Methods and compositions for direct printing with improved recyclability - Patents.com

Ink compositions for digital printing on plastic articles, featuring hydrophilic or acidic components, address the challenge of image removal during recycling by separating at elevated temperatures, enhancing recyclability and compatibility with traditional recycling processes.

JP7580431B2Active Publication Date: 2024-11-11PLASTIPAK PACKAGING INC
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2022124854
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-09-04
Filing Date
2022-08-04
Publication Date
2024-11-11
Estimated Expiration
2036-08-31

AI Technical Summary

Technical Problem

Current digital printing technologies on plastic containers face challenges in ensuring that the printed images can be easily removed during the recycling process without contaminating the plastic material, as they often fail to maintain adhesion during the service life and are not compatible with traditional recycling processes.

Method used

Ink compositions for digital printing on plastic articles are developed, comprising a base ink, an ink removal-promoting additive, and a carrier, which are configured to separate from the plastic surface at elevated temperatures during recycling by incorporating hydrophilic or acidic components that enhance ink separation.

Benefits of technology

The ink compositions effectively facilitate the removal of digital images from plastic containers during recycling, maintaining adhesion during the service life and ensuring compatibility with traditional recycling processes, thereby reducing contamination and improving recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580431000016
    Figure 0007580431000016
  • Figure 0007580431000017
    Figure 0007580431000017
  • Figure 0007580431000001
    Figure 0007580431000001
Patent Text Reader

Abstract

Providing an ink composition for digital printing on the exterior surface of a plastic article [Solution] The present disclosure relates to ink compositions for digital printing on the exterior surface of plastic articles. The ink composition includes an ink removal promoting additive. In some embodiments, the ink removal promoting additive comprises: The image separates or releases from the outer surface of the article when exposed to a liquid-based solution at elevated temperatures The disclosed ink compositions can be used to print images. and a plastic container containing the cured ink. This summary is also provided as a guide for scanning specific areas of technology. It is intended as a tool and not as a limitation of the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is a continuation of U.S. patent application Ser. No. 14 / 846,032, filed Sep. 4, 2015. This application claims priority to U.S. patent application Ser. No. 10 / 299,433, filed Oct. 30, 2014. This is a continuation-in-part of US Pat. No. 4 / 528,324, which was filed June 24, 2011. This is a divisional application of U.S. patent application Ser. No. 13 / 168,181, which is currently U.S. Pat. ,979, which is a part of U.S. Provisional Patent Application No. 6,490,482, filed on July 1, 2010. 1 / 360,512, filed October 20, 2009. This is a continuation-in-part of U.S. patent application Ser. No. 12 / 581,952 filed on October 20, 2008. This application claims priority from U.S. Provisional Patent Application No. 61 / 106,860, filed on the same day as the above-mentioned application. All are incorporated by reference herein as if fully set forth herein. do.

[0002] Technical Field The present invention generally relates to ink compositions for digital printing on the exterior surfaces of plastic articles. The present invention provides a digital image having improved adhesion and / or recycling properties. Plastic articles having digital images printed thereon, including plastic containers, and It also relates to a method for facilitating the recycling of [Background technology]

[0003] The plastic packaging industry continues to take advantage of ever-increasing amounts of recycling. have recently developed a method to compete with and potentially replace previous conventional labeling techniques. We have begun to manufacture containers with digitally printed labels of sufficient image quality and quality. Examples of suitable printing techniques are commonly owned U.S. Pat. Nos. 7,625,059 and 7,7 36,713, which are incorporated herein by reference.

[0004] A potential challenge is the ability to recycle containers with digitally printed labels in traditional container recycling processes. Some of the problems that arise when implementing the present invention are discussed and addressed in U.S. Patent Application Serial No. 12 / 581,952. This is also incorporated by reference in its entirety herein. There is a strong consensus among landowners, end users and local governments on the recycling of plastic containers. There is a clear trend to improve and increase the current recycling efforts. are sufficiently compatible with the standards and processes, or provide sufficient incentives to achieve industry-wide change. It is desirable to provide industry acceptable incentives and / or quantities. At least initially, the current industry standard process, typically caustic hot washing and grinding, will be used. It is desirable to provide a recyclable digitally printed article using a process comprising: As such, it will likely adhere to the article for its useful life without quality problems. but digital images that can be more easily removed during the plastic recycling process. There is a need for digitally printed plastic articles, such as containers, that have Summary of the Invention [Means for solving the problem]

[0005] In an exemplary embodiment, an ink composition for digital printing on a plastic article is disclosed. The ink composition generally comprises a base ink; an ink removal enhancing additive; and an ink removal enhancing agent. The removal-promoting additive comprises a carrier capable of dissolving at least a portion of the removal-promoting additive. The printed digital image is heated to or near a predetermined elevated temperature using a liquid-based (e.g., water-based) When exposed to a solution of 1,000 ppm water, the ink at least partially adheres to the plastic article. Such a predetermined elevated temperature may be configured or selected to separate or release the This may include, but is not limited to, those associated with conventional recycling processes.

[0006] In another embodiment, a recyclable material is provided having an exterior surface on which a digital image is printed with cured droplets of ink. A removable plastic article is disclosed. The ink droplets are coated with a removable additive. The ink composition includes a composition of matter as summarized in the following: Method embodiments for and methods for facilitating such recycling are also disclosed.

[0007] Further advantages of the present invention will be described in part in the following description and in part in the following claims. The advantages of the present invention will become apparent from the description or may be learned by the practice of the invention. The objects of the present invention will be realized and attained by means of the elements and combinations particularly pointed out in the appended claims. It will be understood that both the foregoing general description and the following detailed description are exemplary and explanatory. It should be understood that these are merely illustrative and are not intended to limit the invention as claimed.

[0008] Embodiments of the present invention will now be described, by way of example, with reference to the accompanying drawings, in which: [Brief description of the drawings]

[0009] [Figure 1]1 generally illustrates a side view of a portion of a plastic container having a digital image printed thereon according to an embodiment. [Diagram 2] 1 is a generic representation of a quality review table / matrix that may be used to evaluate the acceptability of a printed image onto a plastic article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In various aspects, reference will now be made in detail to embodiments of the invention, Examples of such are described herein and illustrated in the accompanying drawings. However, it is understood that the present invention is not limited to these embodiments. It will be understood that the present invention is defined by the appended claims. It is intended to cover alternatives, modifications, and equivalents that may fall within the spirit and scope of the invention. will be done.

[0011] In a general, but non-limiting, context, a plastic sheet having an embodiment of a printed image 20 is A portion of a surface 10 of a container (e.g., container) is generally illustrated in FIG. The embodiment shown may consist of multiple basecoat ink droplets 32 and multiple secondary ink droplets 34. The base coat 30 may also include a secondary coat 40, which may consist of ink droplets 42. Includes.

