Floor cushioning and floor construction materials

A dual-layered floor cushioning material with specific elastic modulus ranges for each layer addresses the challenge of effective shock absorption and comfort, achieving reduced impact acceleration and comfortable flooring experience.

JP7580189B2Active Publication Date: 2024-11-11KURARAY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2019177014
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-09-27
Publication Date
2024-11-11
Estimated Expiration
2039-09-27

AI Technical Summary

Technical Problem

Existing floor cushioning materials struggle to achieve both effective shock absorption during a fall collision and comfortable walking or sitting sensation, with many either being too soft and prone to bottoming out or too hard, while also failing to meet the stringent impact mitigation standards of recent specifications.

Method used

A dual-layered floor cushioning material is introduced, comprising a first buffer layer with a compressive elastic modulus of 0.01 to 29 kPa when compressed 10% to 20% and a second buffer layer with a compressive elastic modulus of 30 to 12,000 kPa when compressed 2.5% to 5.0%, arranged such that the second layer is below the first, enhancing shock absorption and comfort.

Benefits of technology

The dual-layered design significantly reduces impact acceleration during a fall collision while providing a comfortable walking and sitting experience, meeting or exceeding impact mitigation standards and ensuring neither excessive hardness nor softness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580189000002
    Figure 0007580189000002
  • Figure 0007580189000003
    Figure 0007580189000003
  • Figure 0007580189000004
    Figure 0007580189000004
Patent Text Reader

Abstract

To provide a floor cushioning material and a floor constitution material useful for mitigating impact.SOLUTION: A floor cushioning material 10 is constituted with at least a first cushioning layer 2 and a second cushioning layer 3 arranged under the first cushioning layer. The first cushioning layer 2 has a compression modulus of elasticity of 0.01-29 kPa when compressed from 10% to 20%, and the second cushioning layer 3 has the compression modulus of elasticity of 30-12,000 kPa when compressed from 2.5% to 5.0%. A floor constitution material has at least the floor cushioning material and a plate.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a floor cushioning material and a floor constituent material that are useful for absorbing shock, and in particular to a floor cushioning material and a floor constituent material that can absorb shock during a fall collision. [Background technology]

[0002] Floor constituent materials are required to be thin, lightweight, and have shock absorbing properties. For example, Patent Document 1 (JP 2016-216928 A) describes a floor constituent material including a buffer layer arranged in the bottommost layer, a plate material arranged adjacent to the upper side of the buffer layer, and a buffer layer arranged in the topmost layer on the opposite side to the buffer layer with the plate material in between. The buffer layer arranged in the topmost layer has a compressive elastic modulus of 100 to 2500 kPa and a thickness of 0.5 to 4 mm, the buffer layer arranged in the bottommost layer has a compressive elastic modulus of 10 to 500 kPa, and the plate material has a product of a bending elastic modulus and a thickness of 1.0×10 4 Thus, a shock absorbing floor component has been disclosed.

[0003] In Patent Document 1, the product of the compressive elastic modulus of the buffer layer placed above the board and the buffer layer placed below the board, and the bending elastic modulus and thickness of the board are adjusted within a specific range to realize a thin shock-absorbing floor component with excellent shock-absorbing properties.

[0004] For example, the Architectural Institute of Japan specifies that the recommended hardness value for floors in kindergartens, hospitals, elderly care facilities, athletic facilities, and other locations where consideration for fall impacts is desired is 100 G or less, and Patent Document 1 meets this recommended value. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-216928 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in recent years, further improvements have been required for shock-absorbing tatami flooring in terms of fall impact resistance, and the recommended hardness value for shock-absorbing tatami flooring specified in JIS A 5917 (2018) is 50G or less. On the other hand, with simply soft cushioning materials such as those used in gymnastics, the thickness needs to be increased to prevent the floor from touching the ground, which creates the problem of a poor walking feel.

[0007] Therefore, an object of the present invention is to provide a floor cushioning material that can further improve the shock mitigation properties against the impact during a fall collision. Another object of the present invention is to provide a floor constituent material which not only achieves the above-mentioned shock absorbing properties but also provides a comfortable stepping and sitting experience which is neither too hard nor too soft. [Means for solving the problem]

[0008] As a result of intensive research into achieving the above-mentioned object, the inventors of the present invention have surprisingly discovered that a cushioning material that combines a first buffer layer whose compressive elastic modulus when compressed from 10% to 20% is in a specific small range and a second buffer layer whose compressive elastic modulus when compressed from 2.5% to 5.0% is in a specific large range, and that arranges the second buffer layer below the first buffer layer, can achieve shock absorption that exceeds that of Patent Document 1, although the reason is unclear. They also discovered that a floor component equipped with such a floor cushioning material can combine not only good shock absorption properties but also good comfort when stepping on and sitting on it, which led to the completion of the present invention.

