Adhesive Film
The (meth)acrylic adhesive film with controlled molecular weight distribution and specific structural units addresses high-temperature adhesive strength and residue issues, providing reliable adhesion and easy peeling in QFN manufacturing.
Patent Information
- Application Number
- JP2020168971
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-06
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-10-06
AI Technical Summary
Existing adhesive films used in QFN manufacturing face issues such as increased adhesive strength and residue formation during high-temperature processes, and silicone-based films cause conductivity issues due to silicone migration.
A (meth)acrylic adhesive film with a base film and an adhesive layer formed by living radical polymerization, containing a (meth)acrylic copolymer with specific structural units and molecular weight distribution, which suppresses excessive adhesive strength and residue formation at high temperatures.
The adhesive film maintains high adhesive strength at high temperatures without excessive increase and minimizes residue, ensuring easy peeling and minimal contamination on adherends.
Smart Images

Figure 0007580234000001 
Figure 0007580234000002 
Figure 0007580234000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive film, and more particularly to an adhesive film having an adhesive layer with excellent heat resistance. [Background technology]
[0002] In recent years, CSP (Chip Size / Scale Package) technology has been attracting attention as a mounting technology for LSI (Large Scale Integration). Among these technologies, packages with lead terminals incorporated inside the package, such as QFN (Quad Flat Non-leaded package), are attracting particular attention in terms of miniaturization and high integration.
[0003] The manufacturing process for such QFNs consists of the steps of attaching an adhesive film to one side of the lead frame, a die bonding process to attach a semiconductor element to the die pad of the lead frame, a wire bonding process to connect the semiconductor element and the lead frame, a molding process to encapsulate and protect the semiconductor element and the die pad of the lead frame with molding resin, a process to peel the adhesive film from the encapsulated lead frame, and a dicing process to cut the lead frame to separate the packages.
[0004] Here, the lead frame and the like are exposed to high temperatures of about 180°C to 250°C in the die bonding and wire bonding processes, and about 160°C to 240°C in the molding process. Therefore, the adhesive film used in the manufacture of QFNs is required to have no increase in adhesive strength after exposure to high temperatures, to be peelable with light force, and to leave no adhesive residue. Furthermore, the adhesive film is also required not to peel off during processes where it is exposed to high temperatures.
[0005] Known examples of the pressure-sensitive adhesive film include silicone-based pressure-sensitive adhesive films in which a silicone-based resin is used in the pressure-sensitive adhesive layer, and (meth)acrylic-based pressure-sensitive adhesive films in which a (meth)acrylic resin is used in the pressure-sensitive adhesive layer.
[0006] For the (meth)acrylic resin, a polymer obtained by polymerizing a radically polymerizable monomer such as a (meth)acrylic monomer is used. As a type of radical polymerization, free radical polymerization is generally used. However, free radical polymerization cannot fully control the molecular weight, molecular weight distribution, copolymer composition, etc., and low molecular weight components are generated, or even in the case of copolymerization, homopolymers are generated, and these components have the disadvantage of causing a decrease in the heat resistance and cohesive strength of the adhesive film, making the adhesive film more likely to peel off, etc. In contrast, the living radical polymerization method makes it easy to control the molecular weight, molecular weight distribution, copolymer composition, etc., and can suppress the generation of low molecular weight components and the generation of homopolymers that are generated without copolymerization.
[0007] Therefore, Patent Document 1 describes the preparation of a copolymer by copolymerizing radically polymerizable monomers by a living radical polymerization method using an organic tellurium compound as a chain transfer agent, and the use of the obtained copolymer as an adhesive (see Patent Document 1 (Claim 1)). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 5256515 Summary of the Invention [Problem to be solved by the invention]
[0009] Silicone-based adhesive films have a problem in that silicone compounds such as low molecular weight silicone resins and silicone oils in the adhesive layer migrate to the adherend, causing poor electrical continuity. In addition, (meth)acrylic adhesive films are not contaminated by silicone, but have problems such as being easily peeled off when exposed to high temperatures.
[0010] The present invention has been made in consideration of the above circumstances, and aims to provide a (meth)acrylic adhesive film that has high adhesive strength even at high temperatures, does not increase its adhesive strength excessively even when exposed to high temperatures, and does not leave adhesive residue even after exposure to high temperatures. [Means for solving the problem]
[0011] The adhesive film of the present invention, which has been able to solve the above-mentioned problems, comprises a base film and an adhesive layer formed on at least one surface of the base film, the adhesive layer being formed from an adhesive composition containing a (meth)acrylic copolymer obtained by living radical polymerization, the (meth)acrylic copolymer comprising a structural unit (a-1) having a cyclic ether group and a structural unit (a-2) having an acidic group, a molecular weight distribution (Mw / Mn) of 3.0 or less, and a gel fraction of the adhesive layer of 30 mass% or more.
[0012] By making the molecular weight distribution of the (meth)acrylic copolymer 3.0 or less, the adhesive strength at high temperatures can be increased. In addition, by making the gel fraction of the adhesive layer 30% by mass or more, the adhesive strength at high temperatures can be increased, and adhesive residue after exposure to high temperatures can be further suppressed. Furthermore, since the (meth)acrylic copolymer has a cyclic ether group and an acidic group, some of the cyclic ether group and acidic group remain even after the adhesive layer is formed. Therefore, when exposed to high temperatures, the remaining cyclic ether group and acidic group react, and the adhesive strength is prevented from increasing excessively when exposed to high temperatures, and adhesive residue after exposure to high temperatures can be further suppressed. Effect of the Invention
[0013] According to the present invention, a (meth)acrylic adhesive film can be obtained which has high adhesive strength even at high temperatures, does not increase excessively in adhesive strength even when exposed to high temperatures, and does not leave adhesive residue even after exposure to high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] <Adhesive film> The pressure-sensitive adhesive film of the present invention has a base film and a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition on at least one surface of the base film. The pressure-sensitive adhesive layer is formed on at least one surface or at least a part of the base film. The pressure-sensitive adhesive layer may be a single layer or a multilayer structure.
[0015] Generally, a "sheet" is defined in JIS as a thin, flat product whose thickness is generally small relative to its length and width, and a "film" is generally a thin, flat product whose thickness is extremely small compared to its length and width, and whose maximum thickness is arbitrarily limited, and which is usually supplied in the form of a roll (Japanese Industrial Standard JIS K6900). For example, in terms of thickness, in the narrow sense, a product with a thickness of 100 μm or more is called a sheet, and a product with a thickness of less than 100 μm is sometimes called a film. However, the boundary between a sheet and a film is unclear, and since there is no need to distinguish between the two in the present invention, in the present invention, when a product is called a "sheet," it is also considered to include a "film," and when a product is called a "film," it is also considered to include a "sheet."
[0016] Each of the components constituting the pressure-sensitive adhesive film of the present invention will be described below.
[0017] (1. Pressure-sensitive adhesive composition) The pressure-sensitive adhesive composition contains a (meth)acrylic copolymer (A) (hereinafter, may be simply referred to as "copolymer (A)"). The copolymer (A) contains a structural unit (a-1) having a cyclic ether group and a structural unit (a-2) having an acidic group, and has a molecular weight distribution (PDI) of 3.0 or less. The pressure-sensitive adhesive composition can form a pressure-sensitive adhesive layer by applying the pressure-sensitive adhesive composition onto a substrate film and reacting the acidic group of the copolymer (A) with the cyclic ether group of the copolymer (A) (or a functional group of a crosslinking agent described below).
[0018] (1-1. (Meth)acrylic copolymer (A)) The copolymer (A) is a (meth)acrylic copolymer having a molecular weight distribution (PDI) of 3.0 or less, and containing a structural unit (a-1) having a cyclic ether group and a structural unit (a-2) having an acidic group.
[0019] The (meth)acrylic copolymer may be any copolymer that contains structural units derived from (meth)acrylic monomers as the main component (50% by mass or more), and may contain structural units derived from vinyl monomers other than (meth)acrylic monomers. The content of structural units derived from (meth)acrylic monomers in the copolymer (A) is preferably 80% by mass or more, more preferably 90% by mass or more, based on the entire copolymer (A). The copolymer (A) may be composed only of structural units derived from (meth)acrylic monomers.
[0020] In the present invention, "(meth)acrylic" refers to "at least one of acrylic and methacrylic". "(meth)acrylic monomer" refers to a monomer having "(meth)acryloyl group" in the molecule. "(meth)acryloyl" refers to "at least one of acryloyl and methacryloyl". "Vinyl monomer" refers to a monomer having a radically polymerizable carbon-carbon double bond in the molecule. "Structural unit derived from (meth)acrylic monomer" refers to a structural unit in which the radically polymerizable carbon-carbon double bond of the (meth)acrylic monomer is polymerized to a carbon-carbon single bond. "Structural unit derived from vinyl monomer" refers to a structural unit in which the radically polymerizable carbon-carbon double bond of the vinyl monomer is polymerized to a carbon-carbon single bond.
[0021] The copolymer (A) may be any one of a random copolymer, a block copolymer, and a graft copolymer, and is preferably a random copolymer.
[0022] The molecular weight distribution (PDI) of the copolymer (A) is 3.0 or less, preferably 2.5 or less, more preferably 2.0 or less. The smaller the PDI, the narrower the molecular weight distribution width, and the copolymer has a uniform molecular weight, and when the value is 1.0, the molecular weight distribution width is the narrowest. That is, the lower limit of the PDI is 1.0. If the PDI is 3.0 or less, the content of the small molecular weight and the large molecular weight is low compared to the molecular weight of the designed copolymer, and when used in a pressure-sensitive adhesive composition, a pressure-sensitive adhesive film with low adherend contamination and high cohesive strength can be obtained. In the present invention, the molecular weight distribution (PDI) is a value calculated by (weight average molecular weight (Mw)) / (number average molecular weight (Mn)), and the measurement method of Mw and Mn will be described later.
[0023] The weight average molecular weight (Mw) of the copolymer (A) is preferably 200,000 or more, more preferably 300,000 or more, even more preferably 400,000 or more, particularly preferably 500,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. If the Mw of the copolymer (A) is 200,000 or more, the cohesive strength is high, the heat resistance is further improved, and contamination of the adherend surface is further reduced, and if it is 2,000,000 or less, the coating workability of the pressure-sensitive adhesive composition is good.