[0012] Containers (including bottles) in connection with this disclosure may be made of plastic materials or resins (e.g., ABS (acrylonitrile butadiene styrene), polyethylene terephthalate (PE T), polystyrene (PS), polyethylene (PE) (high density polyethylene (HDPE) Polypropylene (PP), polyvinyl chloride (PVC), etc. The container may be a single or multi-layer container and may be manufactured by, but not limited to, injection molding, blow molding, or the like. The molded article may be formed using a variety of conventional molding techniques, including molded, thermoforming, and the like. In an embodiment, the outermost layer / surface may be made of virgin plastic material. The container according to the teachings of the present application has a certain degree of recycled content, including a certain percentage of recycled content in the outer layer of the container. Note that percentage recycled content may also be included.

[0013] In an embodiment, the article (e.g., a container) is coated with a first coat or a base coat (e.g., The base coat 30 may include a base coat 30 (shown in FIG. 1). The base coat 30 may be printed on the exterior surface of the article. (e.g. digitally printed by a drop-on-demand inkjet process) The base coat may consist of a plurality of base coat ink droplets 32 that are subsequently cured or cured. The ink may be a UV curable ink, but this is not a limitation. However, it can be applied by a variety of known means including UV or LED lamps. The ink droplets can be monomer-based and can be cured by UV radiation. This helps improve the application of ink droplets (e.g., providing good process properties for printing). ), and / or visual characteristics (e.g., color or texture) of the ink composition. In embodiments, the base coat 30 may include white and / or colorless portions. Furthermore, for the disclosed ink droplets, i.e., those that are monomer-based, curing is The ink droplets can be polymerized. Since the ink used is not solvent-based, the ink Unlike solvents, the ink does not go into solution during the recycling process and does not release volatiles. It can be configured to not emit any harmful substances. The Pollution Agency (EPA) has published guidelines on solvents. Note that the polymer is a solid and does not flash off or release volatile materials. That is, the separation of the ink as disclosed herein occurs when the ink is in a cured polymeric state; It can be physically removed (e.g., in the form of flakes or films) and thus is part of the chemical dissolution. Rather than being contained within, they may be mechanical in nature.

[0014] As summarized above, the ink composition that makes up the ink droplets includes a removal-enhancing additive. In some embodiments, the "removal enhancing additive" comprises at least one hydrophilic or acidic component. The hydrophilic component may include one or more composition elements that exhibit hydrophilicity (water-loving properties). The acidic component may include one or more composition elements that exhibit acidity. In some embodiments, The removal-promoting additive is a combination of a hydrophilic component and an acidic component, i.e., at least two Some ink droplet compositions include a removal-promoting additive. In "binary" compositions, which contain both hydrophilic and acidic components, the composition contains only one additive. A smaller percentage by weight (of the total) is used to provide results equivalent to those achieved by using the composition. may be used.

[0015] Such hydrophilic components include hydrophilic monomers, hydrophilic oligomers, etc. that provide the desired functionality. Hydrophilic monomers often contain a water-dispersible monomer in the backbone structure. In addition to halogens, they are characterized as having oxygen or nitrogen atoms. Such monomers are generally susceptible to attack by polar solvents such as water and ketones. Monomers also tend to be less resistant to thermal degradation. When included in the associated ink droplets, they can be easily removed at a later point in time (e.g., at the time of recycling after use). Improve separation of the image (i.e., cured ink droplets) from the plastic structure of the article By way of example and not limitation, in the cured state, the hydrophilic portions of the polymer can Normally, it will absorb water. When this happens, the water acts as a plasticizer and dissolves the polymer. This can increase the mobility of the chains. Increased mobility softens the polymer, making it more susceptible to removal. As such, removal-enhancing additives (e.g., hydrophilic A plastic article such as a container having an image formed of an ink composition containing a soluble monomer is immersed in a liquid. Upon exposure to a base solution (e.g., agitated water) at elevated temperatures, the ink composition (i.e. This will facilitate the softening of the hydrophilic monomer and separation of the image from the plastic material. The elevated temperature may be any temperature above which the article is generally found in normal use. Further, to the extent desired, the adhesion separation threshold may be a temperature at which the softening and subsequent removal occurs. occurs substantially only at high temperatures (e.g., during the recycling process) and during normal intended use. The aliphatic urethane acrylate may be configured to be substantially prevented during use. The general list of hydrophilic monomers that generally absorb water and can potentially be used as hydrophilic components is given below. Furthermore, they are classified as inkjet / digital printing applications. Some hydrophilic oligomers are suitable for the application of the viscoelastic polymers, provided that the viscosity is adequate (i.e., not too high). may also be used as the hydrophilic component.

[0016] In some embodiments, without limitation, the removal-enhancing additive comprises: That is, the percentage by weight of the relevant ink and removal-promoting additive is approximately 0% to 2% by weight. In some embodiments, the hydrophilic monomer may be in the range of 0 to 10 weight percent. The percent weight of the additive will be within the approximate range of 0-10% of the total weight. Although not intended to be limiting, examples of hydrophilic monomers that may be used include methoxypolyethylene glycol. Monoacrylate (e.g., Sartomer USA, LLC (Sartomer) The CD553 is commercially available from .

[0017] Some water-dispersible monomers are also hydrophilic and appear to absorb water upon curing. Note that in such compositions, water acts as a plasticizer to reduce the viscosity of the cured ink composition ( For example, by softening the hardened ink film on the surface of the container, the ink film can be removed during the recycling process. In an embodiment of the present disclosure, a suitable hydrophilic component is included in the ink composition. This allows the ink to maintain its jettability and adhesion to the article substrate over the life of the article. This makes it possible to impart hydrophilicity to the ink while maintaining the ink-repellent property.

[0018] The acidic component includes acidic monomers that have a measurable acidity value. The measurable amount can be determined by pH, Acid weight percentage, or titration value of alkaline chemicals (e.g., mg KOH / g [mono Note that the concentration may be based on milligrams of potassium hydroxide per gram of mer. Additionally, for example, in the cured state, the acidic moieties of the polymer may be vulnerable to caustic solutions. The reaction between the acidic functionality of the polymer chain and the alkalinity of the solution results in a This may result in a decrease in adhesion to the polymer and promote separation of the polymer. Although not limiting, examples of acidic monomers that may be used include acidic acrylate oligomers (e.g., For example, CN147, commercialized by Sartomer) and monofunctional acid esters (e.g. For example, CD9050, which is commercialized by Sartomer, can be mentioned. When a container containing an acidic component comes into contact with a cleaning solution (e.g., a conventional caustic cleaning solution), the associated bonds Destruction promotes the intended separation of the printed image (ink droplets) from the plastic substrate possible.

[0019] In another embodiment, the removal-promoting additive is capable of promoting the removal of the cured ink composition from the surface of a plastic article. configured or otherwise selected according to desired properties that can facilitate removal of For example, in one embodiment, the removal-enhancing additive may be a scavenging agent that is not normally utilized in conventional recycling processes. Relatively high solvent solubility and It is desirable to exhibit relatively high water solubility. To this end, according to an exemplary embodiment, The removal-promoting additive exhibits a glass transition temperature (Tg) of less than about 130° C. This is in contrast to the removal-promoting additive, which exhibits a glass transition temperature (Tg) of less than about 120° C. Less than about ℃, less than about 110℃, less than about 100℃, less than about 90℃, less than about 80℃, less than about 70℃ , a removal promoter that exhibits a glass transition temperature (Tg) that is less than about 60° C., or even less than about 50° C. In a further embodiment, the ink removal promoting additive can include a catalyst that is capable of reacting with the ink at a temperature of about 50° C. to about 50° C. It has a glass transition temperature (Tg) in the range of about 130° C. In yet another embodiment, the ink removal The accelerator additive is used at about 55°C to about 125°C, or at about 65°C to about 105°C, or at about 55°C to about In yet another embodiment, the ink removal agent has a glass transition temperature (Tg) in the range of about 95° C. The additive may have a glass transition temperature (Tg) in any range derived from any of the exemplary values ​​above. ) may be present.