[0009] That is, the present invention can be configured in the following manner. [Aspect 1] A floor cushioning material comprising at least a first cushioning layer and a second cushioning layer disposed below the first cushioning layer, the compressive elastic modulus of the first buffer layer when compressed from 10% to 20% is 0.01 to 29 kPa (preferably 0.1 to 20 kPa, more preferably 0.5 to 15 kPa); A cushioning material for floors, wherein the second cushioning layer has a compressive elastic modulus of 30 to 12,000 kPa (preferably 50 to 11,000 kPa, more preferably 80 to 10,500 kPa) when compressed from 2.5% to 5.0%. [Aspect 2] A floor cushioning material as described in embodiment 1, wherein the compressive elastic modulus when the second buffer layer is compressed from 2.5% to 5.0% is at least 50 kPa higher (preferably at least 80 kPa higher) than the compressive elastic modulus when the first buffer layer is compressed from 10% to 20%. [Aspect 3] The floor cushioning material according to the first or second aspect, wherein the second cushioning layer has a bending strength of 0.2 N / mm 2 or more (preferably 0.3 to 3 N / mm 2 ) is a cushioning material for floors. Aspect 4 A floor cushioning material according to any one of aspects 1 to 3, wherein the thickness of the first buffer layer is 20 mm or less (preferably 1 to 18 mm, more preferably 3 to 15 mm), and the thickness of the second buffer layer is 0.8 times or more (preferably 0.8 to 6 times, more preferably 0.8 to 5 times) the thickness of the first buffer layer. Aspect 5 In the floor cushioning material according to any one of aspects 1 to 4, the first cushioning layer has an apparent density of 30 to 70 kg / m 3 (Preferably 35 to 65 kg / m 3 , more preferably 40 to 60 kg / m 3 ) nonwoven fiber structure, a cushioning material for floors. Aspect 6 6. The floor cushioning material according to any one of aspects 1 to 5, wherein the first and second cushioning layers can be integrated together by a connecting means. Aspect 7 A floor cushioning material according to any one of aspects 1 to 6, wherein the floor cushioning material has an impact acceleration G value of 45 G or less (preferably 42 G or less, and more preferably 39 G or less) during a fall collision measured in accordance with JIS A 5917 (2018) through a 5.5 mm thick Chinese plywood. Aspect 8 The floor cushioning material according to any one of aspects 1 to 7, wherein the first cushioning layer is a nonwoven fiber structure in which fibers are fixed to each other by fusion of moist heat adhesive fibers. Aspect 9 A floor cushioning material according to any one of aspects 1 to 8, wherein the second cushioning layer is at least one selected from the group consisting of a natural fiber molded board, a synthetic fiber molded board, an inorganic fiber molded board, and a foamed plastic board. Aspect 10 A floor constructing material comprising at least the floor cushioning material according to any one of aspects 1 to 9 and a plate material, with a first cushioning layer being disposed on the underside of the plate material. Aspect 11 A flooring component according to aspect 10, wherein the hardness during daily movement measured in accordance with JIS A 5917 (2018) is 0.6 to 2.0 (preferably 0.6 to 1.5, more preferably 0.7 to 1.4, and even more preferably 0.8 to 1.3). Aspect 12 12. A floor constructing material according to aspect 10 or 11, wherein the flexural modulus of the plate material is 500 to 4000 MPa (preferably 550 to 3000 MPa). Aspect 13 A floor constructing material according to any one of aspects 10 to 12, having a thickness of 100 mm or less (preferably a thickness of 80 mm or less, more preferably 65 mm or less) and an impact acceleration G value measured in accordance with JIS A 6519 of 45 G or less (preferably 42 G or less, more preferably 39 G or less). Aspect 14 A flooring component according to any one of aspects 10 to 13, which is a tatami flooring, a wood flooring, a polymer sheet flooring, a ceramic flooring, or a carpet flooring. In this specification, the term "underside" includes both a case where the part is disposed under the other in a state of direct contact, and a case where the part is disposed under the other without direct contact. Effect of the Invention

[0010] The floor cushioning material of the present invention combines a first cushioning layer which has a moderately small compressive elastic modulus when further compressed from a state already compressed to a certain extent, with a second cushioning layer disposed below the first cushioning layer which has a moderately large compressive elastic modulus at the start of compression, thereby providing floor components equipped with the floor cushioning material with good shock mitigation properties against impacts during a fall collision. Furthermore, by providing the floor cushioning material of the present invention, it is possible to obtain a floor component that not only achieves shock mitigation, but also provides a comfortable stepping and sitting experience that is neither too hard nor too soft. [Brief description of the drawings]

[0011] The present invention will be more clearly understood from the following description of preferred embodiments with reference to the accompanying drawings. However, the embodiments and drawings are merely for illustration and explanation, and should not be used to define the scope of the present invention, which is defined by the appended claims. [Figure 1] FIG. 1 is a schematic cross-sectional view for explaining a laminate (or floor component) of a floor cushioning material and a plate material, which is one embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a floor cushioning material according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing a floor component according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The floor cushioning material of the present invention is composed of at least a first cushioning layer and a second cushioning layer disposed below the first cushioning layer. The floor constructing material of the present invention is composed of at least a board material and the floor cushioning material, and the first cushioning layer is disposed below the board material.

[0013] One embodiment of the present invention will be described with reference to Fig. 1. Fig. 1 is a schematic cross-sectional view for explaining a laminate (or flooring constituent material) of a floor cushioning material and a plate material, which is one embodiment of the present invention. In Fig. 1, the floor cushioning material 10 is composed of a first buffer layer 2 and a second buffer layer 3 disposed below the first buffer layer 2. Furthermore, a plate material 1 is disposed above the floor cushioning material 10, i.e., on the opposite side of the second buffer layer 3 with the first buffer layer 2 interposed therebetween, to form a flooring constituent material 20.

[0014] For example, when pressure is applied locally to plate material 1 due to an impact such as a fall, plate material 1, which is made of a material that is difficult to deform, transmits the received pressure over a large area to first buffer layer 2. Then, first buffer layer 2 transmits part of the pressure from the plate material to second buffer layer 3 while mitigating the received pressure to some extent.

[0015] The second buffer layer 3 has a higher compressive elastic modulus than the first buffer layer 2, and therefore can prevent bottoming out when an impact is applied to the second buffer layer 3, thereby reducing the acceleration G value at the time of impact. Furthermore, although the reason is unclear, by disposing the second buffer layer 3 below the first buffer layer 2, the acceleration G value at the time of impact can be significantly reduced compared to when the first buffer layer 2 and the second buffer layer 3 are each used alone. A floor component including the floor cushioning material of the present invention can reduce the acceleration G value at the time of impact, thereby improving safety during a fall collision.