[0024] The content of the cyclic ether group in the copolymer (A) is preferably 0.03 mmol / g or more, more preferably 0.07 mmol / g or more, even more preferably 0.10 mmol / g or more, and is preferably 1.1 mmol / g or less, more preferably 0.80 mmol / g or less, even more preferably 0.60 mmol / g or less. If the content of the cyclic ether group is 0.03 mmol / g or more, the cohesive failure of the adhesive is further suppressed, and if it is 1.1 mmol / g or less, the reaction with the acidic group during synthesis and gelation are suppressed, and the storage stability is also good. The content of the cyclic ether group is the sum of all the cyclic ether groups in the copolymer (A) and the total number of moles of the cyclic ether group per unit g of the copolymer (A).
[0025] The copolymer (A) preferably has an acidic group content of 0.10 mmol / g or more, more preferably 0.20 mmol / g or more, even more preferably 0.25 mmol / g or more, and preferably 2.1 mmol / g or less, more preferably 1.8 mmol / g or less, even more preferably 1.4 mmol / g or less. If the acidic group content is 0.10 mmol / g or more, the cohesive failure of the adhesive is further suppressed, and if it is 2.1 mmol / g or less, the reaction with the cyclic ether group during synthesis to cause gelation is suppressed, and the storage stability is also good. The acidic group content is the sum of all acidic groups contained in the copolymer (A) and the total number of moles of acidic groups per unit g of the copolymer (A).
[0026] The molar ratio of the cyclic ether group to the acidic group in the copolymer (A) (cyclic ether group / acidic group) is preferably 0.01 or more, more preferably 0.03 or more, even more preferably 0.06 or more, and is preferably 1.0 or less, more preferably 0.95 or less, even more preferably 0.90 or less. If the molar ratio is 0.01 or more, cohesive failure of the pressure-sensitive adhesive can be suppressed, and if it is 1.0 or less, crosslinking failure can be suppressed.
[0027] (1-1-1. Structural unit (a-1)) The structural unit (a-1) is not particularly limited as long as it has a cyclic ether group. The structural unit (a-1) may be one type or two or more types. By having the structural unit (a-1), it is possible to react with the structural unit (a-2) having an acidic group and to perform self-crosslinking. The structural unit (a-1) having a cyclic ether group preferably does not have an acidic group described later.
[0028] The cyclic ether group may be contained in either a structural unit derived from a (meth)acrylic monomer or a structural unit derived from a vinyl monomer other than a (meth)acrylic monomer. The cyclic ether group is not particularly limited as long as it is a cyclic structure containing an ether bond, but is preferably an epoxy group or an oxetane group from the viewpoint of reactivity, and more preferably an epoxy group. In this specification, the epoxy group is not limited to a group consisting of only an epoxy group, but also includes an alicyclic group having an oxacyclopropane structure, which is a three-membered ring ether, that is, a group having an alicyclic group and an oxacyclopropane structure.
[0029] The structural unit (a-1) is preferably a structural unit represented by formula (1).
[0030] [ka] [In formula (1), R 11 R represents an alkylene group or an arylene group which may have a substituent. 12 represents a hydrogen atom or a methyl group.
[0031] R 11 The alkylene group represented by the formula (I) which may have a substituent may be either linear or branched, but is preferably linear. 11 The number of carbon atoms in the alkylene group which may have a substituent, represented by the following formula (I) is preferably 1 to 10, more preferably 1 to 5, and further preferably 1 to 3. Specific examples of the alkylene group which may have a substituent include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, and a 1-methylethylene group.
[0032] R 11 The number of carbon atoms in the arylene group which may have a substituent and is represented by the following formula (I) is preferably 6 to 14, and more preferably 6 to 10. Specific examples of the arylene group which may have a substituent include a phenylene group and a naphthylene group.
[0033] R 11 Examples of the substituent that the alkylene group and arylene group, which may have the substituent represented by the formula (I), have include a linear or branched alkyl group, a cyclic alkyl group such as a cyclohexyl group, an aromatic group, a halogen atom, a hydroxy group, an alkoxy group, an amino group, a nitro group, and a cyano group.
[0034] The monomers that form the structural unit (a-1) are a (meth)acrylic monomer having a cyclic ether group, and a vinyl monomer other than a (meth)acrylic monomer having a cyclic ether group.
[0035] Examples of the (meth)acrylic monomer having a cyclic ether group include glycidyl (meth)acrylate, 2-epoxyethyl (meth)acrylate, 3-epoxypropyl (meth)acrylate, 4-epoxybutyl (meth)acrylate, 5-epoxypentyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 3,4-epoxycyclohexylethyl (meth)acrylate.
[0036] Examples of vinyl monomers having a cyclic ether group other than (meth)acrylic monomers include vinyl glycidyl ether, 4-vinylphenethyl glycidyl ether, allyl glycidyl ether, 4-vinylbenzyl glycidyl ether, 1-vinyl-3,4-epoxycyclohexane, and 3,4-epoxy-1-butene.
[0037] The content of the structural unit (a-1) is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, even more preferably 1.5% by mass or more, particularly preferably 1.9% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 8.0% by mass or less, in the total 100% by mass of the (meth)acrylic copolymer (A). By setting the content of the structural unit (a-1) within the above range, gelation due to reaction with acidic groups during synthesis is suppressed, and storage stability is also improved.
[0038] (1-1-2. Structural unit (a-2)) The structural unit (a-2) having an acidic group may be one type or may have two or more types. The acidic group is a functional group (reactive functional group) that can react with the cyclic ether group of the structural unit (a-1). The acidic group may be, for example, at least one selected from the group consisting of a carboxy group, a sulfonic acid group, a phosphoric acid group, a phosphonic acid group, and a phosphinic acid group, and is preferably a carboxy group. The structural unit (a-2) having an acidic group does not include the structural unit (a-1) having the cyclic ether group.
[0039] The acidic group may be contained in either a structural unit derived from a (meth)acrylic monomer or a structural unit derived from a vinyl monomer other than a (meth)acrylic monomer. The monomer forming the structural unit (a-2) is a (meth)acrylic monomer having an acidic group, or a vinyl monomer having an acidic group other than a (meth)acrylic monomer.
[0040] Examples of the (meth)acrylic monomer having an acidic group include a (meth)acrylic monomer having a carboxy group, a (meth)acrylic monomer having a sulfonic acid group, a (meth)acrylic monomer having a phosphoric acid group, a (meth)acrylic monomer having a phosphonic acid group, and a (meth)acrylic monomer having a phosphinic acid group. Examples of the vinyl monomer other than the (meth)acrylic monomer having an acidic group include a vinyl monomer having a carboxy group. Among these, a (meth)acrylic monomer having a carboxy group is preferred.
[0041] Examples of the (meth)acrylic monomer having a carboxy group include monomers obtained by reacting (meth)acrylates having a hydroxy group, such as 2-(meth)acryloyloxyethyl succinate and 2-(meth)acryloyloxyethyl maleate, with acid anhydrides, such as maleic anhydride and succinic anhydride, (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, etc. Among these, (meth)acrylic acid is preferred.
[0042] Examples of the (meth)acrylic monomer having a sulfonic acid group include ethyl sulfonate (meth)acrylate.
[0043] Examples of the (meth)acrylic monomer having a phosphoric acid group include 2-(phosphonooxy)ethyl (meth)acrylate.
[0044] An example of a (meth)acrylic monomer having a phosphonic acid group is 3-(meth)acryloyloxypropylphosphonic acid.
[0045] An example of a (meth)acrylic monomer having a phosphinic acid group is 3-(meth)acryloyloxypropylphosphinic acid.
[0046] Examples of vinyl monomers having a carboxy group include crotonic acid, maleic acid, itaconic acid, citraconic acid, and cinnamic acid.
[0047] The content of the structural unit (a-2) is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, even more preferably 3.0% by mass or more, and is preferably 15% by mass or less, more preferably 12.5% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the entire (meth)acrylic copolymer (A). If the content of the structural unit (a-2) is 1.0% by mass or more, cohesive failure of the adhesive is suppressed, and if it is 15% by mass or less, reaction with epoxy groups during synthesis to cause gelation is suppressed, and storage stability is also improved.
[0048] The mass ratio ((a-1) / (a-2)) of the structural unit (a-1) to the structural unit (a-2) in the (meth)acrylic copolymer (A) is preferably 0.03 or more, more preferably 0.05 or more, even more preferably 0.10 or more, and is preferably 1.0 or less, more preferably 0.95 or less, even more preferably 0.90 or less. If the mass ratio ((a-1) / (a-2)) is 0.03 or more, cohesive failure of the pressure-sensitive adhesive can be suppressed, and if it is 1.0 or less, crosslinking failure can be suppressed.
[0049] (1-1-3. Structural unit (a-3)) The (meth)acrylic copolymer (A) preferably contains a structural unit (a-3) represented by formula (2).
[0050] [ka] [In formula (2), R 21 R represents a chain or cyclic hydrocarbon group which may have a substituent. 22 represents a hydrogen atom or a methyl group.
[0051] R 21 Examples of the chain-like hydrocarbon group represented by the formula (I) include linear alkyl groups and branched alkyl groups. The linear alkyl group preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably 1 to 5 carbon atoms. Examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-hexyl, n-octyl, n-nonyl, n-decyl, and n-lauryl. The branched alkyl group preferably has 3 to 20 carbon atoms, more preferably 3 to 10 carbon atoms, and even more preferably 3 to 5 carbon atoms. Examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, 2-ethylhexyl, neopentyl, and isooctyl.
[0052] R 21Examples of the substituent that the chain hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a benzoyl group (-COC6H5), and a hydroxy group.
[0053] R 21 Examples of the cyclic hydrocarbon group represented by the formula (I) include a cyclic alkyl group and an aromatic group, and the cyclic alkyl group and the aromatic group may have a chain portion. The number of carbon atoms of the cyclic alkyl group is preferably 4 to 18, more preferably 6 to 12, and even more preferably 6 to 10. Examples of the cyclic alkyl group include a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. The number of carbon atoms of the aromatic group is preferably 6 to 18, more preferably 6 to 12, and even more preferably 6 to 8. Examples of the aromatic group include a phenyl group, a tolyl group, a xylyl group, and a mesityl group. Examples of the cyclic alkyl group having a chain portion and the chain portion of the aromatic group having a chain portion include an alkylene group having 1 to 12 carbon atoms, preferably an alkylene group having 1 to 6 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms.
