of adjusting the surface roughness, the average particle size of the filler in the substrate is preferably 0.5 μm or more, more preferably 1.5 μm or more, and preferably 15 μm or less, and more preferably 10 μm or less.

[0065] <Additives> The substrate may contain any additives as necessary. Examples of the optional additives include various known additives such as heat stabilizers, ultraviolet stabilizers (light stabilizers), dispersants, antistatic agents, antioxidants, fluorescent brighteners, ultraviolet absorbers, dyes, pigments, lubricants, anti-tack agents, anti-blocking agents, and flame retardants. Examples of the heat stabilizers include sterically hindered phenols, phosphorus-based agents, and amine-based agents, which can be blended in an amount of usually 0.001 to 1% by mass. Examples of the light stabilizers include sterically hindered amines, benzotriazoles, and benzophenones, which can be blended in an amount of usually 0.001 to 1% by mass. Examples of the dispersants include silane coupling agents, higher fatty acids such as oleic acid and stearic acid, metal soaps, polyacrylic acid, polymethacrylic acid, and salts thereof, which can be blended in an amount of usually 0.01 to 4% by mass. Examples of the antistatic agents include low molecular weight surfactants such as stearic acid monoglyceride and stearyl diethanolamine, which can be blended in an amount of usually 0.01 to 4% by mass.

[0066] <Substrate structure> The substrate may have either a single layer structure or a multilayer structure. In the case of a multilayer structure, the type and amount of material of each layer may be the same or different. In the case of a multilayer structure, from the viewpoint of adhesion to the print-receiving layer, it is preferable that the layer in contact with the print-receiving layer has the characteristics described above as the <thermoplastic resin film>. From the viewpoint of blocking resistance, the filler content in the surface layer in contact with the print-receiving layer may be higher than that of other layers in order to adjust the surface roughness.

[0067] The substrate may be a non-stretched film or a stretched film. From the viewpoint of increasing the stiffness of the substrate, the substrate is preferably a stretched film stretched at least in one direction, and more preferably a stretched film stretched in two directions (hereinafter, sometimes referred to as a biaxially stretched film). Since the biaxially stretched film is stretched in two directions, it is difficult to stretch when folded, and since it has a high bending elastic modulus, it is difficult to develop a crease. When the substrate has a multi-layer structure, a layer of a non-stretched film and a layer of a stretched film can be combined, or stretched films having the same or different number of stretch axes in each layer can be combined, but from the above viewpoint, it is preferable that at least one layer is a stretched film.

[0068] <<Thickness>> The thickness of the substrate is not particularly limited, but from the viewpoint of providing the recording paper with stiffness suitable for transportation, the thickness is preferably 60 μm or more, more preferably 70 μm or more, and even more preferably 80 μm or more. From the viewpoint of ease of folding, the thickness is preferably 300 μm or less, and more preferably 250 μm or less.

[0069] (Method of manufacturing recording paper) The method for producing the recording paper of the present invention is not particularly limited, but it can usually be produced by laminating a print-receiving layer on a substrate.

[0070] <Formation of the substrate> The substrate is usually obtained by forming a film from a resin composition containing a thermoplastic resin. The film forming method is not particularly limited, and various known forming methods can be used alone or in combination. For example, cast forming, calendar forming, rolling forming, inflation forming, etc., in which a molten resin is extruded into a sheet shape using a single-layer or multi-layer T die, I die, etc. connected to a screw-type extruder, can be mentioned. A film can also be formed by casting or calendaring a mixture of a thermoplastic resin and an organic solvent or oil, and then removing the solvent or oil. Examples of film forming methods for multilayered substrates include film forming methods such as a multilayer die method using a feed block or a multi-manifold, or an extrusion lamination method using multiple dies, and these can also be combined.

[0071] Examples of the film stretching method include a longitudinal stretching method using the difference in peripheral speed between rolls, a transverse stretching method using a tenter oven, a sequential biaxial stretching method combining these, a rolling method, a simultaneous biaxial stretching method using a combination of a tenter oven and a pantograph, or a simultaneous biaxial stretching method using a combination of a tenter oven and a linear motor. In addition, a simultaneous biaxial stretching method (inflation molding) in which a molten resin is extruded into a tube using a circular die connected to a screw-type extruder and then air is blown into the extruded resin can also be used. When manufacturing a multilayer substrate containing multiple stretched films, each layer may be stretched individually before lamination, or may be stretched together after lamination. In addition, the stretched layer may be stretched again after lamination.