[0016] In addition, between the board material 1, the first buffer layer 2, and the second buffer layer 3, there may be another layer (for example, a sheet-like or piece-like material such as a waterproof sheet, a dehumidifying sheet, an anti-mold sheet, an insect-repellent sheet, or a slip-prevention sheet) as appropriate, as long as it does not inhibit the effects of the present invention.

[0017] Furthermore, the components consisting of the plate material 1, the first buffer layer 2, and the second buffer layer 3 may or may not be fixed to each other by a connecting means. If they are fixed, they may be detachable.

[0018] For example, in FIG. 1, (i) the plate material 1 and the first buffer layer 2 may be integrated and placed on the second buffer layer 3 without being fixed, (ii) the first buffer layer 2 and the second buffer layer 3 may be integrated and the plate material 1 may be placed on the first buffer layer 2 without being fixed, or (iii) the plate material 1, the first buffer layer 2 and the second buffer layer 3 may be integrated. From the viewpoint of handling, the above (iii) is preferable. Moreover, the plate material 1, the first buffer layer 2 and the second buffer layer 3 may have the same size or different sizes. For example, the first buffer layer 2 and the second buffer layer 3, which have small areas, may be placed so as to cover them with the plate material 1, which has a large area, or the plate material 1, which has a small area, may be placed on the first buffer layer 2 and the second buffer layer 3, which have large areas. Moreover, the areas of the first buffer layer 2 and the second buffer layer 3 may also be different.

[0019] The connecting means may be adhesive or glue, but it is preferable to use hook-and-loop fasteners so that they can be attached and detached. Alternatively, sewing, a method commonly used for manufacturing tatami mats, may be used. When each part is integrated with a detachable connecting means, not only can each component be manufactured and stored separately, but handling can also be improved by integrating them as needed before use.

[0020] Moreover, Fig. 2 shows a schematic cross-sectional view of a floor cushioning material according to one embodiment of the present invention. Fig. 2 shows a floor cushioning material 10, which is the portion excluding the board material 1 shown in Fig. 1, and the floor cushioning material 10 is composed of a first cushioning layer 2 and a second cushioning layer 3 disposed below it. Such a floor cushioning material 10 can be used as a core material or base material for floor components used in coated floors, stretched floors, and laid floors, in combination with various finishing materials.

[0021] A schematic cross-sectional view showing a floor constructing material according to one embodiment of the present invention is shown in Fig. 3. The floor constructing material 30 includes a floor cushioning material 10 made up of a first cushioning layer 2 and a second cushioning layer 3 disposed thereunder. A board material 1 is disposed on the floor cushioning material 10, a cushioning material 5 is disposed on the board material 1, and a surface decorative material 4 is disposed on the cushioning material 5.

[0022] In addition, between the surface decorative material 4, the cushioning material 5, the board material 1, the first buffer layer 2, and the second buffer layer 3, there may be another layer (for example, a sheet-like or piece-like material such as a waterproof sheet, a dehumidifying sheet, a mold-proof sheet, an insect-proof sheet, or a slip-prevention sheet) as appropriate, as long as it does not inhibit the effects of the present invention.

[0023] Furthermore, the components consisting of the surface decorative material 4, the cushioning material 5, the plate material 1, the first buffer layer 2, and the second buffer layer 3 may or may not be fixed to each other by a connecting means. If they are fixed, they may be detachable.

[0024] For example, in Fig. 3, similarly to Fig. 1, each component may be simply placed on top of each other without being fixed to each other, or may be fixed to each other by a connecting means. For example, the cushion material 5 and the plate material 1 may be integrated and placed on the floor cushioning material 10, or the surface decorative material 4, the cushion material 5 and the plate material 1 may be integrated and placed on the floor cushioning material 10. Alternatively, the surface decorative material 4, the cushion material 5, the plate material 1 and the first buffer layer 2 may be integrated and placed on the second buffer layer 3, or the surface decorative material 4 and the cushion material 5 may be integrated and placed on the plate material 1.

[0025] From the standpoint of ease of handling, in the floor construction material 30, it is preferable that the surface decorative material 4, the cushioning material 5, the board material 1, the first buffer layer 2, and the second buffer layer 3 are integrated together, for example, by a detachable connecting means as necessary.

[0026] The floor cushioning material and floor constituent material of the present invention are not limited to the embodiment shown in Figs. 1 to 3 and may have various configurations, but the following describes each of the constituent members that are typically used.

[0027] (First buffer layer) The first buffer layer may have a compressive elastic modulus of 0.01 to 29 kPa, preferably 0.1 to 20 kPa, and more preferably 0.5 to 15 kPa when compressed from 10% to 20%. Note that the compressive elastic modulus when compressed from 10% to 20% refers to a numerical value measured as the elastic modulus when a test specimen cut into a disk shape having a diameter of 29 mm is compressed from a strain of 10% to 20% by a pressure plate at a test speed of 10 mm / min in accordance with JIS K 7181.

[0028] For the first buffer layer, by measuring the compressive elastic modulus when it is further compressed from a state that has already been compressed to a certain extent, rather than the compressive elastic modulus at the beginning of compression, it is possible to evaluate the shock mitigation properties against a large impact that occurs during a fall collision.

[0029] The thickness of the first buffer layer may be, for example, 20 mm or less, preferably 1 to 18 mm, and more preferably 3 to 15 mm. Here, the thickness may be, for example, a thickness measured in accordance with JIS L 1913 "Testing method for general staple fiber nonwoven fabrics."