[0020] As one of ordinary skill in the art will appreciate, the desired level of water solubility can be determined, for example, by the acid number of the removal-enhancing additive. The acid number can be characterized as a function of the titration value of an alkaline chemical (e.g., mg KOH / g [milligrams of potassium hydroxide per gram of removal-enhancing additive]) and In these embodiments, the removal-promoting additive may be expressed as 110 mg KOH / glucose. Rum, 120mg KOH / gram, 130mg KOH / gram, 140mg KOH / gram, 150mg KOH / gram, 160mg KOH / gram, 170mg K OH / gram, 180mg KOH / gram, 190mg KOH / gram, 200mg KOH / gram, 210mg KOH / gram, 220mg KOH / gram, 230 Approximately 100 mg KOH / gram, including values ​​of 240 mg KOH / gram It may exhibit an acid value ranging from about 250 mg KOH / gram to about 300 mg OH / gram. In one embodiment, the ink removal enhancing additive comprises 175 mg KOH / gram, 185 mg KO Approximately 150 mg KOH / gram, including values ​​of 195 mg KOH / gram and 150 mg H / gram. In yet another embodiment, the ink has an acid value in the range of about 205 mg KOH / gram. The removal-enhancing additive may have an acid number in any range derived from any of the exemplary values ​​above. This can be done.

[0021] In a further aspect, the removal-promoting additive has a glass transition temperature (Tg) of less than about 100° C. and Exhibits an acid value in the range of approximately 100 mg KOH / gram to approximately 250 mg KOH / gram In yet another embodiment, the ink removal promoting additive can be used at a temperature in the range of about 50° C. to about 90° C. Glass transition temperature (Tg) and about 150 mg KOH / gram to about 205 mg KOH / gram In yet another embodiment, the ink removal enhancing additive can exhibit an acid number in the range of: The glass transition temperature (Tg) and any range of acid numbers derived from any of the exemplary values ​​above. It is possible to have.

[0022] Selecting a removal-enhancing additive that exhibits a desired combination of water solubility and glass transition temperature This also facilitates the ink removal process as a prelude to the recycling process. It is possible to provide a curable ink that exhibits desirable adhesion, scratch resistance, and solvent resistance. When exposed to a caustic aqueous environment at a temperature above the Tg of the removal-promoting additive, the softening of the additive occurs. This results in relatively clean peeling of the cured ink layer from the surface of the printed plastic. This could result in separation.

[0023] These removal-promoting additives may be present in amounts of about 1 to about 20 weight percent of the ink composition. It can be present in the composition of 2, 3, 4, 5, 6, 7, 8, 9, 10, Specific weight percent of 11, 12, 13, 14, 15, 16, 17, 18, and 19 The exemplified amounts may further be included. In a further aspect, the ink removal enhancing additive comprises: It can be present in any amount ranging from any of the exemplary values ​​above. For example, the removal-promoting additive may be present in an amount of about 5 to about 20 weight percent of the ink composition. It can be present in the composition.

[0024] In an exemplary embodiment, the present invention provides an ionic liquid that exhibits the above combination of aqueous solubility and relatively low glass transition temperature. The ink removal enhancing additive comprises a styrene maleic anhydride resin. The maleic anhydride resin may be a copolymer of styrene and maleic anhydride. In yet another embodiment, the styrene maleic anhydride is an esterified styrene maleic anhydride. Exemplary, non-limiting, commercially available stearate acids suitable for use as removal enhancing additives are The maleic anhydride resin is manufactured by Total under the Cray Valley trademark SMA. ) 3840 and SMA® 1440F resin.

[0025] In a further embodiment, the ink composition that makes up the ink droplets contains at least one ink removal enhancing additive. The carrier may be monomer-based or may be at least partially solubilized and dissolved. Exemplary Monomers that Can Be Used as Carriers In an exemplary embodiment, suitable acrylic monomers include 1,3-butylene glycol diacrylate, 1,6-hexanediol diacrylate acrylate, 1,3-butylene glycol dimethacrylate, isobornyl acrylate, Examples of the methacrylate include isodecyl methacrylate, and combinations thereof. In one embodiment, the acrylic monomer is 1,3-butylene glycol diacrylate, 1,6 -Hexanediol diacrylate, and 1,3-butylene glycol dimethacrylate As noted above, in embodiments, the removal-promoting additive can be solubilized. The carrier can be solvent-based. Suitable solvents in some aspects are aprotic Specific non-limiting examples of suitable solvent carriers include: Examples include N-methyl-2-pyrrolidone (NMP) and acetone.

[0026] The carrier component is present in the ink composition in an amount of about 1 to about 20 weight percent of the ink composition. This can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 1 Specific exemplified amounts of 3, 14, 15, 16, 17, 18, and 19 weight percent In a further aspect, the carrier can further comprise any of the above exemplary values. For example, the carrier may be present in an amount ranging from about 100 to about 150 parts by weight of the ink composition. It may be present in the ink composition in an amount of from 5 to about 15 weight percent.

[0027] The base ink portion of the ink composition may be any ink known in the art, such as a conventional UV curable ink. The base ink may be any curable ink. , 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 8 Exemplary weight percent values ​​of the ink composition include 2, 83, and 84 weight percent. It may be present in the ink composition in an amount ranging from about 50 to about 85 weight percent. In some embodiments, the base ink has a viscosity of about 100%. For example, the base ink may be present in an amount of about 65 to about 85% by weight of the ink composition. The pigments may be present in the ink composition in any amount up to about 100% by weight percent.

[0028] In one exemplary embodiment, (a) about 65 to about 85 weight percent of the base ink; (b) about About 5 to about 20 weight percent of an ink removal enhancing additive having a glass transition temperature of less than 100°C. and (c) about 500 nm in length capable of dissolving at least a portion of the ink removal enhancing additive. Disclosed herein is an ink composition comprising: According to a preferred embodiment, the base ink can be a base UV white ink, and the ink removal The removal-promoting additive can be a styrene maleic anhydride resin and the carrier can be a solvent-based. It can be N-methyl-2-pyrrolidone (NMP), or acetone, or other The solvent may include any acceptable solvent.