[0072] The stretching temperature when stretching is performed is preferably in the range of the glass transition temperature of the thermoplastic resin or higher when the thermoplastic resin used for the substrate is a non-crystalline resin. When the thermoplastic resin is a crystalline resin, the stretching temperature is preferably in the range of the glass transition temperature of the non-crystalline part of the thermoplastic resin or higher and the melting point of the crystalline part of the thermoplastic resin or lower, specifically, a temperature 2 to 60°C lower than the melting point of the thermoplastic resin is preferable.

[0073] The film stretching speed is not particularly limited, but from the viewpoint of stable stretching, it is preferably within the range of 20 to 350 m / min. The stretching ratio of the film can also be appropriately determined in consideration of the properties of the thermoplastic resin used. For example, when a film containing a propylene homopolymer or copolymer is uniaxially stretched, the stretching ratio is usually about 1.2 times or more, preferably 2 times or more, and usually 12 times or less, preferably 10 times or less. When biaxially stretched, the stretching ratio is usually 1.5 times or more, preferably 10 times or more, and usually 60 times or less, preferably 50 times or less, in terms of area stretching ratio.

[0074] When a film containing a polyester resin is uniaxially stretched, the stretch ratio is usually 1.2 times or more, preferably 2 times or more, and usually 10 times or less, preferably 5 times or less. When a film is biaxially stretched, the stretch ratio is usually 1.5 times or more, preferably 4 times or more, and usually 20 times or less, preferably 12 times or less, in terms of area stretch ratio. Within the above range of stretching ratio, there is a tendency that stable stretch molding can be achieved. Also, in the case of using a resin composition containing a thermoplastic resin and a filler, within the above range of stretching ratio, the desired porosity is obtained, the opacity is easily improved, and the film is less likely to break.

[0075] <Surface treatment> The substrate is preferably subjected to a surface treatment from the viewpoint of enhancing adhesion to an adjacent layer of the substrate, for example, a print-receiving layer. Examples of the surface treatment include corona discharge treatment, flame treatment, plasma treatment, glow discharge treatment, ozone treatment, etc., and these treatments can be combined. Among these, corona discharge treatment or flame treatment is preferred, and corona treatment is more preferred.

[0076] When performing corona discharge treatment, the discharge amount is preferably 600 J / m 2 (10W min / m 2 ) or more, and more preferably 1,200 J / m2 (20W min / m 2 ) or more. The discharge amount is preferably 12,000 J / m 2 (200W min / m 2 ) or less, and more preferably 10,800 J / m 2 (180W min / m 2 The discharge amount when carrying out the flame treatment is preferably 8,000 J / m 2 More preferably, 20,000 J / m 2 The discharge amount is preferably 200,000 J / m or more. 2 or less, more preferably 100,000 J / m 2 The following is the result.

[0077] <Formation of print-receiving layer> The method of forming the print-receiving layer is not particularly limited. For example, a coating liquid is prepared by dispersing or dissolving various components of the print-receiving layer in water, and the coating liquid is applied to a substrate and dried to form the print-receiving layer. For coating, a known coating device such as an air knife coater, a gravure coater, a blade coater, a roll coater, a reverse roll coater, a bar coater, a curtain coater, a die slot coater, a champlex coater, a size press coater, a gate roll coater, or a bill blade coater can be used.

[0078] <Formation of printing layer> A printed layer can be formed by printing characters, lines, pictures, etc. on the print-receiving layer. The printed layer is a layer made of an ink composition transferred by printing.

[0079] The printing method is not particularly limited, and known printing methods such as gravure printing, offset printing, flexographic printing, seal printing, screen printing, etc. can be used. The printed layer can also include conventionally known decorations such as printing by various printers such as inkjet type, electrophotographic type, or liquid toner type, foil stamping such as hot stamping or cold stamping, transfer foil, or holograms.

[0080] For printing, various inks such as ultraviolet curing ink, oil-based ink, oxidation polymerization curing ink, water-based ink, powder toner, or liquid toner (electroink) can be used depending on the printing method.