[0030] The apparent density of the first buffer layer is, for example, 30 to 70 kg / m 3 and preferably 35 to 65 kg / m 3 , more preferably 40 to 60 kg / m 3 Here, the apparent density is a density based on the volume calculated from the external dimensions of the foam, and may be measured by a commonly used measuring method depending on the material. For example, when the first buffer layer is a nonwoven fiber structure, the density may be calculated from the thickness measured in accordance with JIS L 1913 "Testing methods for general staple fiber nonwoven fabrics" and the basis weight measured in accordance with JIS L 1913 "Testing methods for general staple fiber nonwoven fabrics."

[0031] As long as the first buffer layer exhibits such properties, various materials such as plastic foams (e.g., polystyrene foam, polyurethane foam, polyolefin foam, etc.), fiber structures (e.g., nonwoven fiber structures, felt), etc. may be used. These materials may be used alone or in combination of two or more. Among these, fiber structures are preferably used from the viewpoints of not only exhibiting a predetermined compressive elastic modulus even against a relatively large strain, but also excellent durability against repeated impacts.

[0032] Examples of the fiber structure include a physically entangled fiber structure such as felt, a nonwoven fiber structure obtained by mechanically compressing a nonwoven fabric (e.g., needle punching), a nonwoven fiber structure obtained by partially heat-pressure fusing a nonwoven fabric (e.g., heat embossing), and a nonwoven fiber structure in which fibers are fixed to each other by adhesion or fusing with a binder component. The fibers constituting the fiber structure may be natural or synthetic fibers, and examples of the synthetic fibers include polyolefin fibers, (meth)acrylic fibers, polyvinyl alcohol fibers, polyvinyl chloride fibers, polystyrene fibers, polyester fibers, polyamide fibers, polycarbonate fibers, and polyurethane fibers. Among these fibers, polyester fibers, polyamide fibers, or composite fibers containing these fibers are commonly used.

[0033] The average fineness of the subject fibers and / or binder fibers constituting the nonwoven fiber structure can be appropriately set as long as it satisfies the compressive elastic modulus required for the first buffer layer. For example, the average fineness may be in the range of 0.1 to 30 dtex, and preferably in the range of 0.5 to 20 dtex.

[0034] In the present invention, among nonwoven fiber structures, fiber structures in which fibers are fixed to each other by fusion of a binder component (particularly, binder fibers composed of thermal adhesive fibers composed of thermal adhesive resins such as polyester-based, polyamide-based, polyolefin-based, and polyvinyl alcohol-based) are preferred, and from the viewpoint of achieving both impact relaxation and strength, structures containing moist heat adhesive fibers and in which fibers are fixed to each other by fusion of the moist heat adhesive fibers (nonwoven fiber structures containing moist heat adhesive fibers) are particularly preferred. A structure containing moist heat adhesive fibers and in which fibers are fixed to each other by fusion of the moist heat adhesive fibers (hereinafter sometimes referred to as a "nonwoven fiber structure containing moist heat adhesive fibers") can be obtained, for example, by spraying high-temperature steam. The internal structure of the nonwoven fiber structure obtained by spraying high-temperature steam is uniformly bonded in the thickness direction, so that high strength can be ensured while maintaining the fiber structure.

[0035] The heat-and-moisture adhesive fiber is configured to contain at least a heat-and-moisture adhesive resin capable of exerting an adhesive function when high-temperature steam is sprayed. Specific examples of the heat-and-moisture adhesive resin include thermoplastic resins that are softened by hot water (e.g., 80 to 120°C, particularly 95 to 100°C) and can be self-adhesive or adhere to other fibers, such as vinyl alcohol-based polymers such as ethylene-vinyl alcohol-based copolymers, polylactic acid-based resins such as polylactic acid, and (meth)acrylic copolymers containing (meth)acrylamide units. Furthermore, elastomers capable of exerting an adhesive function when high-temperature steam is sprayed (e.g., polyolefin-based elastomers, polyester-based elastomers, polyamide-based elastomers, polyurethane-based elastomers, polystyrene-based elastomers, etc.) may be used. These heat-and-moisture adhesive resins can be used alone or in combination of two or more. Among these, in particular, α-C2- such as ethylene and propylene may be used. 10 A vinyl alcohol polymer containing an olefin unit, in particular an ethylene-vinyl alcohol copolymer, is preferred.

[0036] In the case of composite fibers, the heat-sensitive adhesive resins under moisture may be combined together, or may be combined with a non-heat-sensitive adhesive resin under moisture. Examples of the non-heat-sensitive adhesive resin under moisture include water-insoluble or hydrophobic resins, such as polyolefin resins, (meth)acrylic resins, polyvinyl chloride resins, polystyrene resins, polyester resins, polyamide resins, polycarbonate resins, polyurethane resins, and thermoplastic elastomers. These non-heat-sensitive adhesive resins under moisture may be used alone or in combination of two or more.

[0037] Of these non-moisture heat adhesive resins, from the standpoint of heat resistance and dimensional stability, resins having a higher melting point than the moisture heat adhesive resins (particularly ethylene-vinyl alcohol copolymers), such as polypropylene-based resins, polyester-based resins, and polyamide-based resins, are preferred, with polyester-based resins and polyamide-based resins being particularly preferred because of their excellent balance of heat resistance, fiber formability, etc. Examples of polyester resins include fiber-forming polyester resins made of aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, naphthalene-2,6-dicarboxylic acid, phthalic acid, α,β-(4-carbophenoxy)ethane, 4,4-dicarboxydiphenyl, and 5-sodium sulfoisophthalic acid, aliphatic dicarboxylic acids such as azelaic acid, adipic acid, and sebacic acid, and esters thereof, and diols such as ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexane-1,4-dimethanol, polyethylene glycol, and polytetramethylene glycol, and it is preferable that 80 mol % or more of the constituent units are ethylene terephthalate units. Examples of polyamide resins include aliphatic polyamides mainly composed of nylon 6, nylon 66, and nylon 12, and polyamides containing a small amount of a third component may also be used.