[0054] R 21 Examples of the substituent that the cyclic hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a chain alkyl group, and a hydroxy group.
[0055] Examples of vinyl monomers capable of forming the structural unit (a-3) include (meth)acrylic monomers such as (meth)acrylates having a linear alkyl group, (meth)acrylates having a branched alkyl group, (meth)acrylates having an aromatic group, and (meth)acrylates having an alicyclic hydrocarbon group.
[0056] Specific examples of (meth)acrylates having a linear alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, decyl (meth)acrylate, n-lauryl (meth)acrylate, and n-stearyl (meth)acrylate.
[0057] Specific examples of (meth)acrylates having a branched alkyl group include isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, and isodecyl (meth)acrylate.
[0058] Examples of the (meth)acrylate having an aromatic group include phenyl (meth)acrylate, tribromophenyl (meth)acrylate, and benzyl (meth)acrylate.
[0059] Examples of the (meth)acrylate having an alicyclic hydrocarbon group include (meth)acrylates having a cyclic alkyl group and (meth)acrylates having a polycyclic structure.
[0060] Examples of (meth)acrylates having a cyclic alkyl group include compounds in which a cyclic alkyl group is directly bonded to a (meth)acryloyloxy group.Specific examples of (meth)acrylates having a cyclic alkyl group with a monocyclic structure include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, hexahydrophthalic acid ethyl (meth)acrylate, and hexahydrophthalic acid propyl (meth)acrylate.
[0061] Examples of the (meth)acrylate having a polycyclic structure include a compound in which a cyclic alkyl group having a bridged ring structure is directly bonded to a (meth)acryloyloxy group. Specific examples of (meth)acrylates having a polycyclic structure include bornyl (meth)acrylate, isobornyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, 2-(meth)acryloyloxy-2-(1-adamantyl)propane, 2-(meth)acryloyloxy-2-(1-adamantyl)butane, 3-(meth)acryloyloxy-3-(1-adamantyl)pentane, and tricyclodecanyl (meth)acrylate.
[0062] The content of the structural unit (a-3) is preferably 70% by mass or more and 98.5% by mass or less in 100% by mass of the entire (meth)acrylic copolymer (A).
[0063] In addition, the structural unit (a-3) preferably has a structure derived from at least one (meth)acrylate selected from the group consisting of (meth)acrylates having a linear alkyl group and (meth)acrylates having a branched alkyl group. In this case, the content of the structural unit derived from at least one (meth)acrylate selected from the group consisting of (meth)acrylates having a linear alkyl group and (meth)acrylates having a branched alkyl group is preferably 70% by mass or more and 98.5% by mass or less in 100% by mass of the entire copolymer (A).
[0064] (1-1-4. Structural unit (a-4)) The (meth)acrylic copolymer (A) may have other structural units in addition to the structural units (a-1), (a-2) and (a-3). The other structural units are not particularly limited as long as they are formed from a vinyl monomer capable of copolymerizing with both the vinyl monomers forming the structural units (a-1), (a-2) and (a-3), and may have only one type or two or more types.
[0065] In 100% by mass of the entire copolymer (A), the total content of the structural units (a-1), (a-2) and (a-3) is preferably 71.5% by mass or more, more preferably 73.0% by mass or more, even more preferably 74.5% by mass or more, and particularly preferably 74.9% by mass or more, with the upper limit being 100% by mass.
[0066] Examples of vinyl monomers capable of forming other structural units include (meth)acrylic monomers such as (meth)acrylates having a polyoxyalkylene alkyl ether group, (meth)acrylates having an alkoxy group, (meth)acrylates having an oxygen-containing heterocyclic group, (meth)acrylates having a tertiary amino group, and (meth)acrylamides; vinyl monomers other than (meth)acrylic monomers such as vinyl monomers having a heterocyclic ring, vinyl carboxylates, vinyl monomers having a tertiary amino group, vinyl monomers having a quaternary ammonium base, vinylamides, α-olefins, and dienes.
[0067] Examples of the (meth)acrylate having a polyoxyalkylene alkyl ether group include (meth)acrylates having a polyoxyethylene alkyl ether group, such as polyethylene glycol (degree of polymerization = 2 to 10) methyl ether (meth)acrylate, polyethylene glycol (degree of polymerization = 2 to 10) ethyl ether (meth)acrylate, and polyethylene glycol (degree of polymerization = 2 to 10) propyl ether (meth)acrylate; and (meth)acrylates having a polyoxypropylene alkyl ether group, such as polypropylene glycol (degree of polymerization = 2 to 10) methyl ether (meth)acrylate, polypropylene glycol (degree of polymerization = 2 to 10) ethyl ether (meth)acrylate, and polypropylene glycol (degree of polymerization = 2 to 10) propyl ether (meth)acrylate.
[0068] Examples of the (meth)acrylate having an alkoxy group include methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate.
[0069] The (meth)acrylate having an oxygen-containing heterocyclic group is preferably a (meth)acrylate having a 4- to 6-membered oxygen-containing heterocyclic group. Specific examples of the (meth)acrylate having an oxygen-containing heterocyclic group include tetrahydrofurfuryl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, 2-[(2-tetrahydropyranyl)oxy]ethyl (meth)acrylate, and 1,3-dioxane-(meth)acrylate.
[0070] Examples of the (meth)acrylate having a tertiary amino group include 2-(dimethylamino)ethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate.
[0071] Examples of (meth)acrylamides include dialkyl (meth)acrylamides such as N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, and N,N-diisopropyl (meth)acrylamide; cyclic amides such as N-(meth)acryloylmorpholine; and alkoxyalkyl acrylamides such as N-methoxymethyl acrylamide and N-ethoxymethyl acrylamide.
[0072] Examples of vinyl monomers having a hetero ring include 2-vinylthiophene, N-methyl-2-vinylpyrrole, 2-vinylpyridine, 4-vinylpyridine, N-phenylmaleimide, N-benzylmaleimide, and N-cyclohexylmaleimide. Examples of the vinyl carboxylate include vinyl acetate, vinyl pivalate, and vinyl benzoate. An example of a vinyl monomer having a tertiary amino group is N,N-dimethylallylamine. Examples of vinyl monomers having a quaternary ammonium base include N-methacryloylaminoethyl-N,N,N-dimethylbenzyl ammonium chloride. Examples of the vinyl amides include N-vinylformamide, N-vinylacetamide, 1-vinyl-2-pyrrolidone, and N-vinyl-ε-caprolactam. Examples of the α-olefin include 1-hexene, 1-octene, and 1-decene. Examples of dienes include butadiene, isoprene, 4-methyl-1,4-hexadiene, and 7-methyl-1,6-octadiene.
[0073] (1-1-5. Production method of (meth)acrylic acid-based copolymer (A)) The copolymer (A) can be produced by radical polymerization of a monomer composition containing two or more kinds of vinyl monomers, and is preferably obtained by living radical polymerization (obtained by polymerization using a living radical polymerization method).
[0074] In conventional radical polymerization methods (free radical polymerization methods), not only initiation reactions and propagation reactions, but also termination reactions and chain transfer reactions cause deactivation of the growth ends, and the method tends to produce a mixture of polymers with various molecular weights and non-uniform compositions. The living radical polymerization method maintains the simplicity and versatility of conventional radical polymerization methods, while being less susceptible to termination reactions and chain transfer, and allows growth without being hindered by side reactions that deactivate the growth ends, making it easy to precisely control the molecular weight distribution and produce polymers with uniform composition despite their high molecular weight.
[0075] Therefore, it is considered that the copolymer produced by the living radical polymerization method has an advantage that it has few low molecular weight components (oligomers) and causes little transfer contamination (such as adhesive residue) when used in a pressure-sensitive adhesive composition. In addition, by producing the copolymer (A) by the living radical polymerization method, the structural units ((a-1) to (a-3), etc.) are more uniformly polymerized in each polymer molecule, and the pressure-sensitive adhesive composition using the copolymer (A) has sufficient initial adhesive strength, can suppress peeling when heated, and also suppresses an increase in adhesive strength after heating.
[0076] In the living radical polymerization method, a random copolymer can be obtained by using a mixture (sometimes simply referred to as "vinyl monomers") of a vinyl monomer that forms the structural unit (a-1), a vinyl monomer that forms the structural unit (a-2), and, if necessary, a vinyl monomer that forms the structural unit (a-3), etc.
[0077] Living radical polymerization methods include a method using a transition metal catalyst (ATRP method), a method using a sulfur-based reversible chain transfer agent (RAFT method), and a method using an organic tellurium compound (TERP method), depending on the difference in the method for stabilizing the polymer growth end. Since the ATRP method uses an amine-based complex, it may not be possible to use a vinyl monomer having an acidic group without protecting the acidic group. When using a wide variety of vinyl monomers, the RAFT method may be difficult to achieve a low molecular weight distribution and may have problems such as a sulfur odor or coloring. Among these methods, the TERP method is preferably used from the viewpoints of the diversity of vinyl monomers that can be used, molecular weight control in the polymer region, uniform composition, or coloring.
[0078] The TERP method is a method in which an organic tellurium compound is used as a chain transfer agent to polymerize a radically polymerizable compound (vinyl monomer), and is a method described, for example, in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870.
[0079] Specific polymerization methods of the TERP method include the following (a) to (d). (a) A method of polymerizing a vinyl monomer using an organotellurium compound represented by the general formula (3): (b) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by the general formula (3) and an azo-based polymerization initiator. (c) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by general formula (3) and an organic ditelluride compound represented by general formula (4). (d) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by general formula (3), an azo-based polymerization initiator, and an organic ditelluride compound represented by general formula (4).
[0080] [ka] [In formula (3), R 31R represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group. 32 and R 33 R each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. 34 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, a substituted aryl group, an aromatic heterocyclic group, an alkoxy group, an acyl group, an amido group, an oxycarbonyl group, a cyano group, an allyl group, or a propargyl group. In formula (4), R 31 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group.]
[0081] R 31 The group represented by the following formula (1) is an alkyl group, an aryl group or an aromatic heterocyclic group having 1 to 8 carbon atoms, and specifically is as follows. Examples of the alkyl group having 1 to 8 carbon atoms include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, and octyl groups, and cyclic alkyl groups such as cyclohexyl groups. A linear or branched alkyl group having 1 to 4 carbon atoms is preferred, and a methyl or ethyl group is more preferred. Examples of the aryl group include a phenyl group and a naphthyl group. Examples of the aromatic heterocyclic group include a pyridyl group, a furyl group, and a thienyl group.