[0029] As described herein, the present invention includes a digitally printed image printed directly onto a curved exterior surface. A recyclable plastic article is disclosed, the image being printed as described above in the present specification. In a further aspect, the present invention relates to a method for producing a recyclable plastic article comprising the steps of: The article includes a curved outer surface having a digitally printed image printed directly onto the curved outer surface, the cured droplets of ink being and a composition comprising an ink removal enhancing additive having a glass transition temperature of less than about 100° C. In yet another embodiment, the digitally printed image comprises at least 6 droplets of ink containing the object. With adhesion scores of .0 and up to 9.0, the removal-facilitating additive reduces the chance of digitally printed images When exposed to a basic solution at an elevated temperature of about 70° C., the hardened droplets of the ink are applied to the curved outer surface of the article. The present invention is configured to separate or release the

[0030] In a further aspect, the article comprises a plastic container. In yet another embodiment, the plastic container is a bottle. Of these, polyethylene, polyethylene terephthalate, high density polyethylene, and polypropylene It consists of one or more of the following.

[0031] In a further aspect, the removal-promoting additive present in the ink composition is , exposed to a liquid-based solution, e.g., an aqueous or water-based solution, at a predetermined elevated temperature. Sometimes, it is configured to cause cured droplets of the ink to detach or release from the curved outer surface of the article. For example, the hardened droplets of ink tend to freeze at high temperatures, such as in the range of about 70-90°C, when a digitally printed image is exposed to these temperatures. When exposed to a basic solution having a pH of about 10, 11, 12, or 13, the article In a further aspect, the basic solution can be separated or released from the curved outer surface of the According to an embodiment, the solubility of the solubility-containing cellulose in the cellulose acetate solution is increased by exposing the solubility-containing cellulose in the cellulose acetate solution to a high temperature for a sufficient period of time. After exposure, at least about 90 percent by weight of the cured ink droplets detach from the curved outer surface of the article. In yet another aspect, the digitally printed image comprises a plurality of cured basecoat ink droplets. and a second coat comprising a plurality of cured second coat ink droplets, A subsequent coat is applied over at least a portion of the base coat.

[0032] By way of example and not limitation, UV cured prints having a removal enhancing additive blended therein An embodiment of a polyethylene terephthalate (PET) container containing ink is subjected to an ink removal test. The blended removal-promoting additives in the tested containers were acidic monohydrates of the type described above. mers, i.e., acid acrylate oligomers and / or monofunctional acid esters. The container is unique in the field of plastic container recycling, where the solution is heated to about 85°C. As is commonly known, a pH level of at least 9.0 can aid in label removal. Various samples were exposed to these conditions for 12 minutes. and rated on a scale of 0 to 5 as follows:

[0033] 0 - no improvement in removal compared to control sample

[0034] 1 - Minimal improvement observed, removal only in some areas by abrasion with a metal object Obtained.

[0035] 2 - Some improvement was observed and the entire film could be removed by scraping with a metal object. Done.

[0036] 3 - The cured ink film was removable by scraping it off with a fingernail.

[0037] 4- The cured ink film is easily removable by simply wiping it off with a clean wipe. It was.

[0038] 5 - The cured ink film peeled off during the wash test.

[0039] The test identified, among other things, solutions that exhibited removal performance levels of 4 or 5. However, a level of at least 4 is not always necessary, and in some applications a lower level may be used. Lower removal levels may be acceptable. Test results show that the blended removal-enhancing (acidic) When the additive is included in the ink composition, it reduces the amount of oxidative damage from the plastic (PET) material of the cured ink. Both forms of the acidic additives were shown to provide a significant improvement in the removal of In this test setup, monofunctional acid esters (10% each) showed improvement in ink removal. A somewhat smaller composition percentage of acidic acrylate oligomer was used, as opposed to 15% (p<0.01). and got at least level 4 removal level.

[0040] In embodiments, the ink composition may optionally include a hydrophobic component. The composition may, for example, include a hydrophilic component and a hydrophobic component. Hydrophobicity is generally related to polarity. Many hydrophobic monomers Mers are characterized as having an organic backbone structure composed primarily of hydrogen and carbon; therefore, Therefore, such monomers tend to be non-polar and cannot be dissolved in polar solvents (e.g., water and alcohols). In such two-component embodiments, the polymer provides resistance to hydroxyapatite (H2O), as well as to acids and bases. The ink composition may comprise a hydrophilic component and a hydrophobic component (e.g., a hydrophilic monomer and a hydrophobic monomer). The hydrophobic monomers allow the ink droplets to adhere to the article substrate. Hydrophilic monomers can help the image to remain in the recycling process / bath (e.g., This can aid in softening (and further separation) when exposed to hot, agitated water.

[0041] In the embodiment of the container with the printed image, at least a first base coat 30 (hydrophilic composition) is applied. (which may include minutes) may be applied to the surface of the container at an initial time t1 and an initial temperature T1. Temperature T1 will be in the range of temperatures suitable for application of the relevant base coat. Now, the base coat 30 may be curable (e.g., ultraviolet (UV) curable). , and may be cured prior to application of a second coat.

[0042] In some embodiments, the secondary coat 40 is distributed over at least a portion of the base coat 30. In addition, the ink droplets 42 may be formed by applying a second coat of ink to the ink droplets 42. Additional layers of coating (e.g., a tertiary layer, etc.) may also be applied to the secondary coating 40. In an embodiment of the present disclosure, the second coat ink droplets 42 also comprise an ink composition that includes a hydrophilic component. The composition may be made of a material other than the above-mentioned.

[0043] A plurality of secondary coat ink droplets 42 may collectively form a portion of a coating pattern, The coating pattern may then form all or part of an image. As illustrated, portions of one or more adjacent secondary coat ink droplets 42 overlap one another. The secondary coat 40 and the secondary coat ink droplets 42 of the composition may be mixed or intermixed. includes, but is not limited to, the primary printing colors such as cyan, magenta, and yellow. It may include a variety of known colors. Additionally, overlaps or combinations of specific colors in specific regions may be used. By controlling the combination, additional "process" colors can be provided. The ink droplets 42 may be curable. For example, a UV curable second coat ink droplet may be used. The droplets may contain all or part of the intended image. Curing is accomplished by radiation. In this case, the ink composition may include a photoinitiator. Two bonds - the polar bond between the ink polymer and the plastic, and the microscopic Functionality resulting from plastic surfaces having uneven surfaces at the mechanical level (e.g., microstructure) Note that in many embodiments of the present disclosure, both may be held together primarily by a mechanical connection. In some applications, hydrophilic components attack the mechanical bonds. While the acidic component may work better on polar bonds, the acidic component may work better on polar bonds. Depending on the size of the ink droplets, the secondary coat ink droplets may vary in diameter, for example, from about The thickness of the second coat 40 may range from 10 microns to about 200 microns. At a time t2 and a second temperature T2, a second coat 4 may be applied to the surface 10 of the container. The second temperature T2 at which the base coat 30 is applied is typically the first temperature T1 Lower than.

[0044] In an embodiment of the present invention, the time between application of the base coat and application of the secondary coat (e.g. , t2 minus t1) may be reduced, for example, to just 10 seconds or less. The application time difference will be within 2 to 6 seconds. Further, in an embodiment, the base coat 30 between the temperature at which the second coat 40 is applied to a portion of the base coat 30 and the temperature at which the second coat 40 is applied to a portion of the base coat 30. The application temperature differential, ie, T1 minus T2, can be controlled to be about 10°F or less. In some embodiments, the application temperature differential will be within about 5° F. to about 10° F. In some applications, the application temperatures should be close to each other - i.e. The base coat 30 and the secondary coat 40 are preferably arranged so that the temperature difference between the layers is reduced or minimized. It may be desirable to modify the application and associated temperature of T1. (b) a decrease / reduction in T2, or (c) a combination of (a) and (b). Such time periods for the base coat and the second coat can be achieved. And / or temperature control can provide better adhesion of the printed image to the article. .