[0038] The cross-sectional shape of the heat-and-moisture adhesive fiber (cross-sectional shape perpendicular to the length direction of the fiber) is not limited to a typical solid cross-sectional shape such as a round cross-section or an irregular cross-section (flat, elliptical, polygonal, etc.), but may be a hollow cross-sectional shape. The heat-and-moisture adhesive fiber may be a composite fiber composed of a plurality of resins including at least a heat-and-moisture adhesive resin. The composite fiber may have the heat-and-moisture adhesive resin on at least a part of the fiber surface, but from the viewpoint of adhesiveness, it is preferable that the fiber surface has the heat-and-moisture adhesive resin continuous in the length direction.

[0039] Examples of the cross-sectional structure of the composite fiber in which the heat-and-moisture adhesive resin occupies the surface include a core-sheath type, an island-in-the-sea type, a side-by-side type, a multi-layered type, a radially-laminated type, and a random composite type. Among these cross-sectional structures, a core-sheath type structure in which the heat-and-moisture adhesive resin covers the entire surface of the fiber (i.e., a core-sheath type structure in which the sheath portion is composed of the heat-and-moisture adhesive resin) is preferred because it has high adhesiveness. The core-sheath type structure may be a fiber in which the surface of a fiber composed of another fiber-forming polymer is coated with a heat-and-moisture adhesive resin.

[0040] The nonwoven fiber structure may further contain non-heat-adhesive fibers in addition to the heat-adhesive fibers under moisture. Examples of the non-heat-adhesive fibers under moisture include fibers composed of the non-heat-adhesive resin constituting the composite fiber, as well as cellulosic fibers (e.g., rayon fibers, acetate fibers, etc.). These non-heat-adhesive fibers under moisture can be used alone or in combination of two or more. These non-heat-adhesive fibers under moisture can be used alone or in combination of two or more. These non-heat-adhesive fibers under moisture can be selected according to the desired properties, and when combined with semi-synthetic fibers such as rayon, a fiber structure with relatively high density and high mechanical properties can be obtained.

[0041] The ratio (mass ratio) of the heat adhesive fiber under moisture to the non-heat adhesive fiber under moisture is not particularly limited, but it is preferable that the heat adhesive fiber under moisture / non-heat adhesive fiber be 100 / 0 to 20 / 80, and more preferably 100 / 0 to 50 / 50.

[0042] A nonwoven fiber structure containing such heat-and-moisture adhesive fibers is commercially available from Kuraray Co., Ltd. under the name "Felibendy."

[0043] (Second buffer layer) The second buffer layer may have a compressive elastic modulus of 30 to 12,000 kPa, preferably 50 to 11,000 kPa, and more preferably 80 to 10,500 kPa when compressed from 2.5% to 5.0%. Note that the compressive elastic modulus when compressed from 2.5% to 5.0% refers to a numerical value measured as the elastic modulus when a test specimen cut into a disk shape having a diameter of 29 mm is compressed from a strain of 2.5% to 5.0% by a pressure plate at a test speed of 10 mm / min in accordance with JIS K 7181.

[0044] The second buffer layer's responsiveness to the strain received from the first buffer layer can be accurately evaluated by mainly measuring the compressive modulus at the beginning of compression. By disposing a second buffer layer having a slightly harder compressive modulus under a first buffer layer having a specific softer compressive modulus, it is surprisingly possible to greatly reduce the impact acceleration G value in the laminated state of the first buffer layer and the second buffer layer compared to conventional methods. This is an unexpected effect that could not be predicted, considering that the impact acceleration G values ​​of the first buffer layer and the second buffer layer are about the same as conventional impact acceleration G values.

[0045] Preferably, the compressive modulus of the second buffer layer when compressed from 2.5% to 5.0% may be 50 kPa or more higher than the compressive modulus of the first buffer layer when compressed from 10% to 20%, and more preferably 80 kPa or more higher.

[0046] The thickness of the second buffer layer may be, for example, 5 to 50 mm, preferably 7 to 45 mm, and more preferably 9 to 40 mm. Here, the thickness may be measured by a suitable method depending on the material, and for example, in the case of a nonwoven fiber structure, the thickness may be measured in accordance with JIS L 1913 "Testing method for general staple fiber nonwoven fabrics."

[0047] The thickness of the second buffer layer may be, for example, 0.8 times or more, preferably 0.8 to 6 times, and more preferably 0.8 to 5 times, the thickness of the first buffer layer.

[0048] In terms of receiving the pressure from the first buffer layer, the bending strength of the second buffer layer is, for example, 0.2 N / mm 2 or more, preferably 0.3 to 3 N / mm 2 Here, when the bending strength differs depending on the direction, the bending strength is the bending strength in the direction in which the bending strength is greater. The bending strength is a value measured by the method described in the examples described later.

[0049] As long as the second buffer layer exhibits such properties, various materials can be used for the second buffer layer, including natural fiber (preferably vegetable fiber) molded boards, synthetic fiber molded boards, inorganic fiber molded boards, and foamed plastic boards. Examples of natural fiber and synthetic fiber molded boards include medium density fiberboards (MDF), insulation fiberboards (particularly tatami boards as specified in JIS A 5905), palm boards, kenaf boards, and rice straw tatami mats. Examples of inorganic fiber molded boards include carbon fiber boards and glass fiber boards. Examples of foamed plastic boards include foamed rigid urethane boards, foamed polystyrene boards (particularly extrusion foamed polystyrene boards as specified in JIS A 9511), foamed polyolefin boards, and foamed phenolic resin boards. These materials may be used alone or in combination of two or more.