[0081] In particular, a print-receiving layer containing a low acid value carboxy-containing resin has excellent adhesion to ultraviolet-curable ink and has high printability with ultraviolet-curable ink. The print-receiving layer according to the present invention also has excellent adhesion to ink due to the anchoring effect brought about by the surface irregularities caused by the inorganic filler. In this respect, the print-receiving layer according to the present invention has high printability with offset printing using ultraviolet-curable ink, oil-based ink, or oxidative polymerization curable ink, etc. It has printability not only for offset printing, but also for laser printing using liquid toner or powder toner. EXAMPLES

[0082] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, the terms "parts", "%", and the like are based on mass unless otherwise specified.

[0083] (material) The following materials were used for the print-receiving layer. <Carboxy group-containing resin> (AE986B): Acrylic resin (product name: AE986B, manufactured by E-Tech Co., Ltd.), solid content concentration: 35%, acid value ( mg KOH / g ):5 (ZE-1425): Styrene acrylic resin (product name: Hi-Los-X ZE-1425, manufactured by Seiko PMC Co., Ltd.), solid content concentration: 47%, acid value ( mg KOH / g ):100 <Inorganic filler> (TP-123CS): Light calcium carbonate (product name: Tama Pearl TP-123CS, manufactured by Okutama Kogyo Co., Ltd.), average primary particle size (D50): 0.2 μm, crystal structure: aragonite (Kunipia): Refined bentonite (product name: Kunipia-F, manufactured by Kunimine Kogyo Co., Ltd.), average primary particle size (D50): 2 μm, montmorillonite

[0084] <Antistatic agent> (Sunmorin): Sodium dioctyl sulfosuccinate (product name: Sunmorin OT-70, manufactured by Sanyo Chemical Industries, Ltd.) <Crosslinking agent> (AZ Coat): Ammonium zirconium carbonate (product name: AZ Coat 5800MT, manufactured by San Nopco) <Binders and migration inhibitors> (F220): Isocyanate-modified polyethylene glycol (product name: Melpol F-220, manufactured by Sanyo Chemical Industries, Ltd.) <Antifoaming agent> (Bismar): Defoamer containing ester wax, polyoxylalkylene fatty acid ester, polyoxyethylene alkyl ether fatty acid ester, and higher alcohol (product name: Bismar FX-10F, manufactured by Nisshin Chemical Laboratory)

[0085] Table 1 below lists the materials mentioned above. [Table 1]

[0086] (Preparation of substrate) <Production of Thermoplastic Resin Film (1)> (I) Resin composition a was prepared by mixing 74 parts by mass of propylene homopolymer (product name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation), 8 parts by mass of high-density polyethylene resin (product name: Novatec HD HJ580N, manufactured by Japan Polyethylene Corporation), and 18 parts by mass of heavy calcium carbonate particles (product name: Softon 1800, manufactured by Bihoku Powder Industry Co., Ltd.).

[0087] (II) Next, the resin composition a was melt-kneaded in an extruder set at 260°C and extruded into a sheet from a die. The sheet was cooled by a cooling roll to obtain an unstretched sheet. After heating the unstretched sheet again to 150°C, the speed difference between the rolls was used to stretch the sheet 4.8 times in the machine direction (MD) to obtain a longitudinal uniaxially stretched resin film.

[0088] (III) Separately, 54 parts by mass of an ethylene-propylene random copolymer (product name: Novatec PP FG4AQ, manufactured by Japan Polypropylene Corporation) and 46 parts by mass of heavy calcium carbonate particles (product name: Softon 1800, manufactured by Bihoku Funka Kogyo Co., Ltd.) were mixed to prepare resin composition b.

[0089] This was melt-kneaded in an extruder set at 230° C., extruded through a die into a film on one side of the above-mentioned longitudinally uniaxially stretched film, and laminated to obtain a first surface layer / core layer laminate (b / a). Furthermore, the resin composition b was melt-kneaded in another extruder set at 230°C, extruded from a die into a film, and laminated on the surface of the core layer (a) of the laminate (b / a), thereby obtaining a laminate (b / a / b) having a three-layer structure of a first surface layer / core layer / second surface layer.

[0090] This three-layer laminate was introduced into a tenter oven, heated to 155°C, and then stretched 8 times in the transverse direction (TD) using a tenter. It was then heat-set (annealed) at 164°C, further cooled to 55°C, and the edge portions were slit to obtain a thermoplastic resin film (1) having a thickness of 80 μm. The arithmetic average roughness Ra of the surface of this thermoplastic resin film (1) was measured in accordance with JIS-B-0601:1994 and found to be 0.60 μm.