[0045] In addition to time and temperature, irradiance can also affect the effective cure rate of a printed image. Note that certain factors, i.e., at certain times (e.g., t1 and t2) and At temperatures (e.g., T1 and T2), the associated irradiance, i.e. 、 ε1 and ε2 may be present For example, in an embodiment, the base coat may be cured at an irradiance of ε1, and the associated secondary The coat may be cured at an irradiance of ε. Further, in an embodiment, the effective cure rate is The temperature may be based on a combination of temperature, duration, and irradiance, but the irradiance is generally determined by the following formula: Irradiance (ε)=(dΦ / dA) where Φ = irradiance (measured in watts), and A = area (cm 2 )) can be given by .

[0046] For example, and without limitation, the irradiance range for some embodiments is about 0. 1 watt / cm 2 ~ approx. 10.0 watts / cm 2 It will be between.

[0047] For example, a curable ink (e.g., a UV-curable or radiation-curable ink) is used. In some applications, the associated coat or ink is cured after each printing station. For example, and without limitation, embodiments of the process may include, at least in part, Typically, the process may include applying a base coat; curing; applying a second coat; and curing. Alternatively, and by way of further example and not limitation, the process may comprise, at least in part: , application of base coat; curing process; application of base coat; curing process; application of second coat; and a curing step.

[0048] Furthermore, in an embodiment of the present invention, the manufacturing / subsequent handling rate of the container / bottle is It may be desirable to match or substantially match the flow / process speed of the press(es). There is a gender.

[0049] Additionally, the quality of the printed image is controlled, at least in part, by one or more of the following techniques: It has been found that the performance of the system can be controlled and / or improved. (a) Ink set selection and / or calibration; (b) controlling the substrate (i.e., vessel surface) temperature; and / or (c) Timing control.

[0050] With respect to the selection and / or calibration of the ink set, this is at least in part based on This is achieved by the selection and / or calibration of the ink, including the second coat. The blocks may be combined to provide desired time and / or temperature characteristics, including in combination with one another. For example, it has been discovered that a particular viscosity having a given The choice of ink can indicate or provide a particular desired temperature related effect.

[0051] With respect to controlling the substrate (i.e., vessel surface) temperature, the relevant portion of the side wall (or other portion of the vessel) The temperature of a given part of the container can be manipulated or controlled to a certain extent. The part may be pretreated. Such pretreatment may include, but is not limited to, flame, This can be facilitated using a variety of known techniques, which may include corona and plasma treatment. However, the present invention is not limited to those specific pretreatment techniques.

[0052] With regard to timing control, for example, the times associated with the movement of a container through a manufacturing machine, etc. In addition, the timing of application of the base coat and / or second coat can be controlled. The manufacturing / subsequent handling speed of the container / bottle depends on the flow / process of the associated printing machine(s). It may be desirable to match or substantially match the speed.

[0053] This disclosure relates to the “acceptance” of containers having printed images, such as digitally printed labels. In other words, in an embodiment of the present invention, The system for assessing or evaluating can provide an "adhesion score." can generally be used to assess or evaluate the acceptability of a printed image on a container. Represents a quality review table / matrix. As commonly shown, the Y-axis represents pass or fail. In the illustrated embodiment, the numbers 1-5 represent the containers. Numbers 6-9 indicate that the associated container is receptive, while numbers 7-9 indicate that the associated container is receptive. At least 6 would "pass" as acceptable with respect to this table / matrix, The present invention is not limited to the specific tables / matrices shown or to more scores. may be provided and / or the passing score may be increased or decreased as desired or needed. It is important to note that the rate of decline could have been much higher or lower. A number of tests, which may include a standard test, are represented in columns on the x-axis. For example, in the limit Alternatively, test 1 may include the "Sutherland friction test" and test 2 may include the "3M #610 Tape Test, and Test 3 is the "Simulated Test 4 may include the "3M#810 Tape Test" and Test 5 may include the "3M#810 Tape Test". As generally indicated in the table, the various pass or fail designations are For some of the "standard" tests mentioned above, the tests are may be modified to be suitable for use in conjunction with printed images, as opposed to labels that are distributed For example, various "tape" tests that may comply with ASTM D 3359-08 standard include / Matrix and related tests are performed by cutting the image area with a cutting tool before applying the adhesive tape. That is, in one embodiment, "Test 2" may or may not include cutting the , unless a portion of the image of the container being tested is cross-cut or otherwise may include a "modified" 3M #610 tape test, provided that the container is not separated from the container. In addition, the table in Figure 2 shows the results of the tape test (i.e., the cross-sectional area of ​​the test piece) which is a direct implementation of the modified ASTM standard. A "pass" indication for the test without loss cut / separation is generally 2.0 mm 2 below The ASTM standard is a direct implementation of the tape test. For testing, the indication of "pass" generally means a classification of "4B" or "5B" (ASTM standard (Classification of adhesion test results in Figure 1 below) or contains less than 5% of the printed area removed. It becomes.

[0054] In one embodiment, at a minimum, the tape passes a modified 3M #610 tape test and Containers with printed images (e.g., digitally printed images) that are still "recyclable" It is advisable to provide a digital image printed on the container that conforms to ASTM D 3359. Using the standard #810 tape test, achieve less than a "4B" classification (i.e., 5% of the area Test 2 (modification 3M#610) is considered "recyclable" if Test 3 (3M#810 tape test) and Test 4 (simulated shipping test) were passed. Containers with digital images that fail the 6.0 or 7.0 test should be The print image will achieve an adhesion score of 6.0 or 7.0. Such containers are sufficient for normal / intended use, but preferably are suitable for subsequent recycling. While providing a printed image and associated adhesive that is separable for transportation (i.e. , pass the mock production test) is commercially suitable. In other words, The image and associated adhesion are strong enough for the intended use but do not allow separation during recycling. Do not interfere.

[0055] For such tables / matrices, each test should include appropriate (e.g., statistically significant) After all testing has been completed, The results may be tabulated into a table / matrix to provide an "adhesion" score. The relevance score results can then be correlated.

[0056] Among other things, the teachings of the present disclosure can provide improved recyclability. Recycling ink printed on various items in a cost-effective manner provides benefits to the environment. In addition, it can provide many cost and efficiency advantages. For example, it limits However, the ink composition may at least partially include a hydrophilic component and / or an acidic component. A digital ink composition (which may be formed by curable UV ink or radiation curable ink) The containers bearing the printed images can be conveniently recycled in conjunction with conventional plastic recycling processes. The industry-standard recycling process for plastic packaging has traditionally consisted of removing These flakes are then subjected to a high-temperature caustic cleaning process. drying the cleaned flakes, sorting, and reselling the resin. In an embodiment embodying aspects of the disclosed teachings, The digital image on the vessel may remain on the resin flakes after the grinding process, The image is substantially separated from the resin flakes during the hot caustic washing process, which may be agitated. , thereby not contaminating the clean resin flakes that are to be formed into resin pellets. .