[0050] The second buffer layer can be suitably made of tatami board as specified in JIS A 5905. If necessary, extruded polystyrene foam as specified in JIS A 9511 or an equivalent or higher material can be used under the second buffer layer (e.g., tatami board).

[0051] (plate material) As for the plate material, various materials can be used as long as they are, unlike the buffer layer, materials that do not undergo local deformation in response to a localized impact, such as various natural boards, plywood, plant fiber molded boards, plastic boards, metal boards, ceramic boards, and composite boards.

[0052] From the viewpoint of suppressing local deformation of the plate material, the flexural modulus of the plate material may be, for example, 500 to 4000 MPa, and preferably 550 to 3000 MPa. The flexural modulus is a value measured at a test speed of 10 m / min and changed from 0.25% to 0.5% in accordance with the provisions of JIS K 7171. When the flexural modulus differs depending on the direction, the higher flexural modulus is adopted.

[0053] The thickness of the plate material is not particularly limited as long as it can suppress local deformation, but may be, for example, 3 to 15 mm, and preferably 4 to 13 mm. Furthermore, a cushioning material or a surface decorative material may be disposed on the plate material as necessary.

[0054] The cushioning material is thinner than the first buffer layer from the viewpoint of improving the cushioning property for the plate material while transmitting the impact to the plate material, i.e., mitigating the impact and improving the comfort of sitting, and the thickness of the cushioning material is preferably, for example, about 1 to 5 mm to obtain an appropriate cushioning property. The thickness of the cushioning material may be thicker than, the same as, or thinner than the thickness of the plate material, but is preferably thin.

[0055] The material constituting the cushioning material is not particularly limited as long as it is capable of exhibiting cushioning properties, and may be, for example, the material of the first buffer layer, a rubber or elastomer molded body, a fiber structure (a structure composed of a woven fabric, knitted fabric, nonwoven fabric, etc.), etc.

[0056] Surface decorative materials can be selected from materials used in floor construction materials according to the purpose, and examples include various tatami mat surfaces (rush tatami mat surfaces, resin tatami mat surfaces, Japanese paper tatami mat surfaces), soft floors, fabrics (woven fiber fabrics), cork boards, soft or hard plastic sheets, etc.

[0057] As for the finishing material, board materials and surface decorative materials may be used as they are, or when the surfaces of multiple floor components (or floor cushioning materials) are applied together, various materials used as finishing materials may be used. Examples of finishing materials include synthetic paints and natural paints for painted floors, polymer sheet materials, wood board materials, wood block materials, plastic tile materials, ceramic tile materials, natural stone materials, artificial stone materials, laminated floor materials, and the like for floor coverings, and carpet materials for floor coverings.

[0058] (Floor cushioning and floor construction materials) The floor cushioning material of the present invention has excellent impact resistance even when thin, and may have a thickness of, for example, 80 mm or less, preferably 60 mm or less, more preferably 45 mm or less. The lower limit of the thickness is not limited as long as it can exhibit impact resistance, but may be, for example, about 20 mm.

[0059] The floor component of the present invention is at least composed of a floor cushioning material and a board material, and a first cushioning layer is disposed on the underside of the board material, and since it has excellent impact resistance even if it is thin, it may have a thickness of, for example, 100 mm or less, preferably 80 mm or less, and more preferably 65 mm or less. The lower limit of the thickness is not limited as long as it can exhibit impact resistance, but may be, for example, about 40 mm.

[0060] In addition, the floor constituent material and floor cushioning material of the present invention may have an impact acceleration G value at the time of a fall collision, which is a numerical value indicating impact resistance, measured in accordance with the provisions of JIS A 5917 (2018), of 45 G or less, preferably 42 G or less, and more preferably 39 G or less. The lower limit of the G value is not particularly limited, but may be about 20 G, preferably about 25 G, and more preferably about 30 G.

[0061] In the case of floor components, the G value was measured directly. In the case of floor cushioning materials, a 5.5 mm thick plywood (flexural modulus: 5.5 × 10 3 The flexural modulus of plywood was measured by placing a test piece (width 10 mm, length 100 mm) on the board, with a support distance of 80 mm and a test speed of 10 mm / min, in accordance with JIS K 7171.

[0062] The floor component of the present invention can achieve performance that is neither too hard nor too soft, and therefore the value calculated in a hardness test during daily operations measured in accordance with the provisions of JIS A 5917 (2018) may be, for example, 0.6 to 2.0, preferably 0.6 to 1.5, more preferably 0.7 to 1.4, and even more preferably 0.8 to 1.3.

[0063] In the case of floor components, the hardness test values ​​during daily operation were measured directly. The values ​​that can be imparted by floor cushioning materials were measured by placing a 5.5 mm thick plywood board (flexural modulus: 5.5 × 10 3 The flexural modulus of plywood was measured by placing a test piece (width 30 mm, length 200 mm) on the board, with a support distance of 160 mm and a test speed of 10 mm / min, in accordance with JIS K 7171. The floor components thus obtained can be used to form floors for various buildings (e.g., homes, apartment buildings, stores, dormitories, offices, hotels, school buildings, auditoriums, research institutes, hospitals, clinics, assembly halls, public halls, stadiums, teahouses, etc.) according to their intended use as tatami floors, wood floors, polymer sheet floors, ceramic floors, carpet floors, etc. EXAMPLES

[0064] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Various characteristics of the present invention were evaluated by the following methods.

[0065] [Compressive modulus] In accordance with JISK7181, the first buffer layer was cut into a disk shape with a diameter of 29 mm, and the test speed was 10 mm / min. , based on the initial thickness of the first buffer layer, The value measured as the elastic modulus when compressed from 10% to 20% strain was evaluated as the compressive elastic modulus of the first buffer layer when compressed from 10% to 20%. In addition, in accordance with JISK7181, the second buffer layer was cut into a disk shape with a diameter of 29 mm, and the test speed was 10 mm / min. Based on the initial thickness of the second buffer layer, The value measured as the elastic modulus when compressed from a strain of 2.5% to 5.0% was evaluated as the compressive elastic modulus of the second buffer layer when compressed from 2.5% to 5.0%.