[0082] R 32 and R 33 The groups represented by the following formulae are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, and specific examples of each group are as follows. Examples of the alkyl group having 1 to 8 carbon atoms include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, and octyl groups, and cyclic alkyl groups such as cyclohexyl groups. A linear or branched alkyl group having 1 to 4 carbon atoms is preferred, and a methyl or ethyl group is more preferred.
[0083] R 34 The group represented by the formula (I) is an alkyl group having 1 to 8 carbon atoms, an aryl group, a substituted aryl group, an aromatic heterocyclic group, an alkoxy group, an acyl group, an amido group, an oxycarbonyl group, a cyano group, an allyl group, or a propargyl group, and specifically is as follows: Examples of the alkyl group having 1 to 8 carbon atoms include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, and octyl, and cyclic alkyl groups such as cyclohexyl. A linear or branched alkyl group having 1 to 4 carbon atoms is preferred, and a methyl or ethyl group is more preferred. Examples of the aryl group include a phenyl group and a naphthyl group, with a phenyl group being preferred. Examples of the substituted aryl group include a phenyl group having a substituent, a naphthyl group having a substituent, etc. Examples of the substituent of the aryl group having a substituent include a halogen atom, a hydroxyl group, an alkoxy group, an amino group, a nitro group, a cyano group, -COR 41 A carbonyl-containing group (R 41 Examples of the substituent include an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group or an aryloxy group having 1 to 8 carbon atoms, a sulfonyl group, a trifluoromethyl group, etc. It is preferable that one or two of these substituents are substituted. Examples of the aromatic heterocyclic group include a pyridyl group, a furyl group, and a thienyl group. The alkoxy group is preferably a group in which an alkyl group having 1 to 8 carbon atoms is bonded to an oxygen atom, and examples thereof include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, and an octyloxy group. Examples of the acyl group include an acetyl group, a propionyl group, and a benzoyl group. The amide group is -CONR 421 R 422 (R 421 , R 422 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an aryl group). The oxycarbonyl group is -COOR 43 (R 43 is preferably a group represented by (wherein is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an aryl group), and examples thereof include a carboxy group, a methoxycarbonyl group, an ethoxycarbonyl group, a propoxycarbonyl group, an n-butoxycarbonyl group, a sec-butoxycarbonyl group, a tert-butoxycarbonyl group, an n-pentyloxycarbonyl group, a phenoxycarbonyl group, etc. Preferred oxycarbonyl groups include a methoxycarbonyl group and an ethoxycarbonyl group. The allyl group is -CR 441 R 442 -CR 443 =CR 444 R 445 (R 441 , R 442 each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 443 , R 444 , R 445 are each independently a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an aryl group, and each of the substituents may be connected to form a cyclic structure). The propargyl group is -CR 451 R 452 -C≡CR 453 (R 451 , R 452is a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 453 can be a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, or a silyl group).
[0084] Specific examples of the organotellurium compound represented by formula (3) include (methyltellanylmethyl)benzene, (methyltellanylmethyl)naphthalene, ethyl-2-methyl-2-methyltellanyl-propionate, ethyl-2-methyl-2-n-butyltellanyl-propionate, (2-trimethylsiloxyethyl)-2-methyl-2-methyltellanyl-propionate, (2-hydroxyethyl)-2-methyl-2-methyltellanyl-propionate, and (3-trimethylsilylpropargyl)-2-methyl-2-methyltellanyl-propionate, and all of the organotellurium compounds described in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870.
[0085] Specific examples of the organic ditelluride compound represented by formula (4) include dimethyl ditelluride, diethyl ditelluride, di-n-propyl ditelluride, diisopropyl ditelluride, dicyclopropyl ditelluride, di-n-butyl ditelluride, di-s-butyl ditelluride, di-t-butyl ditelluride, dicyclobutyl ditelluride, diphenyl ditelluride, bis-(p-methoxyphenyl) ditelluride, bis-(p-aminophenyl) ditelluride, bis-(p-nitrophenyl) ditelluride, bis-(p-cyanophenyl) ditelluride, bis-(p-sulfonylphenyl) ditelluride, dinaphthyl ditelluride, and dipyridyl ditelluride.
[0086] The azo polymerization initiator can be any azo polymerization initiator used in normal radical polymerization without any particular limitation. For example, 2,2'-azobis(isobutyronitrile) (AIBN), 2,2'-azobis(2-methylbutyronitrile) (AMBN), 2,2'-azobis(2,4-dimethylvaleronitrile) (ADVN), 1,1'-azobis(1-cyclohexanecarbonitrile) (ACHN), dimethyl-2,2'-azobisisobutyrate (MAIB), 4,4'-azobis(4-cyanovaleric acid) (ACVA), 1,1'-azobis(1-acetoxy-1-phenylethane), 2,2'-azobis(2-methylbutyramide), 2,2'-azobis(4-methoxy- Examples of the azobis(N-cyclohexyl-2-methylpropionamide) include 2,4-dimethylvaleronitrile (V-70), 2,2'-azobis(2-methylamidinopropane) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis(2,4,4-trimethylpentane), 2-cyano-2-propylazoformamide, 2,2'-azobis(N-butyl-2-methylpropionamide), and 2,2'-azobis(N-cyclohexyl-2-methylpropionamide).
[0087] In the polymerization step, in a vessel purged with an inert gas, a vinyl monomer and an organotellurium compound of formula (3) are mixed with an azo-based polymerization initiator and / or an organoditelluride compound of formula (4) for the purpose of promoting the reaction and controlling the molecular weight and molecular weight distribution according to the type of vinyl monomer. Examples of the inert gas used at this time include nitrogen, argon, and helium. Argon and nitrogen are preferred.
[0088] The amount of the vinyl monomer used in the above (a), (b), (c) and (d) may be appropriately adjusted depending on the physical properties of the target copolymer (A). It is preferable to use 200 to 30,000 mol of the vinyl monomer per 1 mol of the organotellurium compound of the formula (3).
[0089] When the organotellurium compound of formula (3) in (b) is used in combination with an azo polymerization initiator, the amount of the azo polymerization initiator is preferably 0.01 mol to 10 mol per mol of the organotellurium compound of formula (3).
[0090] When the organotellurium compound of formula (3) and the organoditelluride compound of formula (4) are used in combination in the above (c), it is preferable to use 0.01 mol to 100 mol of the organoditelluride compound of formula (4) per 1 mol of the organotellurium compound of formula (3).
[0091] When the organotellurium compound of formula (3) in (d), the organic ditelluride compound of formula (4), and the azo polymerization initiator are used in combination, the amount of the organotellurium compound of formula (4) is preferably 0.01 mol to 100 mol per mol of the organotellurium compound of formula (3), and the amount of the azo polymerization initiator is preferably 0.01 mol to 10 mol per mol of the organotellurium compound of formula (4).
[0092] The polymerization reaction can be carried out without a solvent, but it can also be carried out by stirring the mixture using an aprotic or protic solvent that is generally used in radical polymerization. Examples of aprotic solvents that can be used include anisole, benzene, toluene, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetone, 2-butanone (methyl ethyl ketone), dioxane, propylene glycol monomethyl ether acetate, chloroform, carbon tetrachloride, tetrahydrofuran (THF), ethyl acetate, propylene glycol monomethyl ether acetate, or trifluoromethylbenzene. Examples of protic solvents include water, methanol, ethanol, isopropanol, n-butanol, ethyl cellosolve, butyl cellosolve, 1-methoxy-2-propanol, hexafluoroisopropanol, or diacetone alcohol.
[0093] The amount of the solvent used may be appropriately adjusted. For example, it is preferably 0.01 ml or more, more preferably 0.05 ml or more, and even more preferably 0.1 ml or more, per 1 g of vinyl monomer, and is preferably 50 ml or less, more preferably 10 ml or less, and even more preferably 1 ml or less.
[0094] The reaction temperature and reaction time may be appropriately adjusted depending on the molecular weight or molecular weight distribution of the copolymer (A) to be obtained, but usually, the reaction is performed at 0°C to 150°C and for 1 minute to 100 hours with stirring. The TERP method can obtain a high yield and a precise molecular weight distribution even at a low polymerization temperature and a short polymerization time. The pressure is usually normal pressure, but it may be increased or decreased.
[0095] After the polymerization reaction is completed, the reaction mixture obtained can be subjected to a usual separation and purification means to remove the solvent used, the residual vinyl monomer, etc., and the target copolymer (A) can be separated. In addition, the reaction mixture may be used as it is for the pressure-sensitive adhesive composition, provided that it does not affect the physical properties of the pressure-sensitive adhesive composition.
[0096] The growing end of the copolymer obtained by the polymerization reaction is -TeR derived from the tellurium compound. 31 (In the formula, R 31 is R in Eq. (3). 31 ) and is deactivated by handling in air after the polymerization reaction is completed, but tellurium atoms may remain. Since copolymers with tellurium atoms remaining at the terminals tend to be colored and have poor thermal stability, it is preferable to remove the tellurium atoms.
[0097] Methods for removing tellurium atoms include radical reduction methods using tributylstannane or thiol compounds, etc.; adsorption methods using activated carbon, silica gel, activated alumina, activated clay, molecular sieves, polymer adsorbents, etc.; metal adsorption methods using ion exchange resins, etc.; liquid-liquid extraction methods and solid-liquid extraction methods in which tellurium atoms at the ends of the copolymer are oxidized and decomposed by adding a peroxide such as hydrogen peroxide or benzoyl peroxide, or by blowing air or oxygen into the system, and residual tellurium compounds are removed by washing with water or combining with an appropriate solvent; and purification methods in a solution state such as ultrafiltration, which extracts and removes only those having a specific molecular weight or less. These methods can also be used in combination.
[0098] The other end of the copolymer obtained by the polymerization reaction (the end opposite to the growing end) is -CR derived from the tellurium compound. 32 R 33 R 34 (In the formula, R 32 , R 33 and R 34 is R in Eq. (3). 32 , R 33 and R 34 (same as above.)