[0057] The separation technique involves the use of polar and / or mechanical bonds to facilitate the removal of the ink from the article. At least four that can be used alone or in various combinations to attack the This technique involves the use of (1) a hydrophilic component or a hydrophilic component as described herein. For additives having the desired Tg and acid value as described, water or liquid based (2) a solution (e.g., a solution having an acidic component or a Tg and acid number as described herein); (caustic components for additives with desired combinations) - i.e., chemical reactions that break down polar bonds (3) heat or temperature; and / or (4) mechanical force (e.g., high pressure spray (psi)); or any combination thereof Includes:

[0058] This disclosure describes a number of recycling processes that can be used to remove ink from articles. For example, one embodiment of a method for recycling plastic containers includes: and providing a plastic container having a printing image thereon, the ink composition comprising a removal-facilitating additive. an additive (e.g., a hydrophilic or acidic component); one embodiment of the method further comprises: The tal image is then mixed with a liquid-based solution (e.g., water with or without caustic components). ), and optionally agitating the solution. Before or after the exposure, the container is Similar embodiments may be used for dry grinding, cleaning, washing, drying, and It could be said to be along the lines of including purification.

[0059] It may be more similar to conventional industrial recycling and is commercially available (e.g., SOREM A(Italy)) Another process is single washing, wet grinding, centrifugation, screening, and flow "Single wash" may be said to include, for example, high pressure washing (e.g., caustic high temperature wash) and the bottles (e.g. set screw or multi-screw systems) This can be used by transporting the label to aid in label removal. Mechanical force components can be applied. Usually, the bottle is as a whole, i.e., The polymerized ink-containing material is washed away and transported under the conveying mechanism. The waste may fall into the collection or grating system.

[0060] In a further aspect, the present disclosure provides a method for removing cured ink from a plastic container. The method includes: (a) digitally printing a sample by a drop-on-demand inkjet printing process; Curved exterior where the image is printed directly onto the curved exterior of the plastic container, the curved exterior of the plastic container The ink composition may include a hardened droplet of ink applied directly to an exterior surface and may have a viscosity of at least 6.0 and up to about 9.0. An image having an adhesion score and ink removal promotion having a glass transition temperature of less than about 100° C. providing a plastic container having droplets of ink containing the composition including the additive; b) heating at least a portion of the digitally printed image of the plastic container to a high temperature of at least about 70° C. (c) exposing at least a portion of the digitally printed image to a basic solution at room temperature; , removing the image from the curved outer surface on which it is printed.

[0061] In a further aspect, the plastic container is a bottle. The plastic container is made of the following materials: polyethylene, polyethylene terephthalate, high density polyethylene The plastic may be made of one or more of the following materials: polyethylene, polyethylene, and polypropylene.

[0062] In a further aspect, the ink removal enhancing additive comprises a styrene maleic anhydride copolymer. In a further embodiment, the ink removal enhancing additive is a glass paste having a temperature in the range of about 50° C. to about 130° C. In yet another embodiment, the ink removal promoting additive has a transition temperature (Tg) of about 65° C. to about 65° C. The glass transition temperature (Tg) is in the range of about 110° C. In yet another embodiment, the ink removal The enhancing additive has a glass transition temperature (Tg) in the range of about 55° C. to about 65° C. In one embodiment, the ink removal enhancing additive is from about 150 mg KOH / gram to about 205 mg KOH / gram. In yet another aspect, the ink removal enhancing additive has an acid number in the range of: It has an acid value ranging from about 165 mg KOH / gram to about 205 mg KOH / gram.

[0063] In a further embodiment, the basic solution is an aqueous solution having a pH in the range of about 12 to 13; The elevated temperature is in the range of about 70 to 90° C. In yet another embodiment, the removing step comprises removing salt of the image. After exposure to the basic solution, the ink is scraped or wiped from the container. In this embodiment, the ink is mechanically removed in the form of flakes or a film.

[0064] The foregoing descriptions of specific embodiments of the present invention have been presented for purposes of illustration and description. They are not intended to be exhaustive or to limit the invention to the precise forms disclosed. It is to be understood that various modifications and variations are possible in light of the above teachings. This application will now be described in detail, with reference to the principles of the present invention and its practical application, thereby making it suitable for the particular use contemplated. The present invention and its various embodiments, together with various modifications, are intended to enable those skilled in the art to utilize the present invention. The scope of the invention is defined by the appended claims and their equivalents. It is intended to be defined by equivalents. EXAMPLES

[0065] A. Experiment The following examples illustrate the compounds, compositions, articles, devices, and / or methods claimed herein. To provide those of ordinary skill in the art with a complete disclosure and description of how the methods may be made and evaluated. and are purely illustrative and are not intended to limit the present disclosure. Although efforts are made to ensure accuracy of information (e.g., quantity, temperature, etc.), some errors may occur. Differences and deviations should be taken into account. Unless otherwise indicated, parts are parts by weight and temperatures are ° C. or at ambient temperature and the pressure is at or near atmospheric.

[0066] In the following illustrative examples, various ink compositions according to the present disclosure were prepared and applied to plastic objects. The ink composition was first tested for use in direct printing on the exterior surface of an article. By dissolving the removal enhancing additive in a carrier and then adding the carrier solution to the base ink. The prepared ink composition can then be applied directly to the outer surface of a plastic article. Can be used for close printing.

[0067] The performance and recyclability of various ink compositions on plastic articles was also evaluated. An ink composition comprising a UV curable ink having an additive and a carrier was prepared using a polyethylene terephthalate (PET)-based ink. Polyethylene (PET), Polyethylene (PE) and / or High Density Polyethylene (HDPE ) was printed directly onto the surface of the sample and cured.

[0068] The cured ink samples are then tested for one or more of the following properties: adhesion, scratch resistance, and solvent resistance. The samples were subjected to an ink removal test that can include As is commonly known in the art, various bath solutions can be used to aid in label removal, e.g. A bath solution containing a pH level of at least 9.0 and in which the solution is heated to about 75° C. or 85° C. , a period including immediately after (immediately after) and one hour after (1 hour) treatment. And so the test was carried out.

[0069] The materials shown in Table 1 were used to prepare the compositions described and evaluated herein. [Table 1]

[0070] 1. Example 1 In the following examples, the removal enhancing additives in the test samples were waxes and resins. Acetone or N-methyl-2-pyrrolidone (NMP) (Sigma Aldrich) The ink formulations and performance data of the present invention are shown in Tables 2 to 5 below. In the following data, a "pass" indicates that no ink removal was observed; A "Fail" indicates that significant and / or complete ink removal was observed. The given percentage value corresponds to the observed % ink removal. [Table 2-1] [Table 2-2] [Table 2-3] [Table 2-4] [Table 3-1] [Table 3-2] [Table 3-3] [Table 4-1] [Table 4-2] [Table 5-1] [Table 5-2] [Table 5-3] [Table 5-4]

[0071] As the data shows, the SMA3840 and SMA1440F ink formulations showed improved The SMA3840 ink formulation showed some signs of improvement. , showing improved ink removal compared to the control. The SMA1440F ink formulation is typically did not demonstrate any significant symptoms during in-use testing ("in-use"), but did demonstrate strong Tests were repeated several times with PET, EPET, and PE, and all demonstrated removal of the caustic Tests showed good removal.