[0066] [Flexural modulus] This is the value measured as the modulus of elasticity when it changes from 0.25% to 0.5% at a test speed of 10 m / min in accordance with the provisions of JIS K 7171. When the flexural modulus of elasticity differs depending on the direction (e.g., MD direction, CD direction), the higher flexural modulus of elasticity was used.

[0067] [Thickness (mm), apparent density (kg / m 3 )] The basis weight (g / m2) of the nonwoven fiber structure was measured in accordance with 6.1 of JIS L 1913 "General nonwoven fabric test method". 2 ) was measured, and the thickness (mm) of the nonwoven fiber structure was measured in accordance with 6.2 of JIS L 1913 "General nonwoven fabric test method", and the apparent density (kg / m 3 ) was calculated.

[0068] [Flexural strength] In accordance with the provisions of JIS K 7171, the bending strength was measured by a three-point bending test method with a test piece width of 30 mm, a length of 200 mm, a support distance of 160 mm, and a test speed of 10 mm / min.

[0069] [G-value of impact acceleration during a fall collision] In accordance with JIS A 5917 (2018), a steel head (3.75 ± 0.10 kg) was dropped vertically from directly above the test specimen at a drop height of 200 ± 5 mm, and the maximum acceleration G value when it collided with the test specimen was measured and used as an index of hardness during a fall collision. If the test specimen is only a floor cushioning material, the test specimen should be one in which a second cushioning layer is placed under the first cushioning layer and 5.5 mm thick Chinese plywood (flexural modulus: 5545 MPa) is placed on the top of the first cushioning layer. The value obtained in this case is considered to be similar to the value obtained with the floor component of the example.

[0070] [Stiffness during everyday movements] In accordance with JIS A 5917 (2018), when a weight of 40 kg is applied to the test specimen from directly above via a loading plate, the deformation energy U F (N cm), recovery amount D R (cm), recovery time T R The hardness (s) was measured, and the value calculated using the following formula (1) defined in JIS A 5917 (2018) was used as the hardness during everyday movements. log(U F / 9.8-8D R D R T R -1 ) (1) If the floor cushioning material is used as the test specimen, the test specimen should be one in which the second cushioning layer is placed under the first cushioning layer, and 5.5 mm thick linden plywood (flexural modulus: 5545 MPa) is placed on the top of the first cushioning layer. The values ​​obtained in this case are considered to be comparable to those obtained with the floor construction material in the example.

[0071] [Example 1] The surface is made of rush grass tatami mats, and the cushioning material 5 is 2 mm thick and has a density of 10 kg / m 3 The nonwoven fiber structure (Kuraray Co., Ltd.'s "Felivendy" board type) was used, the board material 1 was a 7 mm thick "Galliana board" (flexural modulus: 700 MPa) manufactured by Koyo Sangyo Co., Ltd., and the first buffer layer 2 was a 12 mm thick board with an apparent density of 50 kg / m3 A nonwoven fiber structure containing the above heat-and-moisture adhesive fiber (Kuraray Co., Ltd.'s "Felibendy" board type) was used, and a 15 mm thick palm board (Azeas Co., Ltd.) was used as the second buffer layer 3, and these materials were bonded with an adhesive in the laminated state shown in Figure 3 to obtain a floor component (thin tatami mat). Table 1 shows the physical properties of the first and second buffer layers, as well as the G-value of the impact acceleration during a fall collision and the hardness during everyday operation of the obtained floor component.

[0072] [Example 2] A flooring material (thin tatami mat) was obtained in the same manner as in Example 1, except that a 30 mm thick palm board (manufactured by Azeas Corporation) was used as the second buffer layer 3. Table 1 shows the physical properties of the first and second buffer layers, as well as the G-value of the acceleration upon impact during a fall and the hardness during daily operation of the obtained flooring material.

[0073] [Example 3] A floor constituent material (thin tatami mat) was obtained in the same manner as in Example 1, except that a 10 mm thick kenaf board (manufactured by Yamanaka Sangyo Co., Ltd.) was used as the second buffer layer 3. Table 1 shows the physical properties of the first and second buffer layers, as well as the G-value of the acceleration upon impact during a fall collision and the hardness during everyday movement of the obtained floor constituent material.

[0074] [Example 4] A floor constituent material (thin tatami mat) was obtained in the same manner as in Example 1, except that a 20 mm-thick kenaf board (manufactured by Yamanaka Sangyo Co., Ltd.) was used as the second buffer layer 3. Table 1 shows the physical properties of the first and second buffer layers, as well as the G-value of the acceleration upon impact during a fall collision and the hardness during everyday movement of the obtained floor constituent material.

[0075] [Example 5] A floor constituent material (thin tatami mat) was obtained in the same manner as in Example 1, except that a 30 mm thick tatami board (manufactured by Daiken Corporation) was used as the second buffer layer 3. Table 1 shows the physical properties of the first and second buffer layers, as well as the G-value of the acceleration upon impact during a fall collision and the hardness during everyday movement of the obtained floor constituent material.

[0076] [Example 6] The first buffer layer 2 has a thickness of 8 mm and an apparent density of 50 kg / m 3 A floor constituent material (thin tatami mat) was obtained in the same manner as in Example 1, except that a nonwoven fiber structure containing the above-mentioned heat-and-moisture adhesive fiber ("Felivendy" board type manufactured by Kuraray Co., Ltd.) was used, and a 30 mm-thick tatami board (manufactured by Daiken Corporation) was used as the second buffer layer 3. The physical properties of the first and second buffer layers, and the G-value of the impact acceleration of the obtained floor constituent material during a tumble collision are shown in Table 1.