[0091] <Production of Thermoplastic Resin Film (2)> (I) Resin composition c was prepared by mixing 55 parts by mass of propylene homopolymer (trade name: Novatec PP FY6Q, manufactured by Japan Polypropylene Corporation), 12 parts by mass of propylene homopolymer (trade name: Novatec PP MA3Q, manufactured by Japan Polypropylene Corporation), 10 parts by mass of high-density polyethylene resin (trade name: Novatec HD HJ580N, manufactured by Japan Polyethylene Corporation), and 23 parts by mass of heavy calcium carbonate particles (trade name: Softon 1800, manufactured by Bihoku Powder Industry Co., Ltd.).

[0092] (II) Next, the resin composition c was melt-kneaded in an extruder set at 260°C and extruded into a sheet from a die. The sheet was cooled by a cooling roll to obtain an unstretched sheet. After heating the unstretched sheet again to 150°C, the speed difference between the rolls was used to stretch the sheet in the machine direction (MD) by 4.8 times to obtain a longitudinal uniaxially stretched resin film.

[0093] (III) Separately, 38 parts by mass of a propylene homopolymer (product name: Novatec PP MA3Q, manufactured by Japan Polypropylene Corporation), 3.5 parts by mass of a propylene copolymer (product name: Tafmer PN-2060, manufactured by Mitsui Chemicals, Inc.), and 53 parts by mass of maleic modified propylene light calcium carbonate particles (product name: Calfine YM23, manufactured by Maruo Calcium) were mixed to prepare a resin composition d.

[0094] This was melt-kneaded in an extruder set at 250° C., extruded through a die into a film on one side of the above-mentioned longitudinally uniaxially stretched film, and laminated to obtain a first surface layer / core layer laminate (d / c). Furthermore, the resin composition d was melt-kneaded in another extruder set at 250°C, extruded from a die into a film, and laminated on the surface of the core layer (c) side of the laminate (d / c). This produced a laminate (d / c / d) with a three-layer structure of first surface layer / core layer / second surface layer.

[0095] This three-layer laminate was introduced into a tenter oven, heated to 155°C, and then stretched 8 times in the transverse direction (TD) using a tenter. It was then heat-set (annealed) at 164°C, further cooled to 55°C, and the edge portions were slit to obtain a thermoplastic resin film (2) with a thickness of 110 μm. The arithmetic average roughness Ra of the surface of this thermoplastic resin film (2) was measured in accordance with JIS-B-0601:1994 and found to be 0.20 μm.

[0096] <Production of Thermoplastic Resin Film (3)> (I) Resin composition e was prepared by mixing 14 parts by mass of propylene homopolymer (trade name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation), 60 parts by mass of propylene homopolymer (trade name: Novatec PP FY6, manufactured by Japan Polypropylene Corporation), 10 parts by mass of high-density polyethylene resin (trade name: Novatec HD HJ580N, manufactured by Japan Polyethylene Corporation), and 16 parts by mass of heavy calcium carbonate particles (trade name: Softon 1800, manufactured by Bihoku Powder Industry Co., Ltd.).

[0097] (II) Next, the resin composition e was melt-kneaded in an extruder set at 270°C and extruded into a sheet from a die. The sheet was cooled by a cooling roll to obtain an unstretched sheet. After heating the unstretched sheet again to 140°C, the speed difference between the rolls was used to stretch the sheet 4.8 times in the machine direction (MD) to obtain a longitudinal uniaxially stretched resin film.

[0098] (III) Separately, 53 parts by mass of propylene homopolymer (product name: Novatec PP FG4AQ, manufactured by Japan Polypropylene Corporation) and 47 parts by mass of heavy calcium carbonate particles (product name: Softon 1800, manufactured by Bihoku Funka Kogyo Co., Ltd.) were mixed to prepare resin composition f.

[0099] This was melt-kneaded in an extruder set at 270° C., extruded through a die into a film on one side of the above-mentioned longitudinally uniaxially stretched film, and laminated to obtain a first surface layer / core layer laminate (f / e). Furthermore, the resin composition f was melt-kneaded in another extruder set at 250°C, extruded from a die into a film, and laminated on the surface of the core layer (e) side of the laminate (f / e), thereby obtaining a laminate (f / e / f) having a three-layer structure of first surface layer / core layer / second surface layer.