[0099] (1-2. Crosslinking Agent (B)) The pressure-sensitive adhesive composition may contain a crosslinking agent. By blending a crosslinking agent, the cohesive strength of the pressure-sensitive adhesive can be adjusted, and the adhesive strength, constant load peeling, and adhesive residue can be adjusted. In addition, crosslinking failure can be suppressed. The crosslinking agent (B) is a compound having two or more reactive groups in one molecule that can react with the acidic group of the copolymer (A). The crosslinking agent (B) is not particularly limited, and examples thereof include epoxy-based crosslinking agents, isocyanate-based crosslinking agents, and aziridine-based crosslinking agents. Among these, epoxy-based crosslinking agents are more preferred from the viewpoint of easy control of the degree of progress of the crosslinking reaction and adhesion to the substrate.
[0100] The content of the epoxy-based crosslinking agent in the crosslinking agent (B) is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more. It is also preferable that the pressure-sensitive adhesive composition contains only an epoxy-based crosslinking agent as the crosslinking agent (B).
[0101] The epoxy crosslinking agent is a compound having two or more epoxy groups as reactive groups in one molecule. The epoxy crosslinking agent may be used alone or in combination of two or more kinds.
[0102] Examples of epoxy crosslinking agents include epoxy resins composed of bisphenol A and epichlorohydrin, ethylene glycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, diamine glycidylamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, Examples of suitable glycidyl ethers include glycidyl ether, sorbitol polyglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, and bisphenol-S-diglycidyl ether.
[0103] The isocyanate crosslinking agent is a compound having two or more isocyanate groups (including isocyanate regenerating functional groups in which the isocyanate groups are temporarily protected by a blocking agent or oligomerization) in one molecule as reactive groups. The isocyanate crosslinking agents may be used alone or in combination of two or more kinds.
[0104] Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate. More specifically, for example, lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, and polymethylene polyphenyl isocyanate; trimethylolpropane / tolylene diisocyanate trimer adduct, trimethylolpropane One or more selected from isocyanate adducts such as hexamethylene diisocyanate trimer adducts and isocyanurate bodies of hexamethylene diisocyanate; trimethylolpropane adducts of xylylene diisocyanate; trimethylolpropane adducts of hexamethylene diisocyanate; polyether polyisocyanates, polyester polyisocyanates, and adducts of these with various polyols, polyisocyanates multifunctionalized with isocyanurate bonds, biuret bonds, allophanate bonds, etc. can be used.
[0105] The aziridine crosslinking agent is a compound having two or more aziridine groups as reactive groups in one molecule. The aziridine crosslinking agent may be used alone or in combination of two or more kinds.
[0106] Examples of the aziridine crosslinking agent include tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, tris[1-(2-methyl)-aziridinyl]phosphine oxide, and hexa[1-(2-methyl)-aziridinyl]triphosphatriazine.
[0107] The reactive group content of the crosslinking agent (B) is preferably 0.10 mmol / g or more, more preferably 0.15 mmol / g or more, even more preferably 0.20 mmol / g or more, and is preferably 50 mmol / g or less, more preferably 40 mmol / g or less, even more preferably 30 mmol / g or less. If the reactive group content of the crosslinking agent (B) is 0.10 mmol / g or more, the crosslinking agent is contained to suppress cohesive failure of the adhesive layer, and if the crosslinking agent is contained to be 50 mmol / g or less, the crosslinking density is not too high, and the adhesive strength is good.
[0108] The content of the crosslinking agent (B) in the pressure-sensitive adhesive composition is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.10 parts by mass or more, relative to 100 parts by mass of the copolymer (A), and is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less. If the content of the crosslinking agent (B) is 0.01 parts by mass or more, the cohesive strength of the pressure-sensitive adhesive layer becomes good, and if it is 20 parts by mass or less, the crosslink density is not too high and the adhesive strength is good.
[0109] In the pressure-sensitive adhesive composition, the molar ratio of the reactive groups of the crosslinking agent (B) to the acidic groups of the copolymer (A) (molar amount of reactive groups / molar amount of acidic groups) is preferably 0.002 or more, more preferably 0.01 or more, and even more preferably 0.02 or more, and is preferably 0.20 or less, more preferably 0.15 or less, and even more preferably 0.10 or less.
[0110] In the pressure-sensitive adhesive composition, the molar ratio of the sum of the cyclic ether groups in copolymer (A) and the reactive groups in crosslinking agent (B) to the acidic groups in copolymer (A) (total molar amount of cyclic ether groups and reactive groups / molar amount of acidic groups) is preferably 0.01 or more, more preferably 0.03 or more, and even more preferably 0.06 or more, and is preferably 1.0 or less, more preferably 0.95 or less, and even more preferably 0.90 or less.
[0111] (1-4. Other additives) In addition to the copolymer (A) and the crosslinking agent (B), other additives may be added to the pressure-sensitive adhesive composition. Examples of other additives include crosslinking accelerators, crosslinking retarders, tackifier resins, storage stabilizers, plasticizers, softeners, peeling aids, silane coupling agents, dyes, pigments, dyes, fluorescent brighteners, antistatic agents, wetting agents, surfactants, thickeners, antifungal agents, preservatives, oxygen absorbers, ultraviolet absorbers, antioxidants, near-infrared absorbers, water-soluble quenchers, fragrances, metal deactivators, nucleating agents, alkylating agents, flame retardants, lubricants, processing aids, etc. These are appropriately selected and mixed according to the application and purpose of the pressure-sensitive adhesive film.
[0112] (Crosslinking retarder) The pressure-sensitive adhesive composition may be used by blending a crosslinking retarder as necessary. The crosslinking retarder is a compound capable of suppressing excessive viscosity increase of a pressure-sensitive adhesive composition containing a crosslinking agent by blocking a functional group of the crosslinking agent. The type of crosslinking retarder is not particularly limited, and examples thereof include β-diketones such as acetylacetone, hexane-2,4-dione, heptane-2,4-dione, and octane-2,4-dione; β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, propyl acetoacetate, butyl acetoacetate, octyl acetoacetate, oleyl acetoacetate, lauryl acetoacetate, and stearyl acetoacetate; benzoylacetone; and alcohols. The crosslinking retarder is preferably one that can act as a chelating agent, and is preferably β-diketones or β-ketoesters.
[0113] The content of the crosslinking retarder that can be blended in the pressure-sensitive adhesive composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.5 parts by mass or more, and is preferably 4.0 parts by mass or less, more preferably 3.0 parts by mass or less, even more preferably 1.5 parts by mass or less, based on 100 parts by mass of the copolymer (A). By adjusting the content of the crosslinking retarder within the above range, it is possible to suppress excessive viscosity increase and gelation of the pressure-sensitive adhesive composition after blending the crosslinking agent (B) in the pressure-sensitive adhesive composition, and improve the storage stability of the pressure-sensitive adhesive composition (extend the pot life).
[0114] (tackifier) The pressure-sensitive adhesive composition may be used by blending a tackifier other than the copolymer (A) as necessary. The tackifier is not particularly limited, but examples thereof include rosin-based tackifier resins, terpene-based tackifier resins, phenol-based tackifier resins, and hydrocarbon-based tackifier resins.
[0115] Examples of rosin-based tackifying resins include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin; modified rosins obtained by modifying these unmodified rosins through polymerization, disproportionation, hydrogenation, or the like (polymerized rosin, stabilized rosin, disproportionated rosin, fully hydrogenated rosin, partially hydrogenated rosin, other chemically modified rosins, and the like); and various rosin derivatives.
[0116] Examples of the rosin derivatives include rosin phenol-based resins obtained by adding phenol to rosins (unmodified rosin, modified rosin) using an acid catalyst and thermally polymerizing the resulting mixture; rosin ester-based resins such as rosin ester compounds (unmodified rosin esters) obtained by esterifying unmodified rosin with alcohols, and modified rosin ester compounds (polymerized rosin ester, stabilized rosin ester, disproportionated rosin ester, fully hydrogenated rosin ester, partially hydrogenated rosin ester, etc.) obtained by esterifying modified rosin with alcohols; unsaturated fatty acid modified rosin-based resins obtained by modifying unmodified rosin or modified rosin with unsaturated fatty acid; unsaturated fatty acid modified rosin ester-based resins obtained by modifying rosin ester-based resins with unsaturated fatty acid; rosin alcohol-based resins obtained by reducing the carboxyl groups in unmodified rosin, modified rosin, unsaturated fatty acid modified rosin resins, and unsaturated fatty acid modified rosin ester-based resins; and metal salts of rosin-based resins such as unmodified rosin and modified rosin (particularly rosin ester-based resins).
[0117] Examples of terpene-based tackifying resins include terpene-based resins such as α-pinene polymers, β-pinene polymers, and dipentene polymers, and modified terpene-based resins obtained by modifying these terpene-based resins (phenol-modified, aromatic-modified, hydrogen-modified, hydrocarbon-modified, etc.) (e.g., terpene-phenolic resins, styrene-modified terpene resins, aromatic-modified terpene resins, and hydrogenated terpene resins).
[0118] Examples of phenol-based tackifying resins include condensates of various phenols (e.g., phenol, m-cresol, 3,5-xylenol, p-alkylphenol, resorcinol) with formaldehyde (e.g., alkylphenol-based resins, xylene formaldehyde-based resins), resols obtained by addition reaction of the phenols with formaldehyde using an alkali catalyst, and novolaks obtained by condensation reaction of the phenols with formaldehyde using an acid catalyst.
[0119] Examples of hydrocarbon-based tackifying resins (petroleum-based tackifying resins) include aliphatic hydrocarbon resins [polymers of aliphatic hydrocarbons such as olefins and dienes having 4 to 5 carbon atoms (olefins such as butene-1, isobutylene, and pentene-1; dienes such as butadiene, 1,3-pentadiene, and isoprene)], aliphatic cyclic hydrocarbon resins [alicyclic hydrocarbon resins obtained by cyclizing and dimerizing so-called "C4 petroleum fractions" and "C5 petroleum fractions" and then polymerizing them, cyclic diene compounds (cyclopentadiene, dicyclopentadiene, ethylidene norbornene, dicyclopentadiene ... Examples of such resins include polymers of vinyl groups having 8 to 10 carbon atoms (styrene, vinyltoluene, α-methylstyrene, indene, methylindene, etc.) or their hydrogenated products, alicyclic hydrocarbon resins obtained by hydrogenating the aromatic rings of the aromatic hydrocarbon resins or aliphatic or aromatic petroleum resins described below], aromatic hydrocarbon resins [polymers of vinyl group-containing aromatic hydrocarbons having 8 to 10 carbon atoms (styrene, vinyltoluene, α-methylstyrene, indene, methylindene, etc.)], aliphatic or aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic or alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, and coumarone-indene resins.