[0077] [Example 7] A flooring material (thin tatami mat) was obtained in the same manner as in Example 1, except that a 30 mm-thick extruded polystyrene foam board (manufactured by DuPont-Styro Corporation, "Styrofoam" (TM)) was used as the second buffer layer 3. Table 1 shows the physical properties of the first and second buffer layers, as well as the G-value of the acceleration upon impact during a fall collision and the hardness during everyday movement of the obtained flooring material.

[0078] [Comparative Example 1] A floor constituent material (thin tatami mat) was obtained in the same manner as in Example 1, except that the second buffer layer 3 was not provided. Table 1 shows the physical properties of the first buffer layer, and the G-value of the acceleration upon impact during a fall collision and the hardness during daily movement of the obtained floor constituent material.

[0079] [Comparative Examples 2 to 6] Table 1 shows the acceleration G values ​​at the time of impact during a fall collision measured for the second buffer layer 3 used in Examples 1 to 5.

[0080] [Comparative Example 7] Table 1 shows the impact acceleration G value during a fall collision measured for the second buffer layer 3 used in Example 7.

[0081] [Table 1]

[0082] As shown in Table 1, Comparative Example 1 has the same configuration as Example 1 except that the second buffer layer is not used, and the G value shown in the hardness test during a fall collision was 52 G. Comparative Example 2 uses only the second buffer layer used in Example 1, and the G value shown in the hardness test during a fall collision was 78 G. Example 1, despite being a combination of Comparative Examples 1 and 2, had a G value of 34 G, which was significantly lower than the G values ​​obtained in Comparative Examples 1 and 2.

[0083] Similarly, all of Examples 2 to 7 had G values ​​that were significantly lower than both the G value obtained in Comparative Example 1, which had the same configuration as Example 1 except that the second buffer layer was not used, and the G value of the second buffer layer used alone in each of the Examples, and all of them exhibited excellent impact resistance.

[0084] Furthermore, the hardness during everyday movements was in the range of 0.6 to 2.0 in all of the Examples, indicating a hardness that was neither too hard nor too soft. [Industrial Applicability]

[0085] The floor cushioning material of the present invention can impart good impact resistance to various floor constituent materials. For example, the floor constituent material can be usefully used not only as a floor covering (e.g., tatami flooring, tile carpet, etc.), but also as a stretched floor (e.g., wooden floors such as flooring, polymer sheet floors such as cushion flooring, tile floors such as various tiles, etc.), coated floors (e.g., wooden floors coated with synthetic paint or natural paint, etc.), etc.

[0086] As described above, the preferred embodiments of the present invention have been described. However, various additions, modifications, and omissions can be made without departing from the spirit of the present invention, and such additions, modifications, and omissions are also included within the scope of the present invention. [Explanation of symbols]

[0087] 1 plate material 2 First buffer layer 3 Second buffer layer 4 Surface cosmetic materials 5 Cushioning material 10 Floor cushioning material 20 Floor construction materials 30 Floor construction materials

Claims

1. A floor component comprising at least a floor cushioning material and a board material, The floor cushioning material is at least composed of a first cushioning layer and a second cushioning layer disposed below the first cushioning layer, and the first cushioning layer is disposed below the board material, The compressive elastic modulus of the first buffer layer when compressed from 10% to 20% is 0.01 to 29 kPa; The second buffer layer has a compressive elastic modulus of 30 to 12,000 kPa when compressed from 2.5% to 5.0%; and A floor construction material, wherein the flexural modulus of the plate material is 500 to 4000 MPa.

2. 2. The floor construction material according to claim 1, wherein the compressive modulus of the second buffer layer when compressed from 2.5% to 5.0% is 50 kPa or more higher than the compressive modulus of the first buffer layer when compressed from 10% to 20%.

3. 3. The floor component according to claim 1 or 2, wherein the second buffer layer has a bending strength of 0.2 N / mm 2 That's all for the floor components.

4. The floor component according to any one of claims 1 to 3, wherein the thickness of the first buffer layer is 20 mm or less, and the thickness of the second buffer layer is 0.8 times or more the thickness of the first buffer layer. Floor construction materials.

5. The floor component according to any one of claims 1 to 4, wherein the first buffer layer has an apparent density of 30 to 70 kg / m 3 A floor component which is a nonwoven fiber structure.

6. 6. The floor construction material according to any one of claims 1 to 5, wherein the first buffer layer and the second buffer layer can be integrated with each other by a connecting means.

7. The floor component according to any one of claims 1 to 6, wherein the impact acceleration G value during a fall collision measured in accordance with JIS A 5917 (2018) is 45 G or less.

8. A flooring material according to any one of claims 1 to 7, wherein the first buffer layer is a nonwoven fiber structure in which fibers are fixed to each other by fusion of the moist heat adhesive fiber.

9. The floor construction material according to any one of claims 1 to 8, wherein the second buffer layer is at least one selected from the group consisting of a natural fiber molded board, a synthetic fiber molded board, an inorganic fiber molded board, and a foamed plastic board. A floor construction material.

10. The floor component according to any one of claims 1 to 9, wherein the hardness during daily operation measured in accordance with JIS A 5917 (2018) is 0.6 to 2.

0.

11. 11. The floor construction material according to claim 1, having a thickness of 100 mm or less, and an impact acceleration G value measured in accordance with JIS A 6519 of 45 G or less.

12. The floor construction material according to any one of claims 1 to 11, which is a tatami floor, a wood floor, a polymer sheet floor, a ceramic floor, or a carpet floor.

13. A floor cushioning material used in the floor constituent material according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Impact relieving floor material

    JP2016216928A