[0100] This three-layer laminate was introduced into a tenter oven, heated to 155°C, and then stretched 8 times in the transverse direction (TD) using a tenter. It was then heat-set (annealed) at 163°C, further cooled to 55°C, and the edge portions were slit to obtain a thermoplastic resin film (3) with a thickness of 250 μm. The arithmetic average roughness Ra of the surface of this thermoplastic resin film (1) was measured in accordance with JIS-B-0601:1994 and found to be 0.60 μm.

[0101] (Preparation of Coating Solution for Print Receiving Layer) Coating fluids (A1) to (A4) for the print-receiving layer were prepared as follows.

[0102] <Coating fluid (A1)> 100 parts by mass of an acrylic resin (AE986B) as a carboxy group-containing resin, 100 parts by mass of light calcium carbonate (TP-123CS) as an inorganic filler, 40 parts by mass of refined bentonite (Kunipia) as an inorganic filler, 20 parts by mass of ammonium zirconium carbonate (AZ Coat) as a crosslinking agent, 1 part by mass of isocyanate-modified polyethylene glycol (F-220) as a binder migration inhibitor, and 0.2 parts by mass of an antifoaming agent (Bismer) were mixed, and ion-exchanged water was added to obtain a solids concentration of 10% by mass, to obtain a coating liquid (A1) for a print-receiving layer.

[0103] <Coating liquid (A2)> Each coating liquid (A2) was prepared in the same manner as for the coating liquid (A1), except that 40 parts by mass of purified bentonite (Kunipia) was changed to 4.5 parts by mass of sodium dioctyl sulfosuccinate (Sunmorin).

[0104] <Coating fluid (A3)> Coating Fluid (A3) was prepared in the same manner as Coating Fluid (A1), except that 100 parts by mass of the acrylic resin (AE986B) was changed to 100 parts by mass of a styrene acrylic resin (ZE-1425), which is a carboxyl group-containing resin.

[0105] (Manufacturing of recording paper) <Example 1> The coating liquid (A1) for the print-receiving layer was applied with a bar coater to one side of the substrate, the thermoplastic resin film (1), on which the surface roughness had been measured, and then dried to form a print-receiving layer with a thickness of 0.4 μm, thereby obtaining the recording paper of Example 1. <Example 2> A recording paper of Example 2 was obtained in the same manner as in Example 1, except that a thermoplastic resin film (3) was used as the substrate.

[0106] <Example 3> A recording paper of Example 3 was obtained in the same manner as in Example 2, except that the coating liquid (A1) was changed to the coating liquid (A2).

[0107] <Comparative Example 1> A recording paper of Comparative Example 1 was obtained in the same manner as in Example 1, except that the thermoplastic resin film (1) was changed to the thermoplastic resin film (2).

[0108] <Comparative Example 2> A recording paper of Comparative Example 2 was obtained in the same manner as in Example 2, except that the coating liquid (A1) was changed to the coating liquid (A3).

[0109] (evaluation) Offset printing was carried out on the recording paper of each of the Examples and Comparative Examples, and the printability was evaluated as follows.

[0110] <Ink adhesion> <<Print>> The recording paper of each Example and Comparative Example was cut to A2 size (420 mm x 594 mm) and a pattern including a design was offset printed on one side. For printing, an offset printing machine (product name: SM102, manufactured by Heidelberg) and oxidative polymerization type sheet-fed process ink (product name: Fusion G (black, indigo, red, yellow), manufactured by DIC Corporation) were used. The pattern was printed in four colors, black, indigo, red, and yellow, and the density of each color was 100%. Specifically, 1000 sheets were continuously printed at a speed of 8000 sheets / hour in an environment of a temperature of 23°C and a relative humidity of 50%, to obtain an offset print.

[0111] <<Ink adhesion in dry state>> The ink adhesion of the recording paper in a dry state after printing was evaluated as follows. A 5 cm long piece of cellophane tape manufactured by Nichiban Co., Ltd. was applied to the surface of the print-receiving layer. 2.5 cm of the tape was peeled off by hand at a low speed (2.5 cm / s), and the remaining 2.5 cm was peeled off at a high speed (25 cm / s). After peeling, the adhesion was evaluated according to the degree of peeling of the print-receiving layer using the following criteria. 5 (Excellent): No peeling at both low and high speeds 4 (Good): No peeling at low speed, partial peeling at high speed (less than 50% of the entire high-speed peeled surface) 3 (Fair): No peeling at low speed, peeled completely (more than 50% of the entire high-speed peeling surface) at high speed 2 (Unacceptable): Peeled partially at low speed (less than 50% of the entire low-speed peeling surface), and completely at high speed (more than 50% of the entire high-speed peeling surface). 1 (Fail): Complete peeling at both low and high speeds

[0112] <<Ink adhesion in wet state>> The ink adhesion of the recording paper in a wet state after printing was evaluated as follows. The recording paper was soaked in water at 23°C for 24 hours, then taken out and the moisture on the printed surface was lightly wiped off with a cloth. After 10 minutes, the adhesion of the print-receiving layer to the ink was evaluated using the same method and criteria as in the dry state described above.