[0120] The content of the tackifier that can be blended in the pressure-sensitive adhesive composition is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, and is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, relative to 100 parts by mass of the copolymer (A). By adjusting the content of the tackifier within the above range, sufficient adhesion to the adherend can be ensured.
[0121] (1-5. Method for producing pressure-sensitive adhesive composition) The pressure-sensitive adhesive composition can be produced by mixing the copolymer (A), the crosslinking agent (B) used as necessary, and other additives. The pressure-sensitive adhesive composition may contain a solvent derived from the production of the copolymer (A), or may be a solution diluted with an appropriate solvent to have a viscosity suitable for forming a pressure-sensitive adhesive layer.
[0122] Examples of the solvent include aliphatic hydrocarbons such as hexane and heptane, aromatic hydrocarbons such as toluene and xylene, halogenated hydrocarbons such as methylene chloride and ethylene chloride, ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone, esters such as ethyl acetate and butyl acetate, cellosolve-based solvents such as ethyl cellosolve, and glycol ether-based solvents such as propylene glycol monomethyl ether. These solvents may be used alone or in combination of two or more.
[0123] The amount of the solvent used is not particularly limited and may be appropriately adjusted so that the adhesive composition has a viscosity suitable for coating. From the viewpoint of coatability, however, it is preferable to use the solvent so that the solid content concentration of the adhesive composition is 10% by mass to 95% by mass.
[0124] It is preferable that the pressure-sensitive adhesive composition does not substantially contain a silicone compound. By substantially not containing a silicone compound, adverse effects on electrical components, etc. caused by the silicone compound present in the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition can be prevented. The pressure-sensitive adhesive composition does not substantially contain a silicone compound means that the amount of the silicone compound in the components (solid content) excluding the solvent is 500 μg / g or less, preferably 100 μg / g or less. The silicone compound is a polymer having a main skeleton of a siloxane bond (Si-O-Si) consisting of silicon and oxygen, and an organic group is bonded to the silicon.
[0125] (2. Base Film) The base film can be appropriately selected and used depending on the application of the adhesive film. Examples of the base film include polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN); acrylic resins such as polymethyl methacrylate (PMMA); and films made of plastic materials such as polycarbonate, triacetyl cellulose (TAC), polystyrene, polysulfone, polyethersulfone, polyphenylenesulfone, polyphenylenesulfide, polyetheretherketone, cycloolefin polymers, cycloolefin copolymers, fluoropolymers, polyarylates, polyetherimides, polyimides, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, and ethylene-propylene copolymers. The plastic materials can be used alone or in combination of two or more. Among these, PET is preferred in terms of excellent mechanical strength and dimensional stability. Polyimide is preferred in terms of excellent heat resistance. That is, the base film is preferably a PET film (particularly a biaxially stretched PET film) or a polyimide film.
[0126] The thickness of the base film is not particularly limited and is appropriately selected, but is usually preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, and is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less. If the thickness is less than 5 μm, the strength of the base film is insufficient, and problems such as the film being torn when peeled off occur. In addition, if the thickness of the base film is more than 200 μm, problems such as the film itself being expensive occur.
[0127] The substrate film may be subjected to a surface treatment by an oxidation method, a roughening method, or the like on one or both sides as desired, in order to improve adhesion to a layer provided on the surface. Examples of the oxidation method include corona discharge treatment, plasma treatment, chromic acid treatment (wet), flame treatment, hot air treatment, ozone / ultraviolet light irradiation treatment, and the like. Examples of the roughening method include sandblasting and solvent treatment. These surface treatment methods are appropriately selected depending on the type of substrate film, but generally, corona discharge treatment is preferably used in terms of effectiveness and operability. In addition, the substrate film may be subjected to a primer treatment on one or both sides.
[0128] (3. Adhesive Layer) The gel fraction of the pressure-sensitive adhesive layer is 30% by mass or more, preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 70% by mass to 100% by mass. If the gel fraction is too low, the adhesive strength is likely to increase, and the adherend is likely to be contaminated during peeling. The gel fraction can be controlled by the amount of crosslinking agent in the pressure-sensitive adhesive composition, the crosslinking temperature, and the crosslinking time.
[0129] The thickness of the adhesive layer formed on the base film can be appropriately set depending on, for example, the adhesive strength required for the adhesive film, etc. The thickness of the adhesive layer is generally 1 μm to 100 μm, preferably 5 μm to 50 μm, and more preferably 10 μm to 30 μm.
[0130] It is preferable that the pressure-sensitive adhesive layer does not substantially contain a silicone compound. When the pressure-sensitive adhesive layer does not substantially contain a silicone compound, adverse effects on electrical components and the like can be more effectively prevented. Note that, "substantially not containing a silicone compound" means that the amount of the silicone compound in the pressure-sensitive adhesive layer is 500 μg / m 2 It is preferable that the concentration is 100 μg / m or less. 2 This refers to the following:
[0131] (3-1. Method for forming adhesive layer) The method for forming the pressure-sensitive adhesive layer is not particularly limited, and examples thereof include the following methods (1) and (2) in which a pressure-sensitive adhesive composition is applied and dried. (1) A method in which a pressure-sensitive adhesive composition is applied to one or both sides of a substrate film using various coating devices, the solvent is removed by drying, and curing is performed as necessary. (2) A method in which a pressure-sensitive adhesive composition is applied to the release surface of a release film that has been subjected to a release treatment on its surface using various coating devices, the solvent is dried off, the composition is transferred to one or both sides of a base film, and then cured as necessary.
[0132] Examples of the coating device include a reverse roll coater, a gravure coater, a forward roll coater, a knife coater, a wire bar coater, a doctor blade coater, a slot die coater, a curtain coater, and a dip coater.
[0133] The drying temperature when drying and removing the solvent is preferably 40°C or higher, more preferably 60°C or higher, and preferably less than 150°C, more preferably 140°C or lower, and further preferably 130°C or lower. By setting the drying temperature to less than 150°C, it becomes easier to leave the cyclic ether group and the acidic group in the pressure-sensitive adhesive layer to be formed. The drying time is preferably 5 seconds to 20 minutes, more preferably 10 seconds to 10 minutes. Examples of the drying method include hot air, near infrared rays, infrared rays, and high frequency waves. In addition, examples of the curing conditions include about 3 days to 7 days at 30°C to 50°C. The crosslinking reaction (the reaction between the acidic group of the copolymer (A) and the crosslinking agent (B)) is completed by the drying and removal of the solvent and the curing, and the pressure-sensitive adhesive layer is formed.
[0134] (4. Release film) The pressure-sensitive adhesive film may have a release film (separator) on the surface of the pressure-sensitive adhesive layer until it is used. A release layer may be provided on the opposite side of the base film to the surface on which the pressure-sensitive adhesive layer is laminated, without using a separate release film, and the exposed surface of the pressure-sensitive adhesive layer may be wound in a roll shape or laminated in a tiered shape so that the exposed surface of the pressure-sensitive adhesive layer is in contact with the surface of the release layer. The release film is used as a protective material for the pressure-sensitive adhesive layer, and is peeled off when the pressure-sensitive adhesive film of the present invention is attached to an adherend.
[0135] The release film may be, for example, glassine paper, coated paper, laminated paper, or various plastic films coated with a release agent such as silicone resin. The plastic film used for the release film may be any of the plastic films listed as the base film. The thickness of the release film is not particularly limited, but is usually 10 μm to 150 μm.
[0136] (5. Uses of adhesive film) The adhesive film causes little contamination to the adherend surface, and can be used as a surface protection film, a masking film, or in the manufacturing process of semiconductors, which are peeled off after use. In addition, the adhesive film prevents the adhesive strength from increasing even when exposed to high temperatures while attached to the adherend. Therefore, the adhesive film can be suitably used in applications where it is exposed to 100°C or higher (particularly 150°C or higher) while attached to the adherend. For example, it can be used in high-temperature processing where the adherend is exposed to a high-temperature atmosphere of 150°C or higher.
[0137] In particular, the pressure-sensitive adhesive film is difficult to peel off during use after heat treatment, but is easy to peel off after use, and causes little contamination of the adherend surface after peeling. Therefore, it can be suitably used as a surface protection film for optical components such as polarizing plates, flexible printed circuit (FPC) boards, conductive films in which a thin film such as indium tin oxide (ITO) is formed as a transparent electrode on one side of a transparent base material, and glass substrates. In addition, it can be suitably used as a film supporting a lead frame in the manufacturing process of QFN.
[0138] The adhesive film preferably has an adhesive strength to an adherend at 23°C of 0.1N / 25mm to 10N / 25mm. The adhesive film preferably has an adhesive strength to an adherend after heat treatment (260°C, 0.5 hours) of 0.1N / 25mm to 5.0N / 25mm, more preferably 0.1N / 25mm to 4.0N / 25mm. If the adhesive strength is 10N / 25mm or less, deformation of the adherend can be suppressed when the adhesive film is peeled off from the adherend (e.g., optical member, semiconductor element). If the adhesive strength is 0.1N / 25mm or more, unintentional peeling from the adherend during use is suppressed.
[0139] The pressure-sensitive adhesive film preferably has an enhancement ratio (adhesive strength after heat treatment / adhesive strength before heat treatment) of the pressure-sensitive adhesive layer of 1 or less, more preferably 0.8 or less, and even more preferably 0.6 or less. If the enhancement ratio is 1 or less, the adhesive strength does not increase after heat treatment, the pressure-sensitive adhesive film is easily peeled off after use, the workability is good, and adhesive residue is less likely to occur. The heat treatment conditions for evaluating the enhancement ratio are 260°C and 0.5 hours.
[0140] The pressure-sensitive adhesive film preferably has a ratio (G1 / G2) of the gel fraction (G1) of the pressure-sensitive adhesive layer before heat treatment to the gel fraction (G2) of the pressure-sensitive adhesive film after heat treatment at 150° C. or higher for 3 minutes, which is 1 or less, more preferably 0.9 or less, and even more preferably 0.8 or less. If the ratio (G1 / G2) is 1 or less, the cyclic ether group and acidic group remaining in the pressure-sensitive adhesive layer will react when the pressure-sensitive adhesive film is exposed to a temperature of 150° C. or higher. In other words, the pressure-sensitive adhesive film can be prevented from excessively increasing in adhesive strength when exposed to a temperature of 150° C. or higher. EXAMPLES
[0141] The present invention will be described in more detail below based on specific examples. The present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention. The polymerization rate, weight average molecular weight (Mw) and molecular weight distribution (PDI) of the copolymer, solid content and viscosity of the copolymer solution, gel fraction of the adhesive layer, and adhesive strength before heat treatment, adhesive strength after heat treatment, adhesive residue after heat treatment, and 150°C constant load peeling of the adhesive film were evaluated according to the following methods. The meanings of the abbreviations are as follows.