[0072] 2. Example 2 In this example, an ink composition comprising a white UV curable ink having a removal enhancing additive and a carrier The results are for polyethylene terephthalate (PET) and high density polyethylene (HDPE) samples. The removal-enhancing additive in the tested samples was styrene maleic anhydride. Acetic acid copolymer (SMA1440F, commercially available from Cray Valley USA, LLC) The carrier was N-methyl-2-pyrrolidone (NMP, Sigma-Aldrich) The ink formulations and performance data are shown in the table below. Presented at 6. [Table 6]

[0073] As the data shows, the nearly 100% removal of the ink composition of the present invention is greater than that of the standard ink. Only 50-60% removal was observed in the HDPE samples compared to the control. The ink composition removed 50% of the ink compared to approximately 10% for the standard ink control. The results of the ink composition of the present invention were compared with those of the Association Published by Postconsumer Plastic Recyclers Meets current recycling guidelines.

[0074] Various modifications and variations may be made to the present invention without departing from the scope or spirit of the invention. It will be apparent to those skilled in the art that other embodiments of the invention may be used. It will be apparent to those skilled in the art from consideration of the specification and practice of the invention disclosed. It is to be understood that the specification and examples are merely exemplary and do not represent the true scope and spirit of the invention. It is intended that this be as indicated by the following claims.

[0075] According to a preferred embodiment of the present invention, for example, the following is provided: (Section 1) 1. An ink composition for digital printing on a plastic article, comprising: (a) base ink; (b) an ink removal enhancing additive having a glass transition temperature of less than about 130° C.; and (c) a carrier capable of dissolving at least a portion of the ink removal enhancing additive. The ink composition comprising: (Section 2) The ink removal promoting additive according to the above item 1, comprising a styrene-maleic anhydride copolymer. The ink composition described. (Section 3) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 50° C. to about 110° C. Item 2. The ink composition according to item 1, (Section 4) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 55° C. to about 85° C. 2. The ink composition according to item 1, (Section 5) The ink removal promoting additive has a glass transition temperature (Tg) in the range of about 55° C. to about 65° C. 2. The ink composition according to item 1, (Section 6) The ink removal enhancing additive is from about 150 mg KOH / gram to about 205 mg KOH / gram 2. The ink composition according to claim 1, having an acid value in the range of 1 / gram. (Section 7) The ink removal enhancing additive is from about 165 mg KOH / gram to about 205 mg KOH / gram 2. The ink composition according to claim 1, having an acid value in the range of 1 / gram. (Section 8) The above-mentioned carrier contains a solvent, a monomer, or a combination thereof. The ink composition described. (Section 9) Item 9. The ink composition according to item 8, wherein the solvent comprises at least one aprotic solvent. thing. (Section 10) The solvent is N-methyl-2-pyrrolidone (NMP), or acetone, or 9. The ink composition according to item 8, comprising a combination of the above. (Section 11) Item 9. The ink according to item 8, wherein the monomer comprises at least one acrylic monomer. composition. (Section 12) The acrylic monomer is 1,3-butylene glycol diacrylate, 1,6-hexadecyl glycol diacrylate, Sandiol diacrylate, 1,3-butylene glycol dimethacrylate, isobol decyl acrylate, or isodecyl methacrylate, or a combination thereof. Item 12. The composition according to item 11. (Section 13) Item 2. The ink composition according to item 1, wherein the base ink comprises a UV-curable ink. (Section 14) Item 2. The ink composition according to item 1, wherein the ink composition is UV curable. (Section 15) (a) about 65 to about 85 weight percent of said base ink; (b) about 5 to about 20 weight percent of said composition having a glass transition temperature of less than about 130° C. Ink removal enhancing additive; and (c) about 5 to about 1000 sulphates capable of dissolving at least a portion of the ink removal promoting additive; 15 weight percent of said support Item 2. The ink composition according to item 1, (Section 16) 1. An ink composition for digital printing on a plastic article, comprising: (a) base ink; (b) an acid value in the range of about 100 mg KOH / gram to about 250 mg KOH / gram an ink removal enhancing additive having; and (c) a carrier capable of dissolving at least a portion of the ink removal enhancing additive. The ink composition comprising: (Section 17) Item 16 above, wherein the ink removal promoting additive comprises a styrene-maleic anhydride copolymer. The ink composition according to claim 1. (Section 18) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 50° C. to about 130° C. 17. The ink composition according to item 16, comprising: (Section 19) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 55° C. to about 85° C. 17. The ink composition according to item 16, (Section 20) The ink removal promoting additive has a glass transition temperature (Tg) in the range of about 55° C. to about 65° C. 17. The ink composition according to item 16, (Section 21) The ink removal enhancing additive is from about 150 mg KOH / gram to about 205 mg KOH / gram 17. The ink composition according to item 16, having an acid value in the range of 1 / gram. (Section 22) The ink removal enhancing additive is from about 165 mg KOH / gram to about 205 mg KOH / gram 17. The ink composition according to item 16, having an acid value in the range of 1 / gram. (Section 23) Item 16 above, wherein the carrier comprises a solvent, a monomer, or a combination thereof. The ink composition according to claim 1. (Section 24) 24. The ink composition according to claim 23, wherein the solvent comprises at least one aprotic solvent. Composition. (Section 25) The solvent is N-methyl-2-pyrrolidone (NMP), or acetone, or 24. The ink composition according to item 23, comprising a combination of the above. (Section 26) 24. The ink according to claim 23, wherein the monomer comprises at least one acrylic monomer. Composition. (Section 27) The acrylic monomer is 1,3-butylene glycol diacrylate, 1,6-hexadecyl glycol diacrylate, Sandiol diacrylate, 1,3-butylene glycol dimethacrylate, isobol decyl acrylate, or isodecyl methacrylate, or a combination thereof. 27. The composition according to item 26. (Section 28) 17. The ink composition according to claim 16, wherein the base ink comprises a UV curable ink. (Section 29) Item 17. The ink composition according to item 16, wherein the ink composition is UV curable. (Section 30) (a) about 65 to about 85 weight percent of said base ink; (b) an acid value in the range of about 150 mg KOH / gram to about 205 mg KOH / gram from about 5 to about 20 weight percent of the ink removal enhancing additive; and (c) about 5 to about 1000 sulphates capable of dissolving at least a portion of the ink removal promoting additive; 15 weight percent of said support 17. The ink composition according to item 16, comprising: (Section 31) 1. A recyclable plastic article comprising: A curved outer surface having a digitally printed image printed directly onto said curved outer surface, the image including hardened droplets of ink. said image, and a composition comprising an ink removal enhancing additive having a glass transition temperature of less than about 130° C. said droplets of ink including a composition thereof, the digitally printed image has an adhesion score of at least 6.0 and up to 9.0; and When the digitally printed image is exposed to the basic solution at an elevated temperature of at least about 70° C. The removal-facilitating additive causes the cured droplets of ink to separate or adhere to the curved outer surface of the article. The recyclable plastic article is configured to be released. (Section 32) 32. The plastic article of claim 31, wherein the article comprises a plastic container. (Section 33) Item 33. The plastic article according to item 32, wherein the plastic container is a bottle. (Section 34) Item 31 above, wherein the ink removal promoting additive comprises a styrene-maleic anhydride copolymer. 2. The plastic article according to claim 1 . (Section 35) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 50° C. to about 110° C. 32. The plastic article according to claim 31, having: (Section 36) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 55° C. to about 85° C. 32. The plastic article according to claim 31, comprising: (Section 37) The ink removal promoting additive has a glass transition temperature (Tg) in the range of about 55° C. to about 65° C. 32. The plastic article according to claim 31, comprising: (Section 38) The ink removal enhancing additive is from about 150 mg KOH / gram to about 205 mg KOH / gram 32. The ink composition according to item 31, having an acid value in the range of 1 / gram. (Section 39) The ink removal enhancing additive is from about 165 mg KOH / gram to about 205 mg KOH / gram 32. The ink composition according to item 31, having an acid value in the range of 1 / gram. (Section 40) The article is made of the following materials: polyethylene, polyethylene terephthalate, high density polyethylene Item 31. The plastic according to item 31, which is made of one or more of polyethylene and polypropylene. Goods. (Section 41) The digitally printed image has a pH in the range of about 12 to 13 at an elevated temperature in the range of about 70 to 90° C. When exposed to a basic solution that reacts with the ink, the removal-promoting additive causes the cured droplets of ink to The plug according to claim 31, which is configured to be separated or released from the curved outer surface of the article. Stick items. (Section 42) At least about 90% of the cured ink droplets are cured after exposure to the basic solution at the elevated temperature. The plastic according to claim 41, wherein a percentage of the amount of the adhesive is separated from the curved outer surface of the article. Q items. (Section 43) the digitally printed image comprising a basecoat comprising a plurality of cured basecoat ink droplets; and a secondary coat comprising a plurality of cured secondary coat ink droplets, said secondary coat comprising: Item 32. The plastic article according to item 31, wherein the coating is applied to at least a portion of a base coat. (Section 44) 1. A method for removing cured ink from a plastic container, the method comprising: (a) A digital image is printed on said printhead by a drop-on-demand inkjet printing process. A curved outer surface of the plastic container is printed directly on the curved outer surface of the plastic container. The cured droplets of ink are applied directly to the curved outer surface and are at least 6.0 and up to about 9.0 mm. and an ink having a glass transition temperature of less than about 130° C. a plastic container having said droplets of ink containing a composition including a removal-promoting additive. To do; (b) applying at least a portion of the digitally printed image to the plastic container using at least Exposure to a basic solution at an elevated temperature of about 70°C; and (c) applying at least a portion of the digitally printed image to the curved outer surface on which the image is printed. To remove from The method comprising: (Section 45) 45. The method according to claim 44, wherein the container is a bottle. (Section 46) The ink removal promoting additive includes a styrene-maleic anhydride copolymer. The method described above. (Section 47) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 50° C. to about 110° C. 45. The method according to claim 44, comprising the steps of: (Section 48) The ink removal enhancing additive has a glass transition temperature (Tg) in the range of about 55° C. to about 85° C. 45. The method according to claim 44, comprising: (Section 49) The ink removal promoting additive has a glass transition temperature (Tg) in the range of about 55° C. to about 65° C. 45. The method according to claim 44, comprising: (Section 50) The ink removal enhancing additive is from about 150 mg KOH / gram to about 205 mg KOH / gram 45. The method according to claim 44, having an acid value in the range of 1 / gram. (Section 51) The ink removal enhancing additive is from about 165 mg KOH / gram to about 205 mg KOH / gram 45. The method according to claim 44, having an acid value in the range of 1 / gram. (Section 52) The basic solution is an aqueous solution having a pH in the range of about 12 to 13, and the elevated temperature 45. The method according to item 44, wherein the temperature is in the range of about 70 to 90°C. (Section 53) The plastic container is made of the following materials: polyethylene, polyethylene terephthalate, high Item 44, which is made of one or more of high density polyethylene and polypropylene. method. (Section 54) The removing step comprises removing the ink from the container after exposure of the image to the basic solution. 45. The method according to claim 44, comprising scraping or wiping off the surface of the substrate. (Section 55) 45. The method according to claim 44, wherein the ink is mechanically removed in the form of flakes or a film. Law.