[0113] <Adhesion to substrate> The adhesion strength (kg·cm) between the print-receiving layer and the substrate was measured using an adhesion strength measuring device called "Internal Bond Tester" (product name, manufactured by Kumagai Riki Kogyo Co., Ltd.) in accordance with TAPPI-UM403. Adhesion strength of 1.4kg·cm or more is considered to pass.

[0114] <White page blocking> The evaluation was carried out according to the following procedure. Two sheets of recording paper from each Example or Comparative Example were prepared and stacked so that the print-receiving layer surfaces faced each other, with the MD and TD directions of the two samples coinciding with each other. Two overlapping sheets of recording paper were pressed with a high pressure jack at a pressure of 2.0 kgf for 5 minutes. This resulted in a sample in which the two sheets were intentionally blocked. This sample was pulled in the MD direction of the recording paper at a pulling speed of 50 mm / min using a tensile tester (manufactured by A&D, product name: RTG-11225). The load (gf / 10 cm) required for the sample to separate into one sheet was then measured. 2 The smaller this value, the better the blocking resistance.

[0115] The evaluation results are shown in Table 2. In Table 2, the content of liquid materials is shown in terms of solid content. [Table 2]

[0116] As shown in Table 2, all of Examples 1 to 3, which used a carboxyl group-containing resin with a very low acid value, obtained sufficient adhesion to both the ink and the substrate. In contrast, Comparative Example 2, which used a carboxyl group-containing resin with a high acid value, had low adhesion to the ink in a wet state because the print-receiving layer swelled, and in a dry state, the crosslink density due to the reaction between the carboxyl group-containing resin and the crosslinking agent was high, so the print-receiving layer had a high elastic modulus and low adhesion between the print-receiving layer and the substrate. In addition, when Example 1 is compared with Comparative Example 1, it can be seen that high ink adhesion and high blocking properties can be achieved at the same time by having the arithmetic mean roughness Ra of the surface within a specific range.

[0117] This application claims priority to Japanese patent application No. 2021-59370, filed on March 31, 2021, and incorporates all of the contents of that Japanese patent application by reference. [Explanation of symbols]

[0118] 1 Recording paper, 11 Base material, 12 Print receiving layer

Claims

1. A recording paper having a print-receiving layer on a substrate, The print-receiving layer contains an inorganic filler and a carboxyl group-containing resin having an acid value of 2 to 20 mgKOH / g, The arithmetic mean roughness Ra of the surface of the substrate on the side of the print-receiving layer is 0.3 to 1.0 μm. Recording paper.

2. The print-receiving layer further contains a binder migration inhibitor. The recording paper according to claim 1.

3. The binder migration inhibitor is an isocyanate-modified polyethylene glycol. The recording paper according to claim 2.

4. The inorganic filler includes calcium carbonate and layered silicate. The recording paper according to any one of claims 1 to 3.

5. The content of the carboxyl group-containing resin in the print-receiving layer is 40 to 150 parts by mass per 100 parts by mass of the inorganic filler. The recording paper according to any one of claims 1 to 4.

6. The print-receiving layer has a thickness of 0.2 to 10 μm. The recording paper according to any one of claims 1 to 5.

7. The carboxyl group-containing resin is an acrylic resin (excluding styrene-acrylic resins). The recording paper according to any one of claims 1 to 6.

8. The substrate is a thermoplastic resin film. The recording paper according to any one of claims 1 to 7.

9. The thermoplastic resin film contains a filler. The recording paper according to claim 8.

Citation Information

Patent Citations

  • Sheet for ink-jet recording

    JP2000247020A

  • Electrophotographic media with carboxylic acid polymer

    JP2008522241A

  • Adhesive composition and adhesive film

    JP2018053066A

  • Graphic sheet and illumination system using graphic sheet

    JP2020052225A

  • Tape for electronic device package

    WO2017168829A1