[0142] BTEE: Ethyl 2-methyl-2-n-butyltellanyl-propionate V-70: 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) V-65: 2,2'-azobis(2,4-dimethylvaleronitrile) MA: Methyl acrylate BA: n-butyl acrylate GMA: glycidyl methacrylate AA: Acrylic acid AcOEt: ethyl acetate
[0143] <Evaluation method> (Polymerization rate) Using a nuclear magnetic resonance (NMR) measuring device (Bruker Biospin, model: AVANCE500 (frequency 500 MHz)), 1 H-NMR was measured (solvent: CDCl3, internal standard: TMS). For the obtained NMR spectrum, the integral ratio of the peaks of the vinyl group derived from the monomer and the ester side chain derived from the polymer was obtained, and the polymerization rate of the monomer was calculated.
[0144] (Weight average molecular weight (Mw) and molecular weight distribution (PDI)) The molecular weight was determined by gel permeation chromatography (GPC) using a high performance liquid chromatograph (Tosoh Corporation, model HLC-8320GPC). Two TSKgel Super HZM-M (Tosoh Corporation) columns were used, a tetrahydrofuran solution was used as the mobile phase, and a differential refractometer was used as the detector. The measurement conditions were a column temperature of 40°C, a sample concentration of 10mg / mL, a sample injection amount of 10μm, and a flow rate of 0.2mL / min. A calibration curve was created using polystyrene (molecular weights 2,890,000, 1,090,000, 706,000, 427,000, 190,000, 96,400, 37,900, 10,200, 2,630, and 440) as a standard substance, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were measured. From this measurement, the molecular weight distribution (PDI=Mw / Mn) was calculated.
[0145] (Solids) The copolymer solution with a mass of W1 (approximately 1.0 g) was weighed into an aluminum cup (mass W0) and dried under reduced pressure for 1 hour at 130° C. The mass (W2) of the aluminum cup containing the dried copolymer was measured, and the solid content was calculated using the following formula. Solid content (mass%) = [(W2-W0) / W1] x 100
[0146] (viscosity) The viscosity was measured using a Brookfield viscometer (product name: TVB-15, manufactured by Toki Sangyo Co., Ltd.) with an M3 rotor at 25° C. and a rotor rotation speed of 60 rpm.
[0147] (Gel fraction (120℃)) The pressure-sensitive adhesive composition was applied to a release film, dried at 60° C. for 2 minutes, and further dried at 120° C. for 3 minutes. After that, it was left to stand at 40° C. for 3 days, and then the pressure-sensitive adhesive layer formed on the release film was peeled off. About 0.1 g of the adhesive layer was cut to obtain a test piece (mass W1). This test piece was placed in a stainless steel wire mesh (400 mesh) (mass W0). The stainless steel wire mesh containing the test piece was immersed in ethyl acetate at 60°C for 24 hours, then removed from the ethyl acetate, dried at room temperature for 24 hours, and further dried under reduced pressure at 130°C for 1 hour. The mass W2 of the stainless steel wire mesh containing the dried test piece was then measured, and the gel fraction was calculated using the following formula. Gel fraction (mass%) = [(W2-W0) / W1] x 100
[0148] (Adhesive strength before heat treatment) The adhesive film was pressed onto an adherend (SUSBA steel plate, 1 mm thick, manufactured by Nippon Takuto Co., Ltd.) using a pressing device (roller mass 2 kg), and within 1 minute, the adhesive strength was measured when peeled off at 180° to the adherend. The measurement was performed using a tensile tester at a test temperature of 23°C and a peeling speed of 300 mm / min. The adhesive film had a width of 25 mm and a length of 300 mm. After the measurement started, the measured value for the first 25 mm length was ignored, and the adhesive strength measured values for the 50 mm length peeled off from the test plate were averaged.
[0149] (Adhesive strength after heat treatment) The adhesive film was pressed onto the adherend (manufactured by Nippon Takuto Co., Ltd., SUSBA steel plate, thickness 1 mm) using a pressing device (roller mass 2 kg). The adherend to which this adhesive film was attached was heat treated in a 260 ° C oven for 0.5 hours. After this adherend was allowed to cool to room temperature, the adhesive strength was measured when the adhesive film was peeled off at 180 ° against the adherend. The measurement was performed using a tensile tester, the test temperature was 23 ° C, and the peeling speed was 300 mm / min. The width of the adhesive film was 25 mm and the length was 300 mm. After the measurement started, the measured value of the first 25 mm length was ignored, and the adhesive strength measured value of the 50 mm length peeled off from the test plate was averaged. In addition, the enhancement ratio was calculated using the values of the adhesive strength after heat treatment and the adhesive strength before heat treatment according to the formula (enhancement ratio=adhesive strength after heat treatment / adhesive strength before heat treatment).
[0150] (Adhesive residue after heat treatment) After the heat treatment and measurement of adhesive strength, the presence or absence of adhesive residue on the adherend was judged by visual inspection. Those that had no adhesive residue were rated as "◯", and those that had adhesive residue were rated as "×".
[0151] (150℃ constant load peeling) The adhesive film was pressed onto the adherend (SUSBA steel plate, 1 mm thick, manufactured by Nippon Takuto Co., Ltd.) using a pressing device (roller mass 2 kg). The width of the adhesive film was 25 mm and the length was 50 mm. After aging for 20 minutes at 23°C, a load of 50 g was applied in a 90° direction to the adherend in an atmosphere of 150°C, and the peel time required for peeling over a distance of 50 mm in the length direction was measured. A peel time of 100 seconds or more under constant load was evaluated as "◎", a peel time of 50 seconds or more was evaluated as "◯", and a peel time of less than 50 seconds or cohesive failure was evaluated as "X".
[0152] <Production of copolymer> (Production example 1: Copolymer No. 1) In a flask equipped with an argon gas inlet tube and a stirrer, BA (565.7g), GMA (11.5g), AA (22.8g), V-70 (74.0mg), and AcOEt (448.1g) were charged, and after replacing with argon, BTEE (359.9mg) was added and the reaction was carried out at 33℃ for 22 hours to polymerize. The polymerization rate was 77.8%. After the reaction was completed, AcOEt was added to the reaction solution to obtain a copolymer solution containing copolymer No. 1. The resulting copolymer No. 1 had an Mw of 504,000, a PDI of 1.5, a solid content of the solution of 28.4 mass%, and a viscosity of 17,560 mPa s.
[0153] (Production example 2: Copolymer No. 2) In a flask equipped with an argon gas inlet tube and a stirrer, BA (565.7g), GMA (11.5g), AA (22.8g), V-70 (74.0mg), and AcOEt (448.1g) were charged, and after replacing with argon, BTEE (239.9mg) was added and reacted at 33℃ for 19 hours to polymerize. The polymerization rate was 78.7%. After the reaction was completed, AcOEt was added to the reaction solution to obtain a copolymer solution containing copolymer No. 2. The obtained copolymer No. 2 had an Mw of 640,800, a PDI of 1.6, a solid content of the solution of 21.2 mass%, and a viscosity of 14,720 mPa s.
[0154] (Production Example 3: Copolymer No. 3) In a flask equipped with an argon gas inlet tube and a stirrer, BA (532.2 g), GMA (45.0 g), AA (22.8 g), V-70 (111.0 mg), and AcOEt (448.1 g) were charged, and after replacing with argon, BTEE (359.9 mg) was added and the reaction was carried out at 33°C for 26 hours to polymerize. The polymerization rate was 81.1%. After the reaction was completed, AcOEt was added to the reaction solution to obtain a copolymer solution containing copolymer No. 3. The resulting copolymer No. 3 had an Mw of 527,000, a PDI of 1.9, a solid content of 23.6 mass% and a viscosity of 18,820 mPa s.
[0155] (Production Example 4: Copolymer No. 4) In a flask equipped with an argon gas inlet tube and a stirrer, BA (528.0 g), GMA (24.0 g), AA (48.0 g), V-70 (111.0 mg), and AcOEt (448.1 g) were charged, and after replacing with argon, BTEE (359.9 mg) was added and the reaction was carried out at 33°C for 27 hours to polymerize. The polymerization rate was 89.7%. After the reaction was completed, AcOEt was added to the reaction solution to obtain a copolymer solution containing copolymer No. 4. The resulting copolymer No. 4 had an Mw of 481,000, a PDI of 2.0, a solid content of the solution of 19.2 mass%, and a viscosity of 8,320 mPa s.
[0156] (Production Example 5: Copolymer No. 5) In a flask equipped with an argon gas inlet tube and a stirrer, MA (162.0 g), BA (403.7 g), GMA (11.5 g), AA (22.8 g), V-70 (92.5 mg), and AcOEt (448.1 g) were charged, and after replacing with argon, BTEE (359.9 mg) was added and the reaction was carried out at 33°C for 24 hours to polymerize. The polymerization rate was 87.8%. After the reaction was completed, AcOEt was added to the reaction solution to obtain a copolymer solution containing copolymer No. 5. The obtained copolymer No. 5 had an Mw of 506,000, a PDI of 1.6, a solid content of the solution of 19.9 mass%, and a viscosity of 8,860 mPa s.
[0157] (Production Example 6: Copolymer No. 6) In a flask equipped with an argon gas inlet tube and a stirrer, BA (471.4g), GMA (9.6g), AA (19.0g), V-65 (1.3g), and AcOEt (500.0g) were charged, and after replacing with argon, the mixture was reacted at 55°C for 5 hours, after which V-65 (0.2g) and AcOEt (200.0g) were added and the mixture was reacted for 15 hours to polymerize. The polymerization rate was 96.5%. After the reaction was completed, AcOEt was added to the reaction solution to obtain a copolymer solution containing copolymer No. 6. The obtained copolymer No. 6 had an Mw of 696,000, a PDI of 6.1, a solid content of the solution of 22.2 mass%, and a viscosity of 6,210 mPa s.