Claims

1. 1. A method for removing cured ink from a plastic container, the method comprising: (b) providing a plastic container having a curved exterior surface on which a digital image has been printed directly onto the curved exterior surface of the plastic container by a drop-on-demand inkjet printing process, the image comprising cured droplets of ink applied directly to the curved exterior surface of the plastic container and having an adhesion score of at least 6.0 and up to 9.0, and the droplets of ink comprising a composition comprising (i) an ink removal enhancing additive having a glass transition temperature less than 130° C. comprising a styrene maleic anhydride copolymer and (ii) a carrier solvent comprising acetone or N-methyl-2-pyrrolidone; (c) exposing at least a portion of the digitally printed image on the plastic container to a basic solution at an elevated temperature of at least 70° C.; and (d) removing at least a portion of the digitally printed image from the curved exterior surface on which the image is printed. The method comprising:

2. The method of claim 1 , wherein the container is a bottle.

3. The method of claim 1, wherein the ink removal enhancing additive has a glass transition temperature (Tg) in the range of 50°C to 110°C.

4. The method of claim 1, wherein the ink removal enhancing additive has a glass transition temperature (Tg) in the range of 55°C to 85°C.

5. The method of claim 1, wherein the ink removal enhancing additive has a glass transition temperature (Tg) in the range of 55°C to 65°C.

6. The method of claim 1, wherein the ink removal enhancing additive has an acid value in the range of 150 mg KOH / gram to 205 mg KOH / gram.

7. The method of claim 1, wherein the ink removal enhancing additive has an acid number in the range of 165 mg KOH / gram to 205 mg KOH / gram.

8. 2. The method of claim 1, wherein the basic solution is an aqueous solution having a pH in the range of 12 to 13, and the elevated temperature is in the range of 70° C. to 90° C.

9. 10. The method of claim 1, wherein the plastic container is made of one or more of the following materials: polyethylene, polyethylene terephthalate, high density polyethylene, and polypropylene.

10. The method of claim 1 , wherein the removing step comprises scraping or wiping the ink from the reservoir after exposure of the image to the basic solution.

11. The method of claim 1 , wherein the ink is mechanically removed in the form of flakes or a film.

Citation Information

Patent Citations

  • Removable ink composition and process for removing said ink composition from printed articles

    EP0930349A1

  • Ink composition having elimination performance and method for eliminating ink composition from print

    JP1999209677A

  • Radiation curing type ink composition

    JP1999246811A

  • Water release type ink composition, printed material, molding product and separation of ink composition coating film

    JP2000086951A

  • Easily separable ink composition for laminate printing

    JP2000313833A