[0158] (Production Example 7: Copolymer No. 7) In a flask equipped with an argon gas inlet tube and a stirrer, BA (528.4 g), AA (22.1 g), V-70 (84.8 mg), and AcOEt (410.4 g) were charged, and after replacing with argon, BTEE (329.9 mg) was added and reacted at 33°C for 24 hours to polymerize. The polymerization rate was 86.9%. After the reaction was completed, AcOEt was added to the reaction solution to obtain a copolymer solution containing copolymer No. 7. The resulting copolymer No. 7 had an Mw of 370,300, a PDI of 1.4, a solid content of 27.3 mass% and a viscosity of 1,800 mPa s.
[0159] [Table 1]
[0160] <Production of Pressure-Sensitive Adhesive Composition> (Adhesive composition No. 1) To 100 parts by mass of the solution of copolymer No. 1 obtained in Production Example 1 (28.4 parts by mass of copolymer component, 71.6 parts by mass of AcOEt), 0.031 parts by mass of a crosslinking agent (TETRAD (registered trademark)-C: manufactured by Mitsubishi Gas Chemical Company, Inc., 1,3-bis(N,N-diglycidylaminoethyl)cyclohexane (epoxy group amount: 10.14 mmol / g)) and 50.6 parts by mass of AcOEt were added and stirred to obtain adhesive composition No. 1.
[0161] (Adhesive Compositions No. 2 to 8) Pressure-sensitive adhesive compositions Nos. 2 to 8 were prepared in the same manner as pressure-sensitive adhesive composition No. 1, except that the formulation was changed as shown in Table 2. In Table 2, the amount of solvent listed is the total amount of the solvent contained in the copolymer solution and the solvent added when preparing the pressure-sensitive adhesive composition.
[0162] [Table 2]
[0163] <Manufacturing of adhesive films> (Adhesive Film No.1) The adhesive composition No. 1 was applied onto a polyimide film (PI) film (thickness 25 μm, manufactured by Toray DuPont Co., Ltd., "Kapton (registered trademark) 100V") so that the thickness after drying would be 20 μm. The PI film onto which the adhesive composition was applied was dried at 120°C for 3 minutes to produce adhesive film No. 1 having an adhesive layer. A release film (thickness 25 μm, manufactured by Higashiyama Film Co., Ltd., "HY-PS11") was attached to the obtained adhesive layer, and the film was left to stand at 40°C for 3 days to cure.
[0164] (Adhesive film No. 2~8) Adhesive films Nos. 2 to 8 were produced in the same manner as adhesive film No. 1, except that adhesive composition No. 1 was changed to adhesive compositions Nos. 2 to 8.
[0165] The gel fraction, adhesive strength, adhesive residue after heat treatment, and 150° C. constant-load peel evaluation results for the obtained adhesive film are shown in Table 3.
[0166] [Table 3]
[0167] In the adhesive films No. 1 to No. 5, the adhesive layer is formed from an adhesive composition containing an acrylic copolymer having a structural unit (a-1) with a cyclic ether group and a structural unit (a-2) with an acidic group, and having a molecular weight distribution (PDI) of 3.0 or less obtained by living radical polymerization, and the gel fraction of the adhesive layer is 30% by mass or more. These adhesive films No. 1 to No. 5 have sufficient initial adhesive strength, and peeling during heating is suppressed (excellent constant load peelability at high temperatures). In addition, the increase in adhesive strength after heating is suppressed, and the adhesive strength is actually reduced, allowing for easy peeling without leaving any adhesive residue.
[0168] The adhesive composition No. 3 used in the adhesive film No. 3 had a gel fraction of 99.2% by mass when the drying temperature was changed to 150°C. Specifically, the adhesive composition was applied to a release film, dried at 60°C for 2 minutes, further dried at 150°C for 3 minutes, and then allowed to stand at 40°C for 3 days, after which the gel fraction of the adhesive layer peeled off from the release film was measured. This shows that adhesive film No. 3 has unreacted cyclic ether groups and acidic groups remaining in the adhesive layer, and the gel fraction increases when exposed to high temperatures of 150°C or higher.
[0169] PSA film No. 6 has a gel fraction of less than 30% by mass in the adhesive layer, and when the adhesive film was peeled off from the adherend after heat treatment or at high temperatures, the adhesive layer underwent cohesive failure. PSA film No. 7 is a case where the copolymer contained in the pressure-sensitive adhesive composition is polymerized by a free radical method. This PSA film No. 7 has poor constant-load peelability at high temperatures. The pressure-sensitive adhesive film No. 8 is a case where the copolymer contained in the pressure-sensitive adhesive composition does not contain the structural unit (a-1) having a cyclic ether group. In this pressure-sensitive adhesive film No. 8, the pressure-sensitive adhesive layer underwent cohesive failure when the pressure-sensitive adhesive film was peeled off from the adherend after heat treatment or at high temperatures. [Industrial Applicability]
[0170] The adhesive film of the present invention can be suitably used, for example, as a polarizing plate, a flexible printed circuit (FPC) board, a conductive film having a thin film of indium tin oxide (ITO) or the like formed as a transparent electrode on one side of a transparent substrate, a surface protection film for optical components such as a glass substrate, and a film supporting a lead frame in the manufacturing process of a QFN.
Claims
1. A pressure-sensitive adhesive sheet having a base film and a pressure-sensitive adhesive layer formed on at least one surface of the base film, the pressure-sensitive adhesive layer is formed by applying a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer obtained by living radical polymerization onto a base film, and reacting an acidic group and a cyclic ether group in the (meth)acrylic copolymer, The (meth)acrylic copolymer contains a structural unit (a-1) having a cyclic ether group represented by the following general formula (1) and a structural unit (a-2) having an acidic group, and has a weight average molecular weight of 200,000 or more and a molecular weight distribution (Mw / Mn) of 3.0 or less: the (meth)acrylic copolymer has a molar ratio of a cyclic ether group to an acidic group (cyclic ether group / acidic group) of 0.01 to 1.0; A pressure-sensitive adhesive film, characterized in that the pressure-sensitive adhesive layer has a gel fraction of 60 mass % or more. 【Chemistry 1】 [In formula (1), R 11 represents an alkylene group or an arylene group which may have a substituent. R 12 represents a hydrogen atom or a methyl group.]
2. A substrate film and a pressure-sensitive adhesive layer formed on at least one surface of the substrate film, the pressure-sensitive adhesive layer is formed by applying, onto a base film, a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer obtained by living radical polymerization and a crosslinking agent having in one molecule two or more reactive groups capable of reacting with an acidic group possessed by the (meth)acrylic copolymer, and reacting the acidic group possessed by the (meth)acrylic copolymer with a cyclic ether group possessed by the (meth)acrylic copolymer and a reactive group possessed by the crosslinking agent; The (meth)acrylic copolymer contains a structural unit (a-1) having a cyclic ether group represented by the following general formula (1) and a structural unit (a-2) having an acidic group, and has a weight average molecular weight of 200,000 or more and a molecular weight distribution (Mw / Mn) of 3.0 or less: the pressure-sensitive adhesive composition has a molar ratio of the sum of the cyclic ether groups in the (meth)acrylic copolymer and the reactive groups in the crosslinking agent to the acidic groups in the (meth)acrylic copolymer (total molar amount of cyclic ether groups and reactive groups / molar amount of acidic groups) of 0.01 to 1.0; A pressure-sensitive adhesive film, characterized in that the pressure-sensitive adhesive layer has a gel fraction of 60 mass % or more. 【Chemistry 2】 [In formula (1), R 11 represents an alkylene group or an arylene group which may have a substituent. R 12 represents a hydrogen atom or a methyl group.]
3. The adhesive film described in claim 2, wherein the content of the crosslinking agent in the adhesive composition is 0.01 parts by mass to 20 parts by mass per 100 parts by mass of the (meth)acrylic copolymer.
4. The pressure-sensitive adhesive film according to any one of claims 1 to 3, wherein the (meth)acrylic copolymer has a weight average molecular weight of 200,000 to 2,000,000.
5. The acidic group of the structural unit (a-2) is at least one selected from the group consisting of a carboxyl group, a sulfonic acid group, a phosphoric acid group, a phosphonic acid group and a phosphinic acid group. The pressure-sensitive adhesive film according to any one of claims 1 to 4.
6. The adhesive film according to any one of claims 1 to 5, wherein the content of the structural unit (a-1) is 0.5% by mass to 15% by mass in 100% by mass of the entire (meth)acrylic copolymer.
7. The adhesive film according to any one of claims 1 to 6, wherein the content of the structural unit (a-2) is 1.0% by mass to 15% by mass in 100% by mass of the entire (meth)acrylic copolymer.
8. The pressure-sensitive adhesive film according to any one of claims 1 to 7, wherein the mass ratio ((a-1) / (a-2)) of the structural unit (a-1) to the structural unit (a-2) is 0.03 to 1.
0.
9. The pressure-sensitive adhesive film according to any one of claims 1 to 8, wherein the (meth)acrylic copolymer contains a structural unit (a-3) represented by the following general formula (2): 【Chemistry 2】 [In the general formula (2), R 21 R represents a chain or cyclic hydrocarbon group which may have a substituent. 22 represents a hydrogen atom or a methyl group.
10. The pressure-sensitive adhesive film according to any one of claims 1 to 9, wherein the pressure-sensitive adhesive layer is substantially free of a silicone compound.
11. The pressure-sensitive adhesive film according to any one of claims 1 to 10, which is used for high-temperature processing at 150°C or higher.
12. The pressure-sensitive adhesive film according to any one of claims 1 to 11, wherein the pressure-sensitive adhesive layer is formed by applying a pressure-sensitive adhesive composition and drying at a temperature of less than 150°C.
13. The pressure-sensitive adhesive film according to any one of claims 1 to 12, wherein when the pressure-sensitive adhesive film is heat-treated at 260°C for 0.5 hours, the pressure-sensitive adhesive layer has an enhancement ratio (adhesive strength after heat treatment / adhesive strength before heat treatment) of 1 or less.
Citation Information
Patent Citations
Threeedimensional magnetic head
JP1977056515A
Acrylic resin composition
JP2010053170A
Adhesive
JP2010084068A
Crosslinked polymer and method of producing the same
JP2016003298A
Radiation curable adhesive composition and pressure sensitive adhesive tape
JP2019